Method for preparing activated biochar spheres

By adding wood biochar fragments and metal salts to sodium alginate-based gel spheres to form activated biochar spheres with a turbine layer carbon structure, the problems of low gold ion adsorption efficiency and structural instability in existing technologies are solved, achieving efficient adsorption and recovery of gold ions over a wide pH range.

WO2026232392A1PCT designated stage Publication Date: 2026-11-12TAIWAN CARBON SHUTTLE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/093419
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing technologies struggle to efficiently adsorb and recover gold ions from solutions over a wide pH range, and biochar spheres lack effective pore structures.

Method used

By adding wood biochar fragments, metal salt additives, and thermosetting polymers to sodium alginate-based gel spheres, activated biochar spheres with a turbine-layer carbon structure are formed. Carbonization and physical activation are used to form a porous structure, enhancing the channels and exchange capacity.

Benefits of technology

It achieves efficient adsorption of gold ions in the pH range of 2 to 12, with an adsorption rate of over 60%, and the biochar spheres have a stable structure, making them suitable for recycling and reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025093419_12112026_PF_FP_ABST
    Figure CN2025093419_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A method for preparing activated biochar spheres, comprising: providing a plurality of sodium alginate-based gel spheres, wherein the gel spheres each comprise a plurality of wood biochar fragments, a metal salt additive, and a thermosetting polymer; and carbonizing and physically activating the gel spheres to form a plurality of activated biochar spheres, wherein the activated biochar spheres each comprise a corresponding turbostratic carbon structure, the activated biochar spheres are capable of adsorbing gold ions in a solution, and the pH of the solution ranges from 2 to 12.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing activated biochar balls Technical Field

[0001] This invention relates to an activated biochar ball, and more particularly to a recyclable and reusable activated biochar ball. Background Technology

[0002] To separate gold ions from solution using biochar, and to ensure the biochar can be recycled and reused, current techniques, such as those described in CN 116832774, involve freeze-drying calcium alginate hydrogel spheres, followed by carbonization and acid washing, with a preferred carbonization temperature of 600–700℃. The resulting biomass-derived char particles exhibit a large number of oxygen-containing groups such as quinone and phenolic hydroxyl groups, and operate within a pH range of 1–8. Electron microscopy images at the micrometer scale, as shown in Figures 1 and 2, reveal a smooth and flat surface without obvious pore structures.

[0003] For example, CN 113426385 first utilizes phenolic compounds, aldehyde compounds, chitosan, and sodium alginate to form a homogeneous sol solution, which is then added dropwise to a saturated boric acid solution containing calcium chloride to form gel microspheres. Subsequent aging yields hydrogel microspheres with a double cross-linked structure of calcium alginate and phenolic resin. The hydrogel microspheres are dried at room temperature and pressure and then carbonized, preferably at a carbonization temperature of 850–950℃. The resulting activated biochar microspheres possess a large number of polar groups such as —OH, —NH2, and COOH (COO-). The residual polar groups and heteroatoms can improve the adsorption performance of the carbon aerogel microspheres. At the micrometer scale, electron microscopy images (refer to Figure 3) show that the etched pores have a generally smooth interface. Summary of the Invention

[0004] Activated biochar balls can adsorb gold ions in solution, are recyclable and reusable, and the solution pH should be at least 2–8, or even within the pH 2–12 range. That is, within this pH range, the adsorption rate of standard gold ions using these balls should be at least 60%.

[0005] In one embodiment, a method for manufacturing activated biochar balls includes:

[0006] Multiple sodium alginate-based gel spheres are provided, wherein each gel sphere comprises multiple lignocellulosic biochar fragments, metal salt additives, and thermosetting polymers;

[0007] The gel spheres are carbonized and physically activated to form multiple activated biochar spheres, each of which includes a corresponding turbine layer carbon structure. These activated biochar spheres can adsorb gold ions in the solution, and the pH range of the solution is pH 2 to pH 12.

