Prepreg, method for manufacturing prepreg, and fiber-reinforced composite material
The prepreg manufacturing method involving controlled tension and relaxation of carbon fibers within a specific fiber basis weight range and impregnation process addresses the issue of fiber meandering, enhancing the strength of molded articles by ensuring a uniform prepreg surface.
Patent Information
- Application Number
- PCT/JP2024/022428
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-20
- Filing Date
- 2024-06-20
- Publication Date
- 2024-12-26
AI Technical Summary
Prepregs with uneven thickness can lead to fiber meandering during lamination, resulting in a decrease in the strength of molded articles, particularly noticeable in lightweight prepregs with a fiber basis weight of 20 to 40 g/m².
A prepreg with carbon fibers impregnated in a matrix resin composition, where the fiber basis weight is between 20 to 40 g/m², and the waviness period has an average value of 9 mm or more and a standard deviation of 6 mm or less, is manufactured using a method involving repeated tension and relaxation of the fiber bundle, followed by lamination and impregnation with a resin sheet, to prevent fiber meandering.
This approach ensures a smooth and even prepreg surface, preventing fiber meandering during lamination and resulting in molded products with suppressed strength reduction.
Smart Images

Figure JP2024022428_26122024_PF_FP_ABST
Abstract
Description
Prepreg, method for producing prepreg, and fiber-reinforced composite material
[0001] The present invention primarily relates to a prepreg, a method for producing a prepreg, and a fiber-reinforced composite material.
[0002] Prepregs are known as molding materials for producing molded articles used in aircraft and automobiles. Unidirectional prepregs (UD prepregs), which are formed by impregnating a sheet-like fiber bundle in which the fibers are aligned in one direction with a resin, are a type of prepreg. They are obtained, for example, by spreading fiber bundles fed from a creel into a sheet, laminating a resin sheet on the sheet, and impregnating the sheet with a resin. Patent Document 1 discloses a method and device for spreading reinforcing fiber bundles, which uses a horizontal vibration imparting roll that vibrates in the width direction of the reinforcing fiber bundle and / or a vertical vibration imparting roll that vibrates in a direction intersecting the running direction of the reinforcing fiber bundle, and blows airflows onto both sides of the running direction of the reinforcing fiber bundle to separate and spread the reinforcing fiber bundle. This method and device enable the reinforcing fiber bundle to be spread more quickly and uniformly while preventing uneven spreading and single fiber breakage. Patent Document 2 discloses a method for spreading reinforcing fiber bundles in which a continuously running reinforcing fiber bundle is spread while applying periodic tension fluctuations to the reinforcing fiber bundles using a tension fluctuation means, and by adjusting the ratio between the speed Vr of the contact portion with the reinforcing fiber bundle in the tension fluctuation means and the running speed V of the reinforcing fiber bundle, it is possible to achieve uniform spreading with almost no fuzz generation, and to obtain a low basis weight prepreg with high surface smoothness. Patent Document 3 discloses a method for spreading carbon fiber bundles to be used in a production process of a carbon fiber unidirectional prepreg, in which the carbon fiber bundles are rubbed or brought into contact with a plurality of spreading members arranged so that the yarn path of the carbon fiber bundles is zigzag, and the carbon fiber bundles are spread by one of the plurality of spreading members vibrating in an up and down direction relative to the feeding direction of the carbon fiber bundle, and then the tension of the carbon fiber bundles when introduced into a laminating device is reduced from the tension during spreading, and the carbon fiber bundles are fed to a laminating process.
[0003] Japanese Patent No. 2005-163223, Japanese Patent Application Laid-Open No. 2001-288639, Japanese Patent Application Laid-Open No. 2014-005580
[0004] When prepregs with non-uniform thickness are laminated, the fibers in the laminated prepregs may meander in the thickly overlapping fiber bundle portions. The meandering fiber portions may become the starting point for fracture of the molded body, resulting in a decrease in strength. The inventors have found that this problem occurs when the fiber basis weight of the carbon fiber is, for example, 20 to 40 g / m 2 It has been found that this problem is particularly evident in thin prepregs having a low basis weight. One object of the present invention is to provide a prepreg that can suppress a decrease in strength when molded into a molded article.
[0005] The present invention includes the following embodiments [1] to
[17] . [1] A carbon fiber sheet in which unidirectionally aligned carbon fibers are impregnated with a matrix resin composition, and the fiber basis weight of the carbon fibers is 20 to 40 g / m 2 A prepreg having an average value Tave of the undulation period T measured by the following method of 9 mm or more and a standard deviation Tsdev of the undulation period T of 6 mm or less. <Measurement Method> A test piece is obtained by cutting the prepreg into a 100 mm x 50 mm piece so that the direction parallel to the surface direction and perpendicular to the fiber direction is 100 mm. The test piece is attached to a glass plate and integrated with the glass plate. A 47 mm x 11 mm prepreg image is obtained by scanning 47 mm in a direction parallel to the surface direction and perpendicular to the fiber direction (90 degree direction) using a microscope. The prepreg image is converted into a grayscale image using the following formula (1), and the average brightness value Xi in the fiber direction is calculated to obtain an average brightness value distribution X. The average brightness value distribution X is smoothed using a Gaussian filter to extract the waviness Y. The waviness average Yave expressed by the following formula (2) and the waviness period T expressed by the following formula (3) are calculated, and the average value Tave of the waviness periods T of the three test pieces expressed by the following formula (4) and the standard deviation Tsdev of the waviness periods T of the three test pieces expressed by the following formula (5) are calculated.
[0006]
[0007] R: Red value represented by RGB values, G: Green value represented by RGB values, B: Blue value represented by RGB values, Yi: waviness value of brightness value at the i-th pixel, n: number of waviness Yi data points, L: observed length in a direction perpendicular to the fiber direction of the prepreg image, C: number of intersections between waviness Y and the average Yave of waviness Y, Ti: period value of waviness Y of the i-th test piece. [2] The prepreg according to [1], wherein the content of the matrix resin composition in the prepreg is 20 to 50 mass% relative to the total mass of the prepreg. [3] The prepreg according to [2], wherein the prepreg contains carbon fibers having a fiber diameter of 5 to 15 μm. [4] The prepreg according to any one of [1] to [3], wherein the matrix resin composition contains a thermosetting resin. [5] The prepreg according to any one of [1] to [4], wherein the matrix resin composition contains a curing agent. [6] The prepreg according to [5], wherein the curing agent comprises dicyandiamide. [7] The prepreg according to any one of [1] to [6], wherein the matrix resin composition comprises a thermoplastic resin. [8] A fiber-reinforced composite material obtained by curing the prepreg according to any one of [1] to [7]. [9] A method for producing a prepreg, comprising the following steps: Spreading step: Spreading the fiber bundle by applying an external force that deforms the fiber bundle in a direction intersecting the fiber bundle conveying direction, thereby repeatedly creating tension and relaxation states in the fiber bundle. Tensioning step: Applying a tension of 150 g / weight or more to the spread fiber bundle. Laminating step: Laminating a resin sheet on the spread and tensioned fiber bundle to obtain a laminate. Impregnation step: Applying a load to the laminate to impregnate the fiber bundle with resin.
[10] The method for producing a prepreg according to [9], wherein in the tensioning step, a tension of 1.1 times or more is applied to the spread fiber bundle.
[11] The method for producing a prepreg according to
[10] , wherein the tension applying step applies tension to the fiber bundle between the spreading step and the laminating step using a tension applying device.
[12] The method for producing a prepreg according to
[11] , wherein the tension applied to the fiber bundle in the tension applying step is 3 g / spindle·K or more per 1,000 filaments.
[13] A method for producing a prepreg according to any one of [9] to
[12] , wherein the tension applied to the fiber bundle in the tensioning step is 45 g / spindle×m / g or more per g / m of fiber basis weight.
[14] A method for producing a prepreg according to any one of
[11] to
[13] , wherein the tensioning device includes an abrasion bar.
[15] A method for producing a prepreg according to any one of
[11] to
[14] , wherein the tensioning device includes a brake roll.
