Silicone composite

The silicone composite with specific thermally-conductive fillers and treating agents addresses the reduction in extrusion rates and mechanical properties of thermally-conductive compositions, ensuring high performance in electronic applications.

WO2026232456A1PCT designated stage Publication Date: 2026-11-12DOW SILICONES CORP +10
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/093645
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Thermally-conductive compositions used in electronics face challenges with reduced extrusion rates and mechanical properties like elongation when increasing the content of thermally-conductive fillers.

Method used

A silicone composite comprising organopolysiloxane, thermally-conductive fillers with specific particle sizes, and a filler treating agent, which minimizes the formation of alkoxy groups, thereby maintaining high extrusion rates and excellent elongation.

Benefits of technology

The silicone composite achieves high extrusion rates and improved mechanical properties by suppressing the generation of alkoxy groups, enhancing the performance of thermally-conductive compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2025093645-FTAPPB-I100001
    Figure PCTCN2025093645-FTAPPB-I100001
  • Figure PCTCN2025093645-FTAPPB-I100002
    Figure PCTCN2025093645-FTAPPB-I100002
  • Figure PCTCN2025093645-FTAPPB-I100003
    Figure PCTCN2025093645-FTAPPB-I100003
Patent Text Reader

Abstract

Provided is a silicone composite comprising (A) an organopolysiloxane, (B) a thermally-conductive filler, and (C) a filler treating agent. The (B) TC filler includes (B1) a TC filler having a Dv50 of less than 5 μm, and (B2) a TC filler having a Dv50 of 5 μm or more. The (C) filler treating agent includes (C1) a filler treating agent having as specific structure. The silicone composite has a 1H-NMR spectrum, using deuterated benzene as the solvent, that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm.
Need to check novelty before this filing date? Find Prior Art

Description

SILICONE COMPOSITETECHNICAL FIELD

[0001] The present disclosure relates to a silicone composite, a thermally-conductive composition, a cured product, and a method of producing a silicone composite.BACKGROUND

[0002] This section provides background information related to the present disclosure which is not necessarily prior art.

[0003] An industry drive to smaller and more powerful electronic devices has increased demands on thermally-conductive compositions useful for dissipating heat generated in such devices. For instance, the telecommunications industry is going through a generational shift to 5G networks, which demand highly integrated electrical devices with smaller sizes and that brings a requirement for double the power requirements. The heat generated by the high power in the smaller devices would damage the device if not efficiently dissipated. Thermally conductive interface materials are often used in electronics to thermally couple heat generating components and heat dissipating components.SUMMARY

[0004] Thermally-conductive compositions generally contain a large amount of thermally-conductive fillers to exhibit high thermal conductivity. However, increasing the content of thermally-conductive fillers in the thermally-conductive composition may reduce the extrusion rate when applying the composition to the target part, as well as other mechanical properties such as elongation.

[0005] The present disclosure provides a silicone composite, a thermally-conductive composition, a cured product, and a method of producing a silicone composite. In some embodiments, the present disclosure provides a silicone composite that can be used to prepare a thermally-conductive composition capable of exhibiting high extrusion rate and excellent elongation.

[0006] In a first aspect, a silicone composite is disclosed. The silicone composite according to embodiments disclosed herein comprises: (A) an organopolysiloxane, (B) a thermally-conductive filler, and (C) a filler treating agent, wherein the (B) thermally-conductive filler includes: (B1) a thermally-conductive filler having a Dv50 of less than 5 μm, and (B2) a thermally-conductive filler having a Dv50 of 5 μm or more, wherein the (C) filler treating agent includes (C1) a filler treating agent represented by the following formula (I) : R13SiO- (R22SiO) n-SiR13  (I) where R1 is each independently an alkyl group or an alkoxy group, provided that at least  one R1 is an alkoxy group, R2 is each independently an alkyl group or an aryl group, and n is the average number of (R22SiO) units and has a value of 10 or more and 400 or less, and wherein the silicone composite has a 1H-NMR spectrum, using deuterated benzene as the solvent, that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm.

