Magnetoresistive element and preparation method therefor, and magnetic sensing apparatus

By designing TMR magnetoresistive elements with closed vortex and non-closed magnetization patterns, the complexity and parallelism of the sensor chip rotation package are solved, and magnetic field measurements with high sensitivity and wide linear ranges are achieved.

WO2024250419A1PCT designated stage expired Publication Date: 2024-12-12ZHUHAI MULTI-INNOVATION TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/113162
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2023-08-15
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

In TMR sensors, when preparing a full-bridge structure, the two independent magnetoresistive sensor chips rotate 180 degrees and the mechanical assembly method is complicated and cannot guarantee that the chips are completely parallel, affecting the linear output of the sensor.

Method used

A magnetoresistive element is designed, including a first unit element and a second unit element, through series connection, the first unit element has a sensing layer with a closed vortex magnetization pattern for responding to linear changes in the external magnetic field, and the second unit element has The sensing layer of the non-closed magnetization pattern is used to maintain a constant signal. The magnetization direction of the reference layers is the same, forming a Wheatstone bridge structure, avoiding the rotary packaging process.

Benefits of technology

Magnetic reluctance elements with high sensitivity and wide linear range are realized, simplifying the preparation process and avoiding the impact of mechanical packaging on linear output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023113162_12122024_PF_FP_ABST
    Figure CN2023113162_12122024_PF_FP_ABST
Patent Text Reader

Abstract

A magnetoresistive element and a preparation method therefor, and a magnetic sensing apparatus. The magnetoresistive element comprises first element portions (10) and second element portions (20), wherein each first element portion (10) comprises at least one first unit element (101); each second element portion (20) comprises at least one second unit element (201); the first element portion (10) and the second element portion (20) are connected in series; the first unit element (101) comprises a first reference layer (1012) and a first sensing layer (1014) that has a closed vortex magnetization pattern, and is used for outputting, in response to an external magnetic field, a linearly changing first signal within a preset magnetic field range; the second unit element (201) comprises a second reference layer (2012) and a second sensing layer (2014) that has a non-closed magnetization pattern, and is used for outputting, in response to the external magnetic field and within the preset magnetic field range, a second signal that remains constant; and the second reference layer (2012) and the first reference layer (1012) have the same magnetization direction.
Need to check novelty before this filing date? Find Prior Art

Description

Magnetoresistive element and preparation method thereof, and magnetic sensing device

[0001] Related applications

[0002] This application claims priority to Chinese patent application No. 202310658813.9 filed on June 5, 2023, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the technical field of magnetic sensors, and in particular to a magnetoresistive element and a preparation method thereof, and a magnetic sensor device. Background Art

[0004] TMR sensors are widely used in the field of magnetic field detection due to their magnetoresistance effect.

[0005] In practical applications, TMR sensors are typically implemented using a Wheatstone bridge structure, which offers the advantages of high sensitivity and temperature stability. Based on the resistance variation of the four bridge arms with magnetic field, Wheatstone bridge structures can be categorized as single, half, and full bridges, with the full bridge structure being the most sensitive. However, fabricating a full-bridge TMR sensor requires that the two adjacent bridge arms respond in opposite directions to the same changing magnetic field, making the fabrication of a full-bridge TMR sensor somewhat challenging.

[0006] To achieve a Wheatstone full-bridge structure, the general solution is to rotate one of the two independent magnetoresistive sensor chips 180 degrees relative to the other through external wiring and then package them together. This mechanical assembly method makes the sensor preparation process cumbersome. More importantly, it cannot ensure that the two independent magnetoresistive sensor chips packaged together are completely parallel, which affects the linear output of the sensor.

[0007] Summary of the Invention

[0008] The main purpose of this application is to provide a magnetoresistive element and a preparation method thereof, and a magnetic sensing device, aiming to overcome the above problems existing in the prior art and provide a magnetoresistive element with high sensitivity and a wide linear range.

[0009] To achieve the above objectives, the present application provides a magnetoresistive element for magnetic field measurement, the magnetoresistive element comprising:

[0010] a first element portion including at least one first unit element; and

[0011] a second element portion including at least one second unit element;

[0012] The first element portion and the second element portion are connected in series;

[0013] The first unit element includes a first reference layer and a first sensing layer having a closed vortex magnetization pattern, and is configured to output a linearly varying first signal in response to an external magnetic field within a preset magnetic field range;

[0014] The second unit element includes a second reference layer and a second sensing layer having a non-closed magnetization pattern, and is configured to output a constant second signal in response to an external magnetic field within the preset magnetic field range;

[0015] The second reference layer has the same magnetization direction as the first reference layer.

[0016] In one embodiment, the magnetoresistive element further comprises:

[0017] an electrical connection portion, configured to electrically contact the first element portion and the second element portion, so that each of the first element portions and each of the second element portions in the magnetoresistive element are connected to form a Wheatstone bridge structure;

[0018] The first unit element includes a first bottom electrode layer, a first reference layer, a first insulating layer, a first sensing layer and a first top electrode layer which are arranged in sequence;

[0019] The first reference layer has a first film surface, which is magnetized and fixed in a first direction in the in-plane direction of the first film surface; the first direction is parallel to the easy magnetization direction of the first sensing layer;

[0020] The second unit element includes a second bottom electrode layer, a second reference layer, a second insulating layer, a second sensing layer and a second top electrode layer which are arranged in sequence;

[0021] The second reference layer has a second film surface, which is magnetized in a second direction in the in-plane direction of the second film surface; the second direction is parallel to the easy magnetization direction of the first sensing layer.

[0022] In one embodiment, the first unit element and the second unit element are TMR magnetoresistive elements.

[0023] In one embodiment, the first sensing layer includes a first free layer close to the first insulating layer and a second free layer close to the first free layer. The first free layer is made of a ferromagnetic material, and the second free layer is made of a soft magnetic material.

[0024] In one embodiment, in the second unit element, an antiferromagnetic layer is further included between the second sensing layer and the second top electrode layer, an exchange bias field exists between the antiferromagnetic layer and the second sensing layer, and the magnetization direction of the exchange bias field is parallel to the easy magnetization direction of the first sensing layer.

[0025] In one embodiment, the thickness of the antiferromagnetic layer is 20 nm-30 nm.

