Positive electrode material, positive electrode sheet, and secondary battery
By introducing magnesium into the cathode material of lithium-ion batteries and controlling its gradient distribution, combined with elements such as lithium and titanium, the performance deficiencies of cathode materials in terms of high rate and cycle life are solved, and the electrochemical performance and cycle performance of the battery are improved.
Patent Information
- Application Number
- PCT/CN2025/082199
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-03-12
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium-ion battery cathode materials have insufficient performance in terms of high rate and cycle life, which affects the cycle performance and high rate performance of secondary batteries.
By introducing magnesium into the cathode material, its gradient distribution on the surface and outer region of cobalt-containing particles is controlled to form a stable oxide layer, optimize the conduction path of electrons and ions, reduce internal resistance, and improve the conductivity and structural stability of the material by combining the synergistic effect of elements such as lithium and titanium.
It improves the electrochemical and cycle performance of the cathode material, enhances the high-rate performance and cycle life of the secondary battery, reduces temperature rise and mechanical stress, and optimizes the current density distribution.
Smart Images

Figure CN2025082199_12112026_PF_FP_ABST
Abstract
Description
A positive electrode material, a positive electrode sheet, and a secondary battery Technical Field
[0001] This application relates to the field of energy storage materials, specifically to a cathode material, a cathode sheet, and a secondary battery. Background Technology
[0002] Lithium-ion batteries, as high-efficiency power sources, are widely used in various devices and energy storage systems. In the preparation of cathodes for lithium-ion batteries, cobalt-containing cathode materials such as lithium cobalt oxide (LiCoO2) have attracted attention due to their excellent electrochemical performance and energy density. However, cobalt-containing cathode materials like lithium cobalt oxide still have shortcomings in terms of high-rate operation and cycle life, which can adversely affect the cycle performance and high-rate performance of the battery. Summary of the Invention
[0003] This application provides a positive electrode material, a positive electrode sheet, and a secondary battery. The positive electrode material of this application is not prone to side reactions and not only has good electrochemical and cycle performance, but also good corrosion resistance and conductivity. Therefore, the positive electrode sheet containing the positive electrode material of this application has good interfacial properties, and when used in a secondary battery, it can enhance the cycle performance and high-rate performance of the secondary battery.
[0004] In a first aspect, this application provides a cathode material comprising cobalt-containing particles, wherein the cobalt-containing particles contain magnesium; X-ray photoelectron spectroscopy tests show that the magnesium content on the surface of the cobalt-containing particles is W1%; and the magnesium content in the region 80nm to 120nm from the surface of the cobalt-containing particles is W2%, where W1 > W2.
[0005] In the above technical solution, the inventors discovered that when the above conditions are met, the cathode material is less prone to side reactions, which can reduce the temperature rise of the secondary battery at high rates. Furthermore, the magnesium element on the surface of the cobalt-containing particles can form stable oxides, thereby improving the corrosion resistance and chemical stability of the cathode material. In addition, since the magnesium content on the surface of the cobalt-containing particles is greater than the magnesium content in the 80nm–120nm region, the electron and ion conduction paths in the cathode material can be optimized, reducing the internal resistance of the cathode material and improving its conductivity, resulting in excellent electrochemical performance. When the cathode material in the above solution is used in cathode plates and secondary batteries, it can improve the performance of both the cathode plate and the secondary battery at high rates and their cycle performance.
[0006] In one possible implementation, at a distance D from the surface of the cobalt-containing particles x nm and D y In the region of nm, the magnesium content is W. x % and Wy %, 0.2≤(W) x -W y ) / (D y -D x )≤0.3, and 0≤D x <D y ≤120.
[0007] In the above technical solution, the magnesium content is gradient-distributed in the region 0–120 nm from the surface of the cobalt-containing particles. This alleviates the inhomogeneity of the electrochemical reaction between the inner and outer layers of the cathode material, ensuring a uniform current density distribution and improving the performance of the cathode material at high rates. Furthermore, the gradient-distributed magnesium reduces the mechanical stress caused by concentration changes during charging and discharging, helping to maintain the stability of the cathode material. The gradient-distributed magnesium also reduces interfacial impedance, further enhancing the conductivity of the cathode material and helping to maintain its performance during high-rate charging and discharging. When the cathode material in the above technical solution is used in cathode plates and secondary batteries, the cycle performance and high-rate performance of the secondary battery can be further improved.
[0008] In one possible implementation, the cobalt-containing particles also include lithium, and in the region of the cobalt-containing particles from 0 to 120 nm, the mass ratio of lithium, cobalt, and magnesium is 1:(0.98–1):(0.0005–0.003).
[0009] In the above technical solution, by controlling the mass ratio of lithium, cobalt and magnesium in the surface region of cobalt-containing particles, the conductivity and structural integrity of cobalt-containing particles can be enhanced while maintaining the stability of the crystal structure, thereby improving the performance and cycle life of the secondary battery at high rates.
[0010] In one possible implementation, the magnesium content is 0.05% to 1% based on the mass of the cobalt-containing particles.
[0011] In one possible implementation, the cobalt-containing particles also include titanium, and the mass ratio of magnesium to titanium is 0.25:1 to 3:1.
[0012] In the above technical solution, the synergistic effect of magnesium and titanium not only improves the conductivity and stability of the cathode material, but also forms a more stable solid solution with cobalt by averaging the metal valence states. Furthermore, the combined action of magnesium and titanium at the lattice sites helps reduce the structural strain of the positive-valence material, resulting in superior cycle stability during charge and discharge; effectively suppressing the phase transition of cobalt-containing particles at high potentials, and improving the overall electrochemical performance of the cathode material.
[0013] In one possible implementation, the cobalt-containing particles have Dv90, Dv50 and Dv10 particle sizes of R1μm, R2μm and R3μm, respectively, and the cobalt-containing particles satisfy at least one of the following conditions: (1) 15≤R1≤25; (2) 10≤R2≤20; (3) 3≤R3≤10.