[0007] In a second aspect, a thermally-conductive composition is disclosed. The thermally-conductive composition according to embodiments disclosed herein comprises two components, wherein at least one of the two components is the silicone composite according to the silicone composite of the first aspect of the present disclosure.

[0008] In a third aspect, a cured product is disclosed. The cured product according to embodiments disclosed herein is obtainable from the thermally-conductive composition of the second aspect of the present disclosure.

[0009] These and other embodiments are described in more detail in the Detailed Description.BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 shows an example of the 1H-NMR spectrum of a silicone composite that has a peak within a range of 3.30 ppm and 3.80 ppm.

[0011] Figure 2 shows an example of the 1H-NMR spectrum of a silicone composite that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm.DETAILED DESCRIPTION

[0012] Test methods refer to the most recent test method as of the priority date of this document when a date is not indicated with the test method number. References to test methods contain both a reference to the testing society and the test method number. The following test method abbreviations and identifiers apply herein: ASTM refers to ASTM International methods; EN refers to European Norm; DIN refers to Deutsches Institut für Normung; ISO refers to International Organization for Standards; and UL refers to Underwriters Laboratory.

[0013] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percents are based on weight, all temperatures are in ℃, and all test methods are current as of the filing date of this disclosure.

[0014] Products identified by their tradename refer to the compositions available under those tradenames on the priority date of this document.

[0015] “And / or” means “and, or as an alternative” . All numerical ranges include endpoints unless otherwise indicated.

[0016] Determine particle size of “Dv50” as the volume-weighted median value of particle diameter distribution (Dv50) using a MastersizerTM (trademark of Malvern Instruments Limited) 3000 laser diffraction particle size analyzer from Malvern Instruments.

[0017] “A 1H-NMR spectrum, using deuterated benzene as the solvent, that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm” means that when a silicone composite is extracted with n-hexane and the 1H-NMR of the obtained extract is measured (standard substance: tetramethyl silane) , no peaks are observed in the region of 3.30 ppm to 3.80 ppm, or if peaks are observed in the region of 3.30 ppm to 3.80 ppm, the integral value of the peaks in the region of 3.30 ppm to 3.80 ppm is 0.003%or less of the integral value (100%) of the peaks in the region of -0.3 ppm to 0.5 ppm. The extraction of a silicone composite with n-hexane is done as follows: A sample of a silicone composite (about 0.67 g) is placed in a 12 mL vial. Add 5 g of n-hexane to extract, followed by another 5 g of n-hexane to wash once. Transfer the liquid to another weighed digestion vial (12 mL) and remove the n-hexane to dryness.

[0018] Determine chemical structure for organopolysiloxanes by standard 1H, 13C and 29Si nuclear magnetic resonance (NMR) analysis, such as, described in US Patent 9,593,209, Reference Example 2 at col. 32.

[0019] The term “surface-treat” refers to making a filler treating agent adhere to at least part of the outer surface of a filler.

[0020] The terms “comprising, ” “including, ” “having, ” and their derivatives, are not intended to exclude the presence of any additional component, step or procedure, whether or not the same is specifically disclosed. In order to avoid any doubt, all compositions claimed through use of the term “comprising” may include any additional additive, adjuvant, or compound, whether polymeric or otherwise, unless stated to the contrary. In contrast, the term, “consisting essentially of” excludes from the scope of any succeeding recitation any other component, step or procedure, excepting those that are not essential to operability. The term “consisting of” excludes any component, step or procedure not specifically delineated or listed.

[0021] The use of “for example, ” “e.g., ” and “such as, ” to list illustrative examples does not limit to only the listed examples. Thus, “for example” or “such as” means “for example, but not limited to” or “such as, but not limited to” and encompasses other similar or equivalent examples.