[0026] In one embodiment, the second sensing layer includes a third free layer disposed between the second insulating layer and the second top electrode layer;

[0027] The third free layer is made of ferromagnetic material;

[0028] The third free layer has a shape anisotropy field such that the second sensing layer has a magnetization direction parallel to the first direction.

[0029] In one embodiment, a ratio of a major axis to a minor axis of the third free layer is 3-10, and the major axis is parallel to the first direction.

[0030] In addition, to achieve the above-mentioned purpose, the present application also provides a method for preparing a magnetoresistive element, the method comprising:

[0031] providing a substrate;

[0032] Depositing a magnetic stack on the substrate, and performing tape-out and magnetic field annealing on the magnetic stack to form the magnetoresistive element as described above;

[0033] The magnetoresistive element includes a first element portion including one or more first unit elements, and a second element portion including one or more second unit elements, wherein a first reference layer in the first unit element and a second reference layer in the second unit element have the same magnetization direction;

[0034] The magnetic field annealing comprises:

[0035] Annealing is performed at 340° C.-360° C. and a preset magnetic field for 40 min-80 min.

[0036] In one embodiment, the magnetic field strength of the preset magnetic field is 3000 Oe-5000 Oe.

[0037] In one embodiment, the magnetic field direction of the preset magnetic field is parallel to the easy magnetization direction of the first sensing layer.

[0038] In one embodiment, depositing a magnetic stack on the substrate and taping out the magnetic stack comprises:

[0039] Depositing a magnetic stack on the substrate according to a preset material and a preset thickness; the magnetic stack at least includes a bottom electrode layer, a reference layer, an insulating layer, a sensing layer and an antiferromagnetic layer;

[0040] The magnetic stack is taped out to form at least one first magnetic stack and at least one second magnetic stack, the antiferromagnetic layer is etched and a first top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the first magnetic stack, and a second top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the second magnetic stack.

[0041] In one embodiment, depositing a magnetic stack on the substrate and taping out the magnetic stack comprises:

[0042] Depositing a magnetic stack on the substrate according to a preset material and a preset thickness; the magnetic stack comprises at least a bottom electrode layer, a reference layer, an insulating layer, and a sensing layer; the sensing layer comprises a first sensing layer and a second sensing layer;

[0043] The magnetic stack is taped out to form at least one first magnetic stack and at least one second magnetic stack; a first top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the first magnetic stack, the second sensing layer is etched and a second top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the second magnetic stack, and the sensing layer in the first magnetic stack and the sensing layer in the second magnetic stack have different shapes.

[0044] In addition, to achieve the above-mentioned purpose, the present application also provides a magnetic sensing device, which includes a magnetoresistive element;

[0045] The magnetoresistive element is the magnetoresistive element described above, or is manufactured using the manufacturing method described above;

[0046] The magnetic sensing device is used for at least one of current sensing, speed sensing, direction sensing, rotation angle sensing or proximity sensing.

[0047] The magnetoresistive element provided in the present application includes a first element portion, which includes at least one first unit element; and a second element portion, which includes at least one second unit element; the first element portion and the second element portion are connected in series; the first unit element includes a first reference layer and a first sensing layer having a closed vortex magnetization pattern, which is used to output a linearly changing first signal in response to an external magnetic field within a preset magnetic field range; the second unit element includes a second reference layer and a second sensing layer having a non-closed magnetization pattern, which is used to output a constant second signal in response to an external magnetic field within the preset magnetic field range; the second reference layer and the first reference layer have the same magnetization direction. The magnetoresistive element of the present application integrates the advantages of a vortex structure magnetoresistive sensor, and at the same time, due to the one-piece molding, avoids the performance difference caused by one of the two magnetoresistive sensor chips rotating 180 degrees relative to the other, and has the technical effects of high sensitivity and wide linear range. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] FIG1 is a schematic structural diagram of a magnetoresistive element in a first embodiment of the present application;

[0049] FIG2 is a schematic diagram of the cross-sectional structure of the first unit element in the first embodiment of the present application;

[0050] FIG3 is a schematic diagram of the cross-sectional structure of the second unit element in the first embodiment of the present application;

[0051] FIG4 is a schematic diagram of a cross-sectional structure of a second unit element in a second embodiment of the present application;

[0052] FIG5 is a schematic diagram showing how the resistance of the second unit element changes with the magnetic field in the second embodiment of the present application;

[0053] FIG6 is a schematic diagram showing how the resistance of the first unit element changes with the magnetic field in the second embodiment of the present application;

[0054] FIG7 is a schematic cross-sectional view of the first unit element and the second unit element in the third embodiment of the present application;

[0055] FIG8 is a schematic diagram showing how the resistance of the second unit element changes with the magnetic field in the third embodiment of the present application;

[0056] FIG9 is a schematic diagram showing how the resistance of the first unit element changes with magnetic field in the third embodiment of the present application;

[0057] FIG10 is a schematic flow chart of an embodiment of a method for preparing a magnetoresistive element according to the present application;

[0058] FIG11 is a schematic diagram of a magnetic stack structure according to an embodiment of the present application;

[0059] FIG12 is a schematic diagram of etching a bottom electrode according to an embodiment of the present application;

[0060] FIG13 is a schematic diagram of etching of a first magnetic stack according to an embodiment of the present application;

[0061] FIG14 is a schematic diagram of etching a second magnetic stack according to an embodiment of the present application;

[0062] FIG15 is a schematic diagram comparing the material systems of the first magnetic stack and the second magnetic stack in the first solution involved in an embodiment of the present application;

[0063] FIG16 is a schematic structural diagram of a magnetoresistive element prepared using the first solution according to an embodiment of the present application;

[0064] FIG17 is a schematic diagram comparing the material systems of the first magnetic stack and the second magnetic stack in the second solution according to an embodiment of the present application;

[0065] FIG18 is a schematic structural diagram of a magnetoresistive element prepared using the second solution in an embodiment of the present application.

[0066] Explanation of Figure Numbers

[0067] The realization of the objectives, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0068] It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application.