[16] A method for producing a prepreg according to any one of
[11] to
[15] , wherein a distance L from a point of contact between the fiber bundle and the tensioning device on the most downstream side to a point of contact between the fiber bundle and the resin sheet satisfies L<300 mm.
[17] A method for producing a prepreg according to any one of [9] to
[16] , wherein a load is applied by an impregnation roll at the point of contact between the fiber bundle and the resin sheet to start the impregnation.
[0008] According to one aspect of the present invention, fiber meandering during lamination of prepregs can be prevented, thereby suppressing a decrease in strength when a molded article is formed.
[0009] FIG. 1 is a schematic diagram showing a schematic configuration of a prepreg manufacturing apparatus according to an embodiment. FIG. 2 is a schematic diagram showing an example of a tensioning device. FIG. 3 is a schematic diagram showing an example of a tensioning device. FIG. 4 is a schematic diagram showing an example of a tensioning device. FIG. 5 is a prepreg image measured using a microscope. FIG. 6 is a diagram in which waviness Y is extracted from a prepreg image measured using a microscope. FIG. 7 is a diagram in which average brightness value distribution X is extracted from a prepreg image measured using a microscope.
[0010] The prepreg of this embodiment has unidirectionally aligned carbon fibers impregnated with a matrix resin composition, and has an average value Tave of the undulation period T of 9 mm or more and a standard deviation Tsdev of the undulation period T of 6 mm or less, as measured by the following method. [Measurement Method] A test piece is obtained by cutting the prepreg into a 100 mm x 50 mm piece so that the direction parallel to the surface direction and perpendicular to the fiber direction is 100 mm. The test piece is attached to a glass plate and integrated with the glass plate. A 47 mm x 11 mm prepreg image is obtained by scanning 47 mm in a direction parallel to the surface direction and perpendicular to the fiber direction (90-degree direction) using a microscope. The prepreg image is converted into a grayscale image using the following formula (1), and the average brightness value Xi in the fiber direction is calculated to obtain the average brightness value distribution X. The average brightness value distribution X is smoothed using a Gaussian filter to extract the waviness Y. The waviness average Yave expressed by the following formula (2) and the waviness period T expressed by the following formula (3) are calculated, and the average value Tave of the waviness periods T of the three test pieces expressed by the following formula (4) and the standard deviation Tsdev of the waviness periods T of the three test pieces expressed by the following formula (5) are calculated.
[0011]
[0012] R: Red value indicated by RGB values G: Green value indicated by RGB values B: Blue value indicated by RGB values Yi: Waviness value of brightness value at the i-th pixel n: Number of waviness Yi data L: Observation length in the direction perpendicular to the line axis of the prepreg image C: Number of intersections between waviness Y and the average Yave of waviness Y Ti: Period value of waviness Y of the i-th test piece
[0013] The color of the matrix resin composition used in the prepreg to be measured is preferably transparent, translucent, or milky translucent. Test specimens are obtained by cutting the prepreg into a roughly rectangular shape with a fiber direction of 50 mm, parallel to the surface direction and perpendicular to the fiber direction, i.e., a width direction of 100 mm. Test specimens obtained from prepregs equipped with a film and release paper can be attached to a glass plate by removing the film on the side opposite the release paper. When attaching the test specimen to the glass plate, the entire test specimen is pressed with the pad of a finger to prevent the shape of the fibers from changing. If the prepreg is equipped with release paper, the release paper is peeled off to expose the prepreg surface. When peeling off the release paper, peel it off slowly so that the prepreg does not lift off the glass surface. A 47 mm x 11 mm prepreg image is obtained by scanning 47 mm in the width direction of the prepreg using a microscope. When acquiring the prepreg image, a light is irradiated from the side of the glass plate opposite the prepreg. The light intensity is set to grayscale the composite prepreg image in 256 gradations, with the average brightness of all pixels being 50 to 60. If the average brightness is not within the 50 to 60 range, the light is adjusted again to acquire the prepreg image. If the average brightness is above 60 even when the light intensity is set to the minimum value, a neutral density filter is used to adjust the average brightness so that it is within the 50 to 60 range, and then the prepreg image is acquired. When acquiring the prepreg image, the test piece may be surrounded by a blackout curtain or the like to prevent light from light sources other than transmitted illumination from entering, or the measurement may be performed in a room with the light source blocked. The grayscale of the acquired prepreg image is not limited to any program using Equation (1), but IgorPro 8.04, for example, can be used. An example of a prepreg image is shown in Figure 6. In Figure 6, the range of +10% and -10% of the average waviness value Yave is indicated by a dashed line, and the intersection of the waviness Y and the average waviness value Yave is indicated by a dot. Fig. 7 shows a waveform obtained by extracting the average brightness value distribution X from Fig. 6. Fig. 8 shows a waveform obtained by extracting the waviness Y from Fig. 6. The horizontal axis in Figs. 6 to 8 indicates the pixel number, which can be converted to length (mm) by multiplying the number of pixels by the resolution.The waviness Y in the section exceeding Yave + 10% is considered one peak, and the waviness Y in the section below -10% is considered one valley. The point where Yave intersects with the waviness Y between adjacent peaks and valleys is considered the intersection point of the waviness Y and the average waviness value Yave. The number of intersections C is obtained by counting the intersections in the entire observation section. Even if the waviness Y appears to be a peak or valley, if it does not exceed Yave + 10%, it is not considered a peak of the waviness period. If it does not fall below Yave - 10%, it is not considered a valley of the waviness period, and the intersection point is not counted. The waviness period T is obtained by doubling the measurement length L shown in FIG. 6 and dividing it by (C + 1). The waviness period T was determined from each of the three test pieces, and the average value of the waviness periods T at the three points was defined as Tave, and the standard deviation of the waviness periods T at the three points was defined as Tsdev.
[0014] When the average value Tave of the three-point undulation periods T is 9 mm or more and the standard deviation Tsdev of the three-point undulation periods T is 6 mm or less, the prepreg is smooth and uniform in the width direction and fiber direction, and the prepregs can be laminated without gaps, thereby obtaining a molded product with suppressed strength reduction. From the viewpoint of the surface irregularities of the prepreg in the direction perpendicular to the fiber direction (width direction), the average value Tave of the three-point undulation periods T is preferably 12 mm or more, and more preferably 14 mm or more. From the viewpoint of the surface irregularities of the prepreg in the fiber direction and the direction perpendicular to the surface direction (thickness direction), the standard deviation Tsdev of the three-point undulation periods T is preferably 5 mm or less, and more preferably 4 mm or less.
[0015] In this embodiment, a prepreg having an average value Tave of the three-point undulation periods T of 9 mm or more and a standard deviation Tsdev of the three-point undulation periods T of 6 mm or less can be obtained by, for example, spreading parallel fiber bundles uniformly not only in the microscopic range of the surface roughness level but also in the visible range.
[0016] One example of a method for obtaining a uniformly spread unidirectional prepreg is a method comprising the following steps of spreading, tensioning, laminating, and impregnation. Spreading step: An external force is applied to the fiber bundle to deform it in a direction intersecting the fiber conveyance direction, thereby repeatedly creating tension and relaxation in the fiber bundle and spreading it. Tensioning step: A tension of 150 g / weight or more is applied to the spread fiber bundle. Laminating step: A resin sheet is laminated on the spread and tensioned fiber bundle to obtain a laminate. Impregnation step: A load is applied to the laminate to impregnate the fiber bundle with resin.
[0017] When a prepreg is produced only through a fiber-spreading process in which the fiber bundle is repeatedly subjected to a state of tension and relaxation, without undergoing a tensioning process, the undulation period T becomes large, but a stable undulation period cannot be obtained in the fiber direction, and thickness variations tend to occur in the fiber direction. When a prepreg is produced only through a tensioning process without undergoing a fiber-spreading process in which the fiber bundle is repeatedly subjected to a state of tension and relaxation, the undulation period T tends to be small and a large number of surface irregularities tend to occur. By undergoing the fiber-spreading process and tensioning process in which the fiber bundle is repeatedly subjected to a state of tension and relaxation, a prepreg with a large undulation period and few surface irregularities even in the fiber direction can be obtained.
