Polypropylene-based non-stretched film and laminate using same

The polypropylene-based unstretched film with a propylene random copolymer and specific surface characteristics addresses the challenges of low-temperature heat-sealability and high-temperature blocking resistance, offering improved retort food packaging performance and environmental sustainability.

WO2024252926A1PCT designated stage expired Publication Date: 2024-12-12TORAY ADVANCED FILM CO LTD

Patent Information

Application Number
PCT/JP2024/018779
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-23
Filing Date
2024-05-22
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Current packaging solutions for retort food face challenges with polypropylene films due to poor low-temperature heat-sealability, high-temperature blocking resistance, and bag-making processability, particularly when aiming for reduced layer configurations and environmental sustainability.

Method used

A polypropylene-based unstretched film with a propylene random copolymer having a melting temperature peak between 135°C and 145°C, combined with a base layer containing 50% propylene/ethylene block copolymer and a sealing layer with specific surface roughness and peak count, enhances heat-sealing strength and blocking resistance while maintaining environmental friendliness.

Benefits of technology

The solution provides excellent low-temperature heat-sealability, high-temperature blocking resistance, and improved bag-making processability, ensuring retort suitability and reduced material usage, while maintaining environmental considerations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided are: a polypropylene-based non-stretched film that has, when used in a packaging bag that is for packaging a retort food and has less number of layers in consideration of the environment, excellent low-temperature heat sealability and high-temperature blocking resistance, excellent bag-making processability, and excellent retort suitability; and a laminate using the same. This polypropylene-based non-stretched film contains, as a main component, a propylene-based random copolymer having a melting temperature peak at 135-145°C, and has, as a heat seal surface on at least one surface, a surface that has a film surface average roughness Ra of at least 0.1 µm and a peak count of at least 100 peaks / 10 mm2 for 0.3 µm or higher peaks. Alternatively, the polypropylene-based non-stretched film according to claim 1 is formed of two layers, which are a base layer and a seal layer. The base layer contains at least 50 mass% of a propylene-ethylene block copolymer, and has a melting temperature peak at 150°C or higher. The range of the melting temperature peak of the seal layer is 135-145°C. The polypropylene-based non-stretched film has, as a heat seal surface, a surface in which the seal layer surface has a surface average roughness Ra of at least 0.1 µm, and, in terms of the peak count number RPc, the peak count is at least 100 peaks / 10 mm2 for 0.3 µm or higher peaks. In addition, this laminate has laminated therein a heat resistant base material having a melting point of 160°C or higher, and has a heat seal strength of at least 23 N / 15 mm at 170°C.
Need to check novelty before this filing date? Find Prior Art

Description

Polypropylene-based unstretched film and laminate using the same

[0001] The present invention relates to a polypropylene-based unstretched film for packaging retort food and a laminate using the same.

[0002] Laminates and packaging bags for retort food packaging include those made by laminating a heat-resistant substrate such as biaxially oriented polyethylene terephthalate film (hereinafter sometimes referred to as PET), biaxially oriented polyamide film (hereinafter sometimes referred to as ON), or aluminum foil (hereinafter sometimes referred to as AL foil) with a heat-sealable unoriented polypropylene film (hereinafter sometimes referred to as CPP), such as PET / ON / CPP or PET / ON / AL foil / CPP. The required properties of these packaging bags include heat resistance, impact resistance, high heat-seal strength, blocking resistance, and bag-making processability.

[0003] In recent years, environmentally friendly packaging legislation has come into force, making environmentally conscious design of packaging bags essential. This has led to increased demand for a reduction in the number of layers in the laminate, and bilayer structures such as PET / CPP, ON / CPP, and OPP / CPP are being investigated. Furthermore, there is a growing demand for mono-material packaging bags made of the same material with excellent recyclability. Therefore, laminates of the same material, such as biaxially oriented polypropylene film / non-oriented polypropylene film, with an OPP / CPP structure, are being investigated. However, OPP has lower heat resistance than PET and ON, resulting in poor bag-making processability under conventional bag-making conditions. Therefore, in order to maintain the same bag-making processability as before, there is an increasing demand for non-oriented polypropylene film with low-temperature heat sealability, high-temperature blocking resistance, and retort suitability.

[0004] In order to solve the above problems, Patent Document 1 proposes a laminate in which a heat seal layer is laminated on one side of a biaxially oriented polypropylene film having high heat resistance and elastic modulus, but the laminate has insufficient low-temperature heat sealability, high-temperature blocking resistance, and retort suitability. Also, Patent Document 2 proposes a polypropylene-based multilayer sealant film for retort pouches in which inorganic particles are added to the heat seal layer to define the surface roughness, but there are concerns about particles falling off during the film-forming process or laminating process, and particles being mixed into food. In addition, the film properties of low-temperature heat sealability, high-temperature blocking resistance, and retort suitability are insufficient, and the bag-making processability is also poor.

[0005] JP 2020-7441 A Patent No. 5895590 A

[0006] Therefore, an object of the present invention is to provide a polypropylene-based unstretched film that has excellent low-temperature heat sealing properties, high-temperature blocking resistance, bag-making processability, and retort suitability, and a laminate using the same, as a packaging bag for retort food packaging with a reduced number of layers that is environmentally friendly.

[0007] The present inventors have achieved the above object by providing the following polypropylene-based unstretched film and a laminate using the same.

[0008] That is, the present invention is directed to a film having a propylene-based random copolymer as a main component, the melting temperature peak of which is 135°C or higher and 145°C or lower, and a film having an average surface roughness Ra of 0.1 µm or higher and a peak count of 0.3 µm or higher of 100 or more per 10 mm on at least one side. 2 The surface of the film is a non-stretched polypropylene film, and the heat-sealable surface is a surface of the film.

[0009] The adhesive tape is made up of two layers, a base layer and a seal layer, and the base layer contains 50% by mass or more of a propylene-ethylene block copolymer, has a melting temperature peak of 150°C or higher, and the seal layer has a melting temperature peak in the range of 135°C to 145°C. The seal layer surface has an average surface roughness Ra of 0.1 μm or higher, and the number of peaks of 0.3 μm or higher is 100 / 10 mm. 2 The polypropylene-based non-oriented film has the above surface as a heat seal surface.

[0010] By using a polypropylene-based unstretched film that has excellent low-temperature heat sealing properties and high-temperature blocking resistance for packaging retort foods, and a laminate using the same, it is possible to provide an environmentally friendly packaging bag for packaging retort foods that allows for a reduction in the amount of packaging material used.

[0011] The polypropylene-based non-oriented film and the laminate using the same of the present invention will be specifically described below.

[0012] The non-oriented polypropylene film of the present invention is mainly composed of a propylene random copolymer having a melting temperature peak in the range of 135° C. to 145° C. Here, the term "main component" means that the propylene random copolymer accounts for 50% by mass or more of the total amount of resin in the film.

[0013] If the ratio of the propylene-based random copolymer having a melting temperature peak in the range of 135°C to 145°C is less than 50% by mass, the heat seal strength of 23 N / 15 mm or more at 170°C required for retort food applications cannot be obtained, and when the contents are filled into the bag and heat sterilized at 130°C or higher, scattering or leakage of the contents may occur.

[0014] The peak melting temperature of the propylene random copolymer is in the range of 135°C to 145°C, so that the heat seal strength at 170°C required for retort food applications of 23N / 15mm or more can be obtained, and the blocking shear strength at 130°C is 15N / 12cm. 2 This is preferable because it can be done as follows:

[0015] When the melting temperature peak is less than 135°C, the blocking shear force at 130°C is 15 N / 12 cm 2 If the peak melting temperature exceeds 145°C, when the heat seal surfaces are overlapped and heat sealed, the heat seal initiation temperature at which the heat seal strength is 3 N / 15 mm or more may become 150°C or higher, slowing down the bag making speed.

[0016] The melt flow rate (hereinafter sometimes referred to as MFR) of the propylene random copolymer is preferably in the range of 0.5 to 100 g / 10 min (230°C, load 2.18 N), and more preferably in the range of 2 to 20 g / 10 min, since this allows stable melt extrusion film formation.

[0017] The propylene-based random copolymer having a melting temperature peak in the range of 135°C to 145°C is preferably a propylene-based random copolymer composed of propylene and one or more comonomers, since it can achieve both high-temperature blocking resistance and heat seal strength.