[0069] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0070] It should be noted that all directional indications in the embodiments of the present application (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the various components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0071] In addition, the descriptions of "first", "second", etc. in this application are for descriptive purposes only and should not be understood as indicating or implying their relative importance or implicitly indicating the number of the technical features indicated. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of such features. In addition, the technical solutions between the various embodiments can be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in this field. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0072] Due to their magnetoresistance effect, TMR sensors are widely used in magnetic field detection. In practical applications, TMR sensors are typically implemented using a Wheatstone bridge structure, which offers the advantages of high sensitivity and temperature stability. Based on the resistance variation of the four bridge arms with magnetic field, Wheatstone bridge structures can be categorized as single-bridge, half-bridge, and full-bridge, with the full-bridge structure having the highest sensitivity. However, the fabrication of a full-bridge TMR sensor requires that the two adjacent bridge arms have opposite responses to the same changing magnetic field, making the fabrication of a full-bridge TMR sensor difficult.

[0073] To achieve a Wheatstone full-bridge structure, the general solution is to rotate one of the two independent magnetoresistive sensor chips 180 degrees relative to the other through external wiring and then package them together. This mechanical assembly method makes the sensor preparation process cumbersome. More importantly, it cannot ensure that the two independent magnetoresistive sensor chips packaged together are completely parallel, which affects the linear output of the sensor.

[0074] In order to overcome the above problems existing in the prior art, an embodiment of the present application provides a magnetoresistive element with high sensitivity and a wide linear range.

[0075] Referring to Figure 1 , which is a schematic diagram of the structure of a magnetoresistive element in a first embodiment of the present application, the magnetoresistive element comprises a first element portion 10 and a second element portion 20 , which are connected in series. The first element portion 10 comprises at least one first unit element 101 , and the second element portion 20 comprises at least one second unit element 201 .

[0076] It should be noted that the number of first unit elements 101 in the first element portion 10 can be adjusted according to actual conditions, and this embodiment does not limit this. The number and connection method of the second unit elements 201 in the second element portion 20 are the same as those of the first unit elements in the first element portion.

[0077] The first unit elements 101 in the first component section 10 can be connected in series and / or in parallel. Specifically, a series connection can improve the stability of the first component section at different temperatures and increase the resistance of the first component section; a parallel connection can reduce the resistance of the first component section. Similarly, the second unit elements 201 in the second component section 20 can also be connected in series or in parallel.

[0078] It is understandable that the first unit elements in the first element section 10 can be connected in series in sequence; or, the first unit elements in the first element section can be connected in parallel in pairs to form a plurality of first unit element groups, and then the first unit element groups can be connected in series; or, the first unit elements in the first element section can be connected in parallel in pairs or more to form a plurality of first unit element strings, and then the first unit element strings can be connected in series.

[0079] It is understandable that when two first unit elements are connected in series, one first unit element and the other first unit element only share the top electrode layer or the bottom electrode layer, but do not share the bottom electrode layer or the top electrode layer at the same time; when two first unit elements are connected in parallel, one first unit element and the other first unit element share both the top electrode layer and the bottom electrode layer.

[0080] It should be noted that the shape of the stacked layers of the first unit element may be circular, elliptical or other shapes, which is not limited here.

[0081] In this embodiment, the first unit element 101 includes a first reference layer and a first sensing layer having a closed vortex magnetization pattern, which is used to output a linearly changing first signal in response to an external magnetic field within a preset magnetic field range; the second unit element 201 includes a second reference layer and a second sensing layer having a non-closed magnetization pattern, which is used to output a constant second signal in response to an external magnetic field within a preset magnetic field range; the second reference layer has the same magnetization direction as the first reference layer.

[0082] It should be noted that the first signal and the second signal refer to electrical parameter values, such as voltage values; maintaining constant means that the value of the second signal is basically not affected by the external magnetic field within a certain range, and its numerical value remains unchanged; the first signal can at least change linearly with the magnetic field within the measurable range, and the second signal can at least remain unchanged with the magnetic field within the measurable range.

[0083] It is understood that the closed vortex magnetization pattern on the surface of the first sensing layer only appears when the external magnetic field is lower than its nucleation field. Furthermore, as the external magnetic field gradually decreases, after decreasing to zero and then increasing back toward the annihilation field, the closed vortex magnetization pattern on its surface gradually disappears. This preset magnetic field range is within the nucleation field-annihilation field range.

[0084] It is understood that, to obtain a closed vortex magnetization pattern, the first sensing layer may be in the shape of a circular disk or an elliptical disk, with a ratio of its major axis to its minor axis between 1 and 2. The shape of the second sensing layer may be the same as or different from that of the first sensing layer, and this is not limited here.

[0085] In this embodiment, since the first unit element can generate a linearly varying first signal within a preset magnetic field range, the first element portion, when connected in series or in parallel, can also generate a linearly varying third signal within the preset magnetic field range (which can be assumed to conform to y1 = ax + b, where x is the external magnetic field and y1 is the value of the third signal). Since the second unit element can generate a constant second signal within the preset magnetic field range, the second element portion, when connected in series or in parallel, can also generate a constant fourth signal within the preset magnetic field range (which can be assumed to conform to y2 = c, where y2 is the value of the fourth signal). The value y3 of the fifth signal, obtained by differentiating the third and fourth signals, can conform to y3 = ax + bc, and its value varies linearly with the external magnetic field. Therefore, the magnetoresistive element of this embodiment can achieve linear measurement of the external magnetic field.

[0086] Furthermore, because the second reference layer and the first reference layer have the same magnetization direction, there is no need to intentionally rotate the first and second component parts 180 degrees before proceeding with the packaging process during the electrical connection process between the first and second component parts. The magnetoresistive element can be directly packaged after the stacking, annealing, and wafer fabrication processes. This process is relatively simple, as it does not require rotating the magnetoresistive element 180 degrees before packaging. When used for magnetic field measurement, it is not affected by mechanical packaging, which can prevent its linear range from being affected. Therefore, the magnetoresistive element of the embodiments of the present application can achieve higher sensitivity and a wider linear range.

[0087] In this embodiment, the magnetoresistive element further includes an electrical connection portion, which is used to electrically contact the first element portion and the second element portion, so that each first element portion and each second element portion in the magnetoresistive element can be connected to form a Wheatstone bridge structure.

[0088] Specifically, the electrical connection portion may be a plurality of pads.

[0089] It is understandable that the number of the first component parts can be 2 or more, and the number of the second component parts can be 2 or more. Every two first component parts and every two second component parts can be electrically connected in sequence through the pads of the electrical connection part to form a Wheatstone bridge structure.