[0018] An example of an embodiment of the prepreg manufacturing method is a method in which the steps from the fiber-opening step to the impregnation step are carried out continuously on a line to produce the prepreg. Alternatively, as another example, a laminate may be produced by a laminate manufacturing method in which the fiber-opening step, tensioning step, and lamination step are carried out continuously on a line, and the prepreg may be produced by carrying out the impregnation step on a separate line.
[0019] <Manufacturing Apparatus> An example of a prepreg manufacturing apparatus that can be used in the prepreg manufacturing method will be described below with reference to the drawings. Note that the dimensions and the like in the drawings illustrated in the following description are examples, and the present invention is not necessarily limited thereto, and can be implemented with appropriate changes within the scope that does not change the gist of the present invention.
[0020] As shown in Figure 1, a prepreg manufacturing apparatus 100 (hereinafter also simply referred to as "manufacturing apparatus 100") of this embodiment includes a plurality of yarn suppliers 10, a fiber spreading device 20, a tensioning device 30, a laminating device 40, and an impregnation machine 50. In the following explanation, the positional relationship of each component will be explained with reference to the XYZ Cartesian coordinate system shown in each figure. In this XYZ Cartesian coordinate system, the XY plane is horizontal, the X-axis direction is the feeding direction of the fiber bundle, the Y-axis direction is the width direction of the fiber bundle, and the Z-axis direction is the up-down direction perpendicular to the XY plane.
[0021] The yarn supplier 10 may be any type that can deliver the continuous fiber bundle 1, and an example thereof is one in which the continuous fiber bundle 1 is delivered by external take-up from a bobbin package attached to a creel. Alternatively, the continuous fiber bundle 1 may be delivered by internal take-up from a package from which the bobbin has been removed. The continuous fiber bundles 1 delivered from the multiple yarn suppliers 10 are transported to the fiber spreading device 20 so as to be parallel to each other and spaced apart by a predetermined distance in a direction horizontal and perpendicular to the transport direction (Y-axis direction). Guide rolls, dancer rolls, etc. can be used as appropriate for transporting the continuous fiber bundle 1. The number of yarn suppliers 10 can be set as appropriate depending on the number of filaments in the continuous fiber bundle 1 delivered from each yarn supplier 10, the width of the desired laminate or prepreg, etc.
[0022] The fiber-spreading device 20 shown in FIG. 1 includes a tension fluctuation device 21 and a lateral vibration fiber-spreading device 22 disposed downstream of the tension fluctuation device 21 .
[0023] The tension fluctuation device 21 includes a pair of guide rolls 23, 23 and a vertical vibration bar 24. The pair of guide rolls 23, 23 are arranged so that their rotation axes are both parallel to the Y-axis direction and are spaced apart in the conveying direction (X-axis direction) of the continuous fiber bundle 1. The vertical vibration bar 24 is arranged above and between the pair of guide rolls 23, 23 so that its rotation axis is parallel to the Y-axis direction. The vertical vibration bar 24 reciprocates (vertically vibrates) in the up-down direction (Z-axis direction) while keeping its rotation axis parallel to the Y-axis direction, and can intermittently press down on the continuous fiber bundle 1 passing between the pair of guide rolls 23, 23 from above.
[0024] In the tension fluctuation device 21, the continuous fiber bundle 1 passing above a pair of guide rolls 23, 23 along their peripheral surfaces is intermittently pressed down from above by a vertical vibration bar 24 between the pair of guide rolls 23, 23. In this way, an external force is applied to the continuous fiber bundle 1 to deform it in the vertical direction (Z-axis direction) intersecting the feeding direction, thereby repeatedly generating tension and relaxation in the continuous fiber bundle 1 being fed, and the continuous fiber bundle 1 is expanded and spread in the Y-axis direction.
[0025] The period of the tension fluctuation caused by the vertical vibration bar 24, i.e., the period of tension and relaxation, may be a constant period or an irregular period. The movement of the vertical vibration bar 24 is not limited to a reciprocating movement in the up and down direction, and for example, when pressing down the continuous fiber bundle 1, the vertical vibration bar 24 may also move in the conveying direction (X-axis direction) together with the continuous fiber bundle 1. This reduces friction between the vertical vibration bar 24 and the continuous fiber bundle 1, making it easier to suppress the generation of fluff.
[0026] The angle between the axial direction of the vertical vibration bar 24 and the fiber direction of the continuous fiber bundle 1 when viewed from above is not limited, but can be, for example, 60 to 120°. The distance between the central axis of the vertical vibration bar 24 and the central axis of the guide roll 23 when viewed from above is not limited, but is preferably 15 to 45 mm. When the distance is within the above range, it is easy to attach the vertical vibration bar 24 and the guide roll 23, and it is easy to prevent the opened fiber bundle from re-bundling.
[0027] The outer diameter of the guide roll 23 is not limited, but may be, for example, 12 to 60 mm. The outer diameter of the vertical vibration bar 24 is not limited, but may be, for example, 12 to 60 mm. The surfaces of the guide roll 23 and the vertical vibration bar 24 may be subjected to surface treatment such as matte finish, chrome plating, polishing, etc.
[0028] The vertical vibration bar 24 does not necessarily have to be a bar, but may be a rotating roll. From the viewpoint of minimizing friction between the roll and the continuous fiber bundle and easily suppressing the generation of fuzz, it is preferable that the vertical vibration bar 24 be a rotating roll, and more preferably a free roll. An example of a free roll is one in which the roll body is rotatably attached to a fixed shaft via a bearing or the like. In this case, the shape of the rotating roll does not necessarily have to be circular, and may be an oval, a rounded rectangular shape, a rounded cross shape, or the like.
[0029] The tension fluctuation device 21 may be any device that can periodically fluctuate the tension of the conveyed continuous fiber bundle 1, and is not limited to the embodiment shown in Fig. 1. For example, it may be a device in which an external force is intermittently applied to the continuous fiber bundle 1 by a pair of vertical vibration bars 24 and guide rolls 23. It may also be a device in which an external force is intermittently applied to the continuous fiber bundle 1 by three guide rolls 23 and two vertical vibration bars 24 arranged above and between the respective guide rolls.
[0030] 1, there is one tension fluctuation device 21, but this is not limiting, and two or more tension fluctuation devices 21 may be installed. When multiple tension fluctuation devices are installed, the number of tension fluctuation devices may be, for example, two to four. A hot air device 28 that blows hot air onto the continuous fiber bundle 1 may be provided upstream of the tension fluctuation device 21. By blowing hot air onto the fiber bundle to be spread, the binder that binds the filaments together in the fiber bundle melts, thereby increasing the spread efficiency.
[0031] The laterally vibrating fiber-spreading device 22 includes a plurality of guide rolls 26 and a plurality of laterally vibrating rolls 27, which are arranged alternately in the feeding direction (X-axis direction) of the continuous fiber bundle 1. The rotation axes of the guide rolls 26 and the laterally vibrating rolls 27 are both parallel to the Y-axis direction. The laterally vibrating rolls 27 do not need to be rolls, but may be non-rotating bars. Each laterally vibrating roll 27 is capable of reciprocating (laterally vibrating) horizontally and in a direction perpendicular to the feeding direction of the continuous fiber bundle 1 (Y-axis direction). During the lateral vibration of the laterally vibrating roll 27, its rotation axis is maintained parallel to the Y-axis direction.
[0032] 1 , the continuous fiber bundles 1 are fed so as to come into contact with the upper sides of the alternately arranged guide rolls 26 and the lower sides of the alternately arranged laterally vibrating rolls 27, while the laterally vibrating rolls 27 are laterally vibrated in the Y-axis direction. This causes the continuous fiber bundles 1 to be further widened in the Y-axis direction, filling the gaps between the fiber bundles and forming a sheet-like continuous fiber bundle 2. Note that in the laterally vibration fiber spreader 22, the continuous fiber bundles 1 may also be fed so as to come into contact with the lower sides of the alternately arranged guide rolls 26 and the upper sides of the alternately arranged laterally vibrating rolls 27.