[0014] In the above technical solution, when the cathode material is used in a secondary battery, by controlling the particle size values of cobalt-containing particles Dv90, Dv50 and Dv10, the compaction density and stability of the cathode material can be optimized, which can promote ion diffusion and balance the charge and discharge reaction, and is beneficial to improving the energy density of the secondary battery.
[0015] In one possible implementation, (R1-R3) / R2≤0.4.
[0016] In the above technical solution, the cobalt-containing particles have a relatively uniform particle size distribution, which is beneficial to improving the uniformity of the electrochemical reaction of the cathode material, thereby improving the performance of the secondary battery.
[0017] In one possible implementation, the cobalt-containing particles also include at least one of aluminum, yttrium, lanthanum, or zirconium.
[0018] In the above technical solution, the cobalt-containing particles contain the aforementioned elements, which can form a stable protective layer on the surface of the cobalt-containing particles, further suppressing the side reactions of the cathode material and helping to further improve the electrochemical performance and cycle performance of the cathode material.
[0019] In one possible implementation, based on the mass of the cobalt-containing particles, the cathode material satisfies at least one of the following conditions: (1) the aluminum content is 0.5% to 2%; (2) the yttrium content is 0.01% to 0.5%; (3) the lanthanum content is 0.01% to 0.5%; and (4) the zirconium content is 0.02% to 0.7%.
[0020] Secondly, this application provides a positive electrode sheet comprising the aforementioned positive electrode material. Therefore, the positive electrode sheet of this application also has good performance in use.
[0021] Thirdly, this application provides a secondary battery comprising the aforementioned positive electrode. Therefore, the secondary battery provided by this application exhibits excellent cycle performance and performance at high rates.
[0022] The beneficial effects of this application are:
[0023] This application provides a positive electrode material, a positive electrode sheet, and a secondary battery. The positive electrode material includes cobalt-containing particles containing magnesium. X-ray photoelectron spectroscopy (XPS) analysis shows that the magnesium content on the surface of the cobalt-containing particles is W1%, and the magnesium content in the region 80 nm to 120 nm from the surface of the cobalt-containing particles is W2%, where W1 > W2. By controlling the concentration distribution of magnesium in the cobalt-containing particles, this application makes the positive electrode material less prone to side reactions. The positive electrode material not only has good electrochemical performance and cycle performance, but also good corrosion resistance and conductivity. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments of this application will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 is a graph showing the relationship between the magnesium content in the cathode material provided in Example 1-1 of this application and the distance from the surface of the cobalt-containing particles. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0027] In existing technologies, taking lithium-ion batteries as an example, the cathode material often contains cobalt-containing particles such as lithium cobalt oxide, which can improve the electrochemical performance and energy density of the electrochemical device. However, the performance of secondary batteries using the above-mentioned cathode materials needs to be improved in terms of high-rate and cycle life. Although there are technologies to dope magnesium into cobalt-containing particles such as lithium cobalt oxide, the stability of the cathode material is insufficient, limiting its improvement on the cycle performance and high-rate performance of secondary batteries.
[0028] Based on the aforementioned technical issues, the cathode material provided in this application is less prone to side reactions and possesses not only excellent electrochemical and cycle performance but also good corrosion resistance and conductivity. Therefore, cathode sheets containing the cathode material of this application exhibit excellent interfacial properties, which, when used in secondary batteries, can enhance the cycle performance and high-rate performance of the secondary battery.
[0029] The positive electrode material, positive electrode sheet, and secondary battery of the present application embodiments are described in detail below.
[0030] In a first aspect, this application provides a cathode material comprising cobalt-containing particles containing magnesium. Based on X-ray photoelectron spectroscopy characterization, the magnesium content on the surface of the cobalt-containing particles is W1%, and the magnesium content in the region 80 nm to 120 nm from the surface of the cobalt-containing particles is W2%, where W1 > W2.
[0031] It should be noted that the terms "surface of cobalt-containing particles" and "distance to the surface of cobalt-containing particles" mentioned in this application are calculated using the following standard: The lowest point of the cobalt-containing particle's surface is located exactly on the outer surface of the inscribed sphere. In this case, "surface of cobalt-containing particles" refers to the region of the cobalt-containing particle located outside the inscribed sphere; this region can be called the "surface of cobalt-containing particles," and the distance from this region to the surface of the cobalt-containing particle is 0 nm. The "distance to the surface of cobalt-containing particles" is also defined with the surface of the inscribed sphere as the reference frame; "D nm from the surface of cobalt-containing particles" means that the distance from the inside of the cobalt-containing particle to the surface of the inscribed sphere is D nm. Furthermore, in this application, the equivalent particle size of the cobalt-containing particles is generally at the micrometer level; therefore, the region 0–120 nm from the cobalt-containing particles can be considered the "surface layer" of the cobalt-containing particles. Additionally, for ease of explanation, as an example, the cobalt-containing particles in this application are based on lithium cobalt oxide particles and can be called "modified lithium cobalt oxide particles."
[0032] In the cathode material of this application, the inventors discovered that magnesium in the surface layer of cobalt-containing particles (i.e., the region from 0 to 120 nm) can passivate active sites, making the cathode material less prone to side reactions and reducing the temperature rise of the secondary battery at high rates. The high magnesium content on the surface of the cobalt-containing particles allows for the formation of a stable oxide layer, increasing the corrosion resistance and chemical stability of the cathode material. Furthermore, the magnesium content on the surface of the cobalt-containing particles is higher than in the 80 nm–120 nm region, which optimizes the electron and ion conduction pathways in the cathode material, reduces the internal resistance, and improves the conductivity, resulting in excellent electrochemical performance. When the cathode material of this application is used in cathode sheets, it enables the cathode sheets to have good interfacial properties, and when used in secondary batteries, it can enhance the cycle performance and high-rate performance of the secondary battery.