[0090] Figure 2 is a schematic diagram of the cross-sectional structure of the first unit element in the first embodiment. As shown in Figure 2, the first unit element 101 may include a first bottom electrode layer 1011, a first reference layer 1012, a first insulating layer 1013, a first sensing layer 1014 and a first top electrode layer 1015 arranged in sequence; the first reference layer 1012 has a first film surface 1012a, which is magnetized and fixed in a first direction D1 in the in-plane direction of the first film surface 1012a; the first direction D1 is parallel to the easy magnetization direction of the first sensing layer 1014.

[0091] It should be noted that the first unit element may be a TMR magnetoresistive element. The first unit element further includes a first pinning layer (not shown) for fixing the magnetization of the first reference layer. The first pinning layer is disposed between the first bottom electrode layer and the first reference layer to define and maintain the magnetization direction of the first reference layer. The material, shape, etc. of the first pinning layer are not limited herein.

[0092] It is understandable that the structure of the first sensing layer 1014 can be disc-shaped, the ratio of its major axis length to minor axis length can be 1 to 2, its major axis length can be 0.1 to 10 μm, its thickness can be 0.5 to 500 μm, and the ratio of its thickness to major axis length can be 1 / 500 to 1 / 50.

[0093] In this embodiment, the first sensing layer 1014 may include a first free layer close to the first insulating layer 1013 and a second free layer close to the first free layer, wherein the first free layer is a ferromagnetic material and the second free layer is a soft magnetic material.

[0094] Specifically, the material of the first free layer may be CoFeB, and the material of the second free layer may be Permalloy, amorphous alloy, or microcrystalline alloy.

[0095] Figure 3 is a schematic diagram of the cross-sectional structure of the second unit element in this embodiment. As shown in Figure 3, the second unit element 201 includes a second bottom electrode layer 2011, a second reference layer 2012, a second insulating layer 2013, a second sensing layer 2014 and a second top electrode layer 2015 arranged in sequence; the second reference layer 2012 has a second film surface 2012a, which is magnetized and fixed in a second direction D2 in the in-plane direction of the first film surface 2012a; the second direction D2 is parallel to the easy magnetization direction of the first sensing layer 1014.

[0096] It should be noted that the second unit element may be a TMR magnetoresistive element. The second unit element further includes a second pinning layer (not shown) for fixing the magnetization of the second reference layer. The second pinning layer may be disposed between the second bottom electrode layer and the second reference layer to define and maintain the magnetization direction of the first reference layer.

[0097] In a second embodiment of the present application, as shown in Figure 4, in the second unit element 201, an antiferromagnetic layer 2016 is further included between the second sensing layer 2014 and the second top electrode layer 2015. An exchange bias field exists between the antiferromagnetic layer 2016 and the second sensing layer 2014, and the magnetization direction of the exchange bias field is parallel to the easy magnetization direction of the first sensing layer 1014.

[0098] Specifically, the thickness of the antiferromagnetic layer 2016 may be 20 nm-30 nm.

[0099] Specifically, the material used for the antiferromagnetic layer 2016 may be IrMn material.

[0100] The structures of the first sensing layer and the second sensing layer 2014 can both be soft magnetic materials (such as NiFe) covered with ferromagnetic materials (such as CoFeB), thereby realizing an induced vortex domain structure.

[0101] Specifically, a CoFeB material layer is provided on the side of the first sensing layer 1014 close to the first insulating layer 1013, and a NiFe material layer is covered on the CoFeB material layer, thereby forming an induced vortex domain structure in the first sensing layer 1014, and a closed vortex magnetization pattern can be obtained under a certain magnetic field. Furthermore, a CoFeB material layer is provided on the side of the second sensing layer 2014 close to the second insulating layer 2013, and a NiFe material layer is covered on the CoFeB material layer, thereby forming an induced vortex domain structure in the second sensing layer 2014, and a closed vortex magnetization pattern can be obtained under a certain magnetic field. Simultaneously, an antiferromagnetic layer 2016 is covered on the second sensing layer 2014 to form an exchange bias field, destroying the vortex domain structure and causing the magnetic domains to be arranged in a uniform direction, i.e., a non-closed magnetization pattern is obtained in the second sensing layer.

[0102] It can be understood that in this embodiment, the first sensing layer in the first unit element 101 and the second sensing layer in the second unit element 201 can have the same shape, both being disc-shaped, with a ratio of their major axis length to their minor axis length of 1 to 2, their major axis length of 0.1 μm to 10 μm, their thickness of 0.5 μm to 500 μm, and a ratio of their thickness to their major axis length of 1 / 500 to 1 / 50.

[0103] FIG5 is a schematic diagram showing how the resistance of the second unit element in the second embodiment changes with the magnetic field. It can be seen that within the magnetic field range of -H1 to +H1, the resistance of the first unit element does not change with the change of the magnetic field. Specifically, due to the exchange bias field between the antiferromagnetic layer and the second sensing layer, when a large external magnetic field is applied parallel to the magnetization direction of the second reference layer, the second sensing layer and the second reference layer are parallel in magnetization direction. At this time, the resistance of the first unit element is the minimum value, as shown in ① in FIG5 ; as the magnetic field strength of the external magnetic field gradually decreases, the magnetic domain of the second sensing layer remains stable due to the action of the exchange bias field, as shown in ② in FIG5 ; when the magnetic field continues to decrease to 0 and increases in the opposite direction to the first magnetic field, the magnetic domain of the second sensing layer begins to rotate. Since the magnetization directions of the second sensing layer and the second reference layer are not parallel, the resistance of the first unit element begins to gradually increase, as shown in ③ in FIG5 ; when the external magnetic field continues to increase to the second magnetic field, the second sensing layer is completely reversed. At this time, the second sensing layer The magnetic domains are arranged in opposite directions to the magnetic domains of the second reference layer, the magnetization directions of the second sensing layer and the second reference layer are antiparallel, and the resistance of the first unit element is the maximum value, as shown in ④ in Figure 5; when the external magnetic field continues to increase to the third magnetic field, the resistance of the first unit element continues to maintain the maximum value; when the external magnetic field continues to increase from the third magnetic field, since the external magnetic field exceeds the pinning field of the second reference layer, the magnetic domains of the second reference layer rotate, and the resistance begins to decrease, as shown in ⑤ in Figure 5; when the external magnetic field continues to increase to the fourth magnetic field, the magnetic domains of the second reference layer are completely flipped. At this time, the magnetic domains of the second sensing layer and the second reference layer are arranged in parallel again, and the resistance is the minimum value, as shown in ⑥ in Figure 5; when the external magnetic field gradually decreases from the fourth magnetic field, the relationship between the resistance change and the arrangement of the magnetic domains of the second sensing layer and the second reference layer is shown in ⑦ to 9 in Figure 5. As shown, it is worth noting that due to the effect of the exchange bias field, when the magnetic field is negative, the magnetic domains of the second sensing layer and the second reference layer will be reversed, so the resistance of the second unit element remains stable in the ±H1 magnetic field.