[0008] In one embodiment, a method for manufacturing activated biochar balls includes:

[0009] A sodium alginate-based homogeneous solution and a calcium chloride homogeneous solution are formed, wherein the sodium alginate-based homogeneous solution includes sodium alginate, a thermosetting polymer, a metal salt additive, and multiple wood biochar fragments.

[0010] The sodium alginate-based homogeneous solution was added dropwise to the calcium chloride homogeneous solution to form multiple sodium alginate-based hydrogel spheres;

[0011] Solidify these hydrogel spheres;

[0012] After curing, these hydrogel spheres are heated and dried to form multiple dry gel spheres;

[0013] These dry gel spheres are carbonized and physically activated to form multiple activated biochar spheres. Attached Figure Description

[0014] Figures 1-2 show electron microscope images of biomass-derived char particles at the micrometer scale, as disclosed in CN 116832774.

[0015] Figure 2 is

[0016] Figure 3 shows an electron microscope image of the activated biochar balls disclosed in CN 113426385 at the micrometer scale.

[0017] Figure 4 is a schematic diagram of the layered edge structure.

[0018] Figure 5 is a schematic diagram of the surface hierarchical structure.

[0019] Figure 6 shows electron microscope images of Leucaena leucantha biochar at the micrometer scale.

[0020] Figure 7 shows the spherical appearance of activated biochar balls according to one embodiment of the present invention.

[0021] Figure 8 shows an electron microscope image of the internal structure of the activated biochar spheres according to one embodiment of the present invention.

[0022] Figure 9 shows the spherical appearance of the activated biochar balls according to another embodiment of the present invention.

[0023] Figure 10 shows an electron microscope image of the internal structure of activated biochar balls according to another embodiment of the present invention.

[0024] Figure 11 shows electron microscope images of the biochar fragments added in the embodiment of the present invention at the micrometer scale. Detailed Implementation

[0025] In one embodiment, lignocellulosic biochar fragments, a thermosetting polymer, and a metal salt additive are encapsulated in calcium alginate hydrogel spheres. The lignocellulosic biochar fragments are dispersed in the cross-linked chains of the hydrogel spheres, while the thermosetting polymer and metal salt additive are uniformly dispersed in water within the hydrogel spheres. The hydrogel spheres are then heated. Initially, the thermosetting polymer in the water dissolves and forms a high-molecular-weight cross-linked structure together with the metal salt additive particles, such as clay mineral particles. Upon continued heating, the hydrogel spheres dehydrate to form sodium alginate-based gel spheres. Subsequently, carbonization and physical activation are performed under nitrogen atmosphere to generate porous activated biochar spheres for easy recycling. In one embodiment, the hydrogel spheres are approximately 3 mm in size, and the activated biochar spheres are approximately 1 mm in size. The metal salt additive particles may be particles of clay minerals or their processed derivatives.

[0026] In one embodiment, wood biochar fragments can serve as the primary carbon source for activated biochar balls. Combined with the cross-linked chains of the sodium alginate-based cross-linked structure, they can strengthen the cross-linked structure of the calcium alginate gel balls. The cross-linked chains integrate the cyclic structure of biochar, such as aromatic rings, which can improve the thermal stability of the cross-linked structure. Thermosetting polymers can act as adhesives, connecting and fixing multiple adjacent cross-linked chains within the gel balls, strengthening the spherical structure of the gel balls, preventing disintegration during high-temperature processing, and can also serve as a secondary carbon source for the activated biochar balls. Metal salt additive particles can act as bridging agents, forming a cross-linked structure together with the thermosetting polymer, thus improving thermal stability. Calcium alginate serves as a carrier for the wood biochar fragments and can also be a secondary carbon source for the activated biochar balls.