[0033] The fiber-spreading device is not limited to the fiber-spreading device 20 shown in Fig. 1 . For example, the direction in which the feeding form of the fiber bundle in the fiber-spreading device is deformed may be any direction intersecting the feeding direction (X-axis direction) of the fiber bundle, and is not limited to the up-and-down direction (Z-axis direction). Specifically, the fiber-spreading device may be a device that repeatedly tensions and relaxes the fiber bundle being fed by deforming the feeding form of the fiber bundle in the Y-axis direction or in a direction between the Y-axis and Z-axis directions. Furthermore, another example of a fiber-spreading device does not need to be equipped with a lateral vibration fiber-spreading device.
[0034] The tension applying device 30 is a device that applies tension to the spread continuous fiber bundle 2. It is preferable that the tension applying device 30 is disposed between the spreading device 20 and the laminating device 40, that is, that the tension applying device 30 is a device that directly applies tension to the continuous fiber bundle 2 from after spreading to before lamination with the resin sheet. Note that, as long as it can apply a desired tension to the continuous fiber bundle 2 that is to be laminated with the resin sheet, it may also be a tension applying device that indirectly applies tension to the continuous fiber bundle 2 that is to be laminated with the resin sheet by applying tension to the continuous fiber bundle 1 during or before spreading.
[0035] Specific examples of the tension applying device 30 are shown below, but the present invention is not limited to these. In the tension applying device 30 of the example shown in Fig. 2, a plurality of rubbing bars 31 whose axial directions are parallel to the Y-axis direction are arranged at intervals in the conveying direction (X-axis direction) of the continuous fiber bundle 2. In the tension applying device 30 of this example, tension is applied to the continuous fiber bundle 2 by rubbing the conveyed continuous fiber bundle 2 against the plurality of rubbing bars 31. It is preferable that each rubbing bar 31 does not rotate about its axis, but it may be rotated at a peripheral speed slower than the conveying speed (line speed) of the continuous fiber bundle 2.
[0036] The surface roughness Ra of the peripheral surface of the abrading bar 31 is preferably 0.2 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. If the surface roughness Ra of the peripheral surface of the abrading bar 31 is equal to or greater than the above-mentioned lower limit, the continuous fiber bundle 2 is less likely to stick to the peripheral surface of the abrading bar 31, and tension can be applied more stably to the continuous fiber bundle 2. Furthermore, the surface roughness Ra of the peripheral surface of the abrading bar 31 is preferably 2.0 μm or less, more preferably 1.6 μm or less, and even more preferably 1.3 μm or less. If the surface roughness Ra of the peripheral surface of the abrading bar 31 is equal to or less than the above-mentioned upper limit, the abrading bar is less likely to fluff. The preferred upper and lower limits of the surface roughness Ra of the peripheral surface of the abrading bar 31 can be arbitrarily combined, and for example, 0.5 to 1.3 μm is preferred. The surface roughness Ra can be measured in accordance with JIS B 0601-2001.
[0037] 3, a plurality of brake rolls 32 whose axial directions are parallel to the Y-axis direction are arranged at intervals in the conveying direction (X-axis direction) of the continuous fiber bundle 2. In this example, the tension applying device 30 applies tension to the continuous fiber bundle 2 by conveying the continuous fiber bundle 2 with the plurality of brake rolls 32 that rotate when a torque equal to or greater than a certain level is applied.
[0038] For the same reasons as for the rubbing bar 31, the surface roughness Ra of the peripheral surface of the brake roll 32 is preferably 0.2 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. The surface roughness Ra of the peripheral surface of the brake roll 32 is preferably 2.0 μm or less, more preferably 1.6 μm or less, and even more preferably 1.3 μm or less. The preferred upper and lower limit values of the surface roughness Ra of the peripheral surface of the brake roll 32 can be arbitrarily combined, and for example, 0.5 to 1.3 μm is preferred.
[0039] 4 includes a brake roll 32 and a nip roll 33 that sandwich the conveyed continuous fiber bundle 2 from above and below. In the tension applying device 30 of this example, tension is applied to the continuous fiber bundle 2 by sandwiching the conveyed continuous fiber bundle 2 between the brake roll 32 and the nip roll 33 from above and below.
[0040] 5 includes a brake roll 32 and a nip roll 33 that sandwich the conveyed continuous fiber bundle 2 from above and below, and a tension measuring device 34 that is arranged downstream of the brake roll 32 and the nip roll 33 in the conveying direction of the continuous fiber bundle 2. The tension applying device 30 of this example includes a mechanism that detects the tension of the continuous fiber bundle 2 with the tension measuring device 34 and feeds back the detected tension value to the brake roll 32, thereby controlling the tension applied to the continuous fiber bundle 2.
[0041] The tension applying device 30 is not limited to those shown in Figures 2 to 5, and may be, for example, a combination of two or more of these. In the present invention, the tension applying device preferably has at least a scraping bar or a brake roll.
[0042] The laminating device 40 is a device that laminates a resin sheet 3 on the opened and tensioned continuous fiber bundle 2. The laminating device 40 includes a resin sheet supply body 41 that is arranged above the conveyed continuous fiber bundle 2, and a resin sheet supply body 41 that is arranged below the conveyed continuous fiber bundle 2. The laminating device 40 laminates the resin sheets 3 fed from the resin sheet supply body 41 by bonding them to the top and bottom of the conveyed continuous fiber bundle 2.
[0043] The impregnation machine 50 includes multiple pairs of impregnation rolls 51 that sandwich and apply a load to a laminate 4, which is a laminate of continuous fiber bundles 2 and a resin sheet 3. The conveyed laminate 4 is sandwiched between the multiple pairs of impregnation rolls 51 and pressurized from above and below, whereby the resin that forms the resin sheet 3 is impregnated into the continuous fiber bundles 2.
[0044] 1 , a pair of impregnation rolls 51 on the most upstream side of the impregnation machine 50 also serve as laminating rolls that bond the continuous fiber bundle 2 and the resin sheet 3 in the laminating device 40. That is, in the manufacturing apparatus 100 of this example, the impregnation rolls 51 apply a load at the point of contact between the continuous fiber bundle 2 and the resin sheet 3, thereby starting impregnation. In this way, if impregnation is started at the same time as the continuous fiber bundle 2 and the resin sheet 3 are laminated, misalignment between the continuous fiber bundle 2 and the resin sheet 3 due to a difference in inner and outer circumferences when the transported laminate 4 is embraced by the rolls is suppressed, and defects are less likely to occur.
[0045] The laminating device 40 may include a laminating roll in addition to the pair of impregnation rolls 51 on the most upstream side of the impregnation machine 50. In this case, it is preferable that the laminate 4 is conveyed linearly in the X-axis direction from the contact point between the continuous fiber bundle 2 and the resin sheet 3 laminated by the laminating rolls to the pair of impregnation rolls 51 on the most upstream side of the impregnation machine 50. This configuration also makes it possible to prevent misalignment between the continuous fiber bundle 2 and the resin sheet 3 due to a difference between the inner and outer peripheries when the conveyed laminate 4 is embraced by the rolls.
[0046] The prepreg manufacturing apparatus is not limited to the above-described manufacturing apparatus 100, which includes a yarn supplier, a spreader, a tensioning device, a laminating device, and an impregnation machine, and which continuously performs spreading, tensioning, laminating, and impregnation in a single line. For example, the prepreg manufacturing apparatus may include a laminate manufacturing apparatus including a yarn supplier, a spreader, a tensioning device, and a laminating device, and an impregnation apparatus, on separate lines. In addition, the components in the above-described embodiments may be replaced with well-known components as appropriate, and the above-described modified examples may be combined as appropriate, without departing from the spirit of the present invention.
[0047] <Manufacturing Method> Hereinafter, as an example of a method for manufacturing a prepreg, manufacturing of a prepreg using the manufacturing apparatus 100 shown in FIG. 1 will be described.
