Positive electrode material, secondary battery, and electronic device

By introducing fluorine elements with different binding energies onto the surface of cobalt-containing material particles to form a composite fluoride layer, the instability and safety hazards of secondary batteries under high temperature and mechanical damage are solved, thus improving the stability and safety of the battery.

WO2026188410A9PCT designated stage Publication Date: 2026-11-12NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/081917
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-03-11
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Secondary batteries are prone to instability and capacity decay under high temperature storage and mechanical damage conditions, leading to performance degradation and safety hazards.

Method used

By introducing fluorine elements with different binding energies onto the surface of cobalt-containing material particles, a composite fluoride layer is formed, which improves mechanical strength and toughness, provides a thermal safety barrier, and enhances high-temperature storage performance and safety.

Benefits of technology

It enhances the stability and safety of secondary batteries under high temperature and mechanical damage conditions, extends service life, reduces side reactions and internal stress, and improves overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025081917_12112026_PF_FP_ABST
    Figure CN2025081917_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of battery materials, and provides a positive electrode material, a secondary battery, and an electronic device. The positive electrode material comprises a cobalt-containing material, which has, within a range from 0 nm to 100 nm on the surface thereof, a bimodal feature of fluorine element detected by X-ray photoelectron spectroscopy (XPS), wherein the peak of the first peak is in the range of 687eV to 688eV, corresponding to a high-binding-energy fluoride, and the peak of the second peak is in the range of 684eV to 686eV, corresponding to a low-binding-energy fluoride. In the present application, by introducing fluorine elements having different binding energies into the cobalt-containing material and adjusting the relative content of the two fluorides, the high-temperature storage performance and safety performance of the secondary battery can be improved when such material is used in a secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode materials, secondary batteries and electronic devices Technical Field

[0001] This application belongs to the field of battery materials technology, specifically relating to a cathode material, a secondary battery, and an electronic device. Background Technology

[0002] Rechargeable batteries, which can recover their active materials through charging after discharge, are widely used in mobile electronic devices, electric vehicles, energy storage, and other fields. However, in practical applications, rechargeable batteries are prone to instability and capacity decay under high-temperature storage and mechanical damage conditions, often leading to performance degradation and safety hazards. Therefore, improving the high-temperature storage performance and safety performance under mechanical damage of rechargeable batteries is a technical problem that needs to be solved in this field. Summary of the Invention

[0003] In view of this, this application provides a cathode material, a secondary battery, and an electronic device. By introducing fluorine elements with different binding energies into cobalt-containing material particles, the high-temperature storage performance and safety performance can be improved when applied in a secondary battery, thereby solving the above-mentioned problems.

[0004] In a first aspect, this application provides a cathode material comprising cobalt-containing material particles; the cobalt-containing material particles are tested by X-ray photoelectron spectroscopy, and the cobalt-containing material particles contain fluorine elements in the range of 0 nm to 100 nm from the surface, and the F1s spectrum includes a first peak and a second peak, the peak value of the first peak is in the range of 687 eV to 688 eV, and the peak value of the second peak is in the range of 684 eV to 686 eV. According to X-ray photoelectron spectroscopy (XPS), the cobalt-containing material particles contain two types of fluorine elements with different binding energies in the range of 0 nm to 100 nm from the surface. The high-binding-energy fluorine element can maintain chemical inertness in high-temperature environments, reducing material dissolution and morphological changes, while the low-binding-energy fluorine element helps to provide self-healing ability at high temperatures, repairing microcracks and defects. The two types of fluorine elements with different binding energies work closely together to form a composite fluoride layer, which can improve the mechanical strength and toughness of the cobalt-containing material particles, improve the ability of the secondary battery to resist physical shock, and provide a thermal safety barrier to inhibit the spread of thermal runaway. This improves the high-temperature storage performance and safety performance of the secondary battery when it encounters mechanical damage, ensuring the durability and safety of the secondary battery when used under harsh conditions.

[0005] In some implementations, the peak intensity of the first peak is I. A The peak intensity of the second peak is I. B , 0.2≤I A / I B ≤0.9; preferably, 0.5≤I A / I B≤0.8. This application controls the content ratio of fluorine elements with two binding energies to make the peak intensities of the first and second peaks in the F1s spectrum conform to the above relationship, which helps to improve the thermal stability and surface protection capability of the composite fluoride layer, and further improves the high-temperature storage performance and safety performance of the secondary battery.

[0006] In some embodiments, the fluorine content is m1% based on the mass of the cobalt-containing material particles, where 0.05 ≤ m1 ≤ 1.50. Controlling the fluorine content within this range can further improve the high-temperature storage performance and safety performance of the secondary battery.

[0007] In some embodiments, the cobalt-containing material particles contain aluminum in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of aluminum is m2%, 0.1 ≤ m1 / m2 ≤ 5.0; preferably, 0.5 ≤ m1 / m2 ≤ 2.0. Aluminum can form aluminum fluoride with fluorine, which has a high binding energy, improving the structural and interfacial stability of the cobalt-containing material particles, thereby further improving the high-temperature storage performance and safety performance of the secondary battery.

[0008] In some embodiments, the cobalt-containing material particles contain element D in the range of 0 nm to 100 nm from the surface. Element D includes at least one of yttrium, calcium, lanthanum, or cerium. Based on the mass of the cobalt-containing material particles, the mass content of element D is m3%, with 1 ≤ m1 / m3 ≤ 50; preferably, 5 ≤ m1 / m3 ≤ 30. Using Y, Ca, La, or Ce as doping elements D, and adjusting their mass content with fluorine to conform to the above relationship, can enhance the ionic conductivity and high-temperature performance of the cobalt-containing material particles, thereby further improving the high-temperature storage performance and safety performance of the secondary battery.

[0009] In some embodiments, 0.01 ≤ m³ ≤ 0.50; preferably, 0.05 ≤ m³ ≤ 0.20. When the mass content of element D in the cobalt-containing material particles is within the above range, the high-temperature storage performance and safety performance of the secondary battery can be further improved.

[0010] In some implementations, the cathode material satisfies at least one of the following conditions:

[0011] (1) The cobalt-containing material particles contain magnesium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of magnesium is m. 11 %, 0.1≤m1 / m 11 ≤10.0; preferably, 0.5≤m1 / m 11 ≤5.0;

[0012] (2) The cobalt-containing material particles contain zirconium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of zirconium is m. 12 %, 0.1≤m1 / m 12 ≤20.0; preferably, 1.0≤m1 / m 12 ≤10.0;

[0013] (3) The cobalt-containing material particles contain titanium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of titanium is m. 13 %, 0.1≤m1 / m 13 ≤10.0; preferably, 0.5≤m1 / m 13 ≤5.0;

[0014] (4) The cobalt-containing material particles contain lithium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of lithium is m. 14 %, 0.01≤m1 / m 14 ≤0.50; preferably, 0.05≤m1 / m 14 ≤0.10.

[0015] By selecting the above-mentioned doping elements and adjusting their mass content with fluorine to conform to the above relationship, the structural stability and interfacial stability of cobalt-containing material particles can be further enhanced, thereby improving the high-temperature storage performance and safety performance of secondary batteries.

