Beneficiation method for improving grade of magnesium-containing copper sulfide ore concentrate

By adjusting the pH value and using specific collectors and inhibitors, the problem of magnesium silicate and pyrite affecting the grade of copper concentrate in high-magnesium-containing copper sulfur ores is solved, and copper concentrate is achieved Improvement of ore grade and stability of copper-molybdenum magnesium separation.

WO2024250449A1PCT designated stage expired Publication Date: 2024-12-12KUNMING METALLURGY INST +1

Patent Information

Application Number
PCT/CN2023/115920
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-08
Filing Date
2023-08-30
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Among the high-magnesium-containing copper sulfur ore, the presence of magnesium silicate minerals and pyrite leads to a decrease in the grade of copper concentrate, which is mainly due to the hydrophobicity and wearability of magnesium silicate minerals, which lead to difficulty in adsorption of collectors. The floating property and Cu2+ activation affect the copper-sulfur separation effect.

Method used

Using pretreatment, roughing, copper-molybdenum-sulfur separation and copper concentrate grade enhancement steps, by adjusting pH, using collectors and inhibitors, combined with flotation and remilling processes, the influence of magnesium is reduced and the copper concentrate grade is improved. .

Benefits of technology

It effectively improves the grade of copper concentrate, reduces the impact of magnesium and impurities, improves the production environment for copper-molybdenum magnesium separation, reduces copper metal loss, and improves the quality of copper concentrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023115920_12122024_PF_FP_ABST
    Figure CN2023115920_12122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of beneficiation and grade improvement. Disclosed is a beneficiation method for improving the grade of magnesium-containing copper sulfide ore concentrate. The present invention provides a method for improving the grade of magnesium-containing copper sulfide ore concentrate, comprising: crushing and grinding an ore to -0.074 mm accounting for 55% to 65%; adding a regulator, i.e., lime, collectors, i.e., butyl xanthate and kerosene, and a frother, i.e., MIBC, to obtain copper-molybdenum-sulfur mixed concentrate; re-grinding the copper-molybdenum-sulfur mixed concentrate to -0.048 mm accounting for 75-82%; adding the regulator, i.e., lime, a magnesium-containing silicate inhibitor, a collector, i.e., SG-1, and the frother, i.e., MIBC, to obtain copper-molybdenum mixed concentrate; and adding sodium sulfide, the collector, i.e., kerosene, and the frother, i.e., MIBC, to the copper-molybdenum mixed concentrate, so that high-grade copper concentrate can be obtained. According to the present invention, mixed flotation of copper and molybdenum, regrinding for separating copper and molybdenum from sulfur, and removal of magnesium from copper concentrate for grade improvement are used to improve the grade of copper concentrate.
Need to check novelty before this filing date? Find Prior Art

Description

A mineral processing method for improving the grade of magnesium-containing copper-sulfur ore concentrate Technical Field

[0001] The invention belongs to the technical field of chemical industry, and in particular relates to a mineral processing method for improving the grade of magnesium-containing copper-sulfur ore concentrate. Background Art

[0002] Copper deposits are generally classified into five types: porphyry, skarn, stratigraphic, volcanic, and copper-nickel sulfide. As mining progresses, alteration, such as potash, sericitization, silicification, and chloritization, occurs around some deposits. This diverse range of alteration types complicates ore sorting. For example, the presence of magnesium-containing silicate minerals such as talc, serpentine, and chlorite, as well as pyrite, can significantly impact the grade of copper concentrate. Technical issues

[0003] There are two main aspects that affect the copper concentrate grade in the flotation of high-magnesium copper-sulfide ores. The first is the influence of magnesium-containing silicate minerals. Magnesium-containing silicate minerals are difficult to inhibit, such as talc, serpentine, chlorite, etc., because of their strong hydrophobicity and good natural floatability, they are not easy to be inhibited; magnesium-containing silicate ores themselves are easy to grind and muddy, and it is easy to form sludge covering the surface of the mineral, affecting the adsorption of the collector on the mineral; the sludge is also easily included in the flotation foam machinery, affecting the concentrate grade. The second is the influence of pyrite. Pyrite has good floatability and is easy to float up; pyrite is usually suppressed in a high pH slurry environment, and the foam is easy to become sticky and then entrain other minerals, affecting the quality of the copper concentrate; pyrite is affected by Cu 2+ Activation effect, chalcopyrite is affected by Fe 2+ The inhibitory effect makes it difficult to separate copper and sulfur. Therefore, it is very necessary to develop a method that can solve the above technical problems. Technical Solutions

[0004] The object of the present invention is to provide a mineral processing method for improving the grade of magnesium-containing copper-sulfur ore concentrate.