[0022] <Silicone composite>

[0023] The present disclosure provides a silicone composite. The silicone composite comprises (A) an organopolysiloxane, (B) a thermally-conductive filler (hereinafter, also abbreviated as “ (B) a TC filler” ) , and (C) a filler treating agent (hereinafter, also abbreviated as “ (C) a treating agent” ) . In some embodiments, the silicone composite may comprise a (D) a hydrosilylation reaction catalyst (hereinafter, also abbreviated as “ (D) a catalyst” ) . The silicone composite optionally comprises components other than components (A) to (D) (hereinafter, abbreviated as “Other components” ) .

[0024] The silicone composite of the present disclosure has a 1H-NMR spectrum, using deuterated benzene as the solvent, that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm. As a result, using the silicone composite, a thermally-conductive composition capable of exhibiting high extrusion rate and excellent elongation can be prepared. Although the reason for this is not clear, it is presumed as follows: Figure 1 shows the 1H-NMR spectrum of the extract obtained by extracting the silicone composite (part A) with n-hexane, prepared in Comparative Example 1 described in the specification. Comparative Example 1 involves mixing (A) organopolysiloxanes, surface non-treated (B) TC fillers, and (C) treating agents including the (C1) treating agent under vacuum heating to prepare the silicone composite (hereinafter sometimes referred to as ″in-situ treatment″) . In the 1H-NMR spectrum of Figure 1, two peaks are observed in the range of 3.30 ppm to 3.80 ppm. Analysis of the H-Si HMBC (Heteronuclear Multiple Bond Coherence) spectrum of the same sample revealed that the peak around 3.60 ppm is considered to be derived from the methoxy group of the dimer of the (C1) filler treating agent, and the peak around 3.40 ppm is considered to be derived from the methoxy group produced by the condensation between the formed methanol and the silanol group originated from the (A1) vinyl polymer. According to the inventors, these methoxy groups (alkoxy groups) are presumed to have been generated by mixing the (A) organopolysiloxanes, the surface non-treated (B) TC fillers, and the (C) treating agents under heating conditions (e.g., 60 ℃ or above) . On the other hand, Figure 2 shows the 1H-NMR spectrum of the extract obtained from extracting the silicone composite (part A) with n-hexane, prepared in Inventive Example 1 described in the specification. Unlike Figure 1, no peaks are observed in the range of 3.30 ppm to 3.80 ppm in the 1H-NMR spectrum of Figure 2. In other words, the methoxy groups (alkoxy groups) generated in Comparative Example 1 were not generated in Inventive Example 1. As stated above, by using a silicone composite that substantially lacks peaks in the range of 3.30 ppm to 3.80 ppm in the 1H-NMR spectrum, a thermally-conductive composition exhibiting high extrusion rate and excellent elongation can be prepared. Although the reason for such an effect is not clear, it is considered that, for example, in Comparative Example 1, the two types of methoxy groups (alkoxy groups) mentioned above were a factor in reducing the extrusion rate and mechanical properties such as elongation.

[0025] (A) Organopolysiloxane

[0026] The (A) organopolysiloxane is not particularly limited and any organopolysiloxane can be used. Note that the (A) organopolysiloxane may comprise two or more different organopolysiloxanes, which may be independently selected. The (A) organopolysiloxane may be linear, branched, partly branched, cyclic, resinous (i.e., have a three-dimensional network) , or may comprise a combination of different structures. For example, the (A) organopolysiloxane may comprise any combination of M, D, T and / or Q siloxane units. These siloxane units can be combined in various manners to form cyclic, linear, branched and / or resinous structures.

[0027] Non-limiting examples of the (A) organopolysiloxane include (A1) an organopolysiloxane having an alkenyl group and (A2) an organohydrogenpolysiloxane, and combinations thereof. In other words, the silicone composite may include the (A1) organopolysiloxane and may not include (A2) , may include the (A2) organohydrogenpolysiloxane and may not include the (A1) organopolysiloxane, or may include both the (A1) organopolysiloxane and the (A2) organohydrogenpolysiloxane.