[0016] In some implementations, the cathode material satisfies at least one of the following conditions:

[0017] (1) 0.01≤m 11 ≤2.00; preferably, 0.05≤m 11 ≤0.20;

[0018] (2) 0.05≤m 12 ≤1.00; preferably, 0.07≤m 12 ≤0.20;

[0019] (3) 0.02≤m 13 ≤2.00; preferably, 0.1≤m 13 ≤0.5;

[0020] (4) 4≤m 14 ≤8; preferably, 6≤m 14 ≤7.

[0021] By controlling the mass content of doping elements within the above-mentioned range, this application can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0022] In a second aspect, this application provides a secondary battery, including a positive electrode, a negative electrode, and an electrolyte; the positive electrode includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector; the positive electrode material layer includes the positive electrode material described in the first aspect.

[0023] Thirdly, this application provides an electronic device including the secondary battery described in the second aspect above.

[0024] Based on the cathode material, secondary battery, and electronic device provided in this application, the beneficial effects are at least as follows:

[0025] Fluorine elements with different binding energies are incorporated into the surface of cobalt-containing material particles within a range of 0 nm to 100 nm, corresponding to fluorides with different binding energies. Lower binding energy fluorides, such as lithium fluoride, provide self-healing capabilities at high temperatures, repairing microcracks. Higher binding energy fluorides, such as aluminum fluoride and zirconium fluoride, increase grain boundary strength and stability, reducing structural changes caused by charge-discharge cycles. By controlling the peak intensity ratio of fluorine elements with different binding energies, a stable fluoride layer can be formed on the surface of the cobalt-containing material particles, improving their thermal stability and chemical inertness, reducing the decomposition of the cathode material at high temperatures, and minimizing side reactions with the electrolyte, thus reducing or preventing capacity loss and performance degradation. The fluoride layer also enhances mechanical strength, provides protection against physical damage, and improves the toughness of the cathode material. When the secondary battery suffers physical damage such as puncture, the fluoride layer can act as a barrier to mitigate thermal runaway, improving the safety of the secondary battery. Furthermore, the combination of two fluorine elements with different binding energies can also improve ion conductivity and promote the uniformity of electrochemical reactions. Through the above-mentioned effects, the thermal stability and mechanical damage stability of the cathode material can be improved, and the stability and safety of the secondary battery can be significantly improved under complex and harsh conditions. It also helps to reduce the side reactions and internal stress inside the secondary battery, and improve the overall life and durability of the secondary battery. Attached Figure Description

[0026] Figure 1 shows the F1s spectrum of a cobalt-containing material particle provided in a specific embodiment of this application;

[0027] Figure 2 is a schematic diagram of the structure of a cobalt-containing material particle provided in a specific embodiment of this application. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0029] Cobalt-containing particles in cathode materials can form strong ionic bonds with oxygen, ensuring structural stability. Furthermore, cobalt promotes lithium-ion insertion and extraction, increasing the lithium-ion diffusion rate. Therefore, they are widely used in lithium-ion batteries; for example, lithium cobalt oxide exhibits high energy density and excellent electrochemical performance. However, cobalt-containing particles are prone to structural instability and capacity decay under high-temperature storage and mechanical damage conditions (such as nail penetration tests). Chemical reactions and structural changes on the material surface often lead to battery performance degradation and safety hazards. Surface modification strategies have been proposed to optimize the performance of cobalt-containing particles, particularly by introducing fluorine into the material surface to form a stable fluoride layer, which can improve its heat resistance and mechanical strength. However, how to effectively control the binding energy and distribution of these fluorides still requires further investigation.

[0030] Firstly, this application provides a cathode material comprising cobalt-containing material particles. X-ray photoelectron spectroscopy (XPS) analysis shows that the cobalt-containing material particles contain fluorine in a region of 0 nm to 100 nm from the surface. The F1s spectrum includes a first peak and a second peak, with the first peak ranging from 687 eV to 688 eV and the second peak ranging from 684 eV to 686 eV. This application designs two fluorides with different binding energies within a 0 nm to 100 nm region on the surface of the cobalt-containing material particles. High-binding-energy fluorides, such as aluminum fluoride (AlF3), effectively protect the cobalt-containing material particles from damage caused by high temperatures and chemical reactions, while low-binding-energy fluorides, such as lithium fluoride (LiF), provide self-healing capabilities, improving the material's durability and safety. The close cooperation of these two fluorides with different binding energies enhances the mechanical strength and toughness of the cathode material, improves the secondary battery's resistance to physical shocks, and acts as a thermal barrier. In the event of an internal short circuit caused by physical damage to the secondary battery, it provides a thermal safety barrier, inhibiting the spread of thermal runaway. Furthermore, fluorine elements with both binding energies can participate in the formation of a solid electrolyte interface layer, improving electrode interface characteristics, enhancing lithium-ion conductivity and transport stability, and improving the safety performance of the secondary battery under mechanical damage. Through the above design, this application achieves performance improvement of cobalt-containing material particles under harsh conditions such as high temperature or mechanical damage, extending the service life of the secondary battery and improving overall safety performance.

[0031] In this application, cobalt-containing material particles in the cathode material refer to particulate materials containing cobalt that can participate in electrochemical reactions in battery chemistry, and more particularly, particulate materials with cobalt as one of the main components that can be used as the positive electrode active material in secondary batteries such as lithium-ion batteries. Exemplarily, cobalt-containing material particles may include, but are not limited to: lithium cobalt oxide (LiCoO2, LCO), lithium nickel cobalt manganese oxide (LiNiCoMnO2, NCM), lithium nickel cobalt aluminum oxide (LiNiCoAlO2, NCA), lithium manganese cobalt oxide (LiMnCoO2), and layered lithium transition metal oxides such as LiCo. 1-x M x O2 (where M can be metals such as Ni, Mn, Fe, etc.), spinel-type lithium transition metal oxides such as lithium cobalt oxide spinel (LiCo2O4), etc.

[0032] It should be noted that, in this field, the “surface” of an object is a physical layer with a physical structure. In this context, the surface of a solid refers to the physical layer consisting of one or more atomic layers of the outermost layer of the solid, which is the interface layer where the solid comes into contact with a vacuum or another substance.

[0033] Specifically, X-ray photoelectron spectroscopy (XPS) is a technique for analyzing the chemical properties of a material's surface. It utilizes the absorption and scattering characteristics of X-rays as they pass through an object's surface to detect its internal structure. XPS can measure the elemental composition, empirical formulas, chemical states, and electronic states of elements in materials. It involves exciting a solid surface with a beam of X-rays while simultaneously measuring the kinetic energy of electrons emitted from a region greater than 0 nm and less than or equal to 100 nm from the surface of the material being analyzed; this results in the XPS spectrum. Photoelectron spectroscopy records electrons with energies exceeding a certain threshold. The spectral peaks appearing in the photoelectron spectrum represent the emission of electrons with specific energies from atoms. The energy and intensity of these peaks can be used for qualitative and quantitative analysis of the elements contained in a solid surface.