[0048] First, the continuous fiber bundles 1 delivered from each of the multiple fiber suppliers 10 are transported to the fiber-spreading device 20 so that they are horizontal and parallel to each other at a predetermined interval in a direction perpendicular to the transport direction (Y-axis direction). The transport speed (line speed) of the continuous fiber bundle 1 is not limited, but can be, for example, 0.1 to 50 m / min, preferably 0.5 m / min or more, and more preferably 1 m / min or more. On the other hand, the transport speed of the continuous fiber bundle 1 is preferably 30 m / min or less, more preferably 15 m / min or less, and even more preferably 10 m / min or less. If the transport speed (line speed) of the continuous fiber bundle 1 is equal to or greater than the above-mentioned lower limit, high productivity can be ensured. If the transport speed (line speed) is equal to or less than the above-mentioned upper limit, the tension fluctuation period required for fiber-spreading is reduced, and vibration of the device can be suppressed. The preferred upper and lower limit values of the transport speed of the continuous fiber bundle 1 can be arbitrarily combined.
[0049] In the fiber-spreading device 20, the tension fluctuation device 21 conveys the continuous fiber bundle 1 in the X-axis direction, while a vertical vibration bar 24 intermittently presses the continuous fiber bundle 1 from above between a pair of guide rolls 23, 23. In this way, by applying an external force that deforms the continuous fiber bundle 1 in the vertical direction (Z-axis direction) intersecting the feeding direction of the continuous fiber bundle 1, tension and relaxation states are repeatedly generated in the continuous fiber bundle 1, and the continuous fiber bundle 1 is expanded and spread in the Y-axis direction. In this example, further, in the laterally vibrating fiber-spreading device 22, while conveying each continuous fiber bundle 1 along alternately arranged guide rolls 26 and laterally vibrating rolls 27, the laterally vibrating rolls 27 are laterally vibrated in the Y-axis direction, so that each continuous fiber bundle 1 is further spread and leveled, and gaps between the fiber bundles are filled to form a sheet-like continuous fiber bundle 2 (fiber-spreading process).
[0050] The difference in tension of the continuous fiber bundle 1 between the tensioned state and the relaxed state in the spreading step is preferably 10 g / spindle-K or more per 1,000 filaments, more preferably 30 g / spindle-K or more, and even more preferably 50 g / spindle-K or more. If the tension difference per 1,000 filaments is equal to or greater than the above-mentioned lower limit, the spreadability of the fiber bundle is improved. Furthermore, the difference in tension of the continuous fiber bundle 1 between the tensioned state and the relaxed state in the spreading step is preferably 4,000 g / spindle-K or less per 1,000 filaments, more preferably 3,000 g / spindle-K or less, and even more preferably 2,000 g / spindle-K or less. If the tension difference per 1,000 filaments is equal to or less than the above-mentioned upper limit, the fiber bundle can be stably spread while suppressing vibration of the device. The upper and lower limits of the tension difference can be arbitrarily combined, and, for example, 50 to 2,000 g / spindle-K is preferable. In the unit "g / spindle·K", K means that there are 1000 filaments.
[0051] The difference in tension of the continuous fiber bundle 1 when tensioned and relaxed in the spreading process is preferably 10 g / spindle×m / g or more per g / m of fiber weight, more preferably 30 g / spindle×m / g or more, and even more preferably 50 g / spindle×m / g or more. If the difference in tension per g / m of fiber weight is equal to or greater than the above-mentioned lower limit, the spreadability of the fiber bundle is improved. Furthermore, the difference in tension of the continuous fiber bundle 1 when tensioned and relaxed in the spreading process is preferably 4000 g / spindle×m / g or less per g / m of fiber weight, more preferably 3000 g / spindle×m / g or less, and even more preferably 2000 g / spindle×m / g or less. If the difference in tension per g / m of fiber weight is equal to or less than the above-mentioned upper limit, the fiber bundle can be stably spread while suppressing vibration of the device. The upper and lower limits of the tension difference can be arbitrarily combined, and, for example, 50 to 2000 g / spindle×m / g is preferable. The tension of the fiber bundle when tense and when relaxed in the fiber-spreading step is a value obtained by dividing the tension per spindle of the continuous fiber bundle when tense and when relaxed by the fiber weight (unit: g / m) of the fiber bundle.
[0052] The vertical vibration frequency of the vertical vibration bar 24 is preferably 50 rpm or more, more preferably 100 rpm or more, and even more preferably 200 rpm or more. If the vertical vibration frequency of the vertical vibration bar 24 is equal to or greater than the above-mentioned lower limit, the fiber bundle can be opened more easily. Furthermore, the vertical vibration frequency of the vertical vibration bar 24 is preferably 2000 rpm or less, more preferably 1500 rpm or less, and even more preferably 1000 rpm or less. If the vertical vibration frequency of the vertical vibration bar 24 is equal to or less than the above-mentioned upper limit, the fiber bundle can be opened stably while suppressing vibration of the device. The upper and lower limit values of the vertical vibration frequency of the vertical vibration bar 24 can be arbitrarily combined, and for example, 50 to 2000 rpm is preferable. The amplitude of the bar that applies tension sandwiching one relaxation in the opening process is not particularly limited, but can be, for example, 5 to 20 mm.
[0053] The lateral vibration speed of the lateral vibrating roll 27 is preferably 100 m / min or more, more preferably 200 m / min or more, and even more preferably 300 m / min or more. If the lateral vibration speed of the lateral vibrating roll 27 is equal to or higher than the lower limit, the fiber bundles are likely to be uniformly spread. Furthermore, the lateral vibration speed of the lateral vibrating roll 27 is preferably 1500 m / min or less, more preferably 1200 m / min or less, and even more preferably 1000 m / min or less. If the lateral vibration speed of the lateral vibrating roll 27 is equal to or lower than the upper limit, the fiber bundles can come into contact with the roll without floating, and are therefore likely to be spread. The upper and lower limits of the lateral vibration speed of the lateral vibrating bar 27 can be arbitrarily combined, and, for example, a range of 100 to 1500 m / min is preferred.
[0054] In order to increase the spreading efficiency, hot air may be blown from a hot air device 28 onto the continuous fiber bundle 1 spread by the tension fluctuation device 21. The temperature of the hot air blown onto the continuous fiber bundle 1 is not limited, but can be, for example, 60 to 130°C.
[0055] After the spreading step, for example, in a tension applying device 30 shown in Fig. 2, the spread continuous fiber bundle 2 is conveyed while rubbing against a plurality of rubbing bars 31, thereby applying tension to the continuous fiber bundle 2. Alternatively, in a tension applying device 30 shown in Fig. 3, tension is applied to the continuous fiber bundle 2 by conveying the continuous fiber bundle 2 with a plurality of brake rolls 32. Alternatively, in a tension applying device 30 shown in Fig. 4, tension is applied to the continuous fiber bundle 2 by sandwiching the conveyed continuous fiber bundle 2 from above and below between the brake roll 32 and the nip roll 33. Alternatively, in a tension applying device 30 shown in Fig. 5, tension is applied to the continuous fiber bundle 2 by sandwiching the conveyed continuous fiber bundle 2 from above and below between the brake roll 32 and the nip roll 33, and the value of the tension of the continuous fiber bundle 2 detected by a tension measuring device 34 is fed back to the brake roll 32 to control the tension (tension applying step). By repeatedly tensioning and relaxing the continuous fiber bundle 1 in the tension fluctuation device 21 while applying tension to the continuous fiber bundle 2 in the tension applying device 30, the continuous fiber bundle 2 is repeatedly subjected to a state in which tension is applied and a state in which the tension is reduced.
[0056] After the tensioning step, in the laminating device 40, the resin sheet 3 delivered from one resin sheet supplier 41 and the resin sheet 3 delivered from the other resin sheet supplier 41 are laminated above and below the opened and tensioned continuous fiber bundle 2 (laminating step). The impregnation roll 51 on the most upstream side of the impregnation machine 50 laminates the continuous fiber bundle 2 and the resin sheet 3, and simultaneously applies a load to start impregnation. The fiber bundle is impregnated with resin by multiple pairs of impregnation rolls 51, thereby obtaining a prepreg (UD prepreg) 5 (impregnation step). The obtained prepreg 5 can be wound up, for example, by a winder.