[0027] In one embodiment, the gel spheres are carbonized to form biochar spheres, which further strengthens the sphere structure and makes them less susceptible to damage from corrosion or impact. During carbonization, an activation gas, such as carbon dioxide or water vapor, can be injected into a nitrogen environment to simultaneously activate the spheres.

[0028] In one embodiment, in addition to metal salt additives, during the carbonization process of biochar, the organic matter of the biochar releases metal salts, such as alkali metal carbonates, as part of the thermal decomposition reaction. At a carbonization temperature of 600–650°C, the organic matter of the biochar can release all the metal salts, and the biochar can form an initial turbine layer carbon structure. At the physical activation temperature (700–1000°C), the metal salts dissociate into metal ions, which can flow with the molten metal salts. The biochar fragments themselves already contain metal salts. Thermosetting polymers and calcium alginate also produce metal salts during carbonization.

[0029] In one embodiment, after physical activation, the activated biochar spheres develop a layered, turbine-like carbon structure with a wider front and narrower back interlayer space. Metal ions, embedded in these interlayer spaces along with the flow of molten metal salts, can be used for ion exchange. Under high-pressure nitrogen, metal ions can penetrate deeper into the interlayer space, thereby creating a larger interlayer space and more exchangeable metal ions. The physical activation step not only improves the original properties of biochar, such as specific surface area and pore structure, but also provides additional exchangeable metal ions. However, physical activation can further worsen the thermal weight loss of the biochar, weakening the spherical structure of the gel spheres. The formation of a cross-linked structure of thermosetting polymer-metal salt additive particles within the gel spheres helps maintain their spherical structure during physical activation, preventing them from disintegrating into fragments. In one embodiment, the activated biochar spheres contain more than 70% carbon.

[0030] In one embodiment, calcium alginate hydrogel spheres solidify to form a stable cross-linked structure incorporating biochar fragments. The solidified hydrogel spheres contain thermosetting polymer particles, clay mineral particles, and calcium carbonate particles distributed within the water content of the hydrogel spheres. The solidified hydrogel spheres can be dehydrated and dried using atmospheric pressure heating. Initially, during heating, the thermosetting polymer melts and combines with the clay mineral particles to form a second cross-linked structure (polymer-clay mineral cross-linked structure), which permeates the structural voids of the sodium alginate-based gel spheres. After dehydration, the second cross-linked structure provides internal cohesion to the calcium alginate-biochar fragment spheres, strengthening the sphere structure. In one embodiment, during the carbonization process, bio-calcium carbonate helps to form cyclic structures, such as aromatic ring structures, improving the thermal stability of the biochar.

[0031] In one embodiment, the thermosetting polymer may be a phenolic resin, starch, or a processed derivative of starch, such as wheat starch, corn starch, or paste. The metal salt additive particles may be clay minerals or their derivatives, such as aluminosilicate minerals, mica powder, modified kaolin, or calcium carbonate / biocarbonate. The addition of biocarbonate can promote the formation of cyclic structures, such as aromatic rings, in the biochar during carbonization, thereby improving thermal stability. Physical activation may be carbon dioxide activation or steam activation. Steam activation helps to generate additional oxygen-containing functional groups.

[0032] In one embodiment, the millimeter-sized porous activated biochar spheres, at the micrometer scale, have a carbon framework formed by numerous fragmented carbon particles ranging from 10 to 50 micrometers (µm) in size. These fragmented carbon particles possess a layered edge structure (refer to Figure 4) and a surface hierarchical structure (refer to Figure 5). Referring to Figure 4, the layered edge structure includes an upper surface 1, a lower surface 2, and an edge surface 3 connecting the upper surface 1 and the lower surface 2, wherein the upper surface 1 and the lower surface 2 face approximately opposite directions. Referring to Figure 5, the surface hierarchical structure includes an upper surface 4, a lower surface 5, and an edge surface 6 connecting the upper surface 4 and the lower surface 5, wherein the upper surface 4 and the lower surface 5 face approximately the same direction. A single fragmented carbon particle may have multiple layered edges. The 10-50 micrometer (µm) carbon particles aggregate and stack, forming a multi-sized, irregularly stacked structure with a spherical appearance. The fragmented carbon particles connect to form a porous spherical carbon framework, creating voids between the fragmented carbon particles, which connect to form a porous structure.