[0034] In some embodiments, the peak intensity of the first peak is I. A The peak intensity of the second peak is I. B , 0.2≤I A / I B ≤0.9. For example, I A / I BThe value is within the range of 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or any combination thereof. Fluorides with high binding energy can provide stronger surface protection, but conductivity may decrease. This application controls the content ratio of fluorides with two binding energies to ensure that the peak intensities of the first and second peaks in the F1s spectrum conform to the above relationship, thus balancing the protective ability and ionic conductivity of the fluorides. This helps to improve the thermal stability and surface protection of the composite fluoride layer, further improving the high-temperature storage performance and safety performance of the secondary battery.

[0035] In some preferred embodiments, 0.5 ≤ I A / I B ≤0.8. When the peak intensity ratio of the first and second peaks is within this range, it can provide excellent surface protection and is beneficial to improving the electrical conductivity of cobalt-containing material particles, enhancing the self-healing ability of ion-conducting particles, thereby helping to optimize the chemical and thermal stability of cobalt-containing material particles, improving high-temperature storage performance, and the good protective layer structure is more resistant to physical impact, thus improving safety performance.

[0036] In some embodiments, the fluorine content is m1% based on the mass of the cobalt-containing material particles, where 0.05 ≤ m1 ≤ 1.50. Exemplarily, m1 can be a value within the range of 0.05, 0.15, 0.31, 0.38, 0.50, 0.66, 0.81, 0.89, 1.00, 1.09, 1.32, 1.47, 1.50, or any combination thereof. Controlling the fluorine content within this range provides flexible adjustment and optimization space, allowing customization according to different application requirements. Specifically, when the fluorine content is controlled at a lower level of 0.05% or greater, a basic protective layer can still be formed on the surface, improving thermal stability and resistance to chemical corrosion. When the fluorine content is controlled at a higher level of 1.50% or less, stronger high-temperature and mechanical protection can be provided in harsher environments, while balancing the potential risks of increased surface impedance and capacity reduction, thereby further improving the high-temperature storage performance and safety performance of the secondary battery.

[0037] In some embodiments, the cobalt-containing material particles contain aluminum in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material particles, the mass content of aluminum is m2%, 0.1 ≤ m1 / m2 ≤ 5.0; preferably, 0.5 ≤ m1 / m2 ≤ 2.0. Exemplarily, the value of m1 / m2 is a value within the range of 0.1, 0.4, 1.0, 1.3, 2.2, 2.5, 3.3, 3.8, 4.2, 4.6, 5, or any two of these. Aluminum can form aluminum fluoride with fluorine, which has a high binding energy and can enhance the structure on the surface of the cobalt-containing material particles, helping to improve the chemical inertness and thermal stability of the cobalt-containing material particles, providing protection at high temperatures, improving the corrosion resistance of the cobalt-containing material particles, reducing side reactions, and extending cycle life. In addition, some aluminum elements are doped into the crystal structure of cobalt-containing material particles. By adjusting the mass content of fluorine and aluminum elements to meet the above ratio, the strength at the grain boundaries can be enhanced, and the structural stability and interface stability of cobalt-containing material particles can be improved, thereby further improving the high-temperature storage performance and safety performance of secondary batteries.

[0038] In some embodiments, the cobalt-containing material particles contain element D in the range of 0 nm to 100 nm from the surface. Element D includes at least one of yttrium, calcium, lanthanum, or cerium. Based on the mass of the cobalt-containing material particles, the mass content of element D is m3%, and 1 ≤ m1 / m3 ≤ 50; preferably, 5 ≤ m1 / m3 ≤ 30. Exemplarily, the value of m1 / m3 is a value within the range of 1, 3, 7, 15, 23, 27, 30, 38, 40, 48, 50, or any two of these values. Using Y, Ca, La, or Ce as doping elements D, and adjusting their mass content with fluorine to conform to the above relationship, can enhance the ionic conductivity and high-temperature performance of the cobalt-containing material particles, thereby further improving the high-temperature storage performance and safety performance of the secondary battery.

[0039] In some embodiments, 0.01 ≤ m³ ≤ 0.50; preferably, 0.05 ≤ m³ ≤ 0.20. For example, the value of m³ is within the range of 0.01, 0.04, 0.08, 0.14, 0.18, 0.28, 0.29, 0.34, 0.42, 0.46, 0.5, or any two of these ranges. When the mass content of element D in the cobalt-containing material particles is within the above range, the high-temperature storage performance and safety performance of the secondary battery can be further improved.

[0040] In some embodiments, the cobalt-containing material particles contain magnesium in the range of 0 nm to 100 nm from the surface; the mass content of magnesium is m based on the mass of the cobalt-containing material particles. 11 %, 0.1≤m1 / m 11 ≤10.0; preferably, 0.5≤m1 / m 11≤5.0. For example, m1 / m 11 The value is within the range of 0.1, 0.8, 2.1, 3.1, 3.9, 5.6, 6.1, 7.7, 8.3, 9.3, 10, or any two of these values. Adding magnesium to cobalt-containing material particles allows them to combine with fluorine to form MgF2, enhancing structural stability. By controlling the mass content of these two elements to conform to the aforementioned relationship, the high-temperature storage performance and safety performance of secondary batteries can be further improved.

[0041] In some embodiments, the cobalt-containing material particles contain zirconium in the range of 0 nm to 100 nm from the surface; the mass content of zirconium is m based on the mass of the cobalt-containing material particles. 12 %, 0.1≤m1 / m 12 ≤20.0; preferably, 1.0≤m1 / m 12 ≤10.0. For example, m1 / m 12 The value is within the range of 0.1, 2.3, 4.0, 4.8, 7.2, 10.5, 12.9, 14.5, 16.4, 19.0, 20.0, or any two of these values. Adding zirconium to cobalt-containing material particles allows it to combine with fluorine to form ZrF4, providing excellent corrosion resistance and improving the structural stability of the cobalt-containing material particles. Controlling the mass content of both elements to conform to the aforementioned relationship can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0042] In some embodiments, the cobalt-containing material particles contain titanium elements in the range of 0 nm to 100 nm from the surface; the mass content of titanium elements is m based on the mass of the cobalt-containing material particles. 13 %, 0.1≤m1 / m 13 ≤10.0; preferably, 0.5≤m1 / m 13 ≤5.0. For example, m1 / m 13 The value is within the range of 0.1, 0.9, 1.8, 2.7, 4.1, 5.4, 5.8, 7.2, 8.4, 9.2, 10.0, or any two of these values. Adding titanium to cobalt-containing material particles allows them to combine with fluorine to form TiF4, improving the conductivity and reducing stress of the cobalt-containing material particles, thus enhancing their structural stability. Controlling the mass content of both elements to conform to the aforementioned relationship can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0043] In some embodiments, the cobalt-containing material particles contain lithium in the range of 0 nm to 100 nm from the surface; the mass content of lithium is m based on the mass of the cobalt-containing material particles. 14 %, 0.01≤m1 / m 14≤0.50; preferably, 0.05≤m1 / m 14 ≤0.10. For example, m1 / m 14 The values ​​are within the range of 0.01, 0.06, 0.08, 0.14, 0.22, 0.25, 0.33, 0.36, 0.43, 0.45, 0.5, or any combination thereof. By controlling the mass content of lithium and fluorine to conform to the above ratio, lithium fluoride provides chemical stability, protects the cathode material, provides a thermal barrier, enhances the thermal stability of the electrode, and reduces the decomposition and morphological changes of the cathode material under high-temperature conditions. Lithium fluoride also improves the mechanical strength of the electrode material, helping to resist physical impacts, such as nail penetration tests. In the event of damage, lithium fluoride can slow the propagation of thermal runaway, improve battery safety, and can repair small cracks on the electrode surface, reducing damage accumulation and enhancing the durability of the cathode material. Therefore, it can improve the high-temperature storage performance and safety performance of secondary batteries.