[0018] Examples of the comonomer include ethylene and α-olefins having 4 or more carbon atoms. Examples of the random copolymer include a propylene-ethylene random copolymer of propylene and ethylene, a random copolymer of propylene and an α-olefin having 4 or more carbon atoms, and a random copolymer of propylene, ethylene, and an α-olefin having 4 or more carbon atoms. Examples of the α-olefins having 4 or more carbon atoms constituting the random copolymer include 1-butene, 4-methylpentene-1, 1-octene, 1-hexene, etc., and 1-butene is preferred.

[0019] From the viewpoint of heat seal strength, the copolymerization amount of the comonomer is preferably 1 mol % or more and 10 mol % or less in terms of copolymerization amount. If the copolymerization amount is less than 1 mol %, the heat seal strength may be low, while if it exceeds 10 mol %, the slipperiness may be poor, the film may be prone to wrinkling during winding, and blocking may occur during unwinding, causing film tearing.

[0020] The non-oriented polypropylene film of the present invention has an average surface roughness Ra of 0.1 μm or more on at least one surface to be heat-sealed, preferably in the range of 0.2 to 0.7 μm, because this provides good film slippage and good processability during film formation and lamination.

[0021] The polypropylene-based non-oriented film of the present invention has a peak count of 100 or more peaks of 0.3 μm or more per 10 mm on at least one side of the heat-sealable surface.2 In this case, the blocking shear force at 130°C is 15N / 12cm 2 This is preferable because it is easy to open the bag, easy to fill the contents, and increases the bag-making speed when automatically filling the contents into the bag. 2 , more preferably 500 or more / 10 mm 2 is.

[0022] In order to set the average film surface roughness of the heat seal surface and the peak count of 0.3 μm or more within the preferred ranges, it is preferable that the film surface is not formed using inorganic or organic particles, since this can prevent particles from falling off during film formation and particles from being mixed into the contents.

[0023] In order to set the average surface roughness of the film and the peak count of 0.3 μm or more within the preferred range, for example, the propylene random copolymer may be mixed with at least one polyethylene and an organic peroxide crosslinking agent, and the mixture may be extruded at high temperature and high shear to prepare chips, which may then be used to form a film using a T-die type film forming machine or an inflation film forming machine.

[0024] The polyethylene has a density of, for example, 0.900 g / cm 3 0.945g / cm or more 3 Low density polyethylene, with a density of less than 0.945 g / cm 3 0.970g / cm or more 3 Examples include high density polyethylene with a density of less than 0.900 g / cm 3 If less than this amount of polyethylene is mixed, it may not be possible to form the above-mentioned average surface roughness and peak count of the film.

[0025] As the low density polyethylene, linear low density polyethylene (hereinafter sometimes referred to as LLDPE), which is a copolymer of ethylene and α-olefin, has good dispersibility in propylene-based random copolymers, and the peak count of 0.3 μm or more is 100 or more / 10 mm. 2Examples of the α-olefin constituting the linear low-density polyethylene include 1-butene, 1-hexene, and 1-octene.

[0026] The peak melting temperature of the polyethylene is preferably 100°C or higher and lower than 140°C, more preferably 120°C or higher and lower than 140°C, from the viewpoint of heat seal strength and blocking shear force at 130°C.

[0027] The melt flow rate of the polyethylene measured in accordance with JIS-K7210 (1999) at 190°C under a load of 21.18 N is preferably 0.2 to 10 g / 10 min, more preferably 0.5 to 5 g / 10 min, since this provides good dispersibility in the propylene-based random copolymer and makes it easier to obtain the film surface average roughness and peak count of 0.3 μm or more.

[0028] The amount of the linear low-density polyethylene (LLDPE) mixed into the propylene-based random copolymer is preferably less than 50% by mass, more preferably in the range of 5 to 40% by mass, and even more preferably in the range of 10 to 30% by mass, which makes it easier to obtain the average surface roughness of the film and a peak count of 0.3 μm or more, and the blocking shear force at 130° C. is 15 N / 12 cm 2 The following is likely to be the case, which is preferable.

[0029] The amount of the organic peroxide added is preferably in the range of 0.1 to 10% by mass, more preferably 0.5 to 5% by mass, based on the resin component, because this provides good dispersibility in the resin, allows the crosslinking agent to exert its effect on the polyethylene, and makes it easier to obtain the film surface average roughness and peak count of 0.3 μm or more. If the amount added is less than 1% by mass, the effect of the addition is difficult to see, while if it exceeds 40% by mass, poor dispersion is likely to occur and extrudability may deteriorate.

[0030] The organic peroxide is not particularly limited, and examples thereof include alkyl peroxides, diacyl peroxides, ester peroxides, carbonate peroxides, etc. Examples of alkyl peroxides include dicumyl peroxide, di-tert-butyl peroxide, di-tert-butylcumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(tert-butyl-oxy)hexyne-3, tert-butylcumyl, 1,3-bis(tert-butylperoxyisopropyl)benzene, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxonane, etc.

[0031] Examples of diacyl peroxides include benzoyl peroxide, lauroyl peroxide, decanoyl peroxide, etc. Examples of peroxide esters include 1,1,3,3-tetramethylbutylperoxyneodecanoate, α-cumylperoxyneodecanoate, tert-butylperoxyneodecanoate, tert-butylperoxyneoheptanoate, tert-butylperoxypivalate, tert-hexylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, tert-amylperoxyl-2-ethylhexanoate, tert-amylperoxyl-2-ethylhexanoate, tert-butylperoxypivalate, tert-butylperoxyneodecanoate, tert-butylperoxyneoheptanoate, tert-butylperoxypivalate, tert-hexylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, tert-amylperoxyl-2-ethylhexanoate, tert-butylperoxyneodecanoate, tert-butylperoxyneodecanoate, tert-butylperoxyneoheptanoate, tert-butylperoxypivalate, tert-hexylperoxypivalate, tert-butylperoxy-2-ethylhexanoate, tert-amylperoxyl-2-ethylhexanoate, tert-butylperoxyneodec ... peroxymethyl terephthalate, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxyisobutyrate, di-tert-butylperoxyhexahydroterephthalate, tert-amylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxyacetate, tert-butylperoxybenzoate, and di-butylperoxytrimethyladipate.

[0032] Examples of peroxycarbonates include di-3-methoxybutyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, diisopropyl peroxydicarbonate, tert-butylperoxyisopropyl carbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, dicetyl peroxydicarbonate, and dimyristyl peroxydicarbonate.

[0033] From the viewpoint of food hygiene when packaging retort food, it is preferable that the organic peroxide does not remain in the polypropylene-based unstretched film of the present invention.

[0034] Another method for achieving a preferred range of average film surface roughness Ra and peak count of 0.3 μm or more is to use a film-forming nip roller to impart an embossed shape to one side of the film (heat-sealed surface). There are no particular limitations on the film-forming nip roller as long as it can form the heat-sealed surface of the present invention. For example, the film-forming nip rollers disclosed in International Publication No. 2013 / 80925 and Japanese Patent Application Laid-Open No. 2020-55189 are preferably used. Specifically, an embossing nip roller having an arithmetic mean roughness Ra of 0.2 μm or less, a ten-point mean roughness Rz of 2 to 8 μm, and an average spacing Sm of irregularities of 90 μm or less is preferred.

[0035] The polypropylene-based non-stretched film of the present invention has a blocking shear strength of 15 N / 12 cm between heat-sealed surfaces at 130°C. 2 In this case, the bag is easy to open and the filling of the contents is excellent when automatically filling the contents into the bag. 2 If the time exceeds this, the opening of the bag may not open during automatic filling of the contents into the bag, causing the contents to spill out, and the bag making speed may decrease.

[0036] In addition, in the case of packaging bags such as pouches, when the heat-sealable surfaces are overlapped and heat-sealed, the heat-sealing initiation temperature at which the heat-sealing strength becomes 3 N / 15 mm or more is preferably 150°C or lower, more preferably 145°C or lower.

[0037] The bag-making speed is preferably 40 spm or more, more preferably 45 spm or more. If the bag-making speed is less than 40 spm, the product yield may be poor and the manufacturing cost may increase, which is not preferable.

[0038] The polypropylene-based unstretched film of the present invention is preferred because the blocking shear force and heat seal strength at 130°C are within the preferred ranges of the present invention, and the addition of a thermoplastic elastomer improves the low-temperature heat sealability and impact resistance.

[0039] The content of the thermoplastic elastomer is preferably 5% by mass or more and 40% by mass or less. If the content is less than 5% by mass, the effect of improving low-temperature heat sealability and impact resistance may not be achieved, whereas if the content is more than 40% by mass, the heat seal strength may be significantly reduced during retort treatment or heating in a microwave oven, etc., which may result in liquid leakage from the packaging bag.

