Method for recovering lithium from lithium-containing waste

By using alkali metal oxides and fluoride as calcination additives in lithium-containing waste materials, combined with aerobic roasting and leaching processes, the problems of high energy consumption and equipment corrosion in the prior art are solved, and low-energy consumption and efficient lithium recovery and battery-grade lithium carbonate preparation are achieved.

WO2025086551A1PCT designated stage expired Publication Date: 2025-05-01GEM CO LTD +1

Patent Information

Application Number
PCT/CN2024/084717
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-27
Filing Date
2024-03-29
Publication Date
2025-05-01

AI Technical Summary

Technical Problem

The prior art method of recycling lithium from lithium-containing waste materials has high energy consumption and the use of highly toxic hydrofluoric acid has high requirements for equipment, which is not suitable for large-scale industrial production.

Method used

Alkaline metal oxides and/or alkali metal fluoride are used as calcining additives, mixed with lithium-containing waste materials and calcined aerobic calcination, leaching the calcined powder, leaching it through water or acid, and removing impurities with precipitant agents, and finally preparing battery-grade lithium carbonate.

Benefits of technology

It reduces the energy consumption of lithium recycling, avoids the use of highly toxic hydrofluoric acid, is suitable for large-scale industrial production, and the prepared lithium carbonate meets the battery-grade standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024084717_01052025_PF_FP_ABST
    Figure CN2024084717_01052025_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a method for recovering lithium from lithium-containing waste. The method comprises the following steps: mixing lithium-containing waste with a roasting additive, and then carrying out aerobic roasting on the obtained mixed powder; leaching the powder subjected to the aerobic roasting, and carrying out solid-liquid separation on same to obtain a lithium-containing solution; and performing purification and impurity removal on the obtained lithium-containing solution, and then preparing a lithium salt, wherein the roasting additive comprises an alkali metal oxide and / or an alkali metal fluoride. In the present application, by means of the use of the roasting additive, the temperature required by aerobic roasting is decreased, the energy consumption of recovering lithium from lithium-containing waste is reduced, the preparation of the lithium salt is realized, and the high added-value recycling of lithium-containing waste is realized.
Need to check novelty before this filing date? Find Prior Art

Description

A method for recovering lithium from lithium-containing waste materials Technical Field

[0001] The present application belongs to the technical field of waste treatment, and relates to a method for treating solid waste, and in particular to a method for recovering lithium from lithium-containing waste. Background Art

[0002] Lithium is a soft, silvery-white metallic element widely used in batteries, ceramics, glass, lubricants, refrigerants, the nuclear industry, and optoelectronics. Existing raw materials for lithium production primarily come from spodumene, lepidolite, petalite, and apatite. This production process is complex, energy-intensive, and capital-intensive. Another source of raw material for lithium production is lithium-containing waste or spent products generated during lithium processing, which represent a crucial renewable resource for lithium recovery.

[0003] CN101892394A discloses a method and apparatus for extracting lithium from lepidolite ore to prepare lithium carbonate. The method comprises the following steps: firstly, lepidolite ore: CaO: one or two of Na2CO3 and K2CO3 are mixed in a mass ratio of 1:0.2-0.4:0.1-0.3, and roasted in a U-shaped roaster; then, the clinker is crushed, slaked lime is added, and lithium precipitation mother liquor, water or residue washing liquid are added in a liquid-to-solid ratio of 2-4:1, followed by leaching, filtering and washing; then, sodium carbonate or a mixed salt of sodium carbonate and potassium carbonate is added to the filtrate to precipitate lithium, precipitate, filter and dry to obtain lithium carbonate; finally, the filtered mother liquor is returned to the autoclave dissolution process, and after multiple cycles, roaster gas is introduced into the filtered mother liquor for evaporation, CO2 is introduced for carbonation, and the mixed salt of potassium carbonate and sodium carbonate is precipitated by cooling and crystallization.