[0044] In some embodiments, 0.01 ≤ m 11 ≤2.00; preferably, 0.05≤m 11 ≤0.20. For example, m 11 The value is within the range of 0.01, 0.09, 0.30, 0.66, 0.83, 1.01, 1.33, 1.37, 1.61, 1.89, 2.00, or any two of these ranges. Controlling the magnesium content within the above range can further enhance the structural and interfacial stability of cobalt-containing material particles, thereby improving the high-temperature storage performance and safety performance of secondary batteries.

[0045] In some embodiments, 0.05 ≤ m 12 ≤1.00; preferably, 0.07≤m 12 ≤0.20. For example, m 12 The value is within the range of 0.05, 0.09, 0.21, 0.34, 0.46, 0.49, 0.66, 0.70, 0.81, 0.97, 1.00, or any two of these ranges. Controlling the zirconium content within the above range is beneficial for further improving the stability of cobalt-containing material particles, thereby improving the high-temperature storage performance and safety performance of secondary batteries.

[0046] In some embodiments, 0.02 ≤ m 13 ≤2.00; preferably, 0.1≤m 13 ≤0.5. For example, m 13The value is within the range of 0.02, 0.09, 0.30, 0.66, 0.83, 1.01, 1.33, 1.37, 1.61, 1.89, 2.00, or any two of these ranges. Controlling the mass content of titanium in cobalt-containing material particles to meet the above range is beneficial to further improve the stability of cobalt-containing material particles, thereby improving the high-temperature storage performance and safety performance of secondary batteries.

[0047] In some embodiments, 4≤m 14 ≤8; preferably, 6≤m 14 ≤7. For example, m 14 The value is a value within the range of 4, 5, 6, 7, 8, or any two of these values. Controlling the mass content of lithium in cobalt-containing material particles to conform to the above range can improve the thermal stability and durability of the cathode material, and further improve the high-temperature storage performance and safety performance of the secondary battery.

[0048] In some embodiments, the cobalt-containing material particles have a particle size Dv10 of 1–3 μm, a particle size Dv50 of 3–10 μm, and a particle size Dv90 of 8–20 μm. Controlling the particle size distribution within these ranges optimizes the compaction density and stability of the material, promoting ion diffusion and balanced charge-discharge reactions. Furthermore, a uniform particle size distribution helps maintain the uniformity of the electrochemical reaction, thereby facilitating the enhancement of battery performance by fluorine.

[0049] In this application, the cobalt-containing material particles can be prepared by a method including the following steps:

[0050] Preparation of the precursor solution: Dissolve the cobalt source and lithium source in deionized water in the corresponding proportions to obtain the precursor solution. For example, cobalt nitrate (Co(NO3)2) can be used as the cobalt source, and lithium nitrate (LiNO3) can be used as the lithium source. During the dissolution process, a magnetic stirrer can be used to stir thoroughly until the solution is homogeneous and free of impurities. If necessary, filter to remove insoluble particles.

[0051] High-temperature pyrolysis: The precursor solution is atomized and then subjected to high-temperature pyrolysis to obtain precursor powder. Atomization can be performed using spray drying equipment to atomize the precursor solution into fine droplets. During high-temperature pyrolysis, these fine droplets rapidly evaporate and decompose. By controlling the temperature and time of the high-temperature pyrolysis treatment, the particle size and morphology can be adjusted to obtain precursor powder with a suitable particle size.

[0052] Atomization process: The precursor solution (a mixed solution of cobalt nitrate and lithium nitrate) is atomized into droplets with a particle size of 5 to 50 μm using a spray drying device.

[0053] High-temperature pyrolysis: The atomized droplets are placed in an inert gas (nitrogen or argon) atmosphere and heated to 300-500°C at a heating rate of 5-10°C / min. The temperature is maintained for 2-5 hours to allow the droplets to evaporate and decompose rapidly, yielding precursor powder.

[0054] Primary sintering: The precursor powder is subjected to primary sintering under an inert gas (such as nitrogen or argon) to obtain lithium cobalt oxide powder. The primary sintering temperature is 800–1000℃, the time is 6–12 h, the heating rate is 3–8℃ / min, and then it is naturally cooled to room temperature to obtain lithium cobalt oxide powder with a crystallinity ≥95%.

[0055] Surface coating with fluorine: Obtain a fluorine-containing solution, add lithium cobalt oxide powder to the fluorine-containing solution for dispersion, and then perform a curing and drying process to remove excess water, forming a preliminary coating layer on the surface of the lithium cobalt oxide powder, resulting in coated powder. The fluorine-containing solution can be prepared by dissolving a fluorine source in water. Fluorine sources include, but are not limited to, lithium fluoride (LiF), ammonium fluoride (NH4F), sodium fluoride (NaF), potassium fluoride (KF), magnesium fluoride (MgF2), and zinc fluoride (ZnF2). Any fluorine-containing substance other than the fluorine sources listed above can be used, as long as it does not adversely affect the characteristics of the battery. During the dispersion process, continuous stirring can be performed to ensure that the coating material uniformly covers the surface of the lithium cobalt oxide powder.

[0056] Secondary sintering: The coated powder is subjected to secondary sintering to obtain secondary sintered powder. The temperature of the secondary sintering treatment is 600-1000℃, and the time is 5-12 hours. This application performs secondary sintering at high temperature to further solidify the fluoride coating layer. This process can ensure that the thickness of the fluoride coating layer is uniform and stable, thereby improving the durability of the material.

[0057] Surface coating with other elements (including but not limited to Al, Y, Ca, La, Ce, Mg, Zr, Ti, etc.): The secondary sintered powder is mixed with the element precursors providing the above-mentioned other elements in the corresponding mass ratio to obtain a mixed powder. The mixing method is not limited to a specific method and any known method can be used. Specific examples of mixing methods include manual mixing, mortar and pestle (manual or automatic), ball mill, planetary mill, vibratory mill, rotor mill, hammer mill, dispersion mill, mixer, homogenizer, etc. The mixing step can be carried out in air or in other atmospheres such as an inert atmosphere. Before the mixing treatment, an alcohol solvent (such as ethanol) can be added to the secondary sintered powder or element precursor to form a slurry, thereby improving the uniformity of the mixing treatment. If a solvent is added, the slurry needs to be dried at a lower temperature of 60-80°C until the solvent is completely removed. The element precursor can be an oxide or salt of the corresponding element, such as:

[0058] Aluminum: Aluminum oxide (Al2O3) or aluminum nitrate (Al(NO3)3);

[0059] Lanthanum: Lanthanum oxide (La₂O₃) or Lanthanum nitrate (La(NO₃)₃);

[0060] Zirconium: Zirconium oxide (ZrO2) or zirconium nitrate (Zr(NO3)4);

[0061] Titanium: Titanium oxide (TiO2) or titanium isopropoxide (TTIP);

[0062] Calcium: calcium oxide (CaO) or calcium nitrate (Ca(NO3)2);

[0063] Cerium element: cerium oxide (CeO2) or cerium nitrate (Ce(NO3)3).