[0104] FIG6 is a schematic diagram showing how the resistance of the first unit element varies with the magnetic field in the second embodiment. It can be seen that within the magnetic field range of −H2 to +H2, the resistance of the first unit element varies uniformly with the magnetic field, exhibiting a certain linear variation pattern.

[0105] Taking into account the relationship between the resistance and the magnetic field shown in Figures 5 and 6, if H1 is greater than H2, the signal output of the magnetoresistive element changes linearly with the magnetic field within the range of ±H2; if H2 is greater than H1, the signal voltage output changes linearly with the magnetic field within the range of ±H1.

[0106] In the second embodiment, because the second sensing layer in the second unit element is pinned by the exchange bias effect, the pinned second element portion can maintain a stable output signal within a preset magnetic field range. In contrast, the first unit element, which is not pinned by the antiferromagnetic layer, has a vortex domain structure and changes linearly with the magnetic field within this magnetic field range. Therefore, the second element can output a signal that changes linearly with the external magnetic field within this range. In this way, the magnetoresistive element can achieve linear measurement of the external magnetic field. At the same time, because the magnetization direction of the reference layer in the first element portion and the second element portion is the same, multiple annealing processes are not required during the preparation process, achieving the integrated molding of the magnetoresistive element. Therefore, the magnetoresistive element of this embodiment has high sensitivity and a wide linear range.

[0107] In a third embodiment of the present application, as shown in FIG7 , the first sensing layer 1014 includes a first free layer 10141 adjacent to the first insulating layer 1013 and a second free layer 10142 adjacent to the first free layer 10141. The first free layer 10141 is made of a ferromagnetic material, while the second free layer 10142 is made of a soft magnetic material. The first free layer 10141 and the second free layer 10142 may form a composite free layer structure.

[0108] It should be noted that the ferromagnetic material may be CoFeB. The soft magnetic material may be a permalloy, an amorphous alloy, or a microcrystalline alloy, such as NiFe, CoFeAl, or CoFeCuMo. Soft magnetic materials have minimal impact on the crystallization of the ferromagnetic material, improving linearity and reducing the hysteresis of the first unit element under a magnetic field. The types of the above materials are not limited here.

[0109] In the third embodiment, referring to FIG. 7 , the second sensing layer 2014 includes a third free layer 20141 disposed between the second insulating layer 2013 and the second top electrode layer 2015 ; the third free layer 20141 is made of ferromagnetic material and has a shape anisotropy field such that its magnetization direction is parallel to the first direction D1 .

[0110] It is understood that the ferromagnetic material of the third free layer 20141 can be the same as that of the first free layer 10141, such as CoFeB. Compared to the first sensing layer, the second sensing layer lacks a soft magnetic layer. Due to its composite free layer structure, the first sensing layer 2014 is more likely to be induced to form a closed vortex magnetization pattern under magnetic field conditions, while the possibility of the second sensing layer 2014 forming a closed vortex magnetization pattern under magnetic field conditions is greatly reduced.

[0111] In the third embodiment, the ratio of the major axis to the minor axis of the third free layer 20141 can be 3-10, and its major axis is parallel to the first direction D1. Therefore, the shapes of the sensing layers in the first unit element 101 and the second unit element 201 are different. At the same time, because the ratio of the major axis to the minor axis of the second sensing layer in the second unit element is larger, the second sensing layer has significant shape anisotropy.

[0112] It is understandable that in this embodiment, the second sensing layer only includes the third free layer, and its length-to-short axis ratio is significantly increased, so that the second sensing layer is affected by shape anisotropy, and it is difficult for it to form a closed vortex magnetization pattern, so that the law of change of the resistance of the second unit element with the external magnetic field is also changed accordingly.

[0113] FIG8 is a schematic diagram showing how the resistance of the second unit element changes with the magnetic field in the third embodiment. It can be seen that within the magnetic field range of −H2 to +H2, the resistance of the first unit element does not change with the change of the magnetic field. Specifically, due to the influence of shape anisotropy, when a large external magnetic field is applied parallel to the magnetization direction of the second reference layer, the magnetization direction of the third free layer is parallel to the magnetization direction of the second reference layer. At this time, the resistance of the second unit element is the minimum, as shown in ① in Figure 8; when the magnetic field gradually decreases, the magnetic domains of the third free layer and the pinned layer always remain stable, as shown in ② in Figure 8; when the magnetic field decreases to 0 and increases in the opposite direction to a certain value, the magnetic domains of the third free layer rotate, and the resistance begins to increase, as shown in ③ in Figure 8; when the magnetic field continues to increase to a certain value, the magnetic domains of the third free layer are completely reversed. At this time, the magnetic domains of the third free layer and the magnetic domains of the second reference layer are arranged in opposite directions, and the resistance is the maximum, as shown in ④ in Figure 8; when the magnetic field continues to increase, the magnetic domains of the second reference layer rotate, and the resistance begins to decrease, as shown in ⑤ in Figure 8; when the magnetic field continues to increase to a certain value, the magnetic domains of the second reference layer are completely flipped. At this time, the magnetic domains of the third free layer and the magnetic domains of the second reference layer are arranged parallel again, and the resistance is the minimum, as shown in ⑥ in Figure 8; when the magnetic field begins to decrease, the relationship between the resistance change and the arrangement of the magnetic domains of the third free layer and the second reference layer is as shown in ⑦ to As shown, the resistance of the second unit element can remain unchanged in the ±H2 magnetic field.

[0114] FIG9 is a schematic diagram showing how the resistance of the first unit element varies with the magnetic field in the third embodiment. It can be seen that within the magnetic field range of −H1 to +H1, the resistance of the first unit element varies uniformly with the magnetic field, exhibiting a certain linear variation pattern.