[0005] The object of the present invention is achieved by comprising the steps of pre-treatment, roughing, copper-molybdenum-sulfur separation, and copper concentrate grade improvement, specifically comprising:

[0006] A. Pretreatment: Grind the raw ore and adjust the pH value to 8.5-10 to obtain material a. The grinding fineness is -0.074mm, accounting for 55-65%;

[0007] B. Roughing: Adjust the concentration of material a to 30-40%, add collector and diesel and stir for 2-4 minutes, then add frother and stir for 1-3 minutes, aerate and scrape for 3-5 minutes to obtain flotation foam product mixed with coarse concentrate b;

[0008] C. Copper, molybdenum and sulfur separation:

[0009] 1) Grind the mixed coarse concentrate b and adjust the pH value to 9-10 to obtain material c, with a grinding fineness of -0.048mm accounting for 75-82%;

[0010] 2) The concentration of material c is adjusted to 30-40%, a magnesium silicate inhibitor is added and stirred for 2-4 minutes, a collector SG-1 is added and stirred for 2-4 minutes, a frother is added and stirred for 1-3 minutes, and aeration and scraping are performed for 2-4 minutes to obtain a flotation foam product, a copper-molybdenum mixed coarse concentrate d;

[0011] D. Improvement of copper concentrate grade: Sodium sulfide is added to the copper-molybdenum mixed concentrate d and stirred for 2-4 minutes, diesel is added and stirred for 1-3 minutes, and then a frother is added and stirred for 1-3 minutes. Aeration and scraping for 3-5 minutes are performed to obtain a foam product containing magnesium and molybdenum e and a high-grade copper concentrate f.

[0012] The specific operations are as follows:

[0013] 1. Add ore and water to the rod mill in a solid-liquid ratio of 1:1, and grind the ore fineness from -0.074mm to 55%~65%. At the same time, add lime as an adjusting agent to the mill to obtain a flotation pulp sample. The pH value of the pulp is in the range of 8.5~10.

[0014] 2. Place the above flotation pulp sample into the flotation machine with a flotation concentration of 30% to 40%. Add the collector butyl xanthate and diesel and stir for 3 minutes. Add the foaming agent MIBC and stir for 2 minutes. Aerate and scrape for 4 minutes to obtain the flotation foam product, i.e., mixed coarse concentrate.

[0015] 3. Pour the mixed coarse concentrate into the mill at a liquid-solid ratio of 1:1. The grinding fineness is -0.048mm75%~82%. Lime as an adjusting agent is also added into the mill. The pH value of the slurry is in the range of 9~10.

[0016] 4. Place the above flotation pulp sample into the flotation machine with a flotation concentration of 30% to 40%. Add magnesium silicate inhibitor and stir for 3 minutes, collector SG-1 and stir for 3 minutes, frother MIBC and stir for 2 minutes, and aerate and scrape for 3 minutes to obtain the flotation foam product, i.e., copper-molybdenum mixed coarse concentrate.

[0017] 5. The main components of the collector SG-1 are isobutyl xanthate propylene ester (50%~65%), glycerol monolaurate (10%~20%) and isopropyl alcohol mixture (5%~20%).

[0018] 6. The above-mentioned magnesium silicate inhibitor is a 1:1 combination of inorganic salts and organic inhibitors, wherein the inorganic inhibitor is at least one of sodium sulfite, sodium hexametaphosphate, and water glass, and the organic inhibitor is at least one of sodium carboxymethyl cellulose, starch, and dextrin.