[0028] In some embodiments, the (A1) organopolysiloxane may have at least two alkenyl groups per molecule. The alkenyl groups may react with other functional groups (for example, Si-H groups in the (A2) organohydrogenpolysiloxane) through a hydrosilylation reaction initiated by the (D) catalyst. Non-limiting examples of the alkenyl group include a vinyl group, allyl group, butenyl group, pentenyl group, heptenyl group, hexenyl group, and combinations thereof.

[0029] In some embodiments, the number of the alkenyl groups per molecule in the (A1) organopolysiloxane may be 2 or more. At the same time the number of the alkenyl groups per molecule in the (A1) organopolysiloxane may be 100 or less, optionally 50 or less, optionally 10 or less, optionally 5 or less, or optionally 3 or less. In some embodiments, the number of the alkenyl groups per molecule in the (A1) organopolysiloxane may be from 2 to 100, optionally from 2 to 50, optionally from 2 to 10, optionally from 2 to 5, optionally from 2 to 3, or optionally 2.

[0030] In the (A1) organopolysiloxane, the alkenyl group may be bonded directly to the silicon atom, or the alkenyl group may be bonded to the silicon atom via another group.

[0031] In some embodiments, the (A1) organopolysiloxane may have a silicon-bonded group which does not include an alkenyl group. Non-limiting examples of the silicon-bonded group include a methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, tert-butyl group, pentyl group, neopentyl group, hexyl groups, cyclohexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, phenyl group, tolyl group, xylyl group, naphthyl group, and these groups in which a part or all of the hydrogen atoms is substituted with a halogen atom such as a fluorine atom, a chloride atom, and a bromine atom, or is substituted with nitrogen containing groups such as a cyano or a tertiary amine group. Note that the (A) organopolysiloxane may have two or more different silicon-bonded groups which do not include alkenyl group, which may be independently selected.

[0032] In some embodiments, the (A1) organopolysiloxane may be a linear organopolysiloxane having alkenyl groups at the two terminals. For example, the linear organopolysiloxane may be represented by the following formula (III) : RaRb2SiO- (Rb2SiO) m-SiRaRb2          (III)

[0033] Each Ra group is directly bonded to the silicon atom and may be same or different. Each Ra group is independently selected from alkenyl groups, optionally selected from the group consisting of a vinyl group, allyl group, butenyl group, pentenyl group, heptenyl group, hexenyl group, or optionally Each Ra may be a vinyl group. Ra group may be unsubstituted or substituted with one or more groups that do not interfere with curing.

[0034] Each Rb group is directly bonded to the silicon atom and may be same or different. Each Rb group is independently selected from the group consisting of alkyl groups and aryl groups, optionally selected from the group consisting of alkyl groups having from 1 to 10 carbon atoms and aryl groups having from 6 to 12 carbon atoms, or optionally selected from the group consisting of alkyl groups having from 1 to 10 carbon atoms. Rb group may be unsubstituted or substituted with one or more groups that do not interfere with curing.

[0035] Subscript “m” refers to the average number of (Rb2SiO) units. In some embodiments, subscript “m” may be 10 or more, optionally 20 or more, optionally 30 or more, or optionally 40 or more. At the same time subscript “m” may be 1,000 or less, optionally 500 or less, or optionally 100 or less. In some embodiments, subscript “m” may be from 10 to 1,000, optionally from 20 to 500, optionally from 30 to 500, or optionally from 40 to 100.

[0036] In some embodiments, the (A2) organohydrogenpolysiloxane may have at least two silicon atom-bonded hydrogen atoms per molecule and free of alkenyl groups. The silicon atom-bonded hydrogen atoms can react with the alkenyl groups, for example, of the (A1) organopolysiloxane through a hydrosilylation reaction initiated by the (D) catalyst and a crosslinked structure including components (A1) and (A2) can be formed. In other words, the (A2) organohydrogenpolysiloxane can act as a cross-linker. Note that the (A2) organohydrogenpolysiloxane may comprise two or more different organohydrogenpolysiloxanes, which may be independently selected.