[0033] Furthermore, it should be noted that although this application only specifies that the magnesium content in the region "80nm to 120nm from the surface of the cobalt-containing particles" is less than the magnesium content on the surface, in actual products, to reduce manufacturing difficulty, cobalt-containing particles generally also have the following property: the greater the distance from the surface of the cobalt-containing particles, the lower the magnesium content. Preferably, in some embodiments of this application, the rate of change of magnesium content is as follows:
[0034] D at a distance from the surface of the cobalt-containing particles x nm and D y In the region of nm, the magnesium content is W. x % and W y %, 0.2≤(W) x -W y ) / (D y -D x )≤0.3, and 0≤D x <D y ≤120.
[0035] The content of magnesium on the surface of cobalt particles gradually decreases in the surface layer of cobalt particles, which will have the following effects on the cathode material: (1) It alleviates the non-uniformity of electrochemical reaction in cobalt-containing materials, making the current density distribution of cathode materials more uniform, which is conducive to improving the performance of secondary batteries at high rates; (2) It reduces the mechanical stress caused by concentration changes in cathode materials during charging and discharging, improves the stability of cathode materials, and is conducive to improving the thermal stability of secondary batteries; (3) It reduces the interface impedance, enhances the migration ability of cathode materials for lithium ions, and is conducive to maintaining the performance of secondary batteries during high-rate charging and discharging.
[0036] The magnesium content in this application is typically 0.05% to 1% of the mass of the cobalt particles, specifically 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 0.8%, 1%, or within a range of any two of the above values.
[0037] In some embodiments of this application, in the 0-120 nm region of the cobalt-containing particles, the mass ratio of lithium, cobalt, and magnesium is 1:(0.98-1):(0.0005-0.003). By controlling the proportions of lithium, cobalt, and magnesium on the surface of the cobalt-containing particles, the conductivity of the surface layer of the cobalt-containing material can be enhanced while maintaining the stability of the crystal structure. This can further improve the performance and cycle life of the secondary battery at high rates.
[0038] In addition, in some embodiments of this application, the cobalt-containing particles also include titanium, and the mass ratio of magnesium to titanium is 0.25:1 to 3:1. The synergistic effect of magnesium and titanium not only improves the conductivity and stability of the cathode material, but also forms a more stable solid solution with cobalt by averaging the metal valence state, greatly enhancing the conductivity and stability of the cathode material. Furthermore, the combined action of magnesium and titanium at the lattice positions helps reduce the structural strain of the cathode material, resulting in excellent cycle stability during charge and discharge. Specifically, taking modified lithium cobalt oxide particles as an example, the combined action of magnesium and titanium can effectively suppress the phase transition of lithium cobalt oxide at high potentials, improving the overall electrochemical performance of the cathode material. When the cathode material is used in secondary batteries, it can improve the performance, cycle performance, and other electrochemical properties of the secondary battery at high rates.
[0039] In addition, in some other embodiments of this application, the cobalt-containing particles may also include at least one of aluminum, yttrium, lanthanum, or zirconium. Specifically, based on the mass of the cobalt-containing particles, the aluminum content is 0.5%–2%, the yttrium content is 0.01%–0.5%, the lanthanum content is 0.01%–0.5%, and the zirconium content is 0.02%–0.7%. These elements can synergistically work with the magnesium in the cobalt-containing particles to form a stable protective layer on the surface of the cobalt-containing particles, further suppressing side reactions in the cathode material. When used in secondary batteries, this can further enhance the cycle performance and high-rate performance of the secondary battery. Aluminum is beneficial for improving the surface stability of the cathode material, yttrium is beneficial for enhancing the structural toughness of the cathode material, lanthanum can increase the conductivity and thermal stability of the cathode material, and zirconium can improve the structural stability and cycle life of the cathode material.
[0040] In addition, in some embodiments of this application, the particle size of cobalt-containing particles is also optimized; specifically, the Dv90, Dv50 and Dv10 particle sizes of cobalt-containing particles are R1μm, R2μm and R3μm respectively, and the values of R1, R2 and R3 can be: (1) 15≤R1≤25, for example 15, 17, 19, 20, 24, 25 etc. or within the range of any two of the above values; (2) 10≤R2≤20, for example 10, 12, 15, 18, 20 etc. or within the range of any two of the above values; (3) 3≤R3≤10, for example 3, 5, 7, 8, 9, 10 etc. or within the range of any two of the above values. This can optimize the compaction density and stability of the cathode material, promote ion diffusion and balance charge and discharge reaction, and help improve the energy density of the secondary battery. More preferably, (R1-R3) / R2≤0.4, so that the particle size distribution of cobalt-containing particles is more uniform, which is beneficial to improving the uniformity of the electrochemical reaction of the cathode material, thereby improving the performance of the secondary battery.
[0041] As an example, this application also provides a method for preparing a cathode material, taking a lithium cobalt oxide-based cathode material as an example, the steps of which are as follows:
[0042] S100: Preparation of precursor: Magnesium nitrate (Mg(NO3)2), cobalt nitrate (Co(NO3)2), and lithium nitrate (LiNO3) are dissolved in deionized water to form a mixed solution, and then spray pyrolysis is performed to obtain a powdered precursor.
[0043] During the formation of the mixed solution, a magnetic stirrer is typically used to thoroughly stir the mixture to dissolve all components; filtration may also be performed if necessary to remove insoluble particles. Additionally, to ensure that magnesium is subsequently enriched on the surface of the cobalt-containing particles, 0.5 wt% citric acid is usually added as a magnesium migration promoter during the formation of the mixed solution.
[0044] During spray pyrolysis, the inlet temperature is generally 280℃~300℃, the outlet temperature is generally 650℃~700℃, and the atomization pressure is around 0.3MPa.
[0045] In addition, titanium tetrachloride (TiCl4) can be added in this step to include titanium in the cobalt-containing particles.