[0115] Taking into account the relationship between the change of resistance and magnetic field shown in Figures 8 and 9, if H1 is greater than H2, the magnetoresistive element can achieve a linear change in voltage output with the magnetic field within the range of ±H2; if H2 is greater than H1, the magnetoresistive element can achieve a linear change in voltage output with the magnetic field within the range of ±H1.

[0116] In this embodiment, the first element portion has a composite free layer structure that easily forms a vortex domain structure, which can generate a linearly varying first signal within a preset magnetic field range, while the second element portion has only a ferromagnetic material layer and is a non-vortex domain structure, which can generate a constant second signal within a preset magnetic field range. This allows the differential signal between the first and second element portions of the magnetoresistive element to vary linearly with the external magnetic field within a certain external magnetic field range. At the same time, because the magnetization directions of the first and second reference layers in the magnetoresistive element are the same, there is no need to further flip the first and second element portions after they are formed, thereby achieving an integrated molding of the magnetoresistive element.

[0117] An embodiment of the present application further provides a method for preparing a magnetoresistive element. Referring to FIG. 10 , FIG. 10 is a flow chart of an embodiment of a method for preparing a magnetoresistive element of the present application.

[0118] In this embodiment, the method for preparing the magnetoresistive element includes:

[0119] Step S10: providing a substrate.

[0120] The substrate is a carrier for the deposited film layer and can be in the form of a flat plate. The material of the substrate can be Si(100) / SiO2.

[0121] In step S20 , a magnetic stack is deposited on the substrate, and the magnetic stack is tape-out and magnetic field annealed to form a magnetoresistive element.

[0122] Specifically, the magnetoresistive element includes a first element portion including one or more first unit elements, and a second element portion including one or more second unit elements, the first unit elements and the second unit elements have the same magnetization direction; the first sensing layer in the first element portion and the second sensing layer in the second element portion have different structures.

[0123] Specifically, the magnetic field annealing step may include: performing magnetic field annealing at 340° C.-360° C. and a preset magnetic field for 40 min-80 min.

[0124] It is understandable that the purpose of performing magnetic field annealing is to impart a certain magnetization direction to each reference layer and sensing layer in the magnetoresistive element. The magnitude of the preset magnetic field can be 3000 Oe-5000 Oe.

[0125] It should be noted that this temperature range is higher than the crystallization temperature of CoFeB. The annealing direction can be selected according to actual needs, with the easy axis direction as a reference.

[0126] It should be noted that the magnetic field annealing step can be performed after obtaining the magnetic stack or after tape-out, and there is no limitation here.

[0127] In some feasible implementations (i.e., the first solution), the steps of depositing a magnetic stack on a substrate and taping out the magnetic stack may specifically include:

[0128] Step S211, depositing a magnetic stack on a substrate according to a predetermined material and a predetermined thickness; the magnetic stack at least includes a bottom electrode layer, a reference layer, an insulating layer, a sensing layer, and an antiferromagnetic layer;

[0129] It should be noted that the magnetic stack may also include a pinning structure, a protective layer and other structures that are beneficial to the performance of the magnetoresistive element. The pinning structure can be arranged between the electrode layer and the reference layer, and the protective layer can be arranged above the antiferromagnetic layer.

[0130] It should be understood that the stacking order of the layers in the magnetic stack can be as follows: the bottom electrode layer is deposited above the substrate, the reference layer is deposited above the bottom electrode layer, the insulating layer is deposited above the reference layer, the sensing layer is deposited above the insulating layer, and the antiferromagnetic layer is deposited above the sensing layer.

[0131] Step S212, tape-out the magnetic stack to form at least one first magnetic stack and at least one second magnetic stack, etching an antiferromagnetic layer and depositing a first top electrode layer in a region of the magnetic stack corresponding to the first magnetic stack, and depositing a second top electrode layer in a region of the magnetic stack corresponding to the second magnetic stack;

[0132] It should be noted that etching the antiferromagnetic layer in the area corresponding to the first magnetic stack in the magnetic stack refers to etching the antiferromagnetic layer above the sensing layer to avoid the presence of the antiferromagnetic layer affecting the structure of the first magnetic stack; if the magnetic stack has other structures (for example, a protective layer) above the antiferromagnetic layer, they should also be etched in this step. If necessary, the corresponding materials, such as the protective layer, can be deposited after etching.

[0133] In this solution, a schematic diagram of the cross-sectional structure of the first magnetic stack and the second magnetic stack after etching is shown in FIG15 .

[0134] In this solution, a magnetic stack including a bottom electrode layer, a reference layer, an insulating layer, a sensing layer and an antiferromagnetic layer can be formed on a substrate first, and then the regions are divided by tape-out to form at least one first magnetic stack and at least one second magnetic stack.

[0135] Specifically, the area division is performed through tape-out, including:

[0136] Step S2121: covering corresponding positions of the first magnetic stack and the second magnetic stack in the magnetic stack with photoresist, as shown in FIG11 , and then performing etching so that only the area covered by the photoresist is retained except for the bottom electrode layer in the magnetic stack.

[0137] It should be noted that the depth of the etching corresponds to the area above the bottom electrode layer. The etching can be achieved using IBE (Ion Beam Etching) technology.

[0138] The shapes of the first magnetic stack and the second magnetic stack do not necessarily have to be circular or elliptical, and the region should at least cover all structures of the first element portion and the second element portion.

[0139] Step S2122: Cover the corresponding positions of each first bottom electrode layer and each second bottom electrode layer in the magnetic stack with photoresist, as shown in FIG12 , and then perform etching so that only the areas corresponding to the first bottom electrode layer and the second bottom electrode layer in the magnetic stack are retained.

[0140] The purpose of this step is to obtain a first bottom electrode layer and a second bottom electrode layer, ie, a bottom electrode.

[0141] It should be noted that the etching depth corresponds to the area above the substrate.

[0142] It should be understood that the regions corresponding to the first bottom electrode layer and the second bottom electrode layer should span at least two first magnetic stacks or second magnetic stacks, thereby achieving electrical connection between the two first magnetic stacks or second magnetic stacks.

[0143] It is understandable that after etching the bottom electrode layer, SiO2 with a thickness of 200 nm to 300 nm may be grown in the etched area using ICPCVD (Inductively Coupled Plasma Chemical Vapour Deposition) technology to form an insulating protective layer.