[0037] In some embodiments, the (A2) organohydrogenpolysiloxane may be a linear organohydrogenpolysiloxane. For example, the linear organopolysiloxane may be represented by the following formula (IV) : Rd3 SiO- (Rd2SiO) k-SiRd3 (IV)

[0038] Each Rd group may be same or different and is independently selected from the group consisting of alkyl groups having from 1 to 20 carbon atoms and a hydrogen atom, with the proviso that at least two Rd groups are hydrogen atoms. The alkyl groups having from 1 to 20 carbon atoms for Rd groups may be an alkyl group having from 1 to 10 carbon atoms, optionally a methyl group or a phenyl group, or optionally a methyl group.

[0039] Subscript “k” refers to the average number of (Rd2SiO) units and is an integer. In some embodiments, subscript “k” may be 5 or more, optionally 6 or more, or optionally 8 or more. At the same time subscript “k” may be 300 or less, optionally 200 or less, or optionally 150 or less. In some embodiments, subscript “k” may be from 5 to 300, optionally from 6 to 200, or optionally from 8 to 150.

[0040] In some embodiments, the number of the silicon atom-bonded hydrogen atoms in the (A2) organohydrogenpolysiloxane may be from 2 to 100, optionally from 2 to 50, optionally from 2 to 25, optionally from 2 to 10, or optionally from 2 to 5.

[0041] In some embodiments, the content of the (A) organopolysiloxane in the silicone composite may be 1.00 wt. %or more, optionally 5.00 wt. %or more, optionally 9.00 wt. %or more, optionally 11.00 wt. %or more, or optionally 13.00 wt. %or more, based on the total weight of the silicone composite. At the same time the content of the (A) organopolysiloxane in the silicone composite may be 95.00 wt. %or less, optionally 60.00 wt. %or less, optionally 40.00 wt. %or less, or optionally 30.00 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the content of the (A) organopolysiloxane in the silicone composite may be from 1.00 to 95.00 wt. %, optionally from 5.00 to 60.00 wt. %, optionally from 9.00 to 40.00 wt. %, optionally from 11.00 to 40.00 wt. %, or optionally from 13.00 to 30.00 wt. %, based on the total weight of the silicone composite.

[0042] (B) Thermally-conductive filler

[0043] The (B) thermally-conductive filler includes (B1) a thermally-conductive filler (hereinafter, also abbreviated as “ (B1) a TC filler” ) having a Dv50 of less than 5 μm and (B2) a thermally-conductive filler (hereinafter, also abbreviated as “ (B2) a TC filler” ) having a Dv50 of 5 μm or more. The silicone composite may contain only one type of the (B1) TC filler or multiple types. Similarly, the silicone composite may contain only one type of the (B2) TC filler or multiple types.

[0044] In some embodiments, the Dv50 of the (B1) TC filler may be 0.1 μm or more, or optionally 0.5 μm or more. At the same time the Dv50 of the (B1) TC filler may be 4 μm or less, or optionally 3 μm or less. In some embodiments, the Dv50 of the (B1) TC filler may be from 0.1 to 5 μm, optionally from 0.1 to 4 μm, or optionally from 0.5 to 3 μm. In some embodiments, the Dv50 of the (B2) TC filler may be 7 μm or more, or optionally 8 μm or more. At the same time of Dv50 of the (B2) TC filler may be 100 μm or less, or optionally 50 μm or less. In some embodiments, the Dv50 of the (B2) TC filler may be from 5 to 100 μm, optionally from 7 to 100 μm, or optionally from 8 to 50 μm.

[0045] The materials of the (B1) TC filler and the (B2) TC filler are independent of each other and may be the same or different. Non limiting example of the materials of the (B1) TC filler and the (B2) TC filler include aluminum trihydrate, alumina, aluminum nitride, zinc oxide, magnesium hydroxide, glass beads, and combinations thereof. In some embodiments, the (B1) TC filler may be at least one of alumina and aluminum nitride. In some embodiments, the (B2) TC filler may be alumina.

[0046] The shapes of the (B1) TC filler and the (B2) TC filler are independent of each other and may be same or different. Non limiting example of the shapes of the (B1) TC filler and the (B2) TC filler include spherical, irregular, crushed, platelet, and combinations thereof.