[0040] The thermoplastic elastomer is preferably a copolymer of 55 to 95% by mass of ethylene or propylene as a main component and 5 to 45% by mass of an α-olefin as a copolymerization monomer, specifically one produced using a metallocene catalyst.

[0041] As the α-olefin, ethylene, propylene, 1-butene, 1-hexene, 1-octene, etc., having 2 to 10 carbon atoms can be used, and specific examples of the thermoplastic elastomer include ethylene-propylene copolymer elastomer, ethylene-butene copolymer elastomer, ethylene-octene copolymer elastomer, propylene-ethylene copolymer elastomer, propylene-butene copolymer elastomer, propylene-hexene copolymer elastomer, propylene-octene copolymer elastomer, etc. In particular, it is preferable to additionally add an elastomer containing propylene as a main component in terms of heat seal strength and low-temperature impact resistance.

[0042] The MFR of the thermoplastic elastomer is preferably in the range of 0.5 to 10 g / 10 min at 190° C. under a load of 21.18 N, from the viewpoints of miscibility with the propylene-based random copolymer and blocking resistance.

[0043] The polypropylene-based non-oriented film of the present invention comprises two layers, a base layer and the polypropylene-based non-oriented film as a seal layer, wherein the base layer contains 50% by mass or more of a propylene-ethylene block copolymer, has a melting temperature peak of 150°C or higher, the seal layer has a melting temperature peak in the range of 135°C to 145°C, the seal layer has a surface average roughness Ra based on roughness curve elements of 0.1 μm or higher, and the peak count RPc based on the roughness curve elements is 100 peaks / 10 mm of 0.3 μm or higher. 2 That's all.

[0044] The base layer preferably contains 50% by mass or more of a propylene-ethylene block copolymer. If the propylene-ethylene block copolymer content is less than 50% by mass, the laminate may have poor low-temperature impact resistance when laminated with a heat-resistant substrate and used as a packaging bag.

[0045] In order to obtain the properties of the laminate of the present invention, it is preferable that the propylene-ethylene block copolymer has an intrinsic viscosity [η]CXS of the 20°C xylene soluble portion CXS of 2.5 dl / g or more and 3.5 dl / g or less, the amount of the 20°C xylene soluble portion CXS of 10 mass% or more and 25.0 mass% or less, and the 20°C xylene insoluble portion CXIS of 1.5 dl / g or more and 2.2 dl / g or less.

[0046] Here, with regard to the 20°C xylene insoluble portion CXIS and soluble portion CXS, when the polypropylene film is completely dissolved in boiling xylene, the temperature is lowered to 20°C, and the mixture is left to stand for 4 hours or more, and then the precipitate and solution are separated by filtration, the precipitate is referred to as the 20°C xylene insoluble portion CXIS (hereinafter may be referred to as the xylene insoluble portion CXIS), and the portion obtained by drying the solution portion (filtrate) to dryness and at 70°C under reduced pressure is referred to as the 20°C xylene soluble portion CXS (hereinafter may be referred to as the xylene soluble portion CXS).

[0047] The 20° C. xylene insoluble portion CXIS corresponds to the polypropylene alone, and the xylene soluble portion CXS corresponds to the rubber component.

[0048] If the amount of 20°C xylene soluble portion CXS in the base layer is less than 10% by mass, the low-temperature impact resistance may be poor, and the decrease in heat seal strength of the laminate at 100°C may be small, resulting in poor vapor permeability, while if it exceeds 25.0% by mass, the decrease in heat seal strength at 100°C may be significant, resulting in leakage of liquid from the packaging bag when heated in a microwave oven, etc. The amount of CXS is preferably in the range of 8% to 20.0% by mass.

[0049] If the intrinsic viscosity ([η]CXS) of the 20°C xylene soluble portion CXS in the base layer is less than 2.5 dL / g, the low-temperature impact resistance may decrease, and if it is more than 3.5 dL / g, the dispersibility in the xylene insoluble portion CXIS may decrease, resulting in poor melt extrudability.

[0050] Furthermore, if the intrinsic viscosity ([η]CXIS) of the 20°C xylene-insoluble portion CXIS in the polypropylene film is less than 1.5 dL / g, the low-temperature impact resistance may decrease, and if it is more than 2.2 dL / g, the dispersibility of the xylene-soluble portion CXS may deteriorate.

[0051] The melt flow rate (hereinafter sometimes referred to as MFR) of the propylene-ethylene block copolymer is preferably in the range of 0.5 to 10 g / 10 min at 230° C. under a load of 21.18 N from the viewpoints of extrusion stability and low-temperature impact resistance.

[0052] The base layer preferably contains 10% by mass or more and less than 50% by mass of a propylene-ethylene random copolymer, since this allows adjustment of the low-temperature impact resistance and heat seal strength of the retort packaging laminate.

[0053] The ethylene content of the propylene-ethylene random copolymer is preferably 1% by mass or more and 7% by mass or less, since this provides good miscibility with the propylene-ethylene block copolymer.

[0054] The MFR of the propylene-ethylene random copolymer is preferably in the range of 0.5 to 10 g / 10 min at 230° C. under a load of 21.18 N, from the viewpoints of extrusion stability and melt miscibility with the propylene-ethylene block copolymer.

[0055] The base layer preferably contains 10% by mass or more and 40% by mass or less of an ethylene-α-olefin copolymer (where the total mass of the base layer resin is taken as 100% by mass), which is preferable because it allows adjustment of vapor permeability during microwave heating.

[0056] If the content of the ethylene / α-olefin copolymer is less than 10% by mass, the effect of the copolymer on vapor permeability during microwave heating may not be observed, whereas if the content exceeds 40% by mass, the heat seal strength may be significantly reduced during retort treatment or heating in a microwave oven, etc., which may result in liquid leakage from the packaging bag.

[0057] The melting point of the ethylene / α-olefin copolymer is preferably 110° C. or higher and 140° C. or lower. If the melting point is lower than 110° C., the heat seal strength at high temperatures may decrease, resulting in packaging bags being torn, whereas if the melting point is higher than 140° C., the heat seal strength at high temperatures may increase, resulting in poor steam permeability during microwave heating.

[0058] The ethylene-α-olefin copolymer is a copolymer of 50 to 95% by mass of ethylene as a main component and an α-olefin as a copolymerizable monomer, and specifically, it is preferably produced using a metallocene catalyst.

[0059] As the α-olefin, 1-butene, 1-hexene, 1-octene, etc., each having 4 to 10 carbon atoms, can be used, and a specific example thereof is linear low-density polyethylene (hereinafter sometimes referred to as LLDPE).

[0060] The MFR of the ethylene / α-olefin copolymer is preferably in the range of 0.5 to 10 g / 10 min at 190° C. under a load of 21.18 N, from the viewpoints of miscibility with polypropylene resins and blocking resistance.

[0061] It is preferable to add a thermoplastic elastomer to the polypropylene-based non-stretched film, since this improves the low-temperature heat sealability and impact resistance.

[0062] The content of the thermoplastic elastomer is preferably 5% by mass or more and 40% by mass or less. If the content is less than 5% by mass, the effect of improving low-temperature heat sealability and impact resistance may not be achieved, whereas if the content is more than 40% by mass, the heat seal strength may be significantly reduced during retort treatment or heating in a microwave oven, etc., which may result in liquid leakage from the packaging bag.

[0063] The thermoplastic elastomer is preferably a copolymer of 55 to 95% by mass of ethylene or propylene as a main component and 5 to 45% by mass of an α-olefin as a copolymerization monomer, specifically one produced using a metallocene catalyst.

[0064] As the α-olefin, ethylene, propylene, 1-butene, 1-hexene, 1-octene, etc., having 2 to 10 carbon atoms can be used, and specific examples of the thermoplastic elastomer include ethylene-propylene copolymer elastomer, ethylene-butene copolymer elastomer, ethylene-octene copolymer elastomer, propylene-ethylene copolymer elastomer, propylene-butene copolymer elastomer, propylene-hexene copolymer elastomer, propylene-octene copolymer elastomer, etc. In particular, it is preferable to additionally add an elastomer containing propylene as a main component in terms of heat seal strength and low-temperature impact resistance.

[0065] The MFR of the thermoplastic elastomer is preferably in the range of 0.5 to 10 g / 10 min at 190°C and a load of 21.18 N for an elastomer mainly composed of ethylene, and in the range of 0.5 to 10 g / 10 min at 230°C and a load of 21.18 N for an elastomer mainly composed of propylene, from the viewpoints of miscibility with the polypropylene-based resin that is the main component of the sealing layer and film formation stability.