[0064] Three-stage sintering: The mixed powder is subjected to three sintering processes to obtain cobalt-containing material particles. The temperature of the three-stage sintering process is 600–1000℃, preferably 700–900℃, and the time depends on the specific material properties, generally several hours, for example, 4–9 hours. The three-stage sintering process can be carried out in an atmosphere of air, oxygen, or an inert gas (such as argon) to control the redox reaction.

[0065] Through the above preparation process, lithium, fluorine and other elements interact to form fluorine elements with different binding energies (such as corresponding fluorides AlF3 and LiF) on the surface of cobalt-containing material particles, which can significantly improve the performance of the material, especially the performance of secondary batteries in high-temperature storage tests and nail penetration tests.

[0066] In a second aspect, this application provides a secondary battery, including a positive electrode, a negative electrode, and an electrolyte; the positive electrode includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector; the positive electrode material layer includes the positive electrode material described in the first aspect.

[0067] In this application, there are no particular limitations on the positive electrode, as long as the purpose of this application can be achieved. The aforementioned "positive electrode material layer disposed on at least one surface of the positive electrode current collector" means that the positive electrode material layer can be located on one surface of the positive electrode current collector along its own thickness direction, or on two surfaces of the positive electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire surface area of ​​the positive electrode current collector, or only a part of the surface area; this application has no particular limitations, as long as the purpose of this application can be achieved. This application also has no particular limitations on the positive electrode current collector, as long as the purpose of this application can be achieved. For example, the positive electrode current collector can include aluminum foil, aluminum alloy foil, or composite current collectors (e.g., aluminum-carbon composite current collectors). In this application, the positive electrode active material can also contain non-metallic elements, such as at least one of fluorine, phosphorus, boron, chlorine, silicon, and sulfur.

[0068] In this application, the positive electrode active material layer may further include a positive electrode binder and a conductive agent. This application does not impose any particular limitation on the type of positive electrode binder in the positive electrode active material layer, as long as it achieves the purpose of this application. For example, the positive electrode binder may include, but is not limited to, at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene-butadiene rubber (SBR), or polyurethane. In some embodiments, the polyolefin binder includes at least one of polyethylene, polypropylene, polyolefin ester, polyolefin alcohol, or polyacrylic acid.

[0069] This application does not impose any particular limitation on the type of conductive agent in the positive electrode active material layer, as long as it can achieve the purpose of this application. For example, the conductive agent can be the same type as the conductive agent in the negative electrode active material layer. In some embodiments, the conductive agent includes carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, or carbon fiber; metal-based materials, such as metal powder or metal fiber of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof. This application does not impose any particular limitation on the mass ratio of positive electrode active material, conductive agent, and positive electrode binder in the positive electrode active material layer. Those skilled in the art can choose according to actual needs, as long as it can achieve the purpose of this application. For example, the loading of positive electrode active material in the positive electrode sheet is 4.0 mg / cm³. 2 Up to 10.0 mg / cm 2 .

[0070] This application does not impose any particular limitation on the negative electrode sheet, as long as the purpose of this application can be achieved. For example, the negative electrode sheet includes a negative current collector and a negative electrode material layer disposed on at least one surface of the negative current collector. In this application, the negative electrode material layer can be disposed on one surface or two surfaces in the thickness direction of the negative current collector. It should be noted that the "surface" here can be the entire area of ​​the negative current collector or a part of the negative current collector; this application does not impose any particular limitation, as long as the purpose of this application can be achieved. This application does not impose any particular limitation on the negative current collector, as long as the purpose of this application can be achieved. For example, it can include, but is not limited to, copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foamed nickel, foamed copper, or composite current collectors (e.g., carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector, etc.). In this application, there are no particular limitations on the thickness of the negative current collector, the negative electrode material layer, and the negative electrode sheet, as long as the purpose of this application can be achieved.

[0071] The negative electrode material layer of this application includes a negative electrode active material, which may include, but is not limited to, graphite, mesophase microcarbon spheres (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, and SiO2. x (0.5 < x < 1.6), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate lithiation TiO2-Li4Ti5O 12 At least one of Li-Al alloy and metallic lithium.

[0072] The negative electrode material layer in this application may further include a negative electrode binder and a negative electrode conductive agent, or the negative electrode material layer may further include a negative electrode binder, a negative electrode conductive agent, and a thickener. This application does not particularly limit the types of negative electrode binders and negative electrode conductive agents, as long as they can achieve the purpose of this application. For example, the negative electrode binder may include, but is not limited to, at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid (PAA), styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon.

[0073] The negative electrode conductive agent may include, but is not limited to, carbon-based materials, metal-based materials, conductive polymers, and mixtures thereof. In some embodiments, the carbon-based material is selected from carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer is a polyphenylene derivative. This application does not impose any particular limitation on the mass ratio of negative electrode material, conductive agent, and negative electrode binder in the negative electrode active material layer, as long as the purpose of this application can be achieved. For example, the loading of negative electrode active material in the negative electrode sheet is 1.0 mg / cm³. 2 Up to 1.5 mg / cm 2 .

[0074] This application does not impose any particular limitation on the type of thickener, as long as it can achieve the purpose of this application. For example, the thickener may include, but is not limited to, at least one of sodium carboxymethyl cellulose or carboxymethyl cellulose. This application does not impose any particular limitation on the mass ratio of negative electrode active material, negative electrode conductive agent, negative electrode binder, and thickener in the negative electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of this application can be achieved.

[0075] According to some embodiments of this application, the electrolyte includes lithium salts and non-aqueous solvents. The lithium salts may include, but are not limited to, at least one of: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide {LiN(CF3SO2)2, LiTFSI)}, lithium bis(fluorosulfonyl)imide {Li(N(SO2F)2), LiFSI}, lithium bis(oxalateborate)borate {LiB(C2O4)2, LiBOB}, lithium difluorooxalateborate {LiBF2(C2O4), LiDFOB}, LiNO3, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiC(SO2CF3)3, Li2SiF6, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), or lithium difluoroborate. This application does not limit the content of lithium salts in the electrolyte, as long as the purpose of this application is achieved.

