Method for producing molybdenum dithiocarbamate, molybdenum dithiocarbamate obtained by said production method, and lubricating oil composition or grease composition containing said molybdenum dithiocarbamate
A method for producing molybdenum dithiocarbamate with high sulfur content is achieved through controlled reactions of molybdenum compounds, sulfur sources, and amine compounds, addressing low yield and equipment constraints of existing methods, resulting in improved lubricity and friction reduction.
Patent Information
- Application Number
- PCT/JP2025/014900
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-26
- Filing Date
- 2025-04-16
- Publication Date
- 2025-10-30
AI Technical Summary
Existing methods for producing molybdenum dithiocarbamate suffer from low purity and yield, and require specialized equipment for high-pressure reactions.
A method involving the reaction of molybdenum compounds, sulfur sources like octasulfur and carbon disulfide, and amine compounds in specific organic solvents at controlled conditions to produce a DTC intermediate, followed by reduction to obtain molybdenum dithiocarbamate with high sulfur content.
Facilitates the production of molybdenum dithiocarbamate with high sulfur content in high yield, using readily available equipment and conditions, enhancing its lubricity and reducing friction properties.
Smart Images

Figure JP2025014900_30102025_PF_FP_ABST
Abstract
Description
Method for producing molybdenum dithiocarbamate, molybdenum dithiocarbamate obtained by said method, and lubricating oil or grease composition containing said molybdenum dithiocarbamate
[0001] The present invention relates to a method for producing molybdenum dithiocarbamate, which can produce molybdenum dithiocarbamate with a high sulfur content in high yield.
[0002] In the automotive field, regulations such as fuel economy regulations and exhaust gas regulations, which stem from environmental issues such as global warming, air pollution, and acid rain, as well as the protection of limited resources such as petroleum energy, are becoming stricter every year. To address these issues, for example, in order to promote fuel economy in automobiles, not only improvements to the automobile itself, such as weight reduction of the automobile body and engine improvements, but also improvements to engine oils, such as lowering the viscosity of engine oils to prevent friction loss in the engine and adding good friction modifiers, are important factors. Among friction modifiers, molybdenum dithiocarbamate has excellent lubricity and friction-reducing properties, and is less corrosive to metals, so it is added to various lubricating oils.
[0003] As a method for producing molybdenum dithiocarbamate, Patent Document 1 describes a method in which carbon disulfide and a secondary amine are added to an aqueous solution of pH 8.5 to 11 containing molybdenum trioxide or an alkali metal salt of molybdic acid and an alkali hydrosulfide or alkali sulfide.
[0004] Furthermore, Patent Document 2 describes a method for producing highly sulfurized molybdenum dithiocarbamate, which is believed to provide good antioxidant stability and improved antifriction retention properties, comprising the steps of reacting a metal source, water, at least one reagent amine, and carbon disulfide under pressure at a temperature higher than the normal boiling point of carbon disulfide.
[0005] JP-A-4-182494 Publication Special Publication No. 2009-512735
[0006] According to the method described in Patent Document 1, it is said that an organomolybdenum compound having a relatively high sulfur content compared to conventional organomolybdenum compounds can be obtained, but there is a problem in that the purity and yield of the obtained product are insufficient.
[0007] According to the method described in Patent Document 2, molybdenum dithiocarbamate with a high sulfur content ratio, which is considered to have excellent properties, can be obtained. However, the method described in Patent Document 2 requires special equipment for carrying out the reaction under a heated and pressurized environment. Therefore, there has been a demand for the development of a simpler method for producing molybdenum dithiocarbamate with a high sulfur content ratio.
[0008] Therefore, an object of the present invention is to provide a method for producing molybdenum dithiocarbamate, which can produce molybdenum dithiocarbamate having a high sulfur content in high yield.
[0009] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have discovered that a production method having specific steps can produce molybdenum dithiocarbamate having a high sulfur content in high yield, and have thus completed the present invention. That is, the present invention is a method for producing molybdenum dithiocarbamate, comprising: a DTC step of reacting one or more molybdenum compounds selected from the group consisting of molybdic acid and its salts, a sulfur source including octasulfur and carbon disulfide, and an amine compound represented by the following general formula (1) to obtain a DTC intermediate; and a reduction step of reducing the obtained DTC intermediate in the presence of a reducing agent to obtain a molybdenum dithiocarbamate represented by the following general formula (2):
[0010]
[0011] (In the formula, R 1 ~R 2 each independently represents a hydrocarbon group having 4 to 14 carbon atoms.
[0012]
[0013] (In the formula, R 3 ~R 6 each independently represents a hydrocarbon group having 4 to 14 carbon atoms; X1 ~X 4 each independently represents an oxygen atom or a sulfur atom.
[0014] According to the present invention, there can be provided a method for producing molybdenum dithiocarbamate, which can produce molybdenum dithiocarbamate with a high sulfur content in high yield.
[0015] A. Method for Producing Molybdenum Dithiocarbamate Hereinafter, the method for producing the molybdenum dithiocarbamate of the present invention will be described.
[0016] A1. DTC Formation Step The DTC formation step in the method for producing molybdenum dithiocarbamate of the present invention is a step of reacting one or more molybdenum compounds selected from the group consisting of molybdic acid and its salts, a sulfur source containing octasulfur and carbon disulfide, and an amine compound represented by general formula (1) to obtain a DTC (dithiocarbamate) intermediate.
[0017] (1) Molybdenum Compound In the present invention, the molybdenum compound used in the DTC formation step is one or more selected from the group consisting of molybdic acid and its salts. Examples of molybdic acid include molybdenum trioxide and molybdenum trioxide hydrate. Examples of molybdic acid salts include ammonium molybdate, sodium molybdate, potassium molybdate, sodium hydrogen molybdate, molybdic acid chloride, molybdic acid bromide, and molybdic heteropolyacid. One or more of these can be used. In the present invention, among these, it is preferable to use one or more molybdenum compounds selected from the group consisting of molybdenum trioxide, molybdenum trioxide hydrate, sodium molybdate, and potassium molybdate. It is even more preferable to use one or more molybdenum compounds selected from the group consisting of molybdenum trioxide and molybdenum trioxide hydrate.
[0018] (2) Sulfur Source In the present invention, the sulfur source used in the DTC formation step is a sulfur source containing octasulfur and carbon disulfide. Octasulfur is an inorganic compound composed of eight sulfur elements, represented by the chemical formula S8, and its CAS number is 10544-50-0. In the present invention, the combined use of octasulfur and carbon disulfide makes it possible to easily obtain molybdenum dithiocarbamate with a high sulfur content in a high yield. Other sulfur sources, such as polysulfide compounds, can also be used in the DTC formation step. However, from the viewpoint of easily obtaining molybdenum dithiocarbamate with a high sulfur content in a high yield, the total sulfur content of octasulfur and carbon disulfide in the sulfur source is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 100% by mass (the sulfur source is composed of octasulfur and carbon disulfide) relative to the total sulfur content in the sulfur source. The ratio of octasulfur to carbon disulfide used as the sulfur source is not particularly limited, but from the viewpoint of facilitating the production of molybdenum dithiocarbamate with a high elemental sulfur content in high yield, it is preferable to adjust the mass ratio of the octasulfur to carbon disulfide so that the mass ratio of the elemental sulfur content of the octasulfur to the elemental sulfur content of carbon disulfide is 10:90 to 90:10. The mass ratio of the elemental sulfur content of the octasulfur to the elemental sulfur content of carbon disulfide is more preferably 20:80 to 80:20, even more preferably 30:70 to 70:30, and particularly preferably 40:60 to 60:40.
[0019] In this DTC process, the use of octasulfur in addition to carbon disulfide, which has conventionally been used as a sulfur source, is believed to facilitate easy and efficient production of DTC intermediates represented by the following general formulas (3) to (5), and is believed to facilitate the production of a DTC intermediate represented by general formula (5) having a high sulfur content.
[0020]
[0021] (In the formula, R 7 ~R 10 each independently represents a hydrocarbon group having 4 to 14 carbon atoms.