[0033] In one embodiment, at the micrometer scale, the interface structure between the pore structure and the carbon skeleton of the porous sphere includes multiple irregularly shaped layered edges, forming a non-smooth interface through multi-layered, non-uniform stacking, unlike etched pore structures. The fragmented carbon particles are inconsistent in height, causing adjacent particles to not be on the same plane, resulting in irregular stacking with varying density, forming multi-layered channels that are disordered and exhibit a non-uniform interface structure. Although the carbon skeleton of the biochar sphere originates from a cross-linked structure, at the micrometer scale, the linking pattern of the fragmented carbon particles on the surface of the porous sphere does not exhibit the chain network of a cross-linked structure, nor does it exhibit the channel structure of acacia biochar (refer to Figure 6).

[0034] In one embodiment, at the micrometer scale, small particles approximately 1 micrometer in size contain inorganic salts. These inorganic salt particles aggregate in small areas on the surface of fragmented carbon particles. Overall, the inorganic salt particles are discretely attached to the surface of the carbon particles.

[0035] In the following specific embodiments, unless otherwise specified, the added biochar was obtained from *Leucaena leucocephala*, carbonized at 650°C, and pulverized before being sieved through a 100-mesh screen; the gold ion standard reagent was prepared by adding trivalent gold ions to deionized water at a concentration of 10 ppm; the adsorption rate of gold ions was measured by adding 100 mg of activated biochar balls to 50 mL of the standard reagent, adsorbing for 5 hours, and then measuring the residual amount of trivalent gold ions in the standard reagent; the hydrogel spheres had a particle size of approximately 3 mm; and the mixture was dried under normal pressure. Metal salt additives, such as clay minerals or their processed derivatives, or calcium carbonate / bio-calcium carbonate, were added to a homogeneous aqueous solution based on sodium alginate and stirred to produce uniformly dispersed metal salt additive particles.

[0036] Example 1

[0037] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 10 g of phenolic resin, 36 g of biochar, and 4 g of mica powder. The mixture was stirred until evenly dispersed in the water to form a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, the solid and liquid phases were separated, and the mixture was heated to 80°C and dried for 2 hours. During this time, the starch and phenolic resin also dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 98.4%. Referring to Figure 7, the spherical appearance of the activated biochar balls; referring to Figure 8, an electron microscope image of the internal structure of the spheres at the micrometer scale.

[0038] Example 2

[0039] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of phenolic resin, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until evenly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the phenolic resin dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 76.8%.

[0040] Example 3

[0041] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until evenly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct dropwise addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the starch dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 84.7%.

[0042] Example 4

[0043] 1 liter of tap water was mixed with 10 g of sodium alginate, 10 g of starch, 10 g of phenolic resin, 36 g of biochar, and 4 g of clay minerals. The mixture was stirred until uniformly dispersed in the water to form a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80 g of calcium chloride to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct dropwise addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation was achieved, and the mixture was heated to 80°C and dried for 2 hours. During this process, the starch and phenolic resin dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with steam at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. For a standard reagent at pH 2, the adsorption rate of gold ions was 100%, and for a standard reagent at pH 12, the adsorption rate of gold ions was 71.6%. Referring to Figure 9, the spherical appearance of the activated biochar spheres; referring to Figure 10, an electron microscope image of the internal structure of the spheres at the micrometer scale.