[0004] CN113174480A discloses a method for extracting lithium, rubidium and cesium from silicate minerals containing lithium, rubidium and cesium. The method comprises firstly mixing finely ground silicate ore powder containing lithium, rubidium and cesium with calcium chloride and a chlorine-fixing agent in a certain proportion, then calcining the mixture at a high temperature, and finally leaching the obtained calcined sand. Lithium salts are obtained from the leachate by chemical precipitation, and rubidium salts and cesium salts are obtained from the solution after lithium precipitation by extraction / strip extraction.

[0005] CN114890443A discloses a systematic process method for high-value utilization of lithium-containing waste, comprising the following steps: grinding the lithium-containing waste to a particle size of 60-325 mesh; mixing the lithium-containing waste and auxiliary materials in a certain proportion to obtain a mixed material; placing the obtained mixed material into a high-temperature furnace for high-temperature roasting to obtain a clinker; leaching the obtained clinker and water in a certain proportion to obtain a leachate; removing impurities and purifying the obtained leachate to obtain a purified liquid; evaporating and concentrating the obtained purified liquid to obtain a purified concentrated liquid; and precipitating lithium in the purified concentrated liquid with soda ash, sodium hydroxide or calcium chloride in a certain proportion to obtain a lithium carbonate product, a lithium hydroxide product or a lithium chloride product, respectively.

[0006] While the above methods can recover lithium, they consume a high amount of energy. Furthermore, adding lithium to silicon-based compounds can significantly improve their optical properties. Currently, lithium recovery from silicon-based compounds, primarily composed of silicon dioxide, often involves dissolution with hydrofluoric acid. However, hydrofluoric acid is highly corrosive and toxic, requiring high production equipment and making large-scale recovery difficult.

[0007] Therefore, it is necessary to provide a method for recovering lithium from lithium-containing waste materials with low energy consumption and high efficiency.

[0008] Summary of the Invention

[0009] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0010] The purpose of this application is to provide a method for recovering lithium from lithium-containing waste materials, which can reduce the energy consumption of recovering lithium-containing waste materials, take into account both environmental protection and economic benefits, and is suitable for large-scale industrial production.

[0011] To achieve this goal, this application adopts the following technical solutions:

[0012] The present application provides a method for recovering lithium from lithium-containing waste, the method comprising the following steps:

[0013] (1) mixing lithium-containing waste materials with a roasting additive, and then aerobic roasting the resulting mixed powder;

[0014] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0015] (3) The lithium-containing solution obtained in step (2) is purified and impurities removed, and then the lithium salt is prepared;

[0016] The calcination additive in step (1) includes alkali metal oxide and / or alkali metal fluoride.

[0017] The roasting additive used in the method provided herein includes an alkali metal oxide and / or an alkali metal fluoride, and the roasting additive includes at least one alkali metal fluoride. In other words, the roasting additive described herein is an alkali metal fluoride, or a combination of an alkali metal fluoride and an alkali metal oxide.

[0018] When the roasting additive in step (1) is a combination of an alkali metal fluoride and an alkali metal oxide, the mass ratio of the alkali metal fluoride to the alkali metal oxide is 1:(0.5-1.5), for example, it can be 1:0.5, 1:0.8, 1:1, 1:1.2 or 1:1.5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] The method provided in the present application achieves the directional transformation of lithium in lithium-containing waste materials through the use of roasting additives, making it easy to leach; moreover, in the process of recovering lithium, there is no need to use highly toxic hydrofluoric acid, which reduces the requirements for production equipment, takes into account both environmental protection and economic benefits, and is suitable for large-scale industrial production.

[0020] In one embodiment, the alkali metal oxide comprises MgO and / or CaO.

[0021] In one embodiment, the alkali metal fluoride comprises NaF and / or NH4F.

[0022] In one embodiment, the mass ratio of the lithium-containing waste to the roasting additive in step (1) is 1:(1-5), for example, it can be 1:1, 1:2, 1:3, 1:4 or 1:5, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, and can further be selected as 1:(2-3).

[0023] In one embodiment, the particle size of the lithium-containing waste in step (1) is less than 100 mesh, for example, it can be 120 mesh, 150 mesh, 180 mesh, 200 mesh or 400 mesh, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] The particle size of the lithium-containing waste material is less than 100 mesh in this application, which means that the lithium-containing waste material can pass through a 100 mesh sieve. This application has found that making the particle size of the lithium-containing waste material less than 100 mesh is conducive to the interaction between the lithium-containing waste material and the roasting additive, making it easier for the roasting additive to exert its effect.