[0076] This application does not impose any particular limitation on non-aqueous solvents, as long as they can achieve the purpose of this application. For example, non-aqueous solvents may include, but are not limited to, at least one of carbonate compounds, carboxylic acid ester compounds, ether compounds, or other organic solvents. The aforementioned carbonate compounds may include, but are not limited to, at least one of chain carbonate compounds, cyclic carbonate compounds, or fluorinated carbonate compounds. The aforementioned chain carbonate compounds may include, but are not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, or methyl ethyl carbonate (EMC). The aforementioned cyclic carbonates may include, but are not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, or vinyl ethylene carbonate. The aforementioned fluorocarbonate compounds may include, but are not limited to, at least one of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The aforementioned carboxylic acid ester compounds may include, but are not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valproic acid lactone, or caprolactone. The aforementioned ether compounds may include, but are not limited to, at least one of 1,3-dioxapentane (DOL), ethylene glycol dimethyl ether (1,2-dimethoxyethane, DME), dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran. The aforementioned other organic solvents may include, but are not limited to, at least one of dimethyl sulfoxide, 1,2-dioxapentane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, or trioctyl phosphate.

[0077] The secondary battery of this application also includes a separator. This application does not impose any particular limitation on the separator, as long as it achieves the purpose of this application. For example, the material of the separator may include, but is not limited to, at least one of polyethylene (PE), polyolefins (PO) primarily composed of polypropylene (PP), polyester (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex, and aramid. The type of separator may include at least one of woven membrane, nonwoven membrane, microporous membrane, composite membrane, rolled membrane, and spun membrane. For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, membrane, or composite membrane with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate, and polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is disposed on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixture of polymer and inorganic materials. For example, the inorganic layer includes inorganic particles and a binder. This application does not have any particular limitation on the inorganic particles, which may include at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. This application does not have any particular limitation on the binder, which may be at least one of the above-mentioned positive electrode binders or negative electrode binders. The polymer layer contains a polymer. This application does not have any particular limitation on the polymer, which may include at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, or polyvinylidene fluoride and poly(vinylidene fluoride-hexafluoropropylene). In this application, there is no particular limitation on the thickness of the separator, as long as it can achieve the purpose of this application. For example, the thickness of the separator can be from 5 μm to 500 μm.

[0078] The secondary battery of this application also includes a packaging bag for containing the positive electrode, negative electrode, separator, and electrolyte, as well as other components known in the art for secondary batteries. This application does not limit the aforementioned other components. This application does not impose any particular limitation on the packaging bag; it can be any packaging bag known in the art, as long as it can achieve the purpose of this application.

[0079] The secondary battery described in this application is not particularly limited and may include any device in which an electrochemical reaction occurs. In one embodiment of this application, the secondary battery may include, but is not limited to, a lithium-ion secondary battery, a lithium polymer secondary battery, or a lithium-ion polymer secondary battery.

[0080] This application does not impose any particular limitation on the preparation method of the secondary battery. For example, it may include the following steps: stacking the positive electrode, separator and negative electrode in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode, separator and negative electrode in sequence, and then fixing the four corners of the entire stacked structure to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery.

[0081] Thirdly, this application provides an electronic device including the secondary battery described in the second aspect above.

[0082] The electronic device described in this application is not particularly limited and can be any electronic device known in the prior art. For example, the electronic device may include, but is not limited to, laptops, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors.

[0083] The following uses a lithium-ion battery as an example to illustrate the solution of this application with reference to the specific embodiments. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available products, and the devices or equipment used are all purchased from conventional market sales channels.

[0084] Test methods

[0085] Element content test

[0086] The elemental content of the cobalt-containing material particles in this application can be tested using an X-ray photoelectron spectrometer, referring to the "General Rules for X-ray Photoelectron Spectroscopy Analysis Methods GB / T19500-2004". The surface depth of the cobalt-containing material particles tested during XPS is 0–100 nm.

[0087] High-temperature storage performance test

[0088] The lithium-ion battery was placed in an environment of 25°C and allowed to stand for 5 minutes. Then, it was discharged at a constant current of 0.2C until the voltage reached 3.0V, and allowed to stand for 10 minutes. Subsequently, it was charged at a constant current of 0.7C until the full charge voltage reached 4.52V, and then charged at a constant voltage until the current reached 0.025C, and allowed to stand for 10 minutes. This charging and discharging process was repeated three times, and the discharge capacity of the last charge was recorded as the initial capacity of the lithium-ion battery.

[0089] After placing the lithium-ion battery at a high temperature (45°C), the above charging and discharging process was defined as one cycle, and a total of 200 charge-discharge cycles were performed. The discharge capacity of the 200th cycle was recorded. High-temperature (45°C) cycle capacity retention rate (%) = [(initial capacity - discharge capacity of 200 cycles) / initial capacity] × 100.

[0090] Puncture test

[0091] The lithium-ion battery was placed in a 25°C environment and left to stand for 5 minutes. Then, it was discharged at a constant current of 0.2C until the voltage reached 3.0V, and left to stand for 10 minutes. Subsequently, it was charged at a constant current of 0.7C until the full charge voltage reached 4.52V, and then charged at a constant voltage until the current reached 0.025C, and left to stand for 10 minutes. The lithium-ion battery was photographed, and its internal voltage resistance (1kHz frequency) was measured by directly connecting the probe of a voltage resistance meter to the positive and negative terminals. A temperature sensing wire was attached to the surface of the lithium-ion battery. In a 25°C testing environment, the battery was placed on a test platform, and a 3mm diameter straight nail was used to puncture the battery from its center at a speed of 150mm / s. The battery was completely punctured by the nail, and the test was continued for 30 minutes before photographing. The internal voltage resistance was measured again using the voltage resistance meter. If the battery did not catch fire or explode, it indicated that the lithium-ion battery had passed the puncture performance test. In the puncture performance tests in the following embodiments and comparative examples, 20 batteries were tested, and the number of punctures that passed was recorded in Tables 1 and 2.

[0092] Example 1-1

[0093] Preparation of cobalt-containing material particles:

[0094] Cobalt nitrate and lithium nitrate in corresponding proportions were dissolved in deionized water to obtain a precursor solution. The precursor solution was atomized by spray drying and then subjected to high-temperature pyrolysis at 120°C for 2 hours to obtain precursor powder. The precursor powder was then subjected to a single sintering treatment under an inert gas (such as nitrogen or argon) at a temperature of 800°C for 7 hours to obtain lithium cobalt oxide powder.

[0095] Lithium cobalt oxide powder was dispersed in an ammonium fluoride solution and then cured and dried to obtain coated powder. The coated powder was then subjected to a secondary sintering process at 900℃ for 7 hours to obtain secondary sintered powder.

[0096] The secondary sintered powder and the elemental precursor providing other elements were mixed by mass ratio and milled using a ball mill to obtain a mixed powder, wherein the other elements were aluminum and the elemental precursor was alumina. The mixed powder was then subjected to a third sintering treatment at 1000℃ for 5 hours to obtain cobalt-containing material particles.