[0066] The polypropylene-based non-oriented film of the present invention may contain, within the scope of the object of the present invention, antioxidants, heat stabilizers, neutralizing agents, antistatic agents, hydrochloric acid absorbents, antiblocking agents, lubricants, etc. These additives may be used alone or in combination of two or more.

[0067] Specific examples of the antioxidant include hindered phenols such as 2,6-di-t-butylphenol (BHT), n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate ("Irganox" 1076, "Sumilizer" BP-76), tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Irganox" 1010, "Sumilizer" BP-101), and tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate ("Irganox" 3114, Mark AO-20).

[0068] Examples of phosphite (phosphorus) antioxidants include tris(2,4-di-t-butylphenyl)phosphite ("Irgafos" 168, Mark 2112), tetrakis(2,4-di-t-butylphenyl)-4-4'-biphenylene-diphosphonite ("Sandstab" P-EPQ), bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite ("Ultranox" 626, Mark PEP-24G), and distearyl pentaerythritol diphosphite (Mark PEP-8).

[0069] Among these, 6-[3-(3-t-butyl-4-hydroxy-5-methyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]-dioxaphosphepine ("Sumilizer" GP) and 2[1-2-hydroxy-3,5-di-t-pentylphenyl]ethyl]-4,6-di-t-pentylphenyl acrylate ("Sumilizer" GS), which combine the functions of both hindered phenols and phosphites, are preferred, and the combined use of these two is particularly preferred because it is effective in suppressing resin decomposition during film formation and contributes to achieving both good heat seal strength and good blocking resistance.

[0070] The amount of antioxidant to be added may be set appropriately within the range of 100 to 10,000 ppm, depending on the type of antioxidant used.

[0071] As the neutralizing agent, hydrotalcite compounds, calcium hydroxide, etc. are preferred for reducing smoke generation during film formation.

[0072] The polypropylene-based non-oriented film of the present invention may contain a fatty acid amide-based lubricant in an amount of 100 to 1,000 ppm relative to the total amount of resin composition, as long as the amount does not deteriorate the film-forming property due to contamination in the film-forming process caused by heat scattering during melt extrusion or reduce the heat-sealing strength. If the amount of fatty acid amide-based lubricant added is less than 100 ppm, the slipperiness may be deteriorated, whereas if it exceeds 1,000 ppm, the amount of heat scattering during melt extrusion increases, causing contamination in the film-forming process, resulting in deterioration of the film-forming property and a decrease in the heat-sealing strength.

[0073] Examples of the fatty acid amide lubricants include oleic acid amide, erucic acid amide, stearic acid amide, palmitic acid amide, and behenic acid amide.

[0074] Examples of methods for obtaining the polypropylene-based non-oriented film of the present invention include a method in which the resin and additive composition are melted and kneaded in a single-screw extruder, a twin-screw co-rotating extruder, or a twin-screw counter-rotating extruder, and then extruded from a T-type nozzle onto a cooling drum and cooled to solidify, and a method in which the melt-extruded composition is laminated on a heat-resistant substrate. In the present invention, the method in which the resin and additive composition are extruded from a T-type nozzle onto a cooling drum and then cooled to solidify is preferred because it provides higher heat seal strength.

[0075] The thickness of the polypropylene-based non-oriented film is preferably 20 μm or more and 150 μm or less, and the thickness ratio of the base layer to the seal layer is preferably 9:1 to 3:1. In this case, stable film-forming properties, low-temperature impact resistance, and heat-sealing strength of the film can be obtained, and bag-forming properties can also be maintained.

[0076] In the laminate of the present invention, in which the polypropylene-based unoriented film is laminated with a heat-resistant substrate having a melting point of 160° C. or higher, the heat seal strength at 170° C. is preferably 23 N / 15 mm or higher. If the heat seal strength at 170° C. is less than 23 N / 15 mm, when the laminate is used as a retort packaging material, the heat seal strength may be reduced by a heat treatment at 130° C. or higher, which may result in scattering or leakage of the contents.

[0077] The heat-resistant substrate having a melting point of 160°C or higher is preferably at least one selected from the group consisting of biaxially oriented polyamide film, biaxially oriented polyethylene terephthalate film, biaxially oriented polypropylene film, biaxially oriented polybutylene terephthalate, biaxially oriented polyester / polyamide hybrid film, uniaxially oriented polyamide film, uniaxially oriented polyethylene terephthalate film, uniaxially oriented polypropylene film, and uniaxially oriented polybutylene terephthalate; films obtained by applying at least one gas barrier layer selected from the group consisting of metal vapor deposition, inorganic vapor deposition, transparent metal oxide vapor deposition, and gas barrier resin to these films; and at least one substrate layer selected from the group consisting of synthetic paper and aluminum foil. Of the monomaterials, it is preferable to use a biaxially oriented polypropylene film or uniaxially oriented polypropylene film as the substrate.

[0078] The method for laminating the heat-resistant substrate and the polypropylene-based unstretched film of the present invention is not particularly limited, but a dry lamination method is preferred from the viewpoint of productivity.

[0079] The adhesive for dry lamination is not particularly limited, but examples include two-component reactive aromatic adhesives composed of a first component consisting of one or more polyols selected from the group consisting of polyurethane polyols, polyester polyols, and polyether polyols, and a second component (curing agent) consisting of an isocyanate; two-component reactive aliphatic adhesives; polyurethane adhesives; acrylic adhesives; epoxy adhesives; polyolefin adhesives; elastomer adhesives; and fluorine-based adhesives.

[0080] The thickness of the adhesive layer is preferably 0.5 to 5 μm, more preferably 0.5 to 3 μm. If the thickness of the adhesive layer is 0.5 μm or more, it becomes easy to control the film thickness, and if it is 5 μm or less, it becomes easy to shorten the drying time and reduce production costs while imparting sufficient adhesive strength.

[0081] The laminate can be used by processing it into a flat bag (flat pouch), a standing pouch, etc., with the polypropylene-based non-oriented film of the present invention as the inner surface of the bag to be heat-sealed.

[0082] The present invention will be described in detail below with reference to examples, but the scope of the present invention is not limited thereto. In addition, the measurement values ​​of each evaluation item in the detailed description of the present invention and the examples were measured by the following methods.

[0083] (1) Melting Temperature Peak Using a differential scanning calorimeter (DSC-60 manufactured by Shimadzu Corporation), the temperature was raised from 20°C at a rate of 10°C / min up to 250°C, and the highest peak temperature among the melting peaks when heated was taken as the melting temperature peak.

[0084] (2) Density of polyethylene (unit: g / cm 3 ) Measurement was carried out in accordance with Method A (underwater displacement method) of JIS-K7112:1999.

[0085] (3) Melt flow rate (MFR) In accordance with JIS K7210:1999, the propylene random copolymer, propylene-ethylene block copolymer, and propylene-α-olefin copolymer elastomer were measured at a temperature of 230°C, and the polyethylene resin and ethylene-α-olefin copolymer elastomer were measured at a temperature of 190°C, each under a load of 21.18 N.

[0086] (4) Content of 20°C xylene soluble portion CXS and insoluble portion CXIS 5 g of film or polymer was completely dissolved in 500 ml of boiling xylene (grade 1 manufactured by Kanto Chemical Co., Ltd.), then the temperature was lowered to 20°C and left to stand for 4 hours or more. The precipitate and the solution were then filtered to separate the xylene soluble portion and the xylene insoluble portion. The mass of the xylene insoluble portion was determined by drying the precipitate at 70°C under reduced pressure, and then measuring the mass at 23°C to determine the content (mass%) of the xylene insoluble portion CXS. The filtrate was evaporated to dryness, dried at 70°C under reduced pressure, and then the mass was measured to determine the content (mass%) of the xylene soluble portion CXS.

[0087] (5) Intrinsic Viscosity of Xylene-Insoluble Portion CXIS and Xylene-Soluble Portion CXS of Film and Polymer Using the samples separated by the above method, measurements were carried out in tetralin at 135° C. using an Ubbelohde viscometer.

[0088] (6) Ethylene Content: Ethylene content was determined by infrared spectroscopy according to the method described in Polymer Analysis Handbook (published by Kinokuniya Shoten, 1995), p. 616 et seq.