[0046] S200, Gradient Sintering: The precursor is placed in a high-temperature furnace and sintered in an inert gas atmosphere at 650℃~750℃ for the first stage, followed by a second stage sintering at 950℃~980℃ in an oxygen atmosphere, and then quenched to obtain primary particles; the quenching rate is greater than 50℃ / s. During the first-stage sintering process, the migration of magnesium to the surface of cobalt-containing particles can be promoted; high-temperature sintering can promote the formation of an oxide layer and stabilize the crystal structure; the quenching rate greater than 50℃ / s can lock the concentration gradient distribution of magnesium. By adaptively adjusting the parameters of S100 and S200, the gradient distribution of magnesium in the surface layer of cobalt-containing particles can be well controlled. This application will describe the specific details using Examples 1-1 as examples later. The cathode materials in other examples and comparative examples can be obtained by adjusting conventional values, and will not be described in detail here.
[0047] If the cobalt-containing particles include other elements, the following steps will also be performed:
[0048] S300, Adding other elements: The sintered product is added to a nitrate solution containing aluminum, yttrium, lanthanum and zirconium, and stirred continuously before curing and drying.
[0049] In this step, the nitrate may also include magnesium nitrate, which can replenish the magnesium content on the surface of the primary particles.
[0050] S400, Secondary Sintering: The particles obtained after curing and drying are sintered a second time.
[0051] This step strengthens the magnesium oxide layer on the particle surface, ensuring that the resulting product has a stable structure and good durability.
[0052] Secondly, this application provides a positive electrode sheet, which includes the above-mentioned positive electrode material, and its specific structure is as follows:
[0053] The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer contains the positive electrode material of this application. The positive electrode material of this application is generally used as a positive active material, and the positive active material can be any material capable of reversibly inserting and de-intercalating Li. + Na + Substances containing alkali metal ions are used to ensure that the positive electrode and secondary battery can be charged and discharged normally.
[0054] It should be noted that, in this application, "a positive electrode active material layer disposed on at least one surface of the positive electrode current collector" means that the positive electrode active material layer can be disposed on one surface or on two surfaces in the thickness direction of the positive electrode current collector. Moreover, in this application, "the surface of the positive electrode current collector" can be the entire area of the positive electrode current collector or a part of the positive electrode current collector. This application has no particular limitation, as long as the purpose of this application can be achieved.
[0055] Furthermore, in this application, the positive electrode active material may include not only lithium cobalt oxide (LiCoO2), but also at least one of lithium iron phosphate (LiFePO4), lithium manganese oxide, lithium nickel oxide, and ternary materials, including but not limited to LiNi. x Co y Mn z O2, LiNi x Co y Al z At least one of O2, etc., and the contents of Ni, Co, Mn, Al, etc., can be adjusted to ensure that x+y+z=1. For example, the ternary material can be LiNi. 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.88 Co 0.08 Mn 0.04 O2, LiNi 0.8 Co 0.15 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi0.88 Co 0.1 Mn 0.02 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.88 Co 0.1 Al 0.02 O2, etc.
[0056] In some embodiments, the positive electrode active material layer further includes a positive electrode conductive agent; this application does not limit the type of positive electrode conductive agent, and any known conductive material can be used. Specifically, the positive electrode conductive agent includes, but is not limited to, at least one of the following: acetylene black, Super-P carbon black, or amorphous carbon such as needle coke, or carbon nanotubes, or graphene.
[0057] In some embodiments, the positive electrode active material layer generally also contains a positive electrode binder. There are no particular restrictions on the type of positive electrode binder used in the manufacture of the positive electrode active material layer. In the case of the coating method, any material that can be dissolved or dispersed in the liquid medium used in the electrode manufacturing process is acceptable. Positive electrode binders include, but are not limited to, any one or at least two of the following: resin-based polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose; rubber-like polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, polybutadiene rubber, and ethylene-propylene rubber; thermoplastic elastomers such as styrene-butadiene-styrene block copolymers or their hydrides, ethylene-propylene-diene terpolymers (EPDM), styrene-ethylene-butadiene-ethylene copolymers, and styrene-isoprene-styrene block copolymers or their hydrides; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymers, and propylene-α-olefin copolymers; fluorinated polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and polytetrafluoroethylene-ethylene copolymers; and polymer compositions with ion conductivity of alkali metal ions (especially lithium ions).
[0058] In the positive electrode sheet, there are no particular restrictions on the type of positive current collector; it can be any known material suitable for use as a positive current collector. Materials for the positive current collector include, but are not limited to, metals such as aluminum, stainless steel, nickel plating, titanium, and tantalum. Furthermore, to reduce the electronic contact resistance between the positive current collector and the positive active material layer, conductive additives or conductive coatings can be applied to the surface of the positive current collector. Conductive additives include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. The conductive coating can be a mixture of inorganic oxides, conductive agents, and positive electrode binders.
[0059] In preparing the positive electrode sheet, the components of the aforementioned positive electrode active material layer can be dissolved or dispersed in a liquid solvent to form a positive electrode slurry. This slurry is then coated onto a positive electrode current collector and dried, thereby forming the positive electrode active material layer on the current collector, thus obtaining the positive electrode sheet. When preparing the positive electrode sheet using this method, there are no particular limitations on the solvent in the positive electrode slurry, as long as it can dissolve or disperse the aforementioned components. Specifically, the solvent in the positive electrode slurry includes, but is not limited to, N-methylpyrrolidone (NMP) and ethylene carbonate (EC). Alternatively, in preparing the positive electrode sheet, the various components of the positive electrode active material layer can be dry-mixed to form a sheet, which is then pressed onto the positive electrode current collector.
[0060] Thirdly, this application provides a secondary battery comprising the aforementioned positive electrode. Because the positive electrode in the secondary battery of this application has excellent interfacial properties, the secondary battery of this application also exhibits excellent cycle performance and performance at high rates.
[0061] In the secondary battery of this application, the positive electrode is as shown above, and the other structures are as follows:
[0062] Negative electrode sheet
[0063] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The composition of the negative electrode active material layer includes the negative electrode sheet active material. That is, in this application, the negative electrode active material layer can be disposed on one surface or on two surfaces in the thickness direction of the negative electrode current collector. Moreover, in this application, the "surface of the negative electrode current collector" can be the entire area of the negative electrode current collector or a part of the negative electrode current collector. This application has no particular limitation, as long as the purpose of this application can be achieved.