[0025] In one embodiment, the Li content in the lithium-containing waste in step (1) is greater than 1 wt%, calculated as oxide, for example, 1 wt%, 3 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt% or 30 wt%, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and can be selected from 1 to 20 wt%, and further selected from 1 to 5 wt%.

[0026] In one embodiment, the oxygen calcination in step (1) is carried out in an air atmosphere.

[0027] In one embodiment, the temperature of the oxygen roasting in step (1) is 300-800°C, for example, it can be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 580°C, 600°C, 650°C, 700°C or 800°C, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, and can further be selected as 300-580°C.

[0028] The method provided in the present application can achieve aerobic roasting at conditions as low as 300°C by using specific roasting additives, and the powder after roasting is easy to leach, which facilitates the recovery of lithium from lithium-containing waste and reduces the energy consumption of lithium recovery.

[0029] In one embodiment, the oxygen roasting time in step (1) is 1-5 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] In one embodiment, the leaching comprises water leaching and / or acid leaching.

[0031] In one embodiment, the solid-liquid ratio of the water immersion is (50-200):1, for example, it can be 50:1, 80:1, 100:1, 120:1, 150:1, 180:1 or 200:1, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable. The unit of the solid-liquid ratio is g / L.

[0032] In one embodiment, the water immersion temperature is 30-90°C, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] In one embodiment, the immersion time is 0.5-5 hours, for example, 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] In one embodiment, the concentration of the acid solution used for acid leaching is 0.01-0.1 mol / L, for example, it can be 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.06 mol / L, 0.08 mol / L or 0.1 mol / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] In one embodiment, the acid used in the acid solution includes sulfuric acid and / or hydrochloric acid.

[0036] In one embodiment, the solid-liquid ratio of the acid leaching is (50-200):1, for example, it can be 50:1, 80:1, 100:1, 120:1, 150:1, 180:1 or 200:1, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable. The unit of the solid-liquid ratio is g / L.

[0037] In one embodiment, the acid leaching temperature is 30-90°C, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0038] In one embodiment, the acid leaching time is 0.5-5 hours, for example, 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0039] In one embodiment, the purification and impurity removal in step (3) is to add a precipitant to perform precipitation and impurity removal.

[0040] The impurity ions in the lithium-containing solution obtained in step (2) mainly include Ca 2+ Mg 2+ and Al 3+ The present application uses a precipitant to precipitate and remove impurities, which is beneficial to obtaining battery-grade lithium salt.

[0041] In one embodiment, the precipitating agent is a combination of sodium hydroxide and sodium carbonate.

[0042] In one embodiment, the amount of sodium carbonate added is 1-10 g / L, for example, 1 g / L, 3 g / L, 5 g / L, 8 g / L or 10 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] In one embodiment, the amount of sodium hydroxide added is such that the pH value of the system is 11-12, for example, 11, 11.2, 11.5, 11.6, 11.8 or 12, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] In one embodiment, the lithium salt in step (3) comprises lithium carbonate.

[0045] The method provided in this application can obtain battery-grade lithium carbonate. The method of preparing lithium carbonate after purification and impurity removal is a commonly used method in the field and will not be described in detail in this application.

[0046] As an optional technical solution of the method provided in this application, the method comprises the following steps:

[0047] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:(1-5), and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0048] The particle size of the lithium-containing waste is less than 100 mesh;

[0049] The temperature of the oxygen roasting is 300-580°C and the time is 1-5h;

[0050] The calcination additive includes any one of MgO, CaO, NaF or NH4F or a combination of at least two thereof;

[0051] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0052] The leaching includes water leaching and / or acid leaching;

[0053] The leaching temperature is 30-90° C., the leaching time is 0.5-5 h, the solid-liquid ratio is (50-200):1, and the unit of the solid-liquid ratio is g / L;

[0054] (3) adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and then preparing lithium carbonate;

[0055] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 1-10 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11-12.