[0057] In this embodiment, tension is applied to the spread continuous fiber bundles 2 in the tensioning step, and the resin sheet 3 is then laminated on the tensioned continuous fiber bundles 2 in the laminating step. This provides sufficient tension to the continuous fiber bundles 2 laminated on the resin sheet 3, making it difficult for the fibers to meander or relax locally, thereby suppressing the generation of protrusions on the surfaces of the obtained laminate 4 and prepreg 5. Since it is easy to apply sufficient tension to the continuous fiber bundles 2 laminated on the resin sheet 3, it is preferable to apply tension to the fiber bundles between the spread step and the laminating step using a tensioning device in the tensioning step.
[0058] The tension applied to the fiber bundle in the tensioning step is the same as the tension of the fiber bundle that will be laminated with the resin sheet when the fiber bundle is relaxed in the fiber-spreading step. Even if the tension of the continuous fiber bundle 1 is zero in the relaxed state in the fiber-spreading step, for example, when the vertical vibration bar 24 is separated from the continuous fiber bundle 1 in the example shown in Figure 1, the tension applied in the tensioning step ensures that the continuous fiber bundle 1 has a minimum tension when laminated with the resin sheet. Therefore, the generation of protrusions on the surfaces of the obtained laminate 4 and prepreg 5 is suppressed.
[0059] The tension applied to the fiber bundle in the tensioning step is preferably 3 g / sinker-K or more per 1,000 filaments, more preferably 4 g / sinker-K or more, and even more preferably 5 g / sinker-K or more. If the tension per 1,000 filaments after the tensioning step is equal to or greater than the above-mentioned lower limit, the formation of protrusions on the surfaces of the resulting laminate 4 and prepreg 5 is easily suppressed. Furthermore, the tension applied to the fiber bundle in the tensioning step is preferably 600 g / sinker-K or less per 1,000 filaments, more preferably 400 g / sinker-K or less, and even more preferably 300 g / sinker-K or less. If the tension per 1,000 filaments after the tensioning step is equal to or less than the above-mentioned upper limit, the occurrence of cracks that cause gaps between fibers in the resulting prepreg is easily suppressed. The upper and lower limit values of the tension applied in the tensioning step can be arbitrarily combined, and for example, 5 to 300 g / sinker-K is preferred.
[0060] The tension applied to the fiber bundle in the tensioning step is preferably 45 g / spindle×m / g or more per g / m of fiber basis weight, more preferably 60 g / spindle×m / g or more, and even more preferably 75 g / spindle×m / g or more. If the tension per g / m of fiber basis weight after the tensioning step is equal to or greater than the above-mentioned lower limit, it is easy to suppress the generation of protrusions on the surfaces of the obtained laminate 4 and prepreg 5. Furthermore, the tension applied to the fiber bundle in the tensioning step is preferably 9000 g / spindle×m / g or less per g / m of fiber basis weight, more preferably 6000 g / spindle×m / g or less, and even more preferably 4500 g / spindle×m / g or less. If the tension per mg / m of fiber basis weight after the tensioning step is equal to or less than the above-mentioned upper limit, the obtained prepreg is less likely to crack. The upper and lower limits of the tension applied in the tension application step can be arbitrarily combined, and are preferably, for example, 75 to 4500 g / spindle×m / g. The tension per 1 g / m of fiber basis weight applied in the tension application step is the value obtained by dividing the tension per spindle after being applied to the fiber bundle in the tension application step by the fiber basis weight (unit: g / m) of the fiber bundle.
[0061] In order to prevent cracks from occurring in the resulting prepreg, it is preferable that the distance L from the point of contact with the continuous fiber bundle 2 on the most downstream side of the tensioning device 30 to the point of contact between the continuous fiber bundle 2 and the resin sheet 3 satisfies L<300 mm. The distance L is preferably less than 300 mm, more preferably 200 mm or less, and even more preferably 150 mm or less. From the viewpoint of device layout, the distance L is preferably 0.5 mm or more, more preferably 1 mm or more, and even more preferably 3 mm or more. The upper and lower limits of the distance L can be arbitrarily combined, and for example, a range of 3 mm or more but less than 150 mm is preferable.
[0062] In the case of the tension applying device 30 shown in Fig. 2, the distance L is the distance from the contact point between the most downstream scraping bar 31 and the continuous fiber bundle 2 to the contact point between the continuous fiber bundle 2 and the resin sheet 3. In the case of the tension applying device 30 shown in Fig. 3, the distance L is the distance from the contact point between the most downstream brake roll 32 and the continuous fiber bundle 2 to the contact point between the continuous fiber bundle 2 and the resin sheet 3. In the case of the tension applying device 30 shown in Fig. 4, the distance L is the distance from the contact point between the brake roll 32 and the nip roll 33 and the continuous fiber bundle 2 to the contact point between the continuous fiber bundle 2 and the resin sheet 3.
[0063] The continuous fiber bundle 1 is a long, continuous fiber bundle consisting of an aggregate of reinforcing fibers. The reinforcing fibers are not particularly limited, and examples include various inorganic or organic fibers such as carbon fibers, aramid fibers, nylon fibers, high-strength polyester fibers, glass fibers, boron fibers, alumina fibers, and silicon nitride fibers. Among these, carbon fibers, aramid fibers, glass fibers, boron fibers, alumina fibers, and silicon nitride fibers are preferred in terms of specific strength and specific elasticity, and carbon fibers are particularly preferred in terms of mechanical properties and weight reduction. When carbon fibers are used as reinforcing fibers, they may be surface-treated with a metal. The reinforcing fibers contained in the fiber bundle may be one type or two or more types.
[0064] The fiber diameter of the reinforcing fibers is not limited, but can be, for example, 4 to 20 μm or 5 to 15 μm. The number of filaments per spindle of the continuous fiber bundle 1 is not limited, but can be, for example, 1,000 to 100,000. The fiber weight of the continuous fiber bundle 1 is not limited, but can be, for example, 0.2 to 4 g / m. The fiber weight in the prepreg is 1 to 500 g / m. 2 However, it can be 20 to 40 g / m 2 In this case, the effect of adjusting Tave and Tsdev on the smoothness of the prepreg surface becomes significant.
[0065] The resin sheet 3 is formed by applying the matrix resin composition to a carrier sheet, such as release-treated paper or resin film. The carrier sheet can be peeled off at any time after impregnation. As the resin sheet supplier 41, a carrier sheet on which the resin sheet 3 has been formed in advance may be fed from the first resin sheet supplier and the second resin sheet supplier, or the resin sheet 3 may be formed by feeding a carrier sheet and applying the matrix resin composition to the carrier sheet during transport.
[0066] The resin used in the matrix resin composition forming the resin sheet 3 is not particularly limited and may be a thermosetting resin or a thermoplastic resin. Examples of thermosetting resins include epoxy resins, vinyl ester resins, unsaturated polyester resins, and phenolic resins. Examples of thermoplastic resins to be added to thermosetting resins include polyamides, polyethersulfones, polyimides, polytetrafluoroethylene, polyvinyl formal resins, and phenoxy resins. Examples of thermoplastic resins include polypropylene resins, polyamide resins, polycarbonate resins, polyphenylene sulfide resins, polyvinyl alcohol resins, polyethersulfone resins, polyetherimide resins, polyetheretherketone resins, and polyetherketoneketone resins. The resin used in the resin sheet 3 may be one type or two or more types.
[0067] The matrix resin composition may contain additives such as a curing agent, a flame retardant, a weather resistance improver, an antioxidant, a heat stabilizer, an ultraviolet absorber, a plasticizer, a lubricant, a colorant, a compatibilizer, and a conductive filler, as needed.