[0022]
[0023] (In the formula, R 11 ~R 14 each independently represents a hydrocarbon group having 4 to 14 carbon atoms.
[0024]
[0025] (In the formula, R 15 ~R 18 each independently represents a hydrocarbon group having 4 to 14 carbon atoms.
[0026] R in general formula (3) 7 ~R 10 , R in general formula (4) 11 ~R 14 , R in general formula (5) 15 ~R 18 Examples of the hydrocarbon group having 4 to 14 carbon atoms represented by each of the formulas include linear alkyl groups such as n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-uncyl, n-dodecyl, n-tridecyl, and n-tetradecyl groups; secondary butyl, isobutyl, secondary pentyl, isopentyl, secondary hexyl, isohexyl, secondary heptyl, isoheptyl, secondary octyl, isooctyl, secondary nonyl, isononyl, secondary decyl, isodecyl, and secondary undecyl groups; Examples of the alkyl group include branched alkyl groups such as a soundecyl group, a secondary dodecyl group, an isododecyl group, a secondary tridecyl group, an isotridecyl group, a secondary tetradecyl group, and an isotetradecyl group, unsaturated hydrocarbon groups such as a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, and a tetradecenyl group, alicyclic hydrocarbon groups such as a cyclohexyl group, a methylcyclohexyl group, a dimethylcyclohexyl group, and an ethylcyclohexyl group, and aromatic hydrocarbon groups such as a phenyl group and a benzyl group. 7 ~R 10 , R in general formula (4) 11 ~R 14 , R in general formula (5) 15 ~R 18correspond to the structure of the hydrocarbon group of the amine compound used in the DTC formation step.
[0027] (3) Amine Compound In the present invention, the amine compound used in the DTC formation step is an amine compound having a hydrocarbon group having 4 to 14 carbon atoms and represented by the following general formula (1):
[0028]
[0029] In general formula (1), R 1 ~R 2 each independently represents a hydrocarbon group having 4 to 14 carbon atoms. Examples of the hydrocarbon group having 4 to 14 carbon atoms include linear alkyl groups such as n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-uncyl, n-dodecyl, n-tridecyl, and n-tetradecyl groups; secondary butyl, isobutyl, secondary pentyl, isopentyl, secondary hexyl, isohexyl, secondary heptyl, isoheptyl, secondary octyl, isooctyl, secondary nonyl, isononyl, secondary decyl, isodecyl, secondary undecyl, and isoonyl. Examples of the amine compound used in the DTC formation step include branched alkyl groups such as a decyl group, a secondary dodecyl group, an isododecyl group, a secondary tridecyl group, an isotridecyl group, a secondary tetradecyl group, and an isotetradecyl group, unsaturated hydrocarbon groups such as a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, and a tetradecenyl group, alicyclic hydrocarbon groups such as a cyclohexyl group, a methylcyclohexyl group, a dimethylcyclohexyl group, and an ethylcyclohexyl group, and aromatic hydrocarbon groups such as a phenyl group and a benzyl group. 1 and R 2 Even in the case of an amine compound in which R 1 and R 2 may be an amine compound in which R is a hydrocarbon group different from R. However, from the viewpoint of facilitating the production of a molybdenum dithiocarbamate having a high sulfur content in a high yield, 1 and R 2In the DTC formation step, one type of amine compound or two or more types of amine compounds may be used.
[0030] In the present invention, the amine compound used in the DTC formation step is selected from the amine compounds represented by general formula (1) of which R 1 ~R 2 are each independently a linear alkyl group having 4 to 14 carbon atoms or a branched alkyl group having 4 to 14 carbon atoms, and R 1 ~R 2 are each independently a linear alkyl group having 8 to 13 carbon atoms or a branched alkyl group having 8 to 13 carbon atoms, and 1 ~R 2 are each independently a linear alkyl group having 8 or 13 carbon atoms or a branched alkyl group having 8 or 13 carbon atoms, and 1 ~R 2 It is particularly preferable to use an amine compound in which each of the groups independently represents a branched alkyl group having 8 or 13 carbon atoms.
[0031] (4) Organic Solvent In the DTC formation step, from the viewpoint of facilitating the production of molybdenum dithiocarbamate having a high sulfur content ratio in a higher yield, the molybdenum compound, the sulfur source, and the amine compound are dissolved in an organic solvent having a dispersion term δd in the Hansen solubility parameter of 15.0 to 17.5 (MPa). 1 / 2 , the value of the bipolar term δp is 0 to 6.8 (MPa) 1 / 2 , hydrogen bond parameter δh is 10.0 to 17.5 (MPa) 1 / 2It is preferable to carry out the reaction in the presence of an organic solvent which is a monohydric alcohol having 3 to 8 carbon atoms, such as 1-propanol, 2-propanol, 1-butanol, 2-butanol, t-butyl alcohol, 1-pentanol, 2-pentanol, 3-methyl-1-butanol, 2-methyl-2-butanol, 1-hexanol, 2-hexanol, cyclohexanol, 2-methyl-2-pentanol, 3-methyl-1-pentanol, 1-heptanol, 2-heptanol, 1-octanol, 2-octanol, and 2-ethylhexanol. Examples of suitable organic solvents include glycol ethers such as ethanol, ethylene glycol monobutyl ether, ethylene glycol mono-n-hexyl ether, ethylene glycol mono-2-ethylhexyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monoisopropyl ether, propylene glycol mono-t-butyl ether, dipropylene glycol mono-n-propyl ether, and tripropylene glycol monomethyl ether, and one or more of these can be used. In the present invention, the use of such an organic solvent in the DTC formation step can improve the reactivity of the molybdenum compound with the sulfur source and the amine compound, thereby enabling the DTC formation intermediate to be obtained more efficiently and, as a result, enabling the production of molybdenum dithiocarbamate with a high sulfur content in high yield.
[0032] Furthermore, in the present invention, the use of an organic solvent having a boiling point of 110°C or higher as the organic solvent is preferred, since this can prevent evaporation of the organic solvent and destabilization of the system during the reaction, allowing the target reaction to proceed stably, and enabling the production of molybdenum dithiocarbamate with a higher sulfur content more easily. Among the above-mentioned organic solvents, in the present invention, from the viewpoint of easily and efficiently obtaining a DTC intermediate and a molybdenum dithiocarbamate with a higher sulfur content, an organic solvent having a dispersion term δd in the Hansen solubility parameter of 15.0 to 16.5 (MPa) is preferred. 1 / 2 , the value of the bipolar term δp is 3.0 to 6.5 (MPa) 1 / 2, hydrogen bond parameter δh is 11.0 to 17.0 (MPa) 1 / 2 It is more preferable to use a monohydric alcohol having 3 to 8 carbon atoms, more preferably 1-propanol, 2-propanol, 1-butanol, 2-butanol, 1-hexanol, 2-hexanol, cyclohexanol, 2-ethylhexanol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, it is even more preferable to use 1-propanol, 2-propanol, 1-butanol, 2-butanol, cyclohexanol, 2-ethylhexanol, 2-butanol, and propylene glycol monomethyl ether, and it is particularly preferable to use 1-butanol. In the present invention, the dispersion term δd representing the London dispersion energy, the polar term δp representing the dipole-dipole interaction energy, and the hydrogen bond term δh representing the hydrogen bond energy in the Hansen solubility parameters are values calculated by the van Krevelen & Hoftyzer method based on the atomic group contribution method.
[0033] (5) Reaction Conditions The DTC formation step in the present invention is a step of reacting the molybdenum compound, sulfur source, and amine compound described above. The ratio of the raw materials used in the DTC formation step is not particularly limited, and can be adjusted appropriately as long as it results in a DTC intermediate. In this case, the raw materials may be added in their entirety at once and reacted, or may be added in two or more portions and reacted. The conditions for reacting the molybdenum compound, sulfur source, and amine compound are also not particularly limited, and any reaction temperature and reaction time may be used as long as a DTC intermediate is obtained. For example, the reaction temperature is preferably 10 to 100°C, more preferably 20 to 70°C, and even more preferably 20 to 50°C. The reaction time is preferably 30 minutes to 15 hours, more preferably 1 to 10 hours.