[0089] The ethylene content (mass %) in the 20°C xylene soluble portion of the propylene-ethylene block copolymer (a) was calculated using the following formula: (Ethylene content in 20°C xylene soluble portion) = {(Ethylene content in (a)) - (Ethylene content in 20°C xylene insoluble portion) × (Content of insoluble portion in (a))} × 100 / (Content of 20°C xylene soluble portion in (a)) (unit of content: mass %).

[0090] (7) Density of polyethylene (unit: g / cm 3 ) Measurement was carried out in accordance with Method A (underwater displacement method) of JIS-K7112:1999.

[0091] (8) Film surface average roughness Ra, and peak count of 0.3 μm or more in the peak count number RPc based on roughness curve elements Using a fully automatic microprofile measuring instrument (SURFCORDER ET4000A) manufactured by Kosaka Laboratory Co., Ltd., the film surface was measured in the direction perpendicular to the film flow direction (TD) according to the measurement method specified in JIS B-0601:1982 under the following conditions to determine the film surface average roughness Ra and the peak count of 0.3 μm or more in the peak count number RPc based on roughness curve elements. Measurement length: 2 mm, Y direction measurement length: 10 mm, Y direction measurement pitch: 0.1 mm, number of scans: 100.

[0092] (9) Film Thickness and Thickness Configuration The film thickness was measured at 10 random locations on the film using a dial gauge in accordance with JIS K7130 (1992) A-2 method, and the average value was taken as the film thickness.

[0093] (10) Temperature at which heat seal strength is 3 N / 15 mm or more According to JIS Z1713:1999, samples of polypropylene-based unoriented films were overlapped with each other on their heat-sealed surfaces and heat-sealed at different temperatures, and the heat seal strength was measured at a peeling speed of 300 mm / min using a Tensilon made by Orientec Co., Ltd. A heat seal initiation temperature of 150°C or less at which the heat seal strength at 23°C was 3 N / 15 mm or more according to this measurement method was considered to have good low-temperature heat sealability.

[0094] (11) Heat seal strength at 170°C A heat-resistant substrate layer and a polypropylene-based unstretched film were bonded together by a normal dry lamination method using an aliphatic ester-based adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and a laminate was produced by aging at 40°C for 3 days. The polypropylene-based unstretched films of the laminate were overlapped and heat-sealed at 170°C, and a sample was measured for heat seal strength at a peel rate of 300 mm / min using a Tensilon manufactured by Orientec Co., Ltd., and a value of 23 N / 15 mm or more was deemed suitable for retort packaging.

[0095] (12) Blocking shear strength at 130°C A film sample of 30 mm wide and 100 mm long was prepared from a polypropylene-based unstretched film, and the sealing layers were overlapped in an area of ​​30 mm x 40 mm, and a load of 10 g was placed on the film. After heating for 30 minutes in an oven at 130°C, the film was left in an atmosphere of 23°C and 65% humidity for 30 minutes or more, and then the shear peel strength was measured at a pulling rate of 300 mm / min using a Tensilon manufactured by Orientec Co., Ltd. The shear peel strength measured by this measurement method was 15 N / 12 cm 2 If the temperature was below this, the high-temperature blocking resistance was judged to be good.

[0096] (13) Bag-making speed A heat-resistant substrate layer and a polypropylene-based unstretched film were bonded together by a conventional dry lamination method using an aliphatic ester adhesive (Takelac A385 / Takenate A50, adhesive layer thickness 2.5 μm, manufactured by Mitsui Chemicals, Inc.), and aged for 3 days at 40 ° C. to produce a long laminate. Next, using the laminate, depending on the heat-resistant substrate, a bag-making machine was used under the conditions of a bottom seal temperature (bottom part) of 140 ° C. or higher and 230 ° C. or lower, a vertical seal temperature of 130 ° C. or higher and 230 ° C. or lower, and a top seal temperature (sealed part after filling with contents) of 130 ° C. or higher and 230 ° C. or lower. The number of packaging bags filled with 200 g of saline solution as contents that could be produced per minute was defined as the bag-making speed spm (shots per minute), and a speed of 40 spm or higher was evaluated as good high-speed bag-making performance.

[0097] (14) Bag Breakage Retention Rate (Low-Temperature Impact Resistance) A 60 μm thick polypropylene-based unoriented film was bonded to one side of a heat-resistant substrate layer of a 15 μm thick biaxially oriented polyamide film by a conventional dry lamination method using an aliphatic ester-based adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and the laminate was aged at 40° C. for 3 days to prepare a laminate.

[0098] Using this laminate, a three-sided bag measuring 150 mm long x 130 mm wide was heat-sealed on three sides at 210°C, filled with 160 g of saline solution, and then sealed using an impulse sealer at a setting of 210°C to obtain a packaging bag. The resulting packaging bag was subjected to 10 drops of a 1 kg load from a height of 20 cm (base shape: 152 mm x 152 mm) in a 5°C atmosphere using a DuPont drop impact tester, and the bag breakage retention rate was measured. Laminates with a bag breakage retention rate of 50% or more without liquid leakage were evaluated as having good low-temperature impact resistance, while laminates with a bag breakage retention rate of less than 50% due to bag rupture or liquid leakage from the seal were evaluated as having poor low-temperature impact resistance.

[0099] (15) Heat seal strength in an atmosphere of 100°C (steam permeability when heated in a microwave oven) Using the packaging bag obtained in (14) above, the heat seal strength was measured at a peel rate of 300 mm / min in an atmosphere of 100°C using a Tensilon manufactured by Orientec Co., Ltd. A strength of 30 N / 15 mm or less was evaluated as good steam permeability when heated in a microwave oven, and a strength of 30 N / 15 mm or more was evaluated as poor steam permeability.

[0100] The compositions of the various raw materials used in the present invention are described below. Table 1 also shows the properties of the polypropylene-based unstretched films and laminates produced from the raw material formulations.

[0101] (1) Propylene-ethylene block copolymer (a1) MFR: 2.1 g / 10 min (230°C) CXS content: 20 mass% [η]CXIS: 1.8 dl / g [η]CXS: 3.2 dl / g Melting temperature peak: 163°C (2) Propylene-ethylene block copolymer (a2) MFR: 2.7 g / 10 min (230°C) CXS content: 27 mass% [η]CXIS: 1.9 dl / g [η]CXS: 3.0 dl / g Melting temperature peak: 155°C (3) Propylene-based random copolymer (a3) ​​Ethylene-propylene random copolymer.

[0102] Ethylene content: 4 mass% MFR: 3.0 g / 10 min (230 ° C) Melting temperature peak: 142 ° C. (4) Propylene-based random copolymer (a4) Ethylene-propylene random copolymer Ethylene content: 6 mass% MFR: 3.0 g / 10 min (230 ° C) Melting temperature peak: 135 ° C. (5) Propylene-based random copolymer (a5) Ethylene-propylene-butene random copolymer Propylene content: 90.7 mass%, ethylene content: 2.5 mass%, butene content: 6.8 mass% MFR: 3.5 g / 10 min (230 ° C) Melting temperature peak: 132 ° C. (6) Polyethylene (b1) 1-octene copolymerized linear low-density polyethylene MFR: 0.8 g / 10 min (190 ° C) Density: 0.925 g / cm 3Melting temperature peak: 125°C (7) Polyethylene (b2) High density polyethylene MFR: 1.1g / 10min (190°C) Density: 0.950g / cm 3 Melting temperature peak: 132°C (8) Polyethylene (b3) High-pressure low-density polyethylene MFR: 7.0 g / 10 min (190°C) Density: 0.905 g / cm 3 Peak melting temperature: 106°C (9) Ethylene-butene copolymer elastomer (c1) "TAFMER" (registered trademark) manufactured by Mitsui Chemicals, Inc. MFR: 3.6 g / 10 min (190°C) Peak melting temperature: 66°C (10) Propylene-butene copolymer elastomer (c2) "TAFMER" (registered trademark) manufactured by Mitsui Chemicals, Inc. MFR: 7 g / 10 min (230°C) Peak melting temperature: 75°C.

[0103] [Example 1] The composition of a polypropylene-based unstretched film was prepared by using 67.6% by mass of an ethylene-propylene random copolymer (a3) ​​as a propylene-based random copolymer, which had been thoroughly cooled with liquid nitrogen and then pulverized using an impeller mill to form a powder, 30% by mass of a linear low-density polyethylene (b1), and 2.4% by mass of Perhexa 25B (manufactured by NOF Corporation, chemical name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) as a peroxide.

[0104] To a total of 100 parts by mass of the mixed composition, 0.05 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101) and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) were added, and the mixture was mixed for 3 minutes using a Henschel mixer.