[0044] Example 5

[0045] 1 liter of tap water was mixed with 10g sodium alginate, 10g starch, 10g phenolic resin, 36g biochar, 4g clay minerals, and 4g calcium carbonate. The mixture was stirred until uniformly dispersed in the water, forming a suspension, which served as the first homogenized aqueous solution. 2 liters of tap water were mixed with 80g calcium chloride, dissolving to form a calcium chloride aqueous solution, which served as the second homogenized aqueous solution. The first homogenized aqueous solution was added dropwise to the second homogenized aqueous solution using a direct addition method to generate hydrogel spheres. The hydrogel spheres were left to stand in the calcium chloride aqueous solution for 8 hours to solidify. After solidification, solid-liquid separation occurred, and the mixture was heated to 80°C and dried for 2 hours. During this time, the starch and phenolic resin also dissolved, forming a cross-linked structure. After drying, the resulting dry hydrogel spheres were simultaneously carbonized and activated with carbon dioxide at 900°C under nitrogen atmosphere for 30 minutes. The final product was porous activated biochar spheres. The adsorption rate of gold ions was 100% for a standard reagent at pH 2 and 100% for a standard reagent at pH 12. The electron microscope (SEM) images of the spheres are shown in Figure 1, showing the sphere's appearance, and Figures 2 and 3, showing the sphere's surface structure at the micrometer scale. Referring to Figure 11, the electron microscope image of the wood biochar fragments added in the examples at the micrometer scale shows a smooth interface with a porous surface.

[0046] Component label

[0047] 1. Top surface

[0048] 2 Lower surface

[0049] 3 Edge surfaces

[0050] 4. Top surface

[0051] 5. Lower surface

[0052] 6. Edge surface

Claims

1. A method for manufacturing activated biochar balls, comprising: Multiple sodium alginate-based gel spheres are provided, wherein each gel sphere comprises multiple lignocellulosic biochar fragments, metal salt additives, and thermosetting polymers; The gel spheres are carbonized and physically activated to form multiple activated biochar spheres, each of which includes a corresponding turbine layer carbon structure. These activated biochar spheres can adsorb gold ions in the solution, and the pH range of the solution is pH 2 to pH 12.

2. The manufacturing method as described in claim 1, wherein, The corresponding turbine layer carbon structure includes multiple embedded exchangeable metal ions.

3. The manufacturing method as described in claim 1, further comprising: Multiple sodium alginate-based hydrogel spheres were heated and dried to form these gel spheres.

4. The manufacturing method as described in claim 1, wherein, Each of these gel spheres includes a sodium alginate-based crosslinked structure associated with the bio-carbon fragments.

5. The manufacturing method as described in claim 1, wherein, These gel spheres each comprise a polymeric cross-linked structure associated with the metal salt additive and the thermosetting polymer.

6. A method for manufacturing activated biochar balls, comprising: A sodium alginate-based homogeneous solution and a calcium chloride homogeneous solution are formed, wherein the sodium alginate-based homogeneous solution includes sodium alginate, a thermosetting polymer, a metal salt additive, and multiple wood biochar fragments. The sodium alginate-based homogeneous solution was added dropwise to the calcium chloride homogeneous solution to form multiple sodium alginate-based hydrogel spheres; Solidify these hydrogel spheres; After curing, these hydrogel spheres are heated and dried to form multiple dry gel spheres; These dry gel spheres are carbonized and physically activated to form multiple activated biochar spheres.

7. The manufacturing method as described in claim 10, wherein, The thermosetting polymers include phenolic resins.

8. The manufacturing method as described in claim 10, wherein, This thermosetting polymer includes starch.

9. The manufacturing method as described in claim 10, wherein, These activated biochar balls each include a corresponding turbine layer carbon structure and multiple exchangeable metal ions embedded in the turbine layer carbon structure.

10. The manufacturing method as claimed in claim 10, wherein, Heating and drying the hydrogel spheres includes heating and melting the thermosetting polymer, and generating a corresponding polymeric cross-linked structure in each of the hydrogel spheres, wherein the corresponding polymeric cross-linked structure is associated with the metal salt additive.