[0034] (6) Molar Equivalent Ratio of Each Element and Amine In the DTC formation step, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio (Mo:S) of the Mo element contained in the molybdenum compound to the S element contained in the sulfur source is preferably 1:1.5 to 1:10, more preferably 1:2 to 1:8, even more preferably 1:3 to 1:6, and particularly preferably 1:4 to 1:5. In this case, from the viewpoint of facilitating the production of a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of Mo contained in the molybdenum compound used, S contained in the octasulfur compound used as the sulfur source, and S contained in the carbon disulfide is preferably 1:0.2-5:0.1-6, more preferably 1:0.8-4:1-5, even more preferably 1:1-3:1.1-4, and particularly preferably 1:1.2-2.5:1.2-3.
[0035] In the DTC formation step, from the viewpoint of facilitating the production of a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of Mo contained in the molybdenum compound to the amine compound (Mo:amine) is preferably 1:0.8 to 1:2, more preferably 1:1 to 1:1.5, even more preferably 1:1.01 to 1:1.3, and particularly preferably 1:1.02 to 1:1.2.
[0036] In the DTC conversion step, from the viewpoint of facilitating the production of a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of the S element contained in the sulfur source to the amine compound (S:amine) is preferably 10:2 to 1.5:0.8, more preferably 8:1 to 1:1.5, even more preferably 6:1.01 to 3:1.3, and particularly preferably 5:1.02 to 5:1.2.
[0037] In the DTC formation step, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound used, the S element contained in the sulfur source, and the amine compound, where the molar equivalent of Mo is taken as 1, is preferably 1:1.5-10:0.8-2, more preferably 1:2-8:1-1.5, even more preferably 1:3-6:1.01-1.3, and particularly preferably 1:4-5:1.02-1.2.
[0038] (7) Molar Equivalent Ratio of Each Element and Amine to Organic Solvent When the DTC conversion step is carried out in the presence of the above-mentioned organic solvent, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of the S element contained in the sulfur source used to the organic solvent (S:organic solvent) is preferably 10:0.05 to 1.5:10, more preferably 8:0.1 to 2:5, even more preferably 6:0.2 to 3:3, and particularly preferably 5:0.3 to 4:2.
[0039] When the DTC conversion step is carried out in the presence of the above-mentioned organic solvent, from the viewpoint of facilitating the production of a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of the amine compound to the organic solvent (amine:organic solvent) used is preferably 2:0.05 to 0.8:10, more preferably 1.5:0.1 to 1:5, even more preferably 1.3:0.2 to 1.01:3, and particularly preferably 1.2:0.3 to 1.02:2.
[0040] When the DTC formation step is carried out in the presence of the above-mentioned organic solvent, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of Mo contained in the molybdenum compound used to the organic solvent (Mo:organic solvent) is preferably 1:0.05 to 1:10, more preferably 1:0.1 to 1:5, even more preferably 1:0.2 to 1:3, and particularly preferably 1:0.3 to 1:2.
[0041] When the DTC formation step is carried out in the presence of the above-mentioned organic solvent, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the molar equivalent ratio of the Mo element contained in the molybdenum compound used, the S element contained in the sulfur source, the amine compound, and the organic solvent (Mo:S:amine:organic solvent), where the molar equivalent of Mo is taken as 1, is preferably 1:1.5-10:0.8-2:0.05-10, more preferably 1:2-8:1-1.5:0.1-5, even more preferably 1:3-6:1.01-1.3:0.2-3, and particularly preferably 1:4-5:1.02-1.2:0.3-2.
[0042] A2. Reduction Step The reduction step in the method for producing molybdenum dithiocarbamate of the present invention is a step in which the DTC intermediate obtained in the above-mentioned DTC step is reduced in the presence of a reducing agent to obtain a molybdenum dithiocarbamate represented by the following general formula (2):
[0043]
[0044] (In the formula, R 3 ~R 6 each independently represents a hydrocarbon group having 4 to 14 carbon atoms; X 1 ~X 4 each independently represents an oxygen atom or a sulfur atom.
[0045] (1) Reducing Agent In the present invention, the reducing agent used in the reduction step is not particularly limited as long as it is a compound that can cause a reduction reaction of the DTC intermediate. Examples of the reducing agent include alkali sulfides such as sodium sulfide, sodium polysulfide, potassium sulfide, and ammonium sulfide; alkali hydrosulfides such as sodium hydrosulfide and potassium hydrosulfide; hydrides such as hydrogen iodide, hydrogen sulfide, and sodium borohydride; salts of lower oxygen acids such as sodium sulfite, sodium dithionite, sodium dithionite (hydrosulfide), sodium hydrogensulfite, sodium pyrosulfite, and sodium thiosulfate; salts of metals in a low valence state such as iron(II), tin(II), titanium(III), and chromium(II); aldehydes such as formaldehyde and acetaldehyde; hydrazine, borane, diborane, formic acid, oxalic acid, and ascorbic acid. One or more of these may be used. In the present invention, among these, from the viewpoint of facilitating the production of molybdenum dithiocarbamate having a high sulfur content in high yield, it is preferable to use one or more selected from the group consisting of alkali sulfides, alkali hydrosulfides, and salts of lower oxygen acids, it is more preferable to use one or more selected from the group consisting of alkali hydrosulfides and salts of lower oxygen acids, it is even more preferable to use one or more selected from the group consisting of sodium hydrosulfide, potassium hydrosulfide, sodium pyrosulfite, and sodium thiosulfate, and it is particularly preferable to use sodium hydrosulfide. When sodium hydrosulfide is used as the reducing agent, it is preferably used in the form of a 10% to 70% aqueous solution from the viewpoint of safety.
[0046] The amount of reducing agent used in the reduction step is not particularly limited as long as it is an amount that can reduce the DTC intermediate obtained in the above-mentioned DTC step. However, from the viewpoint of facilitating the high yield of molybdenum dithiocarbamate with a high sulfur content, the amount of reducing agent is preferably 0.5 to 3 mol, more preferably 1 to 2.5 mol, even more preferably 1.2 to 2.2 mol, and particularly preferably 1.4 to 2 mol, per mol of Mo contained in the DTC intermediate.
[0047] (2) Reaction Conditions The reduction step in the present invention is a step in which the DTC intermediate obtained in the above-described DTC step is reduced in the presence of a reducing agent. In this step, the reduction temperature is not particularly limited and can be adjusted as appropriate. However, from the viewpoint of easily obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, the reduction temperature is preferably 40°C to 120°C, more preferably 60°C to 110°C, and even more preferably 70°C to 100°C. Furthermore, the reduction time is not particularly limited and can be adjusted as appropriate. However, from the viewpoint of efficiently obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, reduction is preferably carried out for 0.5 to 20 hours, and more preferably for 1 to 10 hours.
[0048] In the present invention, by carrying out such a reduction step, it is possible to obtain the molybdenum dithiocarbamate represented by the general formula (2) in high yield from the DTC intermediate described above, and in particular, it is possible to easily obtain a molybdenum dithiocarbamate with a high sulfur content, which is considered to have excellent properties among the molybdenum dithiocarbamates represented by the general formula (2), in high yield. Here, the molybdenum dithiocarbamate with a high sulfur content is a molybdenum dithiocarbamate represented by the general formula (2) in which X 1 ~X 4 Molybdenum dithiocarbamates with a high ratio of sulfur atoms in X 1 ~X 4 The molybdenum dithiocarbamate refers to a molybdenum dithiocarbamate in which the ratio of the number of oxygen atoms to the number of sulfur atoms in the formula (I) is 1.8-0:2.2-4.
[0049] A3. Other Steps In addition to the DTC formation step and reduction step described above, the method for producing molybdenum dithiocarbamate of the present invention may include other steps, such as a dehydration step, a reflux step, and a purification step, depending on the purpose. Furthermore, in the present invention, in the DTC formation step, reduction step, and other steps, the solution may be neutralized by adding an acid such as hydrochloric acid, nitric acid, nitrous acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, or perchloric acid. In the present invention, from the viewpoint of obtaining a molybdenum dithiocarbamate having a high sulfur content in high yield, at least one acid selected from the group consisting of hydrochloric acid, nitric acid, and sulfuric acid is added in the DTC formation step or reduction step in an amount that is 0.001 to 2.0 moles, and more preferably 0.01 to 1.0 moles, where the molar equivalent of Mo contained in the molybdenum compound used is taken as 1. In this case, the acid may be added in the form of an aqueous solution, if necessary.