[0097] X-ray photoelectron spectroscopy (XPS) was performed on the cobalt-containing material particles of Example 1-1. The F1s spectrum of the cobalt-containing material particles prepared in Example 1-1 is shown in Figure 1. The cobalt-containing material particles contain fluorine in the range of 0 nm to 100 nm from the surface. The F1s spectrum includes a first peak and a second peak. The peak value of the first peak is in the range of 687 eV to 688 eV, and the peak value of the second peak is in the range of 684 eV to 686 eV. The peak intensity of the first peak is I. A The peak intensity of the second peak is I. B I A / I B =0.26.

[0098] In this application, the F1s spectrum refers to the spectral peaks of fluorine in XPS, and the chemical state of fluorine can be confirmed by the peak positions (binding energies). In this application, the F1s spectrum is obtained using a method including the following steps:

[0099] 1. XPS test conditions

[0100] • Instrument model: Thermo Scientific ESCALAB Xi+ X-ray photoelectron spectrometer;

[0101] • Excitation source: Monochromatic Al Kα rays (hv = 1486.6 eV);

[0102] • Analysis mode: High-resolution narrow scan (Pass Energy = 20 eV, Step Size = 0.1 eV);

[0103] • Charge neutralization: Neutralization is achieved using a combination of a low-energy electron gun (≤5eV) and an Ar+ beam;

[0104] • Calibration reference: C1s (284.8eV) is used as the internal standard to correct the binding energy.

[0105] 2. F1s spectral peak fitting parameters

[0106] • Software: Avantage v5.9, using the Shirley background subtraction method;

[0107] • Peak shape function: 70% Gaussian + 30% Lorentzian mixed peak shape;

[0108] Peak-splitting strategy:

[0109] Peak 1 (high binding energy peak):

[0110] ■ Binding energy range: 687.0-688.0 eV;

[0111] ■ Classification by chemical state: such as AlF3;

[0112] Peak 2 (low binding energy peak):

[0113] ■ Binding energy range: 684.0-686.0 eV;

[0114] ■ Classified by chemical state: such as LiF.

[0115] 3. Peak intensity ratio calculation

[0116] • Intensity definition: Peak area is used, rather than peak height.

[0117] • Calculation formula: I A / I B = Peak area of ​​the first peak (687-688eV) / Peak area of ​​the second peak (684-686eV).

[0118] 4. Surface Depth Analysis

[0119] Splashing conditions: Ar + Beam (2keV, 1μA / cm) 2 Sputtering rate = 0.5 nm / s;

[0120] • Depth range: 0-100nm.

[0121] Please refer to Figure 2 for a schematic diagram of the structure of the cobalt-containing material particles. A specific embodiment of this application provides a cobalt-containing material particle comprising a lithium cobalt oxide core, with a first outer layer and a second outer layer on the surface of the lithium cobalt oxide core, wherein the first outer layer is located between the lithium cobalt oxide core and the second outer layer. The first outer layer comprises lithium fluoride, corresponding to the low binding energy of fluorine, and the second outer layer comprises lithium fluoride and other elemental fluorides (MF). x M includes, but is not limited to, Al, Y, Ca, La, Ce, Mg, Zr, Ti, etc., and other element fluorides correspond to fluorine elements with higher binding energies.

[0122] Preparation of the positive electrode:

[0123] A positive electrode slurry was prepared by dissolving the aforementioned cobalt-containing material particles (97 wt%), conductive carbon black (1.5 wt%), and polyvinylidene fluoride (1.5 wt%) in N-methylpyrrolidone. The positive electrode slurry was uniformly coated onto one surface of a 10 μm thick aluminum foil used as the positive electrode current collector. The aluminum foil was dried at 120°C to obtain a positive electrode sheet with an 80 μm thick positive electrode material layer coated on one side. The above steps were repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of the positive electrode material layer. The coated aluminum foil was dried, pressurized, and then cut to the specified size to fabricate the positive electrode.

[0124] Preparation of the isolation membrane: A 12μm thick polyethylene (PE) microporous membrane was selected as the isolation membrane.

[0125] Preparation of the negative electrode:

[0126] A mixture of artificial graphite (96 wt%), styrene-butadiene rubber (2 wt%), polyacrylic acid (0.5%), carbon nanotubes (0.5%), and carboxymethyl cellulose (1%) was prepared by mixing deionized water as a solvent and stirring until homogeneous, resulting in a negative electrode slurry with a solid content of 45 wt%. This negative electrode slurry was uniformly coated onto one surface of a 6 μm thick copper foil current collector, and then dried to obtain a negative electrode sheet with a single-sided coating of the negative electrode mixture. The above steps were repeated on the other surface of the copper foil to obtain a negative electrode sheet with a double-sided coating of the negative electrode mixture. The coated copper foil was dried, pressurized, and then cut to the specified size to fabricate the negative electrode.

[0127] Electrolyte preparation:

[0128] In an argon atmosphere glove box with a water content of less than 10 ppm, dimethyl carbonate and ethylene carbonate (dimethyl carbonate and ethylene carbonate in a mass ratio of 1:2) are mixed to obtain a base solvent. Then, lithium salt LiPF6 is added to the base solvent and mixed evenly to obtain an electrolyte. The mass content of LiPF6 is 12.5% ​​based on the mass of the electrolyte.

[0129] Battery making:

[0130] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. The electrode assembly is then wound up. After welding the tabs, the electrode assembly is placed in an outer aluminum-plastic film. After removing the moisture at 80°C, the electrolyte is injected. The lithium-ion battery is obtained through vacuum sealing, settling, formation, shaping, and capacity testing.

[0131] Examples 1-2 to 1-26, Comparative Examples 1 to 2

[0132] Except for adjusting the parameters according to Table 1, everything else is the same as in Example 1-1. By adjusting the duration of the secondary and tertiary sintering processes, the I1 in the F1s spectrum of the cobalt-containing material particles is adjusted. A / I B The values ​​are shown in Table 1. By adjusting the amount of fluorine source, the type and amount of other element precursors, the mass content of fluorine and the type or mass content of other elements are as shown in Table 1. In Comparative Example 1, no element precursors providing other elements were used, and the secondary sintering powder was directly subjected to a third sintering treatment. In Comparative Example 2, lithium cobalt oxide powder was first mixed with element precursors providing other elements, and then subjected to a third sintering treatment, so that aluminum was directly doped into the lithium cobalt oxide crystal phase and did not form high-binding-energy fluorides with fluorine. Then, fluorine was coated on the surface and subjected to a second sintering treatment.

[0133] Table 1

[0134] As shown in Table 1, the F1s spectrum regulated in this application includes a first peak and a second peak. The peak value of the first peak is in the range of 687 eV to 688 eV, and the peak value of the second peak is in the range of 684 eV to 686 eV. This allows the two fluorine elements with different binding energies to combine, thereby improving the high-temperature storage performance and puncture safety performance of the secondary battery. In particular, regulating the peak intensities of the first and second peaks satisfies 0.2 ≤ I A / I B ≤0.9 is beneficial for further improving the high-temperature storage performance and puncture safety performance of secondary batteries; preferably, when 0.5≤I A / I B When the value is ≤0.8, the high-temperature storage performance and puncture safety performance of the secondary battery can be improved more significantly.