[0064] The negative electrode active material layer generally contains a negative electrode active material, and this application does not impose any particular limitation on the negative electrode active material. Specifically, the negative electrode active material may include at least one of carbon materials or silicon-based materials. More specifically, carbon materials include, but are not limited to, at least one of natural graphite, artificial graphite, mesophase microcarbon spheres, hard carbon, or soft carbon; silicon-based materials include, but are not limited to, at least one of silicon, silicon-oxygen composite materials, or silicon-carbon composite materials.
[0065] In some embodiments, the negative electrode active material layer typically also contains a negative electrode conductive agent. This application does not particularly limit the type of negative electrode conductive agent, as long as it achieves the purpose of this application. For example, negative electrode conductive agents include, but are not limited to, at least one of acetylene black, Ketjen black, carbon nanotubes, carbon fibers, carbon dots, or graphene.
[0066] In some embodiments, the negative electrode active material layer may also contain a negative electrode binder and a thickener. This application does not impose any particular limitation on the types of negative electrode binders and thickeners, as long as they can achieve the purpose of this application. For example, the negative electrode binder may include, but is not limited to, at least one of polyvinyl alcohol, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, styrene-butadiene rubber, or acrylated styrene-butadiene rubber; the thickener in the negative electrode slurry may include, but is not limited to, at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose.
[0067] In the negative electrode sheet, the material of the negative electrode current collector includes, but is not limited to, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a polymer substrate coated with a conductive metal, etc., and this application does not have any particular limitations. Among them, the conductive metal includes, but is not limited to, copper, nickel, or titanium, and the material of the polymer substrate includes, but is not limited to, at least one of polyethylene, polypropylene, ethylene propylene copolymer, polyethylene terephthalate, polyethylene terephthalate, or poly(p-phenylene terephthalamide).
[0068] Furthermore, in this application, there are no particular limitations on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the purpose of this application can be achieved. For example, the thickness of the negative electrode current collector is 4 μm to 12 μm, and the thickness of the single-sided negative electrode active material layer is 30 μm to 160 μm.
[0069] Furthermore, similar to the preparation of the positive electrode sheet, the preparation of the negative electrode sheet can be achieved either by preparing a negative electrode slurry, coating the slurry onto a negative electrode current collector, and drying it to form a negative electrode active material layer on the current collector, thus obtaining the negative electrode sheet; or by dry mixing the components of the negative electrode active material layer to form a sheet, which is then pressed onto the negative electrode current collector to form the negative electrode active material layer, thereby obtaining the negative electrode sheet. The solvent in the negative electrode slurry includes any one of aqueous solvents and organic solvents. Aqueous solvents include, but are not limited to, mixtures of alcohol and water or water itself. Organic solvents include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; and aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide. In some other embodiments, when using aqueous solvents, the negative electrode slurry composition may also include a thickener and styrene-butadiene rubber (SBR) emulsion to slurry the negative electrode slurry, thereby adjusting its viscosity. The types of thickeners in the positive electrode slurry include, but are not limited to, at least one of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and their salts.
[0070] electrolyte
[0071] Electrolytes play a role in transporting lithium ions and electrons, ensuring the formation of internal pathways in secondary batteries. Electrolytes typically contain lithium salts, solvents, and additives. It should be noted that this application does not impose specific restrictions on the amount of each component in the electrolyte, as long as the purpose of this application can be achieved.
[0072] Specifically, lithium salts can dissolve in solvents to form ionic conductors and be used as conductive media and lithium-ion transport media; lithium salts include, but are not limited to, at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium perchlorate, lithium bis(oxalate-borate), lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorooxalate-borate), and lithium bis(fluorosulfonyl)imide.
[0073] Solvents can dissolve lithium salts and additives. Solvents can be at least one of carbonates, carboxylic esters, ethers, and alcohols. Carbonates can be classified as cyclic carbonates and linear carbonates. Cyclic carbonates specifically include, but are not limited to, at least one of ethylene carbonate and propylene carbonate; linear carbonates specifically include, but are not limited to, at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate; carboxylic esters include, but are not limited to, at least one of methyl formate, methyl acetate, methyl butyrate, ethyl propionate, propyl propionate, and propyl acetate; ethers include, but are not limited to, at least one of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, and 4-methyl-1,3-dioxolane; and alcohols include, but are not limited to, at least one of ethanol, ethylene glycol, and glycerol.
[0074] Additives include, but are not limited to, nitriles, sulfones, sulfoxides, fluoronitriles, and fluoroesters.
[0075] Separating membrane
[0076] To prevent short circuits, a separator is typically placed between the positive and negative electrodes. In this case, the electrolyte of this application is typically used after penetrating into the separator.
[0077] There are no particular limitations on the material and shape of the separator, as long as it does not significantly impair the effectiveness of this application. The separator material can be resin, glass fiber, inorganic materials, etc., formed from materials stable to the electrolyte of this application. In some embodiments, the separator includes a porous sheet or non-woven fabric-like material with excellent liquid retention properties. Examples of resin or glass fiber separator materials include, but are not limited to, polyolefins, aromatic polyamides, polyimide (PI), polyamide (PA), polytetrafluoroethylene, polyethersulfone, spandex, or aramid. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The above-mentioned separator materials can be used alone or in any combination.
[0078] The separator can also be a material formed by laminating the above-mentioned materials, examples of which include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in that order.
[0079] Inorganic materials include, but are not limited to, oxides such as alumina and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.). The forms of inorganic materials include, but are not limited to, particulate or fibrous forms.
[0080] The separator can be in the form of a thin film, including but not limited to non-woven fabric, woven fabric, and microporous membranes. In the thin film form, the pore size of the separator is 0.01 μm to 1 μm, and the thickness is 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators can also be used: separators formed by using a resin-based adhesive to form a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or negative electrode, for example, a separator formed by using fluororesin as an adhesive to form a porous layer of alumina particles with a particle size of less than 1 μm on both sides of the positive electrode.