[0050] B. Molybdenum Dithiocarbamate The molybdenum dithiocarbamate of the present invention is a molybdenum dithiocarbamate represented by the following general formula (2), which is obtained by the above-described method for producing molybdenum dithiocarbamate.
[0051]
[0052] R in general formula (2) 3 ~R 6each independently represents a hydrocarbon group having 4 to 14 carbon atoms, and examples of such hydrocarbon groups having 4 to 14 carbon atoms include linear alkyl groups such as n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-uncyl, n-dodecyl, n-tridecyl, and n-tetradecyl groups; secondary butyl, isobutyl, secondary pentyl, isopentyl, secondary hexyl, isohexyl, secondary heptyl, isoheptyl, secondary octyl, isooctyl, secondary nonyl, isononyl, secondary decyl, and isodesyl groups. branched alkyl groups such as a butenyl group, a secondary undecyl group, an isoundecyl group, a secondary dodecyl group, an isododecyl group, a secondary tridecyl group, an isotridecyl group, a secondary tetradecyl group, and an isotetradecyl group; unsaturated hydrocarbon groups such as a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, an undecenyl group, a dodecenyl group, a tridecenyl group, and a tetradecenyl group; alicyclic hydrocarbon groups such as a cyclohexyl group, a methylcyclohexyl group, a dimethylcyclohexyl group, and an ethylcyclohexyl group; and aromatic hydrocarbon groups such as a phenyl group and a benzyl group.
[0053] X in general formula (2) 1 ~X 4 each independently represents an oxygen atom or a sulfur atom. 1 ~X 4 The ratio of the number of oxygen atoms to the number of sulfur atoms in X is not particularly limited and can be adjusted depending on the purpose. However, from the viewpoint of various properties such as friction reduction properties of molybdenum dithiocarbamate, 1 ~X 4 The ratio of the number of oxygen atoms to the number of sulfur atoms in the formula (I) is preferably 1.8 to 0:2.2 to 4, more preferably 1.7 to 0:2.3 to 4, even more preferably 1.2 to 0:2.8 to 4, and particularly preferably 1 to 0.4:3 to 3.6.
[0054] The molybdenum dithiocarbamate of the present invention can be used in any application in which a conventional molybdenum dithiocarbamate is used, without any particular limitation. For example, the molybdenum dithiocarbamate can be used in lubricating oils such as engine oil, gear oil, turbine oil, hydraulic oil, flame-retardant hydraulic fluid, refrigeration oil, compressor oil, vacuum pump oil, bearing oil, insulating oil, slideway oil, rock drill oil, metal working oil, plastic working oil, and heat treatment oil; and greases such as bearing grease, gear grease, gear grease, joint grease, and bearing grease.
[0055] C. Lubricating Oil Composition When the molybdenum dithiocarbamate of the present invention is added to a base oil to be used as a lubricating oil composition, the amount of molybdenum dithiocarbamate blended is not particularly limited, but from the viewpoint of making it easier to exhibit the properties of the molybdenum dithiocarbamate of the present invention, the amount of molybdenum dithiocarbamate blended relative to the total amount of the lubricating oil composition is preferably an amount that results in an elemental molybdenum content of 10 to 3,000 ppm by mass, more preferably an amount that results in ...
[0056] When the molybdenum dithiocarbamate of the present invention is used in a lubricating oil composition, the base oil of the lubricating oil composition is not particularly limited, and can be appropriately selected from mineral base oils, chemically synthesized base oils, animal and vegetable base oils, and mixed base oils thereof, etc., depending on the purpose and conditions of use. Here, examples of mineral base oils include paraffinic crude oils, naphthenic crude oils, intermediate crude oils, aromatic crude oils, etc., and further, distillate oils obtained by atmospheric distillation of these, distillate oils obtained by vacuum distillation of residual oils from atmospheric distillation, and refined oils obtained by refining these according to conventional methods, specifically solvent refined oils, hydrogenated refined oils, dewaxed oils, clay-treated oils, etc. can also be used.
[0057] Examples of chemically synthesized base oils include poly-α-olefins, polyisobutylene (polybutene), monoesters, diesters, polyol esters, silicate esters, polyalkylene glycols, polyphenyl ethers, silicones, fluorinated compounds, alkylbenzenes, and GTL base oils. Among these, examples of poly-α-olefins include polymers or oligomers of 1-hexene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, and the like, as well as hydrogenated versions of these. Examples of diesters include diesters of dibasic acids such as glutaric acid, adipic acid, azelaic acid, sebacic acid, and dodecanedioic acid with alcohols such as 2-ethylhexanol, octanol, decanol, dodecanol, and tridecanol. Examples of polyol esters include esters of polyols such as neopentyl glycol, trimethylolethane, trimethylolpropane, pentaerythritol, dipentaerythritol, and tripentaerythritol with fatty acids such as caproic acid, caprylic acid, lauric acid, capric acid, myristic acid, palmitic acid, stearic acid, and oleic acid, and refined base oils thereof can also be used.
[0058] Examples of animal and vegetable base oils include vegetable oils such as castor oil, olive oil, cacao butter, sesame oil, rice bran oil, safflower oil, soybean oil, camellia oil, corn oil, rapeseed oil, palm oil, palm kernel oil, sunflower oil, cottonseed oil, and coconut oil; and animal oils such as beef tallow, lard, milk fat, fish oil, and whale oil. If necessary, highly refined base oils obtained by highly refining these base oils to reduce the amount of impurities such as sulfur may also be used.
[0059] The base oil used in the lubricating oil composition can be one or more of the various base oils described above. The kinematic viscosity of the base oil used in the lubricating oil composition is not particularly limited and can be adjusted appropriately depending on the purpose. For example, a base oil having a kinematic viscosity at 40°C of 1.0 to 600 cSt can be used. From the viewpoint of the friction characteristics and other properties of the resulting lubricating oil composition, it is preferable to use a base oil having a kinematic viscosity at 40°C of 2.0 to 200 cSt, more preferably 4.0 to 100 cSt, and even more preferably 6.0 to 50 cSt.
[0060] The lubricating oil composition containing the molybdenum dithiocarbamate of the present invention may contain known lubricating oil additives depending on the intended use from the viewpoints of friction properties, wear properties, oxidation stability, temperature stability, storage stability, detergency, rust prevention, corrosion prevention, ease of handling, etc. Examples of such lubricating oil additives include known antioxidants, friction reducers, anti-wear agents, oiliness improvers, detergents, ashless dispersants, viscosity index improvers, rust inhibitors, corrosion inhibitors (metal deactivators), antifoaming agents, etc., and one or more of these may be used.