[0056] Compared with the prior art, this application has the following beneficial effects:

[0057] The method provided herein employs a calcination additive comprising an alkali metal oxide and / or an alkali metal fluoride, with the calcination additive comprising at least one alkali metal fluoride. By using the calcination additive, the method provided herein achieves a targeted transformation of lithium from lithium-containing waste, facilitating leaching. Furthermore, the lithium recovery process eliminates the need for highly toxic hydrofluoric acid, reducing production equipment requirements and balancing environmental and economic benefits, making it suitable for large-scale industrial production.

[0058] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0060] FIG1 is an XRD spectrum of lithium carbonate obtained by the method provided in Example 1. DETAILED DESCRIPTION

[0061] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.

[0062] In order to clearly illustrate the technical solution of the present application, the lithium-containing waste in the specific embodiment of the present application is a lithium-containing waste silicon-based compound, whose main components include 5.27wt% Li2O, 35.2wt% SiO2, 5.68wt% Al2O3, 2.85wt% K2O, 1.06wt% CaO, 1.33wt% MgO and 6.92wt% Na2O; the particle size of the lithium-containing waste silicon-based compound treated in the specific embodiment is 100 mesh-200 mesh, that is, the lithium-containing waste silicon-based compound can pass through a 100 mesh sieve but cannot pass through a 200 mesh sieve.

[0063] The above-mentioned composition limitations and parameter limitations of lithium-containing waste are only for clarifying the technical solution of the present application and are not regarded as further limitations on lithium-containing waste.

[0064] Example 1

[0065] This embodiment provides a method for recovering lithium from lithium-containing waste materials, the method comprising the following steps:

[0066] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:2.5, and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0067] The oxygen roasting temperature is 550°C and the time is 3 hours;

[0068] The roasting additive is NH4F;

[0069] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0070] The leaching is water leaching;

[0071] The leaching temperature is 60° C., the leaching time is 3 h, the solid-liquid ratio is 100:1, and the unit of the solid-liquid ratio is g / L;

[0072] (3) Adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and the Ca in the solution 2+ Mg 2+ and Al 3+ Reduce to below 1 ppm, and then use conventional methods to prepare battery-grade lithium carbonate;

[0073] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 5 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11.5.

[0074] The XRD spectrum of the lithium carbonate obtained in this example is shown in FIG1 .

[0075] Example 2

[0076] This embodiment provides a method for recovering lithium from lithium-containing waste materials, the method comprising the following steps:

[0077] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:2, and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0078] The temperature of the oxygen roasting is 580°C and the time is 1 hour;

[0079] The roasting additive is NH4F;

[0080] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0081] The leaching is water leaching;

[0082] The leaching temperature is 30° C., the leaching time is 5 h, the solid-liquid ratio is 200:1, and the unit of the solid-liquid ratio is g / L;

[0083] (3) Adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and the Ca in the solution 2+ Mg 2+ and Al 3+ Reduce to below 1 ppm, and then use conventional methods to prepare battery-grade lithium carbonate;

[0084] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 1 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11.

[0085] Example 3

[0086] This embodiment provides a method for recovering lithium from lithium-containing waste materials, the method comprising the following steps:

[0087] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:3, and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0088] The temperature of the oxygen roasting is 300°C and the time is 5 hours;

[0089] The roasting additive is NH4F;

[0090] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0091] The leaching is water leaching;

[0092] The leaching temperature is 90° C., the leaching time is 0.5 h, the solid-liquid ratio is 50:1, and the unit of the solid-liquid ratio is g / L;

[0093] (3) Adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and the Ca in the solution 2+ Mg 2+ and Al 3+ Reduce to below 1 ppm, and then use conventional methods to prepare battery-grade lithium carbonate;

[0094] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 10 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 12.