[0081] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the separator is within the above ranges, insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.
[0082] In this application, the diaphragm may include a substrate and a surface treatment layer. The substrate may be a nonwoven fabric or composite membrane with a porous structure, and the material of the substrate may include at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing polymers and inorganic materials. For example, the inorganic layer includes inorganic particles and a binder. This application does not have any particular limitation on the aforementioned inorganic particles, and may include at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. This application does not have any particular limitation on the aforementioned binders, and may include at least one of the aforementioned binders. The polymer layer contains a polymer, the polymer material of which includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, or poly(vinylidene fluoride-hexafluoropropylene).
[0083] The secondary battery of this application also includes a packaging bag for containing the positive electrode, separator, negative electrode, and electrolyte, as well as other components known in the art for secondary batteries. This application does not limit the aforementioned other components. This application does not have any particular limitation on the packaging bag; it can be any packaging bag known in the art, as long as it can achieve the purpose of this application.
[0084] The application of the secondary battery in this application is not particularly limited, and it can be used in any electronic device known in the prior art. In some embodiments, the secondary battery of this application can be used in, but is not limited to, laptops, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors, etc.
[0085] Example
[0086] The following uses lithium-ion batteries as an example to illustrate this application in more detail with examples and comparative examples. Those skilled in the art will understand that the preparation methods described in this application are merely examples, and any other suitable preparation methods are within the scope of this application.
[0087] Test methods and equipment:
[0088] Cyclic performance test
[0089] The cycle stability of lithium-ion batteries is evaluated by the capacity retention rate after 400 cycles at 45°C. A higher capacity retention rate after 400 cycles at 45°C indicates better cycle stability of the lithium-ion battery.
[0090] The lithium-ion battery was placed in a 45°C constant temperature chamber and left to stand for 30 minutes to allow it to reach a constant temperature. The battery was then charged at 45°C with a constant current of 0.2C to 4.5V, followed by constant voltage charging at 4.5V to 0.05C. After standing for 5 minutes, it was discharged at a constant current of 0.2C to 3.0V, and left to stand for 5 minutes. The initial discharge capacity C0 of the lithium-ion battery was then tested. Next, the battery was charged at a constant current of 1.8C to 4.15V, followed by constant voltage charging at 4.15V to 1C. It was then charged at a constant current of 1C to 4.25V, followed by constant voltage charging at 4.25V to 0.8C. It was then charged at a constant current of 0.8C to 4.5V, followed by constant voltage charging at 4.5V to 0.05C. After standing for 5 minutes, it was discharged at a constant current of 1C to 3.0V and left to stand for 5 minutes. This completes one charge-discharge cycle. The discharge capacity C1 of the lithium-ion battery after 400 cycles was measured by following the above charge / discharge cycle steps.
[0091] The capacity retention rate after 400 cycles at 45°C is calculated as C1 / C0 × 100%. The higher the capacity retention rate after 400 cycles at 45°C, the better the high-temperature cycle stability of the lithium-ion battery. The specific data on the high-temperature cycle stability of the lithium-ion batteries in each embodiment and comparative example are shown in the table.
[0092] Performance testing at high magnification
[0093] 2C discharge capacity retention test:
[0094] (1) Preparation of test equipment: battery test system (accuracy ±0.1%), constant temperature chamber (temperature control accuracy ±1℃), data logger, standard weighing instrument (accuracy 0.01g).
[0095] (2) Test steps
[0096] Secondary battery pretreatment: The secondary battery is placed in a 25℃ constant temperature chamber for 2 hours to ensure temperature uniformity. It is then charged at a constant current of 0.2C to 4.5V, then switched to constant voltage charging until the current is ≤0.05C, and left to stand for 30 minutes.
[0097] Initial capacity calibration (C0): Discharge at a constant current of 0.2C to 3.0V and record the discharge capacity C0.
[0098] Rate test: Charge at 0.2C constant current to 4.5V, switch to constant voltage charging until current ≤0.05C, let stand for 10 minutes, then discharge at 2C constant current to 3.0V, record the discharge capacity C1. Then let stand for 10 minutes.
[0099] Capacity retention rate calculation: 2C capacity retention rate = (C1 / C0) × 100%.
[0100] 6C discharge cell surface temperature rise test:
[0101] Test equipment preparation
[0102] High-rate charge / discharge equipment (supports ≥10C pulse)
[0103] Infrared thermal imager (accuracy ±1℃) or thermocouple (patent type, response time <1s)
[0104] Foam insulation testing fixture (reduces environmental interference)
[0105] Data Synchronous Acquisition System
[0106] Test steps
[0107] Initial state calibration
[0108] The battery cells were left to stand in a 25°C constant temperature chamber until the surface temperature stabilized (temperature difference ≤ 0.5°C).
[0109] Record the initial surface temperature T0℃ (take the average value of multiple measurements).
[0110] Charging pretreatment
[0111] Charge at a constant current of 1C to 4.5V, then switch to constant voltage until the current is ≤0.05C, and let stand for 10 minutes.
[0112] 6C discharge test
[0113] Discharge to 3.0V at a constant current of 6C.
[0114] Real-time monitoring:
[0115] Surface temperature is recorded every second (full area scan by infrared thermal imager).
[0116] Simultaneously record voltage and current curves.
[0117] Temperature rise calculation
[0118] Maximum temperature rise ΔT max =T max -T0
[0119] Average temperature rise ΔT max =(∫T(t)dt / t total )-T0
[0120] Determination of magnesium content in cobalt-containing particles
[0121] X-ray photoelectron spectroscopy (XPS) was used to characterize the magnesium content at different depths of cobalt-containing particles.