[0061] The antioxidant can be any antioxidant used in lubricating oils without any particular limitation, and examples thereof include 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, 2,4-dimethyl-6-t-butylphenol, 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-bis(2,6-di-t-butylphenol), 4,4'-bis(2-methyl-6-t-butylphenol), 2,2'-methylene Bis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 4,4'-isopropylidenebis(2,6-di-t-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis(4-methyl-6-nonylphenol), 2,2'-isobutylidenebis(4,6-dimethylphenol), 2,6-bis(2'-hydroxy-3'-t-butyl-5'-methylphenol) (4-hydroxy-3,5-di-t-butylphenyl)propionate, octyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, stearyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, oleyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, dodecyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, decyl 3-(4-hydroxy-3,5-di-t-butylphenyl)propionate, Tetrakis{3-(4-hydroxy-3,5-di-t-butylphenyl)propionyloxymethyl}methane, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid glycerol monoester, ester of 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid and glycerol monooleyl ether, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid butylene glycol diester, 3-(4-hydroxy-3,5-di-t-butylphenyl)propionic acid thiodiglycol diester, 4,4'-thiobis(3-methyl-6-t-butylphenol), 4,4'-thiobis(2-methyl-6-t-butylphenol), 2,2'-thiobis(4-methyl-6-t-butylphenol), 2,6-di-t-butyl-α-dimethylamino-p-cresol, 2,6-di-t-butyl-4-(N,N'-dimethylaminomethylphenol), bis(3,5-di-t-butyl-4-hydroxybenzyl)sulfide, tris{(3,5-di-t-butyl-4-hydroxyphenyl)propionyl} propionyl-oxyethyl} isocyanurate, tris(3,5-di-t-butyl-4-hydroxyphenyl) isocyanurate, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl) isocyanurate, bis{2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl}sulfide, 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, tetraphthaloyl-di(2,6-dimethylbenzyl)isocyanurate, ethyl-4-t-butyl-3-hydroxybenzyl sulfide), 6-(4-hydroxy-3,5-di-t-butylanilino)-2,4-bis(octylthio)-1,3,5-triazine, 2,2-thio-{diethyl-bis-3-(3,5-di-t-butyl-4-hydroxyphenyl)}propionate, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinamide), 3,5-di-t-butyl-4-hydroxy-benzyl-phosphate diester, bis(3 -methyl-4-hydroxy-5-t-butylbenzyl)sulfide, 3,9-bis[1,1-dimethyl-2-{β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis{3,phenolic antioxidants such as 3'-bis-(4'-hydroxy-3'-t-butylphenyl)butyric acid glycol ester; naphthylamine-based antioxidants such as 1-naphthylamine, phenyl-1-naphthylamine, p-octylphenyl-1-naphthylamine, p-nonylphenyl-1-naphthylamine, p-dodecylphenyl-1-naphthylamine, and phenyl-2-naphthylamine; N,N'-diisopropyl-p-phenylenediamine, N,N'- Diisobutyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N,N'-di-β-naphthyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine, dioctyl-p-phenylenediamine, phenylhexyl-p-phenylenediamine, phenyloctyl-p phenylenediamine-based antioxidants such as p,p'-phenylenediamine; dipyridylamine, diphenylamine, p,p'-di-n-butyldiphenylamine, p,p'-di-t-butyldiphenylamine, p,p'-di-t-pentyldiphenylamine, p,p'-dioctyldiphenylamine, p,p'-dinonyldiphenylamine, p,p'-didecyldiphenylamine, p,p'-didodecyldiphenylamine, p,p'-distyryldiphenylamine, p,p'-dimethyldiphenylamine; Examples of antioxidants include diphenylamine-based antioxidants such as p-isopropoxydiphenylamine, 4,4'-bis(4-α,α-dimethylbenzoyl)diphenylamine, p-isopropoxydiphenylamine, and dipyridylamine; and phenothiazine-based antioxidants such as phenothiazine, N-methylphenothiazine, N-ethylphenothiazine, 3,7-dioctylphenothiazine, phenothiazine carboxylic acid esters, and phenoselenazine, and the lubricating oil composition may contain one or more of these antioxidants. The amount of these antioxidants to be added is not particularly limited, but is preferably 0.01 to 5 mass %, and more preferably 0.02 to 4 mass %, based on the total amount of the lubricating oil composition.
[0062] The friction reducer can be any friction reducer used in lubricating oils without particular limitation, and examples thereof include organic molybdenum compounds such as molybdenum dithiophosphate and molybdenum amine salts; ashless friction modifiers such as aliphatic amines, fatty acid esters, fatty acid amides, fatty acids, aliphatic alcohols, and aliphatic ethers, each having at least one alkyl or alkenyl group having 6 to 30 carbon atoms in the molecule; oils and fats, amines, amides, and sulfurized esters, and one or more of these may be contained. The amount of these friction reducers to be added is not particularly limited, but is preferably 0.01 to 10% by mass, and more preferably 0.02 to 5% by mass, based on the total amount of the lubricating oil composition.
[0063] The anti-wear agent can be any anti-wear agent used in lubricating oils without any particular limitation, and examples thereof include sulfurized fats and oils, olefin polysulfides, sulfurized olefins, dibenzyl sulfide, ethyl-3-[[bis(1-methylethoxy)phosphinothioyl]thio]propionate, tris-[(2, or 4)-isoalkylphenol]thiophosphate, 3-(di-isobutoxy-thiophosphorylsulfanyl)-2-methyl-propionic acid, triphenylphosphorothionate, and β-dithiophosphorylated propionate. sulfur-based additives such as acetic acid, methylenebis(dibutyldithiocarbamate), O,O-diisopropyl-dithiophosphorylethylpropionate, 2,5-bis(n-nonyldithio)-1,3,4-thiadiazole, 2,5-bis(1,1,3,3-tetramethylbutanethio)1,3,4-thiadiazole, and 2,5-bis(1,1,3,3-tetramethyldithio)-1,3,4-thiadiazole; monooctyl phosphate, dioctyl phosphate, trioctyl phosphate, monobutyl phosphate, dibutyl phosphate, phosphate, tributyl phosphate, monophenyl phosphate, diphenyl phosphate, triphenyl phosphate, tricresyl phosphate, monoisopropyl phenyl phosphate, diisopropyl phenyl phosphate, triisopropyl phenyl phosphate, monotertiary butyl phenyl phosphate, di-tert-butyl phenyl phosphate, tri-tert-butyl phenyl phosphate, triphenyl thiophosphate, monooctyl phosphite, dioctyl phosphorus-based compounds such as phosphite, trioctyl phosphite, monobutyl phosphite, dibutyl phosphite, tributyl phosphite, monophenyl phosphite, diphenyl phosphite, triphenyl phosphite, monoisopropylphenyl phosphite, diisopropylphenyl phosphite, triisopropylphenyl phosphite, mono-tert-butylphenyl phosphite, di-tert-butylphenyl phosphite, and tri-tert-butylphenyl phosphite;Organometallic compounds such as metal dithiophosphates (Sb, Mo, etc.), metal dithiocarbamates (Zn, Sb, W, etc.), metal naphthenates, metal fatty acid salts, metal phosphates, metal phosphate esters, and metal phosphites; and other compounds such as boron compounds, alkylamine salts of mono- and dihexyl phosphates, amine salts of phosphate esters, and mixtures of triphenylthiophosphates and tert-butylphenyl derivatives, of which one or more may be contained. The amount of these antiwear agents to be added is not particularly limited, but is preferably 0.01 to 5 mass %, and more preferably 0.02 to 3 mass %, based on the total amount of the lubricating oil composition.
[0064] The oiliness improver can be any oiliness improver used in lubricating oils without particular limitation, and examples thereof include higher alcohols such as oleyl alcohol and stearyl alcohol; fatty acids such as oleic acid and stearic acid; esters such as oleyl glycerin ester, stearyl glycerin ester, and lauryl glycerin ester; amides such as laurylamide, oleylamide, and stearylamide; amines such as laurylamine, oleylamine, and stearylamine; and ethers such as lauryl glycerin ether and oleyl glycerin ether, and the lubricating oil composition may contain one or more of these. The amount of these oiliness improvers to be blended is not particularly limited, and is preferably 0.01 to 5 mass %, and more preferably 0.02 to 3 mass %, of the total amount of the lubricating oil composition.
[0065] The detergent can be any detergent used in lubricating oils without particular limitation. Examples include basic salts and overbased salts of metals such as calcium, magnesium, and barium, such as sulfonates, phenates, salicylates, and phosphates. One or more of these can be contained. The TBN (total base number) of these compounds is not particularly limited, but a TBN of 30 to 800 mgKOH / g is preferred. The amount of detergent to be added is not particularly limited, but is preferably 0.5 to 10 mass%, more preferably 1 to 8 mass%, based on the total amount of the lubricating oil composition. Among these, it is preferable to contain one or more detergents consisting of a basic or overbased salt of calcium and a basic or overbased salt of magnesium, and it is more preferable to contain a basic or overbased salt of calcium and a basic or overbased salt of magnesium. In this case, the content of calcium atoms derived from the detergent in the lubricating oil composition is not particularly limited, but from the viewpoint of detergency etc., the content of calcium atoms derived from the detergent in the lubricating oil composition is preferably 100 to 3,000 ppm by mass, more preferably 200 to 2,500 ppm by mass. In addition, the content of magnesium atoms derived from the detergent in the lubricating oil composition is not particularly limited, but from the viewpoint of detergency etc., the content of magnesium atoms derived from the detergent in the lubricating oil composition is preferably 50 to 2,000 ppm by mass, more preferably 100 to 1,000 ppm by mass.