[0135] In particular, when the mass content of aluminum and fluorine in cobalt-containing material particles is adjusted to meet the condition of 0.1≤m1 / m2≤5.0, the high-temperature storage performance and safety performance of the secondary battery can be further improved; especially when the condition of 0.5≤m1 / m2≤2.0 is met, the high-temperature storage performance and safety performance of the secondary battery are improved even more significantly.

[0136] In particular, when the cobalt-containing material particles include at least one of yttrium, calcium, lanthanum, or cerium, it is beneficial to further improve the high-temperature storage performance and safety performance of the secondary battery. Specifically, when calcium and at least one of lanthanum or cerium are included simultaneously, the high-temperature storage performance and safety performance of the secondary battery are even better. Especially when the mass content of the above-mentioned doping elements and fluorine satisfies 1 ≤ m1 / m3 ≤ 50, preferably 5 ≤ m1 / m3 ≤ 30, the high-temperature storage performance and safety performance of the secondary battery can be improved even more significantly. In particular, when the mass content of the above-mentioned doping elements satisfies 0.01 ≤ m3 ≤ 0.50, preferably 0.05 ≤ m3 ≤ 0.20, the secondary battery exhibits even better high-temperature storage performance and safety performance.

[0137] Examples 2-1 to 2-24

[0138] Except for adjusting the parameters according to Table 2, the rest is the same as in Examples 1-19. By adjusting the amount of fluorine source and the types and amounts of other element precursors, the mass content of fluorine and the types or mass contents of other elements are as shown in Table 2.

[0139] Table 2

[0140] As shown in Table 2, the mass content of fluorine and magnesium in this application is controlled to satisfy 0.1 ≤ m1 / m 11 ≤10.0, preferably 0.5≤m1 / m 11 A magnesium content ≤5.0 can improve the high-temperature storage performance and safety performance of secondary batteries. In particular, adjusting the magnesium content to meet the requirement of 0.01 ≤ m 11 ≤2.00, preferably 0.05≤m 11 ≤0.20 can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0141] Specifically, this application controls the mass content of fluorine and zirconium to satisfy 0.1 ≤ m1 / m 12 ≤20.0, preferably 1.0≤m1 / m 12 A concentration ≤10.0 can improve the high-temperature storage performance and safety performance of secondary batteries. In particular, adjusting the zirconium content to meet the requirement of 0.05 ≤ m... 12 ≤1.00, preferably 0.07≤m 12 ≤0.20 can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0142] Specifically, this application controls the mass content of fluorine and titanium to satisfy 0.1 ≤ m1 / m 13 ≤10.0, preferably 0.5≤m1 / m13 A concentration ≤5.0 can improve the high-temperature storage performance and safety performance of secondary batteries. In particular, adjusting the mass content of titanium to meet the requirement of 0.02 ≤ m 13 ≤2.00, preferably 0.1≤m 13 ≤0.5 can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0143] Examples 3-1 to 3-8

[0144] Except for adjusting the parameters according to Table 3, the rest is the same as in Examples 2-24. By adjusting the amount of lithium source, the mass content of lithium element is as shown in Table 3.

[0145] Table 3

[0146] As shown in Table 3, the mass content of fluorine and lithium elements in this application is controlled to satisfy 0.01 ≤ m1 / m 14 ≤0.50, preferably 0.05≤m1 / m 14 A concentration ≤0.10 can improve the high-temperature storage performance and safety performance of secondary batteries. In particular, adjusting the lithium mass content to satisfy 4≤m 14 ≤8, preferably 6≤m 14 ≤7 can further improve the high-temperature storage performance and safety performance of secondary batteries.

[0147] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the principles of this application should be included within the protection scope of this application.

Claims

1. A positive electrode material, characterized in that, The cathode material includes a cobalt-containing material; the cobalt-containing material is tested by X-ray photoelectron spectroscopy, and the cobalt-containing material contains fluorine in the range of 0 nm to 100 nm from the surface. The F1s spectrum includes a first peak and a second peak, the peak value of the first peak is in the range of 687 eV to 688 eV, and the peak value of the second peak is in the range of 684 eV to 686 eV.

2. The cathode material according to claim 1, characterized in that, The peak intensity of the first peak is I A The peak intensity of the second peak is I. B , 0.2≤I A / I B ≤0.9; preferably, 0.5≤I A / I B ≤0.

8.

3. The cathode material according to claim 1 or 2, characterized in that, Based on the mass of the cobalt-containing material, the mass content of the fluorine element is m1%, where 0.05 ≤ m1 ≤ 1.

50.

4. The cathode material according to claim 3, characterized in that, The cobalt-containing material contains aluminum in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material, the mass content of the aluminum element is m2%, 0.1 ≤ m1 / m2 ≤ 5.0; preferably, 0.5 ≤ m1 / m2 ≤ 2.

0.

5. The positive electrode material according to claim 3, characterized in that, The cobalt-containing material contains element D in the range of 0 nm to 100 nm from the surface, and element D includes at least one of yttrium, calcium, lanthanum or cerium; based on the mass of the cobalt-containing material, the mass content of element D is m3%, 1 ≤ m1 / m3 ≤ 50; preferably, 5 ≤ m1 / m3 ≤ 30.

6. The cathode material according to claim 5, characterized in that, 0.01≤m3≤0.50; preferably, 0.05≤m3≤0.

20.

7. The cathode material according to claim 3, characterized in that, The cathode material satisfies at least one of the following conditions: (1) The cobalt-containing material contains magnesium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material, the mass content of the magnesium element is m. 11 %, 0.1≤m1 / m 11 ≤10.0; preferably, 0.5≤m1 / m 11 ≤5.0; (2) The cobalt-containing material contains zirconium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material, the mass content of the zirconium element is m. 12 %, 0.1≤m1 / m 12 ≤20.0; preferably, 1.0≤m1 / m 12 ≤10.0; (3) The cobalt-containing material contains titanium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material, the mass content of the titanium element is m. 13 %, 0.1≤m1 / m 13 ≤10.0; preferably, 0.5≤m1 / m 13 ≤5.0; (4) The cobalt-containing material contains lithium in the range of 0 nm to 100 nm from the surface; based on the mass of the cobalt-containing material, the mass content of the lithium is m. 14 %, 0.01≤m1 / m 14 ≤0.50; preferably, 0.05≤m1 / m 14 ≤0.

10.

8. The cathode material according to claim 7, characterized in that, The cathode material satisfies at least one of the following conditions: (1) 0.01≤m 11 ≤2.00; preferably, 0.05≤m 11 ≤0.20; (2) 0.05≤m 12 ≤1.00; preferably, 0.07≤m 12 ≤0.20; (3) 0.02≤m 13 ≤2.00; preferably, 0.1≤m 13 ≤0.5; (4) 4≤m 14 ≤8; preferably, 6≤m 14 ≤7.

9. A secondary battery, characterized in that, It includes a positive electrode, a negative electrode, and an electrolyte; the positive electrode includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector; the positive electrode material layer includes the positive electrode material according to any one of claims 1 to 8.

10. An electronic device, characterized in that, Includes the secondary battery as described in claim 9.