[0122] Test equipment and parameters
[0123] Instrument Model: Thermo Scientific K-Alpha+XPS System
[0124] X-ray source: Monochromatic Al Kα (1486.6 eV)
[0125] Vacuum degree of analysis chamber ≤5×10 -9 mbar
[0126] Energy resolution: 0.5 eV (Ag 3d5 / 2 peak)
[0127] Sputtering ion gun: Ar + Beam (1keV, 1μA / cm2)
[0128] Sample pretreatment
[0129] Surface cleaning:
[0130] Surface contaminants were removed by sputtering with an argon cluster ion beam (500 eV, 45° incident angle) for 60 seconds.
[0131] Confirm C1s pollution carbon peak intensity < 5% of total signal
[0132] Charge compensation:
[0133] Using dual-beam electrons / low-energy Ar + Neutralization Gun (e-Flood Mode)
[0134] Adjust the compensation voltage to keep the peak value of Au4f7 / 2 at 84.0±0.1eV.
[0135] Determination of the rate of change in magnesium content
[0136] In-depth analysis of test steps
[0137] Surface layer analysis (0nm):
[0138] Acquired Mg 1s spectra (scanning range 1303-1293 eV).
[0139] Points accumulation time: 300 seconds / point
[0140] Pass Energy: 20 eV
[0141] Step size: 0.1eV
[0142] Sputtering parameter control:
[0143] Sputtering rate calibration: using Ta2O5 standard wafers (calibrated at 1 nm / min).
[0144] Five depth points are selected as examples:
[0145] D1 = 20nm
[0146] D2 = 50nm
[0147] D3 = 80nm
[0148] D4 = 100nm
[0149] D5 = 120nm
[0150] Data processing methods
[0151] Peak area calculation:
[0152] Using Avantage software:
[0153] Shirley background removal
[0154] Mg 1s peak area integral (1298.5±1.5eV)
[0155] Co 2p 3 / 2 Peak area as internal standard (779.0 eV)
[0156] Concentration calculation:
[0157] W Mg (%) = (I) Mg / S Mg ) / Σ(I i / S i )×100%
[0158] I: Elemental peak area intensity
[0159] S: Relative sensitivity factor (Mg 1s = 0.18, Co 2p) 3 / 2 =2.25)
[0160] Calculation of gradient rate of change:
[0161] a1=(W a -W b ) / (D b -D a )×100%, in % / nm, where W a and W b These are the distances from the surface of the cobalt-containing particles, D. a Place and D b The magnesium concentration at that location.
[0162] Particle size testing of cobalt-containing particles
[0163] Test equipment and parameters
[0164] Instrument model: Malvern Mastersizer 3000 (compliant with ISO 13320 standard)
[0165] Measurement range: 0.01-3500μm (using a red / blue dual light source system)
[0166] Dispersion Module: Wet Dispersion Unit (Hydro MV)
[0167] Analysis software: Mastersizer 3000 (v3.62)
[0168] Sample pretreatment
[0169] Drying process:
[0170] The sample was placed in a vacuum drying oven (60℃×4h) to remove adsorbed water.
[0171] After cooling to room temperature, pass through a 200-mesh sieve (75μm).
[0172] Decentralized system construction:
[0173] A 0.05% sodium hexametaphosphate aqueous solution was selected as the dispersion medium.
[0174] Ultrasonic pretreatment: Disperse for 3 min using a Branson 5510 ultrasonic cleaner (40kHz, 300W).
[0175] Test steps
[0176] Background measurement:
[0177] Add dispersion medium until the shading rate is 5-10% as indicated.
[0178] Perform automatic background subtraction (measurement time 30s).
[0179] Sample loading:
[0180] Gradually add sample until the shading rate stabilizes in the range of 12-18%.
[0181] Real-time monitoring of particle size distribution curve stability (RSD < 2% for 3 consecutive measurements)
[0182] Dynamic distributed control:
[0183] Turn on the mixer (2400 rpm).
[0184] Ultrasonic power adjusted to 60% (built-in ultrasonic probe)
[0185] Maintain dispersion temperature at 25±1℃
[0186] Data collection:
[0187] Calculations were performed using Mie theory (refractive index set: particles 2.42, dispersion medium 1.33).
[0188] Each sample was measured five times consecutively, and the last three stable measurements were taken.
[0189] Example 1-1
[0190] <Preparation of Electrolyte>
[0191] In an argon-atmospheric glove box with a water content of less than 10 ppm, methyl ethyl carbonate and ethyl acetate were mixed at a mass ratio of 1:1 to prepare a base solvent, and then lithium hexafluorophosphate (LiPF6) was added. Based on the total mass of the electrolyte, the mass percentage of LiPF6 was 12.5%, with the remainder being the base solvent.
[0192] <Preparation of the positive electrode>
[0193] The positive electrode material, conductive carbon black, and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 95:2:3. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 70 wt%. The positive electrode slurry was uniformly coated on the upper and lower surfaces of a 9 μm thick aluminum foil for the positive electrode current collector. After drying and pressure treatment, the foil was cut into the specified size to obtain the positive electrode sheet.
[0194] The preparation method of the cathode material is shown below, and the relevant parameters of the obtained cathode material are shown in Table 1:
[0195] Step 1: Preparation of precursor
[0196] Lithium nitrate, cobalt nitrate, magnesium nitrate, and citric acid were dissolved in deionized water and magnetically stirred for 4 hours to form a homogeneous solution of 0.5 mol / L. This solution was then subjected to spray pyrolysis to obtain precursor powder. The inlet temperature during spray pyrolysis was 250℃, the outlet temperature was 600℃, and the atomization pressure was 0.3 MPa.
[0197] Step 2: Gradient sintering
[0198] The precursor was placed in a high-temperature furnace and subjected to first-stage sintering and second-stage sintering sequentially. It was then cooled in the furnace to 200°C before being removed. Specific conditions were as follows:
[0199] First-stage sintering: Nitrogen atmosphere, heating to 750℃ at 5℃ / min, holding for 2 hours, which promotes magnesium diffusion to the surface. Second-stage sintering: Switching to oxygen atmosphere, heating to 950℃ at 2℃ / min, holding for 10 hours, which promotes the formation of a surface oxide layer and stabilizes the crystal structure.