[0095] Example 4

[0096] This embodiment provides a method for recovering lithium from lithium-containing waste materials, the method comprising the following steps:

[0097] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:2.5, and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0098] The oxygen roasting temperature is 550°C and the time is 3 hours;

[0099] The roasting additive is NH4F;

[0100] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0101] The leaching is hydrochloric acid leaching;

[0102] The leaching temperature is 90° C., the time is 0.5 h; the solid-liquid ratio is 200:1, and the unit of the solid-liquid ratio is g / L; the concentration of the acid solution used for leaching is 0.01 mol / L;

[0103] (3) Adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and the Ca in the solution 2+ Mg 2+ and Al 3+ Reduce to below 1 ppm, and then use conventional methods to prepare battery-grade lithium carbonate;

[0104] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 5 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11.5.

[0105] Example 5

[0106] This embodiment provides a method for recovering lithium from lithium-containing waste materials, the method comprising the following steps:

[0107] (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:2.5, and then aerobically roasting the resulting mixed powder in an air atmosphere;

[0108] The oxygen roasting temperature is 550°C and the time is 3 hours;

[0109] The roasting additive is NH4F;

[0110] (2) leaching the powder after oxygen roasting, separating the solid and liquid, and obtaining a lithium-containing solution;

[0111] The leaching is hydrochloric acid leaching;

[0112] The leaching temperature is 30°C, the time is 5 hours; the solid-liquid ratio is 50:1, and the unit of the solid-liquid ratio is g / L; the concentration of the acid solution used for leaching is 0.1 mol / L;

[0113] (3) Adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and the Ca in the solution 2+ Mg 2+ and Al 3+ Reduce to below 1 ppm, and then use conventional methods to prepare battery-grade lithium carbonate;

[0114] The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 5 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11.5.

[0115] Example 6

[0116] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the roasting additive is NaF, the rest is the same as that of Example 1.

[0117] Example 7

[0118] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the roasting additive is a combination of NH4F and CaO, the rest is the same as that of Example 1.

[0119] In this embodiment, the mass ratio of NH4F to CaO is 1:1.

[0120] Example 8

[0121] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the roasting additive is a combination of NH4F and MgO, the rest is the same as that of Example 1.

[0122] In this embodiment, the mass ratio of NH4F to MgO is 1:1.

[0123] Example 9

[0124] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the mass ratio of the lithium-containing waste materials to the roasting additive is 1:1, the rest is the same as that of Example 1.

[0125] Example 10

[0126] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the mass ratio of lithium-containing waste materials to roasting additives is 1:5, the rest is the same as that of Example 1.

[0127] Example 11

[0128] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the mass ratio of lithium-containing waste materials to roasting additives is 1:0.5, the rest is the same as that of Example 1.

[0129] Example 12

[0130] This embodiment provides a method for recovering lithium from lithium-containing waste materials. Except that the mass ratio of lithium-containing waste materials to roasting additives is 1:6, the rest is the same as that of Example 1.

[0131] Comparative Example 1

[0132] This comparative example provides a method for recovering lithium from lithium-containing waste materials, which is the same as Example 1 except that the roasting additive is CaO.

[0133] Comparative Example 2

[0134] This comparative example provides a method for recovering lithium from lithium-containing waste materials. Except that the roasting additive is MgO, the rest is the same as Example 1.

[0135] The lithium leaching rate and the recovery rate of lithium from lithium-containing waste materials in the methods provided in Examples 1-12 and Comparative Examples 1-2 were measured, and the results are shown in Table 1.

[0136] Table 1

[0137] In summary, the method provided by this application achieves a directional transformation of lithium in lithium-containing waste materials through the use of a roasting additive, making it easy to leach. Moreover, in the process of recovering lithium, there is no need to use highly toxic hydrofluoric acid, which reduces the requirements for production equipment, takes into account both environmental protection and economic benefits, and is suitable for large-scale industrial production. Moreover, the method provided by this application can achieve aerobic roasting at conditions as low as 300°C, and the powder after roasting is easy to leach, which facilitates the recovery of lithium from lithium-containing waste materials and reduces the energy consumption of lithium recovery.

[0138] The above description is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Those skilled in the art should understand that any changes or replacements that can be easily thought of by those skilled in the art within the technical scope disclosed in the present application fall within the protection scope and disclosure scope of the present application.