[0068] The curing agent promotes the curing reaction of the curable resin. For example, curing agents for epoxy resins include dicyandiamides, imidazoles, acid hydrazide compounds, and urea compounds. These may be used alone or in combination. Amines may also be included as other curing agents. Dicyandiamides may be, for example, dicyandiamide or those pre-reacted with epoxy resins. Urea compounds include, for example, aromatic ureas in which a ureido group is bonded to an aromatic ring, and aliphatic ureas in which a ureido group is bonded to an aliphatic chain. Imidazoles include imidazole, imidazole adducts, clathrated imidazole, microencapsulated imidazole, and imidazole compounds coordinated with a stabilizer.
[0069] From the viewpoint of improving the mechanical properties of the fiber-reinforced composite material and the adhesion to the carbon fiber, the content of the matrix resin composition in the prepreg is preferably 15 to 50 mass%, more preferably 20 to 50 mass%, and even more preferably 25 to 40 mass%, relative to the total mass of the prepreg.
[0070] [Fiber-reinforced composite material] A fiber-reinforced composite material is obtained by curing a prepreg. That is, the fiber-reinforced composite material contains a cured product of a matrix resin composition contained in the prepreg and carbon fibers. The fiber-reinforced composite material may also be a cured product of a laminate in which two or more prepregs are stacked. The fiber-reinforced composite material can be obtained, for example, by laminating two or more of the above-mentioned prepregs and then molding the laminate by a method such as heat-curing the matrix resin composition while applying pressure to the obtained laminate.
[0071] The present invention will now be described in more detail with reference to examples.
[0072] Example 1 Using the prepreg manufacturing apparatus 100 shown in FIG. 1, a prepreg having a fiber basis weight of 29 g / m 2Seven continuous carbon fiber bundles (manufactured by Mitsubishi Chemical Corporation, product name "TR50S15L AD", number of filaments: 15,000, fiber basis weight: 1000 mg / m) were used as the continuous fiber bundles 1, and the interval between each continuous fiber bundle 1 in the Y-axis direction conveyed to the fiber-spreading device 20 (fiber-spreading process) was 34.5 mm. The matrix resin composition used was a one-component curing epoxy resin composition for prepreg prepared by preliminarily dissolving 45 parts by mass of bisphenol A epoxy resin "Epikote 828" (epoxy equivalent: 184-194, liquid at room temperature) manufactured by Mitsubishi Chemical Corporation, 35 parts by mass of bisphenol A epoxy resin "Epikote 1002" (epoxy equivalent: 600-700, solid at room temperature) manufactured by Yuka Shell Epoxy Co., Ltd., and 30 parts by mass of phenol novolac epoxy resin "Epiclon N775" (softening point 70-80°C) manufactured by DIC Corporation to prepare a homogeneous mixed resin, and then kneading this with 6 parts by mass of dicyandiamide "Epicure DICY7" (molecular weight: 84) manufactured by Mitsubishi Chemical Corporation and 4 parts by mass of "DCMU-99" (molecular weight: 233) manufactured by Hodogaya Chemical Co., Ltd. The one-component curing epoxy resin composition was applied to release paper using a roll coater to prepare a resin film, and the resin sheet was laminated onto a sheet of aligned carbon fibers (lamination process). The one-component curing epoxy resin composition was impregnated using an impregnation roll to obtain a prepreg (impregnation process). The conveying speed (line speed) of the continuous fiber bundle 1 was 2 m / min. The rotation speed of the vertical vibration bar 24 of the tension fluctuation device 21 in the fiber-spreading process was 6 m / min, and the time interval between tensions between one relaxation period was 0.175 seconds. The maximum tension after tension application was 190 g / spindle·K, and the minimum tension was 60 g / spindle·K.
[0073] Example 2 A UD prepreg was produced in the same manner as in Example 1, except that the interval between the continuous fiber bundles 1 in the Y-axis direction was set to 43.5 mm.
[0074] [Comparative Example 1] Seven continuous carbon fiber bundles (manufactured by Mitsubishi Chemical, product name "TR50S15L JJ", number of filaments: 15,000, fiber weight: 1000 mg / m) were used as the continuous fiber bundles 1, and the interval in the Y-axis direction between the continuous fiber bundles 1 fed to the fiber-spreading device 20 was 34.5 mm. The production method was the same as in Example 1 up to the tension fluctuation device, and a UD prepreg was produced by performing the lamination step and the impregnation step without passing through the tension application step.
[0075] [Comparative Example 2] Fiber basis weight 23 g / m 2 A UD prepreg having a resin content of 40% by mass was produced. Seven continuous carbon fiber bundles (manufactured by Mitsubishi Chemical Corporation, product name "TR50S15L JJ", number of filaments: 15,000, fiber basis weight: 1000 mg / m) were used as the continuous fiber bundles 1, and the interval between each continuous fiber bundle 1 in the Y-axis direction transported to the fiber spreading device 20 was 45.0 mm. Otherwise, the UD prepreg was produced in the same manner as in Comparative Example 1.
[0076] [Comparative Example 3] Fiber basis weight 23 g / m 2 A UD prepreg having a resin content of 40% by mass was produced. 122 continuous carbon fiber bundles (manufactured by Mitsubishi Chemical Corporation, product name "MR 30 3L AE," number of filaments: 3,000, fiber basis weight: 190 mg / m) were used as the continuous fiber bundles 1, and the UD prepreg was produced in the same manner as in Example 1, except that abrasion spreading was performed without using the tension fluctuation device 21. The interval between each continuous fiber bundle 1 in the Y-axis direction was 8.3 mm.
[0077] [Comparative Example 4] Fiber basis weight 29 g / m 2 A UD prepreg having a resin content of 40% by mass was produced. The UD prepreg was produced using 145 continuous carbon fiber bundles (manufactured by Mitsubishi Chemical Corporation, product name "TR 30 3L AE", number of filaments: 3,000, fiber basis weight: 200 mg / m) as the continuous fiber bundles 1. The spacing between the continuous fiber bundles 1 in the Y-axis direction was 6.9 mm. The UD prepreg was otherwise produced in the same manner as in Comparative Example 3.
[0078] [Comparative Example 5] Fiber basis weight 25 g / m 2A UD prepreg having a resin content of 25% by mass was produced. 250 carbon fibers 1 (number of filaments: 2,000, fiber basis weight: 100 mg / m) were used as the continuous fiber bundles 1 to produce the UD prepreg. The interval between each continuous fiber bundle 1 in the Y-axis direction was 4 mm. Otherwise, the UD prepreg was produced in the same manner as in Comparative Example 3.
[0079] [Comparative Example 6] Fiber basis weight 29 g / m 2 A UD prepreg having a resin content of 40% by mass was produced. Seven continuous carbon fiber bundles (manufactured by Mitsubishi Chemical, product name "TR50S15L AD", number of filaments: 15,000, fiber basis weight: 1000 mg / m) were used as the continuous fiber bundles 1, and the interval between each continuous fiber bundle 1 in the Y-axis direction transported to the fiber spreading device 20 was 34.5 mm. The tension applying device used was the device shown in FIG. 5. The tension in the tension applying step was constant at 5 g / spindle·K. Otherwise, the UD prepreg was produced in the same manner as in Comparative Example 1.
[0080] [Method for measuring the average value Tave and standard deviation Tsdev of the waviness period T] The average value Tave of the waviness periods at three points and the standard deviation Tsdev of the waviness periods at three points were calculated using the following method. The prepreg was cut into 100 mm lengths in the direction perpendicular to the fiber direction (90 degree direction) and 50 mm lengths in the direction parallel to the fiber direction (0 degree direction) so that the fibers were present over the entire surface, to obtain a test specimen. The film on the side opposite the release paper surface of the test specimen was peeled off, and the carbon fiber surface was pressed against a transparent glass plate with a thickness of 3 mm or less and fixed so as not to peel off. The release paper was peeled off to expose the other carbon fiber surface. The glass plate was fixed so as to be in contact with the measurement table of a microscope (Keyence Digital Microscope VHX-7000), and a light built into the microscope was irradiated from the glass plate side. The light was set so that the average brightness of all pixels when the composited prepreg image was converted to a grayscale of 256 levels using the formula (1) described below was 50 to 60. The resolution was 5.2 μm / pix. Images were composited while scanning 47 mm in the direction perpendicular to the fiber direction, and a prepreg image of 47 mm in the direction perpendicular to the fiber direction and 11 mm in the fiber direction was obtained. The photographing conditions were a magnification of 20x, a shutter speed of 33 ms, and a gain of 0 dB. The prepreg image was obtained by bright-field observation behind a blackout curtain or the like to prevent light from light sources other than transmitted illumination from entering. The prepreg image was converted to a grayscale using IgorPro 8.04 using the following formula (1).