[0066] The ashless dispersant may be any ashless dispersant used in lubricating oils, and may be any suitable ashless dispersant. Examples include nitrogen-containing compounds having at least one linear or branched alkyl or alkenyl group having 40 to 400 carbon atoms in the molecule, or derivatives thereof. Specific examples include succinimides, succinic acid amides, succinic acid esters, succinic acid ester-amides, benzylamines, polyamines, polysuccinimides, and Mannich bases. Derivatives thereof include those obtained by reacting these nitrogen-containing compounds with boron compounds such as boric acid and borates, phosphorus compounds such as thiophosphoric acid and thiophosphates, organic acids, and hydroxypolyoxyalkylene carbonates. The lubricating oil composition may contain one or more of these compounds. The amount of these ashless dispersants to be added is not particularly limited, and is preferably 0.5 to 10 mass %, more preferably 1 to 8 mass %, of the total amount of the lubricating oil composition.
[0067] The viscosity index improver can be any viscosity index improver used in lubricating oils without particular limitation. Examples include poly(C1-18) alkyl (meth)acrylate, (C1-18) alkyl acrylate / (C1-18) alkyl (meth)acrylate copolymer, diethylaminoethyl (meth)acrylate / (C1-18) alkyl (meth)acrylate copolymer, ethylene / (C1-18) alkyl (meth)acrylate copolymer, polyisobutylene, polyalkylstyrene, ethylene / propylene copolymer, styrene / maleic acid ester copolymer, and styrene / isoprene hydrogenated copolymer. One or more of these may be contained. The weight average molecular weight is approximately 10,000 to 1,500,000. The amount of these viscosity index improvers to be added is not particularly limited, but is preferably 0.1 to 20 mass%, more preferably 0.3 to 15 mass%, based on the total amount of the lubricating oil composition.
[0068] The rust inhibitor can be any rust inhibitor used in lubricating oils without particular limitation, and examples thereof include sodium nitrite, oxidized paraffin wax calcium salt, oxidized paraffin wax magnesium salt, tallow fatty acid alkali metal salt, alkaline earth metal salt or amine salt, alkenyl succinic acid or alkenyl succinic acid half ester (the molecular weight of the alkenyl group is about 100 to 300), sorbitan monoester, nonylphenol ethoxylate, lanolin fatty acid calcium salt, etc., and the lubricating oil composition can contain one or more of these. The amount of these rust inhibitors to be added is not particularly limited, and is preferably 0.01 to 3 mass %, and more preferably 0.02 to 2 mass %, based on the total amount of the lubricating oil composition.
[0069] The corrosion inhibitor can be any corrosion inhibitor used in lubricating oils without any particular limitation. Examples of the corrosion inhibitor include triazole, tolyltriazole, benzotriazole, benzimidazole, benzothiazole, benzothiadiazole, and derivatives of these compounds, such as 2-hydroxy-N-(1H-1,2,4-triazol-3-yl)benzamide, N,N-bis(2-ethylhexyl)-[(1,2,4-triazol-1-yl)methyl]amine, N,N-bis(2-ethylhexyl)-[(1,2,4-triazol-1-yl)methyl]amine, and 2,2'-[[(4 or 5 or 1)-(2-ethylhexyl)-methyl-1H-benzotriazole-1-methyl]imino]bisethanol, bis(poly-2- Examples of the corrosion inhibitor include tetraalkylthiuram disulfide, N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide, 3-(3,5-di-t-butyl-hydroxyphenyl)-N'-(3-(3,5-di-tert-butyl-hydroxyphenyl)propanoyl)propanehydrazide, esters of tetrapropenylsuccinic acid and 1,2-propanediol, disodium sebacate, (4-nonylphenoxy)acetic acid, alkylamine salts of mono- and dihexyl phosphate, sodium salt of tolyltriazole, and (Z)-N-methyl-N-(1-oxo-9-octadecenyl)glycine, and the lubricating oil composition may contain one or more of these. The amount of these corrosion inhibitors to be added is not particularly limited, but is preferably 0.01 to 3 mass %, more preferably 0.02 to 2 mass %, based on the total amount of the lubricating oil composition.
[0070] The antifoaming agent can be any antifoaming agent used in lubricating oils without particular limitation, and examples thereof include polydimethylsilicone, dimethylsilicone oil, trifluoropropylmethylsilicone, colloidal silica, polyalkyl acrylate, polyalkyl methacrylate, alcohol ethoxy / propoxylate, fatty acid ethoxy / propoxylate, and sorbitan partial fatty acid ester, and one or more of these can be contained. The amount of these antifoaming agents to be added is not particularly limited, and is preferably 0.0001 to 0.1 mass%, and more preferably 0.001 to 0.01 mass%, based on the total amount of the lubricating oil composition.
[0071] D. Grease Composition When the molybdenum dithiocarbamate of the present invention is added to a base oil to be used as a grease composition, the amount of molybdenum dithiocarbamate blended is not particularly limited, but from the viewpoint of making it easier to exhibit the properties of the molybdenum dithiocarbamate of the present invention, the amount of molybdenum dithiocarbamate blended relative to the total amount of the grease composition is preferably an amount that results in an elemental molybdenum content of 0.01 to 1 mass%, more preferably an amount that results in an amount that results in an amount that results in an elemental molybdenum content of 0.02 to 0.7 mass%, and even more preferably an amount that results in an amount that results in an elemental molybdenum content of 0.03 to 0.5 mass%.
[0072] When the molybdenum dithiocarbamate of the present invention is added to a base oil to form a grease composition, known grease additives may be used in combination, if necessary. Examples of grease additives include antioxidants such as amine-based antioxidants, phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; detergents such as basic salts and overbased salts of metals such as calcium, magnesium, and barium, such as sulfonates, phenates, salicylates, and phosphates; oiliness improvers such as higher alcohols, higher fatty acids, higher fatty acid glycerol esters, higher fatty acid amides, and higher alkylamines; dispersants such as alkenyl succinimides; extreme pressure agents such as phosphate esters, zinc dialkyldithiophosphates, and zinc dialkyldithiocarbamates; other organic molybdenum compounds such as dialkyldithiophosphates, molybdenum long-chain amine salts, and molybdenum alkenyl succinimide complexes; viscosity index improvers, pour point depressants, rust inhibitors, corrosion inhibitors, and antifoaming agents. These additives may also be mixed with the molybdenum dithiocarbamate of the present invention before being incorporated into the grease.
[0073] When the molybdenum dithiocarbamate of the present invention is used in a grease composition, the base oil of the grease composition is not particularly limited, and for example, the base oils exemplified for the lubricating oil composition can be used. Among these, the base oil used in the grease composition preferably contains at least a mineral oil or a hydrocarbon-based synthetic oil, since the lubrication-improving effect of the molybdenum dithiocarbamate is more likely to be exhibited. More preferably, the base oil used contains a paraffin-based highly refined mineral oil, a poly-α-olefin-based or GTL-based chemically synthetic base oil, or a mixed base oil thereof. In this case, it is preferable to contain 50 mass% or more of these base oils out of the total amount of base oil, since this allows the properties of the molybdenum dithiocarbamate to be more effectively exhibited, and it is even more preferable for the base oil to contain 90 mass% or more of these base oils out of the total amount of base oil.
[0074] When the molybdenum dithiocarbamate of the present invention is added to a base oil to prepare a grease composition, the grease composition may further contain a thickener such as a soap-based or complex soap-based thickener, an organic non-soap-based thickener, or an inorganic non-soap-based thickener, and the like, and the grease composition may contain one or more of these.