[0019] 7. Place the above flotation pulp sample into a flotation machine with a flotation concentration of 20% to 30%. Add the inhibitor sodium sulfide and stir for 3 minutes. Add the frother MIBC and stir for 1 minute. Aerate and scrape for 3 minutes. Filter the product at the bottom of the flotation machine to obtain copper concentrate with improved quality. The foam product is the magnesium-molybdenum-containing product.

[0020] The present invention adopts mixed flotation, regrinding copper-sulfur separation, and copper-molybdenum-talc separation, and realizes the improvement of copper concentrate grade through the coordination of reagents and processes, which has reference significance for the treatment of similar ores. Beneficial effects

[0021] The technical principle characteristics of the present invention are as follows:

[0022] 1. Add magnesium-containing silicate inhibitors in the copper-molybdenum-sulfur separation stage to further reduce the magnesium content and weaken the impact of high magnesium content on process stability during the circulation process.

[0023] 2. Add more selective collectors in the copper-molybdenum-sulfur separation stage to reduce the sulfur content and the impact of some impurities, creating a more favorable production environment for copper-molybdenum-magnesium separation.

[0024] 3. Add a collector with strong collection ability and weak selectivity in the roughing stage to recover as much recyclable metal as possible and reduce the loss of copper metal in the roughing stage; add a collector with strong selectivity in the copper-molybdenum-sulfur separation stage to further reduce the impact of impurity content. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] FIG1 is a schematic diagram of a closed-circuit test process according to Example 1 of the present invention;

[0026] FIG2 is a schematic diagram of a full-open circuit test process according to embodiment 2 of the present invention. Modes for Carrying Out the Invention

[0027] The present invention is further described below with reference to the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention fall within the scope of protection of the present invention.

[0028] The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate of the present invention includes pretreatment, roughing, copper-molybdenum-sulfur separation, and copper concentrate grade improvement steps, specifically including:

[0029] A. Pretreatment: Grind the raw ore and adjust the pH value to 8.5-10 to obtain material a. The grinding fineness is -0.074mm, accounting for 55-65%;

[0030] B. Roughing: Adjust the concentration of material a to 30-40%, add collector and diesel and stir for 2-4 minutes, then add frother and stir for 1-3 minutes, aerate and scrape for 3-5 minutes to obtain flotation foam product mixed with coarse concentrate b;

[0031] C. Copper, molybdenum and sulfur separation:

[0032] 1) Grind the mixed coarse concentrate b and adjust the pH value to 9-10 to obtain material c, with a grinding fineness of -0.048mm accounting for 75-82%;

[0033] 2) The concentration of material c is adjusted to 30-40%, a magnesium silicate inhibitor is added and stirred for 2-4 minutes, a collector SG-1 is added and stirred for 2-4 minutes, a frother is added and stirred for 1-3 minutes, and aeration and scraping are performed for 2-4 minutes to obtain a flotation foam product, a copper-molybdenum mixed coarse concentrate d;

[0034] D. Improvement of copper concentrate grade: Sodium sulfide is added to the copper-molybdenum mixed concentrate d and stirred for 2-4 minutes, diesel is added and stirred for 1-3 minutes, and then a frother is added and stirred for 1-3 minutes. Aeration and scraping for 3-5 minutes are performed to obtain a foam product containing magnesium and molybdenum e and a high-grade copper concentrate f.

[0035] In step A, the pH value is adjusted by using lime as an adjusting agent.

[0036] The collector described in step B is butyl xanthate.

[0037] The foaming agent described in step B is methyl isobutyl carbinol MIBC.

[0038] C. In step 1), the pH value is adjusted by using lime as an adjusting agent.

[0039] C. The magnesium silicate inhibitor in step 2) is composed of inorganic and organic types.

[0040] The mass ratio of the inorganic and organic materials is 1:1.

[0041] The inorganic type is one or more of sodium sulfite, sodium hexametaphosphate and water glass; the organic type is one or more of sodium carboxymethyl cellulose, starch and dextrin.

[0042] The collector SG-1 described in step C2) is composed of isobutyl xanthate propylene ester, glycerol monolaurate and isopropyl alcohol.