[0081] The average brightness value Xi was calculated by averaging all pixel brightness in the fiber direction for each pixel, and the average brightness value distribution X in the direction perpendicular to the fiber direction was obtained. Using a Gaussian filter defined in JIS B 0632:2001, the average brightness value distribution X was smoothed with a cutoff wavelength of 2.5 mm to extract the waviness Y. From the extracted waviness Y, Yave, the average waviness represented by the following formula (2), was calculated. The waviness Y in a section exceeding Yave + 10% was considered to be one peak, and the waviness Y in a section below -10% was considered to be one valley. A point where Yave intersects with adjacent peaks and valleys was considered to be the end of the peak or valley, and this was counted across the entire observation section to obtain the number of intersections C. The observation length in the direction perpendicular to the fiber direction of the prepreg image was defined as L, and the waviness period T represented by formula (3) was calculated. The waviness period T is calculated from three different test pieces, and the average value Tave of the waviness period T expressed by equation (4) and the standard deviation Tsdev of the waviness period T expressed by equation (5) are calculated.
[0082]
[0083] R: Red value indicated by RGB values G: Green value indicated by RGB values B: Blue value indicated by RGB values Yi: Waviness value of brightness value at the i-th pixel n: Number of waviness data points L: Observation length in the direction perpendicular to the fiber direction of the prepreg image C: Number of intersections between waviness Y and the average value Yave of waviness Y Ti: Period value of waviness Y of the i-th test piece
[0084] [Evaluation] The UD prepregs of Examples 1 and 2, which were obtained by spreading carbon fiber bundles to a target fiber width using a tension fluctuation device in the spreading step, applying tension to the fiber bundles in the tensioning step, and then laminating a resin sheet, had a larger average value Tave of the three-point undulation periods and a smaller standard deviation Tsdev of the three-point undulation periods than Comparative Examples 1 and 2, which did not have a tensioning step, and Comparative Examples 3 to 5, which did not use a tension fluctuation device. The prepregs of the Examples showed little thickness unevenness in the spread carbon fiber bundles both in the direction perpendicular to the width direction and in the direction perpendicular to the width direction, indicating that they were prepregs with a uniform thickness. Since fiber meandering did not occur even when prepregs with a uniform surface were laminated, it is believed that it is possible to obtain a molded product with suppressed strength reduction.
[0085] This application claims priority based on Japanese Patent Application No. 2023-100649, filed on June 20, 2023, the contents of which are incorporated herein by reference.
[0086]
[0087] 10... yarn supplier, 20... fiber spreading device, 21... tension fluctuation device, 22... laterally vibrating fiber spreading device, 23... guide roll, 24... vertically vibrating bar, 26... guide roll, 27... laterally vibrating roll, 30... tension applying device, 31... scraping bar, 32... brake roll, 33... nip roll, 40... laminating device, 41... resin sheet supplier, 50... impregnation machine, 51... impregnation roll, 100... prepreg manufacturing apparatus.
Claims
1. Carbon fibers aligned in one direction are impregnated with a matrix resin composition, and the fiber weight of the carbon fibers is 20 to 40 g / m 2 A prepreg having an average value Tave of the undulation period T of 9 mm or more and a standard deviation Tsdev of the undulation period T of 6 mm or less, as measured by the following method. <Measurement method> The prepreg is cut into a size of 100 mm x 50 mm so that the direction parallel to the surface direction and perpendicular to the fiber direction is 100 mm, to obtain a test piece. The test piece is attached to a glass plate and integrated with the glass plate. A microscope is used to obtain a 47 mm x 11 mm prepreg image by scanning 47 mm in a direction parallel to the surface direction and perpendicular to the fiber direction (90 degree direction). The prepreg image is converted into a grayscale image using the following formula (1), and the average brightness value Xi in the fiber direction is calculated to obtain the average brightness value distribution X. The waviness Y is extracted by smoothing the average luminance value distribution X using a Gaussian filter. The waviness average Yave expressed by the following formula (2) and the waviness period T expressed by the following formula (3) are calculated, and the average value Tave of the waviness period T of the three points on the test piece expressed by the following formula (4) and the standard deviation Tsdev of the waviness period T of the three points on the test piece expressed by the following formula (5) are calculated. R: Red value indicated by RGB values G: Green value indicated by RGB values B: Blue value indicated by RGB values Yi: Waviness value of brightness value at the i-th pixel n: Number of waviness Yi data L: Observation length in the direction perpendicular to the fiber direction of the prepreg image C: Number of intersections between waviness Y and the average Yave of waviness Y Ti: Periodic value of waviness Y of the i-th test piece 2. The prepreg according to claim 1, wherein the content of said matrix resin composition in said prepreg is 20 to 50 mass % based on the total mass of the prepreg.
3. The prepreg according to claim 2, wherein the prepreg contains carbon fibers having a fiber diameter of 5 to 15 μm.
4. The prepreg of claim 1, wherein the matrix resin composition comprises a thermosetting resin.
5. The prepreg of claim 1, wherein the matrix resin composition includes a curing agent.
6. The prepreg of claim 5, wherein the curing agent comprises dicyandiamide.
7. The prepreg of claim 1, wherein the matrix resin composition comprises a thermoplastic resin.
8. A fiber-reinforced composite material obtained by curing the prepreg according to claim 1.
9. A method for manufacturing a prepreg, comprising the following steps: Spreading step: An external force is applied to the fiber bundle to deform it in a direction intersecting the conveying direction, thereby repeatedly creating and relaxing states in the fiber bundle to spread it. Tensioning step: A tension of 150 g / weight or more is applied to the spread fiber bundle. Laminating step: A resin sheet is laminated on the spread and tensioned fiber bundle to obtain a laminate. Impregnation step: A load is applied to the laminate to impregnate the fiber bundle with resin.
10. A method for producing a prepreg as described in claim 9, wherein in the tension applying step, a tension that is 1.1 times or more the tension of the spread fiber bundle is applied.
11. The method for producing a prepreg according to claim 10, wherein, as the tension applying step, tension is applied to the fiber bundles between the opening step and the lamination step by a tension applying device.
12. The method for producing a prepreg according to claim 11, wherein the tension applied to the fiber bundle in the tension application step is 3 g / spindle·K or more per 1,000 filaments.
13. The method for producing a prepreg as described in claim 9, wherein the tension applied to the fiber bundle in the tension application step is 45 g / weight×m / g or more per 1 g / m of fiber basis weight.
14. The method of claim 11, wherein the tensioning device comprises a scraping bar.
15. The method of claim 11, wherein the tensioning device comprises a brake roll.
16. The method for producing a prepreg according to claim 11, wherein a distance L from a point of contact between the fiber bundle and the tension applying device on the most downstream side to a point of contact between the fiber bundle and the resin sheet satisfies L < 300 mm.
17. The method for producing a prepreg according to claim 9, wherein the impregnation is initiated by applying a load at the contact point between the fiber bundle and the resin sheet using an impregnation roll.
Citation Information
Patent Citations
Opening of strand and opening apparatus
JP1998110346A
Device for opening carbon fiber bundle and its opening and production of prepreg
JP1998292238A
Method for opening bundle of reinforcing fiber and manufacturing method of prepreg
JP2001288639A
Method for producing opened fiber sheet, method for producing thermoplastic resin-impregnated prepreg sheet with the same as reinforcing base, and production machine for the opened fiber sheet, and thermoplastic rein impregnator for the opened fiber sheet
JP2005029912A
Manufacturing method and manufacturing device of laminate, and manufacturing method and manufacturing device of prepreg
JP2023131571A