[0105] The mixture was then fed into a twin-screw extruder whose temperature was controlled to 260°C and melt-kneaded, and then extruded from a T-die at 250°C at 60 m / min. The mixture was brought into contact with a cooling roll at 45°C to be cooled and solidified, and one side of the mixture was subjected to a corona discharge treatment to obtain a 60 μm-thick unstretched polypropylene film.

[0106] The unstretched polypropylene film was laminated to a 12 μm thick transparent vapor-deposited biaxially oriented polyethylene terephthalate film (Barrierox SBR2 (registered trademark)) as a heat-resistant substrate by a conventional dry lamination method using an aliphatic ester adhesive (Takelac A385 / Takenate A50 manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and then aged at 40° C. for 3 days to obtain a laminate.

[0107] Using the laminate, the heat seal strength at 170°C was confirmed, and bag formability was confirmed by evaluating the number of packaging bags filled with 200 g of saline solution using a bag making machine at a bottom seal temperature (bottom part) of 210°C, a vertical seal temperature of 210°C, and a top seal temperature (sealed part after filling with contents) of 210°C, as the bag making speed (spm) (shots per minute). The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 1.

[0108] The polypropylene-based unstretched film has a melting temperature peak of 142°C, an average film surface roughness Ra of 0.29 µm on the heat seal surface, and a peak count of 2690 peaks / 10 mm of 0.3 µm or more. 2 The peak count is very high, and when the heat seal surfaces are overlapped and heat sealed, the heat seal strength reaches 3N / 15mm or more at 144°C, which is excellent in low-temperature heat sealability, and the blocking shear strength at 130°C is 2.4N / 12cm. 2 The film had excellent high-temperature blocking resistance, a high heat seal strength of 60 N / 15 mm at 170°C, making it suitable for retort packaging, and a bag-making speed of 45 spm, providing excellent bag-making properties, satisfying all of the required properties of the present invention.

[0109] Example 2 An unstretched polypropylene film was obtained in the same manner as in Example 1, except that the ethylene-propylene random copolymer of the propylene random copolymer (a3) ​​in Example 1 was replaced with an ethylene-propylene random copolymer of the propylene random copolymer (a4). Furthermore, a laminate was obtained in the same manner as in Example 1, except that a 20 μm thick biaxially oriented polypropylene film (Pylen Film-OT (registered trademark)) P2171 commercially available from Toyobo Co., Ltd. was used as the heat-resistant substrate and biaxially oriented polypropylene film. The heat seal strength at 170°C was confirmed using the laminate, and bag formability was evaluated in the same manner as in Example 1, with a bottom seal temperature (bottom edge) of 145°C, a vertical seal temperature of 145°C, and a top seal temperature (sealed portion after filling with contents) of 150°C. The properties of the obtained unstretched polypropylene film and the properties of the laminate with the heat-resistant substrate are shown in Table 1.

[0110] [Example 3] A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the propylene-based random copolymer (a3) ​​was changed to 87.6% by mass of an ethylene-propylene random copolymer and the polyethylene (b1) was changed to 10% by mass of a linear low-density polyethylene. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 1.

[0111] Example 4 A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the mixed composition in Example 1 was changed to 89 mass% of ethylene-propylene random copolymer as propylene-based random copolymer (a3), 10 mass% of linear low-density polyethylene as polyethylene (b1), and 1 mass% of Perhexa 25B (manufactured by NOF Corporation, chemical name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) as a peroxide, totaling 100 mass parts. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 1.

[0112] Example 5 A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the mixed composition in Example 1 was changed to 67.6 mass% of an ethylene-propylene random copolymer (a3), 20 mass% of a linear low-density polyethylene (b1), 10 mass% of an ethylene-butene copolymer elastomer (c1), and 2.4 mass% of Perhexa 25B (manufactured by NOF Corporation, chemical name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) as a peroxide, totaling 100 mass parts. Furthermore, a laminate was obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 1.

[0113] [Example 6] A composition of a polypropylene-based unstretched film was prepared by adding 0.05 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101) and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) to 100 parts by mass of a mixed resin of 70% by mass of an ethylene-propylene random copolymer (a3), 20% by mass of a linear low-density polyethylene (b1), and 10% by mass of an ethylene-butene copolymer elastomer (c1), and mixing the mixture for 3 minutes using a Henschel mixer.

[0114] The mixture is then fed into a twin-screw extruder whose temperature is controlled at 260°C, melted and kneaded, and extruded. A stainless steel core having a heat transfer medium flow path is coated with HTV silicone rubber to a thickness of 8 mm, and then covered with a PFA heat-shrinkable tube having a thickness of 0.2 mm. The PFA surface is buffed and then sprayed with steel spheres to form a surface with a depth of 1.0 μm and a number of recesses of 10 mm. 2 Using an embossing rubber roller with 1,400 rollers per roller, the film was extruded between a mirror-finished metal roll and the embossing rubber roller to obtain a polypropylene-based non-stretched film with a thickness of 60 μm. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based non-stretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 1.

[0115] [Comparative Example 1] The composition of the polypropylene-based unstretched film was 100 parts by mass of a mixed resin consisting of 70% by mass of an ethylene-propylene random copolymer (propylene-based random copolymer (a3)), 20% by mass of a linear low-density polyethylene (polyethylene (b1)), and 10% by mass of an ethylene-butene copolymer elastomer (c1). The mixed resin contained 0.4 parts by mass of spherical silica having a particle size of 2 μm and tetrakis[methylene-3-(3,5-di-t- 0.05 parts by mass of (butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101) and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) were added, and the mixture was mixed for 3 minutes in a Henschel mixer. The mixture was then fed into a twin-screw extruder temperature-controlled at 260°C and melt-kneaded. The extruded film was then extruded at 60 m / min through a T-die at 250°C and cooled and solidified by contacting it with a cooling roll at 45°C. One side of the film was then corona discharge-treated to obtain a 60 μm-thick unstretched polypropylene film. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained unstretched polypropylene film and the properties of the laminate with the heat-resistant substrate are shown in Table 1.

[0116] The polypropylene-based non-stretched film has a melting temperature peak of 142°C, an average roughness Ra of the heat seal surface of 0.04µm, and a peak count of 0.3µm or more of 68 / 10mm. 2 Therefore, the blocking shear force at 130°C is 42N / 12cm 2 The bag-making speed was 35 spm, and the bag-making properties were poor.

[0117] [Comparative Example 2] A polypropylene-based non-oriented film was obtained in the same manner as in Example 1, except that the ethylene-propylene random copolymer of the propylene-based random copolymer (a3) ​​was changed to an ethylene-propylene-butene random copolymer of the propylene-based random copolymer (a5) in the composition of the polypropylene-based non-oriented film. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based non-oriented film and the properties of the laminate with the heat-resistant substrate are shown in Table 1.

[0118] The polypropylene-based non-stretched film has a peak melting temperature of 132°C, and therefore the blocking shear force at 130°C is 17 N / 12 cm 2 The product had poor high-temperature blocking resistance, a low heat seal strength of 20 N / 15 mm at 170°C, leakage of the contents occurred during retort treatment at 130°C, and the bag-making speed was 32 spm, indicating poor bag-making properties.

[0119] [Comparative Example 3] A polypropylene-based non-oriented film was obtained in the same manner as in Example 1, except that the linear low-density polyethylene (b1) was changed to a high-pressure low-density polyethylene (b3) in the composition of the polypropylene-based non-oriented film. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based non-oriented film and the properties of the laminate with the heat-resistant substrate are shown in Table 1.

[0120] The polypropylene-based non-stretched film has a low average roughness Ra of 0.08 μm, and the melting temperature of the mixed high-pressure low-density polyethylene is low at 106 ° C., so the blocking shear force at 130 ° C. is 25 N / 12 cm 2 The heat seal strength at 170°C was as low as 20 N / 15 mm, causing leakage of the contents during retort treatment at 130°C, and the bag-making speed was 37 spm, resulting in poor bag-making properties.

[0121] Comparative Example 4 A polypropylene-based non-oriented film was obtained in the same manner as in Example 1, except that the composition of the polypropylene-based non-oriented film was 100 parts by mass of a mixed resin of 85% by mass of an ethylene-propylene block copolymer of a propylene-based block copolymer (a1), 5% by mass of high-density polyethylene, and 10% by mass of an ethylene-butene copolymer elastomer (c1). A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based non-oriented film and the properties of the laminate with a heat-resistant substrate are shown in Table 1.