[0144] Step S2123: Covering the corresponding regions outside each first magnetic stack in the magnetic stack with photoresist, as shown in FIG13 , and then etching the regions corresponding to each first unit element to remove the antiferromagnetic layer and the structure above it in the first unit element;

[0145] Step S2124: Covering the corresponding regions outside each second magnetic stack in the magnetic stack with photoresist, as shown in FIG14 , and then etching the region corresponding to the second unit element in the second magnetic stack to remove the structure above the antiferromagnetic layer in the second unit element;

[0146] It should be noted that step S2124 can be executed before or after step S2123.

[0147] Step S2125: Deposit a first top electrode layer and a second top electrode layer above the corresponding areas of each first magnetic stack and each second magnetic stack, respectively, and deposit a plurality of pads (i.e., electrodes) for connecting each first magnetic stack and each second magnetic stack, as shown in FIG16 .

[0148] It should be noted that each pad may be in electrical contact with a portion of the first top electrode layer and the second top electrode layer. The number and connection method of each magnetic stack are not limited to those shown in FIG16. Each first magnetic stack may be electrically connected in series and / or in parallel.

[0149] Figure 15 is a schematic diagram comparing the material systems of the first magnetic stack and the second magnetic stack in this scheme. It can be seen from Figure 15 that the different areas of the material systems of the first magnetic stack and the second magnetic stack are only in the top two layers. By controlling the etching time of the openings in different areas, the preparation of different material systems on the same substrate can be achieved.

[0150] Specifically, the first magnetic stack and the second magnetic stack both include a bottom electrode layer (i.e., a metal layer), a pinning layer (i.e., AFM, FM, metal layer) for pinning the reference layer, a reference layer (FM), an insulating layer, and a sensing layer (FM, FM) stacked in sequence. The second magnetic stack also includes an antiferromagnetic layer (AFM) for affecting the sensing layer and a metal layer for protection.

[0151] It should be noted that the material system of the first magnetic stack and the second magnetic stack is not limited to that shown in FIG. 15 .

[0152] Figure 16 is a schematic diagram of the structure of the magnetoresistive element prepared using the first scheme. The two first element parts 10 and the two second element parts 20 can respectively serve as bridge arms in the Wheatstone bridge structure and are connected in sequence through pads (or electrodes) to form a Wheatstone bridge structure.

[0153] In some other feasible implementations (i.e., the second solution), the steps of depositing a magnetic stack on a substrate and taping out the magnetic stack may include:

[0154] Step S221 , depositing a magnetic stack on a substrate according to a predetermined material and predetermined thickness; the magnetic stack at least includes a bottom electrode layer, a reference layer, an insulating layer, and a sensing layer;

[0155] Specifically, the sensing layer includes a first sensing layer and a second sensing layer.

[0156] It should be noted that the first sensing layer and the second sensing layer are made of different materials, which is not limited here.

[0157] The preset material and preset thickness in this solution refer to the material and thickness of each layer in the magnetic stack, which can be set according to actual needs.

[0158] It should be noted that the magnetic stack is not limited to a bottom electrode layer, a reference layer, an insulating layer, and a sensing layer, but may also include a pinning structure, which may be disposed between the electrode layer and the reference layer. Without considering the pinning structure, the stacking order of the layers in the magnetic stack may be: the bottom electrode layer is deposited above the substrate, the reference layer is deposited above the bottom electrode layer, the insulating layer is deposited above the reference layer, the sensing layer is deposited above the insulating layer, and the antiferromagnetic layer is deposited above the sensing layer.

[0159] Step S222, tape out the magnetic stack to form at least one first magnetic stack and at least one second magnetic stack; deposit a first top electrode layer in the area corresponding to the first magnetic stack in the magnetic stack, etch two sensing layers and deposit a second top electrode layer in the area corresponding to the second magnetic stack in the magnetic stack, and the sensing layer in the first magnetic stack and the sensing layer in the second magnetic stack have different shapes.

[0160] Specifically, in this solution, a magnetic stack including a bottom electrode layer, a reference layer, an insulating layer, a sensing layer 1, and a sensing layer 2 can be formed on the substrate first, and then the area can be divided by wafer taping to form at least one first magnetic stack and at least one second magnetic stack.

[0161] It should be noted that the sensing layer in the first magnetic stack and the sensing layer in the second magnetic stack have different shapes. For example, the first magnetic stack shape can be set to an ellipse with a long-short axis ratio of 1-2, and the second magnetic stack shape can be set to an ellipse with a long-short axis ratio of 3-10.

[0162] Figure 17 is a schematic diagram comparing the material systems of the first magnetic stack and the second magnetic stack in the second scheme. It can be seen from Figure 17 that the only difference between the material systems of the first magnetic stack and the second magnetic stack is that the top layers also include a metal layer and an AFM. By controlling the etching time for opening holes in different areas, different material systems can be prepared on the same substrate.

[0163] FIG18 is a schematic structural diagram of a magnetoresistive element prepared using the second solution. The two first element portions 10 and the two second element portions 20 can serve as bridge arms in a Wheatstone bridge structure, respectively, and are connected in sequence through pads to form a Wheatstone bridge structure.

[0164] It should be noted that the shapes of the first unit element and the second unit element shown in FIG. 18 schematically illustrate the shapes corresponding to the sensing layer.

[0165] Therefore, in this solution, by controlling the timing of etching the openings in different areas and combining the advantages of the vortex structure magnetoresistive sensor, the integrated molding of the Wheatstone bridge structure is achieved, reducing the performance difference caused by the two magnetoresistive sensor chips being molded and assembled at different times.

[0166] The present application also provides a magnetic sensing device comprising the aforementioned magnetoresistive element, or a magnetoresistive element obtained using the aforementioned method for preparing a magnetoresistive element. The magnetic sensing device can be used for at least one of current sensing, speed sensing, direction sensing, rotation angle sensing, or proximity sensing.

[0167] This magnetic sensing device inherits the advantages of high sensitivity and wide linear range of magnetoresistive elements, and is more suitable for current measurement, speed measurement, direction measurement, rotation angle measurement and proximity measurement, and can further reduce its measurement error.

[0168] It should be noted that, in this document, the terms "comprises," "includes," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or system comprising a series of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or system. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of other identical elements in the process, method, article, or system comprising the element.