[0043] The mass ratio of isobutyl xanthate propylene ester, glycerol monolaurate and isopropyl alcohol is (50-65): (10-20): (5-20).

[0044] C. The foaming agent in step 2) is methyl isobutyl carbinol MIBC.

[0045] The present invention will be further described below with reference to specific implementation cases:

[0046] Example 1

[0047] Roughing stage: 3 kg of ore (copper content 0.45%, molybdenum content 0.010%, magnesium oxide content 11.81%) was taken and added to the mill as a conditioning agent. The ore was crushed and ground to -0.074 mm, accounting for 65%. The pH value of the flotation feed slurry was 9.5. The slurry sample was placed in an 8L flotation tank, and butyl xanthate + diesel (40 + 20g / t) was added and stirred for 3 minutes. The frother MIBC 40g / t was added and stirred for 2 minutes. The foaming agent was aerated and scraped for 4 minutes to obtain the flotation foam product, namely the mixed coarse concentrate.

[0048] Copper-molybdenum-sulfur separation stage: The concentration of the copper-molybdenum-sulfur mixed concentrate slurry sample is adjusted to 50%, and lime as an adjusting agent is added. The pH value is controlled at 9, and the grinding fineness is -0.045mm, accounting for 75%. The ground slurry sample is placed in a 1.5L flotation machine, and a magnesium silicate inhibitor of 300g / t is added and stirred for 3 minutes; a collector SG-1 (20g / t) is stirred for 3 minutes; a foaming agent MIBC (10g / t) is added, stirred for 2 minutes, and aerated and scraped for 4 minutes. The foam product is subjected to one-time selection to obtain a copper-molybdenum mixed concentrate.

[0049] Copper concentrate grade improvement stage: copper-molybdenum mixed concentrate slurry sample is placed in a 0.75L tank, 500g / t of sodium sulfide is added, and stirred for 3 minutes; 20g / t of diesel is added, and stirred for 2 minutes; frother MIBC (20g / t) is added, and stirred for 2 minutes; aeration and scraping are carried out for 4 minutes, and the slurry sample in the flotation machine is swept once to obtain high-grade copper concentrate.

[0050] The results of the closed-circuit test are shown in Figure 1. After multiple cycles, two sets of data were taken after reaching the equilibrium value (see Table 1 and Table 2) to analyze the effect of improving the quality of the copper-molybdenum mixed concentrate. With little change in the copper recovery rate, the copper grade increased by 5-6 percentage points.

[0051] Table 1

[0052]

[0053] Table 2

[0054]

[0055] Example 2

[0056] Roughing stage: 3 kg of ore (copper content 0.46%, molybdenum content 0.010%, magnesium oxide content 11.81%) was taken and added to the mill as a conditioning agent. The ore was crushed and ground to -0.074 mm, accounting for 65%. The pH value of the flotation feed slurry was 8.5. The slurry sample was placed in an 8L flotation tank, and butyl xanthate + diesel (30 + 15g / t) was added and stirred for 3 minutes. MIBC 40g / t of frother was added and stirred for 2 minutes. The foam was aerated and scraped for 4 minutes to obtain the flotation foam product, namely the mixed coarse concentrate.

[0057] Copper-molybdenum-sulfur separation stage: The concentration of the copper-molybdenum-sulfur mixed concentrate slurry sample is adjusted to 50%, and lime is added as an adjusting agent. The pH value is controlled at 9, and the grinding fineness is -0.045mm, accounting for 81%. The ground slurry sample is placed in a 1.5L flotation machine, and a magnesium silicate inhibitor of 200g / t is added and stirred for 3 minutes; a collector SG-1 (10g / t) is stirred for 3 minutes; a foaming agent MIBC (10g / t) is added, stirred for 2 minutes, and aerated and scraped for 4 minutes. The foam product is subjected to one-time selection to obtain a copper-molybdenum mixed concentrate.