[0122] The polypropylene-based unstretched film had an average roughness Ra that satisfied the range specified in the present invention, but the peak count of 0.3 μm or more was below the range specified in the present invention, and the blocking shear force at 130° C. was 40 N / 12 cm 2 The melting temperature of the main component, an ethylene-propylene block copolymer, was as high as 163°C, and therefore the temperature at which the heat seal strength reached 3 N / 15 mm or more was as high as 170°C, resulting in poor low-temperature heat sealability. The heat seal strength at 170°C was as low as 4 N / 15 mm, and it was not possible to obtain a bag under the above bag-making conditions.

[0123] [Example 7] As the base layer composition of a polypropylene-based unstretched film, 100 parts by mass of a mixed resin of 50% by mass of a propylene-ethylene block copolymer (a1), 20% by mass of a propylene-ethylene random copolymer (a3), and 30% by mass of a linear low-density polyethylene as a polyethylene-based resin (b1) was used, and 500 ppm of "Sumilizer" GP and 750 ppm of "Sumilizer" GS were used as antioxidants. The mixture was mixed in a Henschel mixer for 3 minutes, and the mixture was supplied to a twin-screw extruder whose temperature was controlled to 260°C, and melt-kneaded.

[0124] The sealing layer composition was prepared by thoroughly cooling with liquid nitrogen and then pulverizing the mixture with an impeller mill to form a powder, using 57.5% by mass of a propylene-ethylene random copolymer (a3) ​​having a melting temperature peak of 142°C, 40% by mass of a linear low-density polyethylene (b1), and 2.5% by mass of Perhexa 25B (registered trademark) (manufactured by NOF Corporation, chemical name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) as a peroxide. To a total of 100 parts by mass of the mixed composition, 0.05 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101) and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) were added, and the mixture was mixed for 3 minutes in a Henschel mixer. The mixture was then fed into a twin-screw extruder controlled at 260°C and melt-kneaded to prepare master chips.

[0125] Next, 25% by mass of the propylene-ethylene random copolymer (a3) ​​was mixed with 75% by mass of the master chips, and the mixture was fed into a twin-screw extruder controlled at 260° C. and melt-kneaded.

[0126] Next, the melt-kneaded base layer resin and seal layer resin were extruded at a ratio of 6:1 from a multi-layer T-type two-layer die at 250°C and 60 m / min, and then brought into contact with a cooling roll at 45°C to cool and solidify.The base layer surface was then corona discharge treated to obtain a 60 μm thick polypropylene-based unstretched film.

[0127] The above-mentioned polypropylene-based unstretched film was bonded to a 15 μm-thick biaxially oriented polyamide film as a heat-resistant substrate by a conventional dry lamination method using an aliphatic ester-based adhesive (Takelac A385 / Takenate A50, manufactured by Mitsui Chemicals, Inc., adhesive layer thickness 2.5 μm), and then aged at 40° C. for 3 days to obtain a laminate.

[0128] Using the above laminate, the heat seal strength at 170°C was confirmed, and bag formability was confirmed by evaluating the number of packaging bags filled with 200 g of saline solution using a bag making machine at a bottom seal temperature (bottom part) of 210°C, a vertical seal temperature of 210°C, and a top seal temperature (sealed part after filling with contents) of 210°C, as the bag making speed (spm) (shots per minute). The properties of the obtained polypropylene-based unoriented film and the properties of the laminate with a heat-resistant substrate are shown in Table 2.

[0129] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0130] [Example 8] A polypropylene-based unstretched film and a laminate were obtained in the same manner as in Example 7, except that the base layer contained 60% by mass of propylene-ethylene block copolymer (a1), 20% by mass of propylene-ethylene random copolymer (a3), and 20% by mass of linear low-density polyethylene (b1). The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0131] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0132] Example 9 A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the propylene-ethylene block copolymer (a1) having a melting temperature peak of 162°C in the base layer in Example 7 was replaced with a propylene-ethylene block copolymer (a2) having a melting temperature peak of 155°C. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0133] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0134] [Example 10] A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that in Example 7, the propylene-ethylene random copolymer (a3) ​​having a peak melting temperature of 142°C of the seal layer was changed to a propylene-ethylene random copolymer (a4) having a peak melting temperature of 135°C. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0135] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0136] Example 11 A polypropylene-based non-oriented film was obtained in the same manner as in Example 1, except that in Example 7, the propylene-ethylene random copolymer (a3) ​​was changed to 87.5% by mass and the linear low-density polyethylene of the polyethylene-based resin (b1) was changed to 10% by mass in the seal layer. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based non-oriented film and the properties of the laminate with the heat-resistant substrate are shown in Table 2. The polypropylene-based non-oriented film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for retort packaging.

[0137] [Example 12] A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that in Example 7, the seal layer was changed to a mixed composition of 89 mass% propylene-ethylene random copolymer (a3), 10 mass% linear low-density polyethylene of the polyethylene-based resin (b1), and 1 mass% Perhexa 25B, totaling 100 parts by mass. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 2.

[0138] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0139] [Example 13] A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the seal layer in Example 7 was changed to a mixed composition of 77.5 mass% of propylene-ethylene random copolymer (a1), 15 mass% of linear low-density polyethylene as the polyethylene-based resin (b1), 5 mass% of ethylene-butene copolymer elastomer (c1), and 2.5 mass% of Perhexa 25B, totaling 100 parts by mass. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 2.

[0140] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0141] Example 14 The seal layer composition used in Example 7 was 60% by mass of a propylene-ethylene random copolymer (a3) ​​and 40% by mass of a linear low-density polyethylene (b1). 500 ppm of "Sumilizer" GP and 750 ppm of "Sumilizer" GS were added as antioxidants to a total of 100 parts by mass of the mixed composition in a Henschel mixer for 3 minutes, and the mixture was fed to a twin-screw extruder controlled at 260°C for melt-kneading.

[0142] Next, a stainless steel core metal having a heat transfer medium flow path is coated with HTV silicone rubber to a thickness of 8 mm, and then covered with a PFA heat-shrinkable tube having a thickness of 0.2 mm. After buffing the surface of the PFA, steel spheres are sprayed onto the PFA to form a surface with a depth of 1.0 μm and a number of recesses of 10 mm. 2 The film was extruded at 50 m / min through a multilayer T-die between an embossing rubber roller (1,400 per roller) and a mirror-finished metal roll, with the sealing layer facing the rubber roll, to obtain a 60 μm-thick unstretched polypropylene film. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained unstretched polypropylene film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0143] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0144] [Example 15] In Example 7, the base layer composition was 100 parts by mass of a mixed resin containing 72% by mass of a propylene-ethylene block copolymer (a1), 18% by mass of a linear low-density polyethylene of a polyethylene-based resin (b1), and 10% by mass of a propylene-butene copolymer elastomer, and 500 ppm of "Sumilizer" GP and 750 ppm of "Sumilizer" GS were mixed in a Henschel mixer for 3 minutes, and the mixture was supplied to a twin-screw extruder controlled at a temperature of 260°C and melt-kneaded.

[0145] The sealing layer composition was prepared by thoroughly cooling with liquid nitrogen and then pulverizing the mixture with an impeller mill to form a powder, using 87.5% by mass of a propylene-ethylene random copolymer (a3) ​​having a peak melting temperature of 142°C, 10% by mass of a high-density polyethylene (b2), and 2.5% by mass of Perhexa 25B (registered trademark) (manufactured by NOF Corporation, chemical name: 2,5-dimethyl-2,5-di(t-butylperoxy)hexane) as a peroxide. To a total of 100 parts by mass of the mixed composition, 0.05 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101) and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) were added, and the mixture was mixed for 3 minutes in a Henschel mixer. The mixture was then fed into a twin-screw extruder controlled at 260°C and melt-kneaded to prepare master chips.

[0146] Next, 70% by mass of the master chips were mixed with 20% by mass of a propylene-ethylene block copolymer and 10% by mass of a propylene-butene copolymer elastomer, and the mixture was fed into a twin-screw extruder controlled at 260°C for melt-kneading.

[0147] Next, the melt-kneaded base layer resin and seal layer resin were extruded at a ratio of 6:1 from a multi-layer T-type two-layer die at 250°C and 60 m / min, and then brought into contact with a cooling roll at 45°C to cool and solidify.The base layer surface was then corona discharge treated to obtain a 60 μm thick polypropylene-based unstretched film.