Claims

1. A method for recovering lithium from lithium-containing waste materials, comprising the steps of: (1) mixing lithium-containing waste and a roasting additive, and then aerobic roasting the resulting mixed powder; (2) leaching the powder after oxygen roasting, separating the solid and the liquid, and obtaining a lithium-containing solution; (3) The lithium-containing solution obtained in step (2) is purified and impurities removed, and then lithium salt is prepared; The calcination additive in step (1) includes alkali metal oxides and / or alkali metal fluorides.

2. The method according to claim 1, wherein: The alkali metal oxide includes MgO and / or CaO; Optionally, the alkali metal fluoride comprises NaF and / or NH4F.

3. The method according to claim 1 or 2, wherein: The mass ratio of the lithium-containing waste material to the roasting additive in step (1) is 1:(1-5); Optionally, the particle size of the lithium-containing waste in step (1) is less than 100 mesh; Optionally, the Li content in the lithium-containing waste in step (1) is above 1 wt %, calculated as oxide.

4. The method according to any one of claims 1 to 3, wherein: The oxygen calcination in step (1) is carried out in an air atmosphere.

5. The method according to any one of claims 1 to 4, wherein: The temperature of the oxygen roasting in step (1) is 300-800°C, and can be further 300-580°C; Optionally, the aerobic roasting time in step (1) is 1-5 hours.

6. The method according to any one of claims 1 to 5, wherein: The leaching includes water leaching and / or acid leaching.

7. The method according to claim 6, wherein: The solid-liquid ratio of the water immersion is (50-200):1, and the unit of the solid-liquid ratio is g / L; Optionally, the water immersion temperature is 30-90°C; Optionally, the water immersion time is 0.5-5h; Optionally, the concentration of the acid solution used for the acid leaching is 0.01-0.1 mol / L; Optionally, the acid used in the acid solution includes sulfuric acid and / or hydrochloric acid; Optionally, the solid-liquid ratio of the acid leaching is (50-200):1, and the unit of the solid-liquid ratio is g / L; Optionally, the acid leaching temperature is 30-90°C; Optionally, the acid leaching time is 0.5-5h.

8. The method according to any one of claims 1 to 7, wherein: The purification and impurity removal in step (3) is to add a precipitant to perform precipitation and impurity removal; Optionally, the precipitant is a combination of sodium hydroxide and sodium carbonate; Optionally, the amount of sodium carbonate added is 1-10 g / L; Optionally, the amount of sodium hydroxide added is such that the pH value of the system is 11-12.

9. The method according to any one of claims 1 to 8, wherein: The lithium salt in step (3) includes lithium carbonate.

10. The method according to any one of claims 1 to 9, wherein: The method comprises the following steps: (1) mixing lithium-containing waste and a roasting additive in a mass ratio of 1:(1-5), and then aerobically roasting the resulting mixed powder in an air atmosphere; The particle size of the lithium-containing waste is less than 100 mesh; The temperature of the oxygen roasting is 300-580°C and the time is 1-5h; The calcination additive includes any one of MgO, CaO, NaF or NH4F or a combination of at least two thereof; (2) leaching the powder after oxygen roasting, separating the solid and the liquid, and obtaining a lithium-containing solution; The leaching includes water leaching and / or acid leaching; The leaching temperature is 30-90°C, the time is 0.5-5h; the solid-liquid ratio is (50-200):1, and the unit of the solid-liquid ratio is g / L; (3) adding a precipitant to the lithium-containing solution obtained in step (2) to precipitate and remove impurities, and then preparing lithium carbonate; The precipitant is a combination of sodium hydroxide and sodium carbonate; the amount of sodium carbonate added is 1-10 g / L, and the amount of sodium hydroxide added is such that the pH value of the system is 11-12.

Citation Information

Patent Citations

  • Process of producing lithium carbonate

    CA1297265C

  • Method for selectively extracting lithium from waste lithium ion battery materials

    CN110835683A

  • Composite additive for treating lepidolite ore and application thereof

    CN111534705A

  • Method for extracting lithium, rubidium and caesium from silicate mineral containing lithium, rubidium and caesium

    CN113174480A

  • Method for extracting lithium from waste lithium iron phosphate battery

    CN116814984A

Cited By

  • Preparation method and device of high-purity metal lithium

    CN122168914A