[0058] Copper concentrate grade improvement stage: copper-molybdenum mixed concentrate slurry sample is placed in a 0.75L tank, 500g / t of sodium sulfide is added, and stirred for 3 minutes; 20g / t of diesel is added, and stirred for 2 minutes; 20g / t of frother MIBC is added, and stirred for 2 minutes; aeration and scraping are performed for 4 minutes, and the slurry sample in the flotation machine is swept once to obtain high-grade copper concentrate.

[0059] The full open circuit test yielded the results shown in Figure 2. Analysis of the effect of quality improvement on the copper-molybdenum mixed concentrate revealed that the copper grade increased by 5-6 percentage points with little change in copper recovery. See Table 3 for specific data.

[0060] Table 3

[0061] .

Claims

1. A method for improving the grade of magnesium-containing copper-sulfide ore concentrate, characterized in that: It includes pre-treatment, roughing, copper-molybdenum-sulfur separation, and copper concentrate grade improvement steps, specifically including: A. Pretreatment: Grind the raw ore and adjust the pH value to 8.5~10 to obtain material a, with a grinding fineness of -0.074mm accounting for 55~65%; B. Roughing: adjust the concentration of material a to 30-40%, add collector and diesel and stir for 2-4 minutes, then add frother and stir for 1-3 minutes, aerate and scrape for 3-5 minutes to obtain flotation foam product mixed with coarse concentrate b; C. Copper, molybdenum and sulfur separation: 1) Grind the mixed coarse concentrate b and adjust the pH value to 9-10 to obtain material c, with a grinding fineness of -0.048mm accounting for 75-82%; 2) The concentration of material c is adjusted to 30-40%, a magnesium silicate inhibitor is added and stirred for 2-4 minutes, a collector SG-1 is added and stirred for 2-4 minutes, a frother is added and stirred for 1-3 minutes, and aeration and foaming are performed for 2-4 minutes to obtain a flotation foam product of copper-molybdenum mixed rough concentrate d; D. Improvement of copper concentrate grade: Sodium sulfide is added to the copper-molybdenum mixed concentrate d and stirred for 2-4 minutes, diesel is added and stirred for 1-3 minutes, and then a frother is added and stirred for 1-3 minutes, and aeration and scraping are performed for 3-5 minutes to obtain a foam product containing magnesium-molybdenum product e and a high-grade copper concentrate f.

2. The method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: In step A, the pH value is adjusted by using lime as an adjusting agent.

3. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: The collector described in step B is butyl xanthate.

4. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: The foaming agent described in step B is methyl isobutyl carbinol MIBC.

5. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: C. In step 1), the pH value is adjusted by using lime as an adjusting agent.

6. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: C. The magnesium silicate inhibitor in step 2) is composed of inorganic and organic types.

7. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 6, characterized in that: The mass ratio of the inorganic and organic materials is 1:

1.

8. The ore dressing method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 6 or 7, characterized in that: The inorganic type is one or more of sodium sulfite, sodium hexametaphosphate and water glass; the organic type is one or more of sodium carboxymethyl cellulose, starch and dextrin.

9. The method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 1, characterized in that: C. The collector SG-1 described in step 2) is composed of isobutyl xanthate propylene ester, glycerol monolaurate and isopropyl alcohol.

10. The method for improving the grade of magnesium-containing copper-sulfur ore concentrate according to claim 9, characterized in that: The mass ratio of isobutyl xanthate propylene ester, glycerol monolaurate and isopropanol is (50-65): (10-20): (5-20).

Citation Information

Patent Citations

  • Flotation separation method of low / extra-low grade copper-molybdenum ore or chat

    CN104722409A

  • Beneficiation method for low-grade mixed copper ore containing molybdenum

    CN105435953A

  • Mineral beneficiation method of complex and refractory high-grade copper sulfide ore

    CN107855211A

  • High-efficiency flotation collecting agent for high-sulfur iron easily-argillized fine-grained complex embedded copper-molybdenum ore as well as preparation method and application thereof

    CN112264194A

  • Magnesium-containing silicate mineral inhibitor and application thereof

    CN112495590A

Cited By

  • Sulfur suppression flotation method for mixed sulfur concentrate in low dissolved oxygen environment

    CN119819494A