[0148] A laminate was obtained with the above-mentioned polypropylene-based unstretched film and a biaxially oriented polyamide film having a thickness of 15 μm in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0149] The polypropylene-based unstretched film had excellent low-temperature heat sealing properties, excellent high-temperature blocking resistance, and, as a laminate, had high heat sealing strength at 170°C, excellent low-temperature impact resistance, excellent bag formability, and excellent steam permeability when heated in a microwave oven, satisfying all of the required properties of the present invention for use in retort packaging.

[0150] Comparative Example 5 A polypropylene-based unstretched film was obtained in the same manner as in Example 7, except that the propylene-ethylene block copolymer (a1) was 40% by mass and the propylene-ethylene random copolymer (a3) ​​was 30% by mass in the base layer. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0151] The above-mentioned polypropylene-based unstretched film has a low content of propylene-ethylene block copolymer in the base layer, so that some bags may leak when heat-treated at 130°C, and also has poor low-temperature impact resistance.

[0152] Comparative Example 6 A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that in Example 7, the base layer was made of a mixed resin of 70 mass% of propylene-ethylene random copolymer (a3) ​​and 30 mass% of linear low-density polyethylene (b1), a polyethylene-based resin. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0153] The above-mentioned polypropylene-based non-oriented film has a low melting temperature peak of the base layer, so that the heat during bag making causes deformation of the bag product, which reduces the bag making speed and results in a low bag break retention rate.

[0154] [Comparative Example 7] In Example 7, for the seal layer, 80% by mass of the ethylene-propylene random copolymer (a5) and 20% by mass of the linear low-density polyethylene (b1) were mixed with 100 parts by mass of the total resin mixture, and 0.4 parts by mass of spherical silica having a particle size of 2 μm, 0.05 parts by mass of tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane ("Sumilizer" BP-101), and 0.01 parts by mass of Irganox 1076 (manufactured by Ciba Specialty Chemicals) were added as inorganic particles to the mixture. The mixture was mixed for 3 minutes using a Henschel mixer, and then fed to a twin-screw extruder adjusted to a temperature of 260 ° C. for melt-kneading. The mixture was then extruded from a T-die at 250 ° C. at 60 m / min and cooled and solidified by contacting with a 45 ° C. cooling roll. One side of the film was then subjected to a corona discharge treatment to obtain a 60 μm thick unstretched polypropylene film. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained unstretched polypropylene film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0155] The polypropylene-based non-stretched film has a seal layer with a melting temperature peak of 150°C, an average roughness Ra of 0.04µm, and a peak count of 0.3µm or more of 68 / 10mm. 2 Therefore, the blocking shear force at 130°C is 42N / 12cm 2 The bag-making speed was 35 spm, which meant poor bag-making properties, and the heat-seal strength in an atmosphere of 100°C was high, resulting in poor steam permeability when heated in a microwave oven.

[0156] Comparative Example 8 A polypropylene-based unstretched film was obtained in the same manner as in Example 7, except that the propylene-ethylene random copolymer (a3) ​​having a melting temperature peak of 142°C in the seal layer was changed to an ethylene-propylene-butene random copolymer, i.e., a propylene-ethylene random copolymer (a6) having a melting temperature peak of 132°C. A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with a heat-resistant substrate are shown in Table 2.

[0157] The polypropylene-based non-stretched film has a sealing layer with a peak melting temperature of 132°C, and therefore has a blocking shear force of 17 N / 12 cm at 130°C. 2 The laminate had poor high-temperature blocking resistance, and the heat seal strength at 170°C was low at 20 N / 15 mm. When the produced bag was retorted at 130°C, leakage of the contents occurred, and the bag production speed was 32 spm, indicating poor bag production properties.

[0158] Comparative Example 9 A polypropylene-based unstretched film was obtained in the same manner as in Example 7, except that the linear low-density polyethylene of the polyethylene-based resin (b1) in the seal layer was changed to a high-pressure low-density polyethylene of the polyethylene-based resin (b3). A laminate was also obtained in the same manner as in Example 1. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0159] The polypropylene-based non-oriented film has a low average roughness Ra of 0.08 μm for the seal layer, and a low melting temperature of 106° C. for the mixed high-pressure low-density polyethylene, so that the blocking shear force at 130° C. is 25 N / 12 cm 2 The laminate had a low heat seal strength of 20 N / 15 mm at 170°C, and the contents leaked during retort treatment at 130°C in the produced bags. The bag production speed was 37 spm, which indicated poor bag production properties.

[0160] Comparative Example 10 A polypropylene-based unstretched film was obtained in the same manner as in Example 1, except that the seal layer in Example 7 contained 85 mass% of ethylene-propylene block copolymer (a1), 5 mass% of high-density polyethylene, and 10 mass% of ethylene-butene copolymer elastomer (c1), with a total mixed resin amount of 100 mass parts. A laminate was also obtained in the same manner as in Example 7. The properties of the obtained polypropylene-based unstretched film and the properties of the laminate with the heat-resistant substrate are shown in Table 2.

[0161] The above polypropylene-based unoriented film satisfied the ranges specified in the present invention for the average roughness Ra of the seal layer and the peak count of 0.3 μm or more. However, because the melting temperature was as high as 162°C, the temperature at which the heat seal strength reached 3 N / 15 mm or more was as high as 162°C, resulting in poor low-temperature heat sealability. The heat seal strength of the laminate at 170°C was as low as 4 N / 15 mm, and it was not possible to obtain a bag product under the above bag-making conditions.

[0162]

[0163]

[0164] The present invention can provide a polypropylene-based unstretched film and a laminate using the same, which can be used as a packaging bag for retort food packaging with a reduced number of layers in consideration of the environment, and which has excellent low-temperature heat sealing properties, high-temperature blocking resistance, and excellent bag-making processability, and which has high heat sealing strength at 170°C as a laminate, excellent low-temperature impact resistance, excellent steam permeability when heated in a microwave oven, and excellent suitability for retort.

Claims

1. The film is mainly composed of a propylene-based random copolymer having a melting temperature peak of 135°C to 145°C, and has a film surface average roughness Ra of 0.1 μm or more and a peak count of 0.3 μm or more per 10 mm on at least one side. 2 The surface of the polypropylene-based non-oriented film that is the heat seal surface is a surface that is the heat seal surface.

2. The blocking shear force between the heat-sealed surfaces at 130°C is 15N / 12cm 2 The polypropylene-based non-oriented film according to claim 1, wherein:

3. It is made up of two layers, a base layer and a seal layer, the base layer contains 50% by mass or more of a propylene-ethylene block copolymer and has a melting temperature peak of 150°C or higher, the seal layer has a melting temperature peak in the range of 135°C to 145°C, the average surface roughness Ra of the seal layer surface is 0.1 μm or more, and the peak count of 0.3 μm or more is 100 / 10 mm 2 A non-stretched polypropylene film having the above surface as a heat seal surface.

4. A polypropylene-based non-oriented film according to claim 1 or 3, in which, when the heat seal surfaces are overlapped and heat sealed, the heat seal initiation temperature at which the heat seal strength becomes 3 N / 15 mm or more is 150°C or less.

5. The polypropylene-based non-oriented film according to claim 1, having a film thickness of 20 μm or more and 150 μm or less.

6. The polypropylene-based non-oriented film according to claim 3, wherein the film thickness is 20 μm or more and 150 μm or less, and the thickness ratio of the base layer to the seal layer is 9:1 to 3:

1.

7. A laminate comprising the polypropylene-based non-oriented film according to claim 1 or 3 and a heat-resistant substrate having a melting point of 160°C or higher, the heat seal strength at 170°C being 23 N / 15 mm or higher.

8. The laminate according to claim 7, wherein the heat-resistant substrate is at least one selected from the group consisting of any one of biaxially oriented polyamide film, biaxially oriented polyethylene terephthalate film, biaxially oriented polypropylene film, biaxially oriented polybutylene terephthalate film, biaxially oriented polyester / polyamide hybrid film, uniaxially oriented polyamide film, uniaxially oriented polyethylene terephthalate film, uniaxially oriented polypropylene film, and uniaxially oriented polybutylene terephthalate film; any one of these films subjected to metal vapor deposition, inorganic vapor deposition, transparent metal oxide vapor deposition, or gas barrier resin; synthetic paper; and aluminum foil.

Citation Information

Patent Citations

  • Heat-sealable matte film

    JP1993329992A

  • Sealant composition and its use

    JP2002294216A

  • Polypropylene resin composition, and film produced thereby

    JP2012236973A

  • Polypropylene resin composition for rough surface film, and film

    JP2017145299A

  • Sealant film for power storage device exterior material and power storage device exterior material using the same

    JP2024057587A

Cited By

  • Food packaging film and food packaging bag

    WO2025164501A1