[0075] Examples of soap-based thickeners include soaps obtained by reacting higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, arachic acid, behenic acid, dsomalic acid, oleic acid, linoleic acid, linolenic acid, and ricinoleic acid with bases such as lithium, sodium, potassium, aluminum, barium, and calcium; and complex soap thickeners obtained by further reacting the above-mentioned fatty acids and bases with acetic acid, benzoic acid, sebacic acid, azelaic acid, phosphoric acid, boric acid, and the like.
[0076] Examples of organic non-soap thickeners include terephthalate-based thickeners, urea-based thickeners, and fluorine-based thickeners such as polytetrafluoroethylene and fluorinated ethylene-propylene copolymers, with urea-based thickeners being preferred. Examples of urea-based thickeners include monourea compounds obtained by reacting a monoisocyanate with a monoamine, diurea compounds obtained by reacting a diisocyanate with a monoamine, ureaurethane compounds obtained by reacting a diisocyanate with a monoamine and a monool, and tetraurea compounds obtained by reacting a diisocyanate with a diamine and a monoisocyanate.
[0077] Examples of inorganic non-soap thickeners include carbon black, boron nitride, organo clay, and silica gel.
[0078] The present disclosure includes the following aspects.
[0079] [1] A method for producing molybdenum dithiocarbamate, comprising: a DTC conversion step of reacting one or more molybdenum compounds selected from the group consisting of molybdic acid and its salts, a sulfur source including octasulfur and carbon disulfide, and an amine compound represented by general formula (1) to obtain a DTC conversion intermediate; and a reduction step of reducing the obtained DTC conversion intermediate in the presence of a reducing agent to obtain a molybdenum dithiocarbamate represented by general formula (2).
[0080] [2] X in general formula (2) 1 ~X 4The method for producing molybdenum dithiocarbamate according to [1], wherein the ratio of oxygen atoms to sulfur atoms (O:S) is 1.8 to 0:2.2 to 4.
[0081] [3] The DTC process is carried out in a condition where the value of the dispersion term δd in the Hansen solubility parameter is 15.0 to 17.5 (MPa). 1 / 2 , the value of the bipolar term δp is 0 to 6.8 (MPa) 1 / 2 , and the hydrogen bond term δh is 10.0 to 17.5 (MPa) 1 / 2 The method for producing molybdenum dithiocarbamate according to [1] or [2], wherein the compound is a monohydric alcohol having 3 to 8 carbon atoms, and the organic solvent is a monohydric alcohol having 3 to 8 carbon atoms.
[0082] [4] The method for producing molybdenum dithiocarbamate according to any one of [1] to [3], wherein the mass ratio of the sulfur element content of the octasulfur to the sulfur element content of the carbon disulfide is 10:90 to 90:10.
[0083] [5] The method for producing molybdenum dithiocarbamate according to any one of [1] to [4], wherein the reducing agent is one or more selected from the group consisting of sodium hydrosulfide, potassium hydrosulfide, sodium pyrosulfite, and sodium thiosulfate.
[0084] [6] The method for producing molybdenum dithiocarbamate according to any one of [1] to [5], wherein the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur source, and the amine compound is 1:1.5 to 10:0.8 to 2, where the molar equivalent of the Mo element is taken as 1.
[0085] [7] A molybdenum dithiocarbamate obtained by the production method according to any one of [1] to [6].
[0086] [8] A lubricating oil composition or a grease composition containing the molybdenum dithiocarbamate according to [7].
[0087] The present invention will be described in more detail below with reference to examples. In the following examples, percentages are by weight unless otherwise specified.
[0088] Example 1 A flask equipped with a stirrer, a thermometer, a nitrogen tube, and a reflux condenser was charged with 45.2 g (0.31 mol) of molybdenum trioxide, 20.1 g (0.078 mol) of octasulfur, 39.8 g (0.16 mol) of di-2-ethylhexylamine, 62.7 g (0.16 mol) of di-isotridecylamine, 16.4 g (0.22 mol) of 1-butanol, and 4.43 g (0.02 mol) of 35% sulfuric acid, and 29.5 g (0.39 mol) of carbon disulfide was added dropwise at 20 to 55°C over 1 hour to react the raw materials, thereby producing a green MoDTC intermediate. In this DTC conversion process, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur compound, and the amine compound was 1:4.4:1.05, where the molar equivalent of the Mo element was 1. Subsequently, 100.0 g (0.53 mol) of a 30% aqueous solution of sodium hydrosulfide was added, and the mixture was reduced at 95°C for 3 hours. The aqueous layer was then removed, washed with water, and dehydrated under reduced pressure. Then, 293.7 g of mineral oil (naphthenic mineral base oil, kinematic viscosity at 100°C: 2.2 mm / s) was added, and the mixture was filtered to obtain 454.8 g of an amber-colored viscous liquid product consisting of mineral oil and a molybdenum compound. The resulting viscous liquid product was analyzed using high-performance liquid chromatography, inductively coupled plasma mass spectrometry, a nuclear magnetic resonance spectrometer, and a matrix-assisted laser desorption / ionization time-of-flight mass spectrometer. The resulting viscous liquid product was found to be a compound represented by the general formula (2), in which R 3 ~R 6 is an isotridecyl group or a 2-ethylhexyl group (the ratio of isotridecyl groups to 2-ethylhexyl groups is 2:2), and X 1 ~X 4 The product was a viscous liquid containing 157.6 g (yield 94.6%) of molybdenum dithiocarbamate having an oxygen atom:sulfur atom ratio of 1.6:2.4.
[0089] Example 2 A flask equipped with a stirrer, a thermometer, a nitrogen tube, and a reflux condenser was charged with 45.0 g (0.31 mol) of molybdenum trioxide, 20.3 g (0.079 mol) of octasulfur, 39.7 g (0.16 mol) of di-2-ethylhexylamine, 63.1 g (0.17 mol) of di-isotridecylamine, 17.2 g (0.23 mol) of 1-butanol, and 4.41 g (0.02 mol) of 35% sulfuric acid, and 29.2 g (0.38 mol) of carbon disulfide was added dropwise at 20 to 55°C over 1 hour to react the raw materials, thereby producing a green MoDTC intermediate. In this DTC conversion process, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur compound, and the amine compound was 1:4.4:1.05, where the molar equivalent of Mo element was 1. Subsequently, 147.5 g (0.79 mol) of a 30% aqueous solution of sodium hydrosulfide was added, and reduction was carried out at 95°C for 3 hours. After removing the aqueous layer, washing with water, and dehydrating under reduced pressure, 297.0 g of mineral oil (naphthenic mineral base oil, kinematic viscosity at 100°C: 2.2 mm / s) was added, and filtration was carried out to obtain 446.9 g of an amber-colored viscous liquid product consisting of mineral oil and a molybdenum compound. The resulting viscous liquid product was analyzed using high-performance liquid chromatography, inductively coupled plasma mass spectrometry, a nuclear magnetic resonance spectrometer, and a matrix-assisted laser desorption / ionization time-of-flight mass spectrometer. The resulting viscous liquid product was found to be a compound represented by the general formula (2), in which R 3 ~R 6 is an isotridecyl group or a 2-ethylhexyl group (the ratio of isotridecyl groups to 2-ethylhexyl groups is 2:2), and X 1 ~X 4 The product was a viscous liquid containing 131.3 g (yield 79.1%) of molybdenum dithiocarbamate having an oxygen atom:sulfur atom ratio of 1.6:2.4.