[0200] Step 3: Add other elements
[0201] The particles from step 2 were immersed in a 0.1 mol / L magnesium nitrate solution for 5 min to replenish the surface magnesium content; after centrifugation, they were vacuum dried at 120 °C for 2 h.
[0202] Step 4: Secondary sintering
[0203] The product obtained in step 3 was heat-treated at 400°C for 3 hours in an oxygen atmosphere to strengthen the surface magnesium oxide layer.
[0204] <Preparation of Negative Electrode Sheets>
[0205] Artificial graphite, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carbon nanotubes (CNTs): carboxymethyl cellulose (CMC) were mixed in a mass ratio of 95.8:2.4:0.5:0.5:0.8. Deionized water was then added as a solvent and the mixture was stirred until homogeneous, resulting in a negative electrode slurry with a solid content of 45 wt%. The negative electrode slurry was uniformly coated onto the upper and lower surfaces of a 6 μm thick copper foil used as a negative electrode current collector. After drying and pressure treatment, the foil was cut into specified sizes to obtain the negative electrode sheet.
[0206] <Isolation membrane>
[0207] A porous polyethylene film with a thickness of 15μm was used as the separator.
[0208] <Preparation of Lithium-ion Batteries>
[0209] The prepared positive electrode, separator, negative electrode, and separator are stacked in sequence, with the separator positioned between the positive and negative electrodes to act as a separator. The electrodes are then wound to obtain the electrode assembly. After welding the tabs, the electrode assembly is placed in an aluminum-plastic film packaging bag and dried in an 85°C vacuum oven for 12 hours to remove moisture. The prepared electrolyte is then injected, and the lithium-ion battery is obtained through vacuum sealing, settling, formation, shaping, and capacity testing.
[0210] Examples 1-2 to 1-21
[0211] Except for adjusting the relevant parameters of the cathode material according to Table 1, the rest is the same as in Example 1-1.
[0212] Comparative Example 1
[0213] Compared to Example 1-1, in step 2: gradient sintering, two-stage sintering is performed first, followed by one-stage sintering. The parameters of the obtained cathode material are shown in Table 1, and the rest are the same as in Example 1-1.
[0214] Comparative Example 2
[0215] Compared to Example 1-1, in the process of preparing the cathode material, the raw materials were mixed by solid-state method and then sintered. In the cathode material obtained, the magnesium element was uniformly distributed on the surface of the cobalt-containing particles without a gradient concentration, as shown in Table 1. The rest was the same as in Example 1-1.
[0216] Table 1
[0217] Examples 2-1 to 2-13
[0218] Except for adjusting the particle size of the cobalt-containing particles in the cathode material according to Table 2, the rest is the same as in Examples 1-2.
[0219] Table 2
[0220] Examples 3-1 to 3-20
[0221] Except for adjusting the types and contents of other elements in the cathode material according to Table 3, the rest is the same as in Examples 1-2.
[0222] Table 3
[0223] As shown in Table 1, the cathode material of this application not only has good electrochemical performance and cycle performance, but also good corrosion resistance and conductivity. When used in secondary batteries, it can enhance the cycle performance and high-rate performance of secondary batteries.
[0224] In particular, as shown in Table 2, by controlling the particle size of the cobalt-containing particles in the cathode material, the cycle performance and high-rate performance of the secondary battery can be further improved.
[0225] In particular, as shown in Table 3, when the cobalt particles in the cathode material contain a specific amount of other elements, the cycle performance and high-rate performance of the secondary battery can be further improved.
[0226] The above are merely embodiments of this application and are not intended to limit the scope of protection of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.
Claims
1. A positive electrode material, characterized in that, It includes cobalt-containing particles, and the cobalt-containing particles include magnesium. X-ray photoelectron spectroscopy (XPS) analysis revealed that the magnesium content on the surface of the cobalt-containing particles was W1%, and the magnesium content in the region 80 nm to 120 nm from the surface of the cobalt-containing particles was W2%, where W1 > W2.
2. The cathode material according to claim 1, characterized in that, D at a distance from the surface of the cobalt-containing particles x nm and D y In the region of nm, the magnesium content is W. x % and W y %, 0.2≤(W) x -W y ) / (D y -D x )≤0.3, and 0≤D x <D y ≤120.
3. The cathode material according to claim 1, characterized in that, The cobalt-containing particles also include lithium, and in the region of the cobalt-containing particles from 0 to 120 nm, the mass ratio of lithium, cobalt, and magnesium is 1:(0.98-1):(0.0005-0.003).
4. The cathode material according to claim 1, characterized in that, Based on the mass of the cobalt-containing particles, the magnesium content is 0.05% to 1%.
5. The cathode material according to claim 1 or 4, characterized in that, The cobalt-containing particles also include titanium, and the mass ratio of magnesium to titanium is (0.25:1) to (3:1).
6. The cathode material according to claim 1, characterized in that, The cobalt-containing particles have Dv90, Dv50, and Dv10 particle sizes of R1μm, R2μm, and R3μm, respectively, and the cobalt-containing particles satisfy at least one of the following conditions: (1)15≤R1≤25; (2)10≤R2≤20; (3)3≤R3≤10。 7. The cathode material according to claim 6, characterized in that, (R1-R3) / R2≤0.
4.
8. The cathode material according to claim 1, characterized in that, The cobalt-containing particles also include at least one of aluminum, yttrium, lanthanum, or zirconium.
9. The cathode material according to claim 8, characterized in that, Based on the mass of the cobalt-containing particles, the cathode material satisfies at least one of the following conditions: (1) The content of aluminum element is 0.5% to 2%; (2) The content of yttrium is 0.01% to 0.5%; (3) The content of the lanthanum element is 0.01% to 0.5%; (4) The zirconium content is 0.02% to 0.7%.
10. A positive electrode plate, characterized in that, It includes the cathode material as described in any one of claims 1 to 9.