[0169] The serial numbers of the above-mentioned embodiments of the present application are for description only and do not represent the advantages or disadvantages of the embodiments.

[0170] The above are only preferred embodiments of the present application and do not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A magnetoresistive element, wherein: For magnetic field measurement, the magnetoresistive element comprises: a first element portion including at least one first unit element; and A second element portion including at least one second unit element; The first element portion and the second element portion are connected in series; The first unit element includes a first reference layer and a first sensing layer having a closed vortex magnetization pattern, and is used to output a linearly varying first signal in response to an external magnetic field within a preset magnetic field range; The second unit element includes a second reference layer and a second sensing layer having a non-closed magnetization pattern, and is used for outputting a constant second signal in response to an external magnetic field within the preset magnetic field range; The second reference layer has the same magnetization direction as the first reference layer.

2. The magnetoresistive element according to claim 1, wherein The magnetoresistive element further comprises: an electrical connection portion, which is used to electrically contact the first element portion and the second element portion, so that each of the first element portions in the magnetoresistive element is connected to each of the second element portions to form a Wheatstone bridge structure; The first unit element comprises a first bottom electrode layer, a first reference layer, a first insulating layer, a first sensing layer and a first top electrode layer arranged in sequence; the first reference layer has a first film surface, which is magnetized and fixed in a first direction in the in-plane direction of the first film surface; the first direction is parallel to the easy magnetization direction of the first sensing layer; The second unit element comprises a second bottom electrode layer, a second reference layer, a second insulating layer, a second sensing layer and a second top electrode layer arranged in sequence; the second reference layer has a second film surface, which is magnetized and fixed in a second direction in the in-plane direction of the second film surface; The second direction is parallel to the easy magnetization direction of the first sensing layer.

3. The magnetoresistive element according to claim 2, wherein: The first sensing layer includes a first free layer close to the first insulating layer and a second free layer close to the first free layer; the first free layer is a ferromagnetic material, and the second free layer is a soft magnetic material.

4. The magnetoresistive element according to claim 2 or 3, wherein: In the second unit element, an antiferromagnetic layer is further provided between the second sensing layer and the second top electrode layer, an exchange bias field exists between the antiferromagnetic layer and the second sensing layer, and a magnetization direction of the exchange bias field is parallel to an easy magnetization direction of the first sensing layer.

5. The magnetoresistive element according to claim 4, wherein: The thickness of the antiferromagnetic layer is 20nm-30nm.

6. The magnetoresistive element according to claim 3, wherein: The second sensing layer includes a third free layer disposed between the second insulating layer and the second top electrode layer; The third free layer is made of ferromagnetic material; The third free layer has a shape anisotropy field so that the second sensing layer has a magnetization direction parallel to the first direction.

7. The magnetoresistive element according to claim 6, wherein: The ratio of the major axis to the minor axis of the third free layer is 3-10, and the major axis is parallel to the first direction.

8. A method for preparing a magnetoresistive element, wherein: The preparation method comprises: providing a substrate; Depositing a magnetic stack on the substrate, performing tape-out and magnetic field annealing on the magnetic stack to form a magnetoresistive element as described in any one of claims 1 to 7; The magnetoresistive element comprises a first element portion including one or more first unit elements, and a second element portion including one or more second unit elements, wherein a first reference layer in the first unit element and a second reference layer in the second unit element have the same magnetization direction; The magnetic field annealing comprises: Annealing is performed at 340° C.-360° C. and a preset magnetic field for 40 min-80 min.

9. The preparation method according to claim 8, wherein: The magnetic field strength of the preset magnetic field is 3000Oe-5000Oe, and the magnetic field direction of the preset magnetic field is parallel to the easy magnetization direction of the first sensing layer; Depositing a magnetic stack on the substrate and taping out the magnetic stack comprises: Depositing a magnetic stack on the substrate according to a preset material and a preset thickness; the magnetic stack at least includes a bottom electrode layer, a reference layer, an insulating layer, a sensing layer and an antiferromagnetic layer; The magnetic stack is taped out to form at least one first magnetic stack and at least one second magnetic stack, the antiferromagnetic layer is etched and a first top electrode layer is deposited in a region of the magnetic stack corresponding to the first magnetic stack, and a second top electrode layer is deposited in a region of the magnetic stack corresponding to the second magnetic stack.

10. The preparation method according to claim 8, wherein: The magnetic field strength of the preset magnetic field is 3000Oe-5000Oe, and the magnetic field direction of the preset magnetic field is parallel to the easy magnetization direction of the first sensing layer; Depositing a magnetic stack on the substrate and taping out the magnetic stack comprises: Depositing a magnetic stack on the substrate according to a preset material and a preset thickness; the magnetic stack at least includes a bottom electrode layer, a reference layer, an insulating layer, and a sensing layer; the sensing layer includes a first sensing layer and a second sensing layer; The magnetic stack is taped out to form at least one first magnetic stack and at least one second magnetic stack; a first top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the first magnetic stack, the second sensing layer is etched and a second top electrode layer is deposited in an area of ​​the magnetic stack corresponding to the second magnetic stack, and the sensing layer in the first magnetic stack and the sensing layer in the second magnetic stack have different shapes.

11. A magnetic sensing device, wherein: The magnetic sensing device includes a magnetoresistive element; The magnetoresistive element is a magnetoresistive element according to any one of claims 1 to 7; The magnetic sensing device is used for at least one of current sensing, speed sensing, direction sensing, rotation angle sensing or proximity sensing.

12. A magnetic sensing device, wherein: The magnetic sensing device includes a magnetoresistive element; The magnetoresistive element is made by the preparation method according to any one of claims 8 to 10; The magnetic sensing device is used for at least one of current sensing, speed sensing, direction sensing, rotation angle sensing or proximity sensing.

Citation Information

Patent Citations

  • Device, magnetic sensor device and method

    CN104749536A

  • Magnetic sensor device and method for a magnetic sensor device having a magneto-resistive structure

    CN107046095A

  • Magnetoresistive element and magnetic sensor

    CN113574694A

  • Magnetoresistive element, preparation method of magnetoresistive element and magnetic sensing device

    CN116018048A

  • Magnetoresistive element, preparation method thereof and magnetic sensing device

    CN116449261A

Cited By

  • Magnetic field transducer

    EP4814518A1