[0090] Example 3 To a flask equipped with a stirrer, a thermometer, a nitrogen tube, and a reflux condenser were added 45.0 g (0.31 mol) of molybdenum trioxide, 10.1 g (0.039 mol) of octasulfur, 39.7 g (0.16 mol) of di-2-ethylhexylamine, 63.1 g (0.17 mol) of di-isotridecylamine, 17.0 g (0.23 mol) of 1-butanol, and 4.42 g (0.02 mol) of 35% sulfuric acid, and 53.0 g (0.70 mol) of carbon disulfide was added dropwise at 20 to 55°C over 1 hour to react the raw materials, thereby producing a green MoDTC intermediate. In this DTC conversion process, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur compound, and the amine compound was 1:5.4:1.05, where the molar equivalent of the Mo element was 1. Subsequently, 101.7 g (0.54 mol) of a 30% aqueous solution of sodium hydrosulfide was added, and the mixture was reduced at 95°C for 3 hours. The aqueous layer was then removed, washed with water, and dehydrated under reduced pressure. Then, 296.4 g of mineral oil (naphthenic mineral base oil, kinematic viscosity at 100°C: 2.2 mm / s) was added, and the mixture was filtered to obtain 446.9 g of an amber-colored viscous liquid product consisting of mineral oil and a molybdenum compound. The resulting viscous liquid product was analyzed using high-performance liquid chromatography, inductively coupled plasma mass spectrometry, a nuclear magnetic resonance spectrometer, and a matrix-assisted laser desorption / ionization time-of-flight mass spectrometer. The resulting viscous liquid product was found to be a compound represented by the general formula (2), in which R 3 ~R 6 is an isotridecyl group or a 2-ethylhexyl group (the ratio of isotridecyl groups to 2-ethylhexyl groups is 2:2), and X 1 ~X 4 The product was a viscous liquid containing 152.3 g (yield 91.8%) of molybdenum dithiocarbamate having an oxygen atom:sulfur atom ratio of 1.8:2.2.
[0091] Comparative Example 1: 45.0 g (0.31 mol) of molybdenum trioxide, 39.6 g (0.16 mol) of di-2-ethylhexylamine, 62.8 g (0.16 mol) of di-isotridecylamine, 16.5 g (0.22 mol) of 1-butanol, and 4.56 g (0.02 mol) of 35% sulfuric acid were added to a flask equipped with a stirrer, thermometer, nitrogen tube, and reflux condenser, and 28.8 g (0.38 mol) of carbon disulfide was added dropwise over 1 hour at 20 to 55°C to react the raw materials, thereby obtaining a DTC intermediate. In this DTC conversion step, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur compound, and the amine compound was 1:2.4:1.05, where the molar equivalent of Mo was taken as 1. Subsequently, 100.8 g (0.54 mol) of a 30% aqueous solution of sodium hydrosulfide was added, followed by reduction at 95° C. for 3 hours. The aqueous layer was then removed, the mixture was washed with water, and dehydrated under reduced pressure. 296.2 g of mineral oil (naphthenic mineral base oil, kinematic viscosity at 100° C. 2.2 mm / s) was added, followed by filtration, yielding 411.8 g of an amber-colored viscous liquid product consisting of mineral oil and a molybdenum compound. The resulting viscous liquid product was analyzed using high-performance liquid chromatography, inductively coupled plasma mass spectrometry, and nuclear magnetic resonance spectroscopy. It was found that the resulting viscous liquid product contained the molybdenum compound represented by general formula (2), where R 3 ~R 6 is an isotridecyl group or a 2-ethylhexyl group (the ratio of isotridecyl groups to 2-ethylhexyl groups is 2:2), and X 1 ~X 4 The product was a viscous liquid containing 99.2 g (yield 59.8%) of molybdenum dithiocarbamate having an oxygen atom:sulfur atom ratio of 1.8:2.2.
[0092] Comparative Example 2: 45.1 g (0.31 mol) of molybdenum trioxide, 39.7 g (0.16 mol) of di-2-ethylhexylamine, 62.7 g (0.16 mol) of di-isotridecylamine, 17.0 g (0.23 mol) of 1-butanol, and 4.42 g (0.02 mol) of 35% sulfuric acid were added to a flask equipped with a stirrer, thermometer, nitrogen tube, and reflux condenser, and 76.8 g (1.01 mol) of carbon disulfide was added dropwise over 1 hour at 20 to 55°C to react the raw materials, thereby obtaining a DTC intermediate. In this DTC conversion step, the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur compound, and the amine compound was 1:6.4:1.05, where the molar equivalent of Mo was taken as 1. Subsequently, the mixture was reacted at 95°C for 3 hours, the aqueous layer was removed, washed with water, and dehydrated under reduced pressure. 297.6 g of mineral oil (naphthenic mineral base oil, kinematic viscosity at 100°C 2.2 mm / s) was added, and the mixture was filtered to obtain 447.9 g of a reddish-purple viscous liquid product consisting of mineral oil and a molybdenum compound. The resulting viscous liquid product was analyzed using high-performance liquid chromatography, inductively coupled plasma mass spectrometry, and nuclear magnetic resonance spectroscopy, and the presence of the molybdenum dithiocarbamate represented by general formula (2) was not confirmed in the resulting viscous liquid product.
[0093] As can be seen from the above results, the present invention can produce molybdenum dithiocarbamate with a high sulfur content in high yield. On the other hand, in Comparative Examples 1 and 2, in which a raw material containing no octasulfur was used as the sulfur source, the yield of molybdenum dithiocarbamate was low, or molybdenum dithiocarbamate could not be produced. In these Comparative Examples, it is believed that the DTC intermediates represented by general formulas (3) to (5) could not be sufficiently obtained in the DTC conversion step, and therefore the target molybdenum dithiocarbamate represented by general formula (2) could not be obtained in the subsequent reduction step. Furthermore, the molybdenum dithiocarbamate with a high sulfur content obtained in high yield by the present invention is expected to have excellent properties and can therefore be suitably used in lubricating oil compositions and grease compositions.
Claims
1. A method for producing molybdenum dithiocarbamate, comprising: a DTC conversion step in which one or more molybdenum compounds selected from the group consisting of molybdic acid and its salts, a sulfur source including octasulfur and carbon disulfide, and an amine compound represented by the following general formula (1) are reacted to obtain a DTC conversion intermediate; and a reduction step in which the obtained DTC conversion intermediate is reduced in the presence of a reducing agent to obtain a molybdenum dithiocarbamate represented by the following general formula (2). (In the formula, R 1 ~R 2 each independently represents a hydrocarbon group having 4 to 14 carbon atoms. (In the formula, R 3 ~R 6 each independently represents a hydrocarbon group having 4 to 14 carbon atoms; X 1 ~X 4 each independently represents an oxygen atom or a sulfur atom.
2. X in general formula (2) 1 ~X 4 2. The method for producing molybdenum dithiocarbamate according to claim 1, wherein the ratio of oxygen atoms to sulfur atoms (O:S) is 1.8 to 0:2.2 to 4.
3. The DTC process is carried out in a condition where the dispersion term δd in the Hansen solubility parameter is 15.0 to 17.5 (MPa). 1 / 2 , the value of the bipolar term δp is 0 to 6.8 (MPa) 1 / 2 , and the hydrogen bond term δh is 10.0 to 17.5 (MPa) 1 / 2 2. The method for producing molybdenum dithiocarbamate according to claim 1, wherein the method is carried out in the presence of an organic solvent which is a monohydric alcohol having 3 to 8 carbon atoms.
4. The method for producing molybdenum dithiocarbamate according to claim 1, wherein the mass ratio of the elemental sulfur content of the octasulfur to the elemental sulfur content of the carbon disulfide is 10:90 to 90:
10.
5. The method for producing molybdenum dithiocarbamate according to claim 1, wherein the reducing agent is one or more selected from the group consisting of sodium hydrosulfide, potassium hydrosulfide, sodium pyrosulfite, and sodium thiosulfate.
6. The method for producing molybdenum dithiocarbamate according to claim 1, wherein the molar equivalent ratio (Mo:S:amine) of the Mo element contained in the molybdenum compound, the S element contained in the sulfur source, and the amine compound is 1:1.5-10:0.8-2, where the molar equivalent of Mo is 1.
7. Molybdenum dithiocarbamate obtained by the method according to any one of claims 1 to 6.
8. A lubricating oil composition or a grease composition containing the molybdenum dithiocarbamate according to claim 7.
Citation Information
Patent Citations
Organomolybdenum compound and use thereof
JP1992182494A
New organic molybdenum compound, friction regulating agent composed thereof and lubricating composition containing the same
JP2008189562A
Method for preparing molybdenum dialkyldithiocarbamate sulfide
JP2009512735A
Molybdenum dithiocarbamate and method for producing molybdenum dithiocarbamate
WO2019208301A1