[0047] The content of the (B1) TC filler in the silicone composite may be 5.00 wt. %or more, optionally 10.00 wt. %or more, optionally 15.00 wt. %or more, or optionally 20.00 wt. %or more, based on the total weight of the silicone composite. At the same time the content of the (B1) TC filler in the silicone composite may be 40.00 wt. %or less, optionally 35.00 wt. %or less, optionally 30.00 wt. %or less, or optionally 25.00 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the content of the (B1) TC filler in the silicone composite may be from 5.00 to 40.00 wt. %, optionally from 10.00 to 35.00 wt. %, optionally from 15.00 to 30.00 wt. %, or optionally from 20.00 to 25.00 wt. %, based on the total weight of the silicone composite.

[0048] The content of the (B2) TC filler in the silicone composite may be 35.00 wt. %or more, optionally 40.00 wt. %or more, optionally 45.00 wt. %or more, or optionally 50.00 wt. %or more, based on the total weight of the silicone composite. At the same time the content of the (B2) TC filler in the silicone composite may be 75.00 wt. %or less, optionally 70.00 wt. %or less, optionally 65.00 wt. %or less, or optionally 60.00 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the content of the (B2) TC filler in the silicone composite may be from 35.00 to 75.00 wt. %, optionally from 40.00 to 70.00 wt. %, optionally from 45.00 to 65.00 wt. %, or optionally from 50.00 to 60.00 wt. %, based on the total weight of the silicone composite.

[0049] (C) Filler treating agent

[0050] The (C) treating agent is useful to assist dispersing and stabilizing the dispersion of fillers such as the (B) TC filler in the silicone composite. The (C) treating agent includes (C1) a filler treating agent (hereinafter, also abbreviated as “ (C1) a treating agent” ) represented by the following formula (I) : R13SiO- (R22SiO) n-SiR13  (I)

[0051] Each R1 is directly bonded to the silicon atom and may be same or different. Each R1 is independently selected from an alkyl group and an alkoxy group, provided that at least R1 is an alkoxy group. The alkyl group of R1 may be an alkyl group having from 1 to 10 carbon atoms, optionally an alkryl group having from 1 to 3 carbon atoms, or optionally a methyl group. The alkoxy group of R1 may be an alkoxy group having from 1 to 10 carbon atoms, optionally an alkoxy group having from 1 to 3 carbon atoms, or optionally a methoxy group.

[0052] Each R2 is directly bonded to the silicon atom and may be same or different. Each R2 is independently selected from an alkyl group and an aryl group. The alkyl group of R2 may be an alkyl group having from 1 to 10 carbon atoms, optionally an alkyl group having from 1 to 3 carbon atoms, or optionally a methyl group. The aryl group of R2 may be an aryl group having from 6 to 12 carbon atoms, or optionally a phenyl group.

[0053] Subscript “n” refers to the average number of (R22SiO) units and has a value of 10 or more and 400 or less. In some embodiments, subscript “n” may be 30 or more, optionally 60 or more, or optionally 90 or more. At the same time subscript “n” may be 300 or less, optionally 220 or less, or optionally 140 or less. In some embodiments, subscript “n” may be from 30 to 300, optionally from 60 to 220, or optionally from 90 to 140.

[0054] In some embodiments, the (C1) treating agent may be a mono-trialkoxysiloxy terminated diorganopolysiloxane. The mono-trialkoxysiloxy terminated diorganopolysiloxane may be represented by the formula: R43SiO- (Rs2SiO) n-Si (OR6) 3 where each R4, R5 and R6 is independently selected from alkyl group having one or more, and can have 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, even 8 or more carbon atoms while at the same time typically contain 10 or fewer, 8 or fewer, 6 or fewer, 4 or fewer, even 2 or fewer carbon atoms, and subscript “n” has the same meaning as the “n” in the above formula (I) .

[0055] The content of the (C1) treating agent in the silicone composite may be 0.25 wt. %or more, optionally 0.40 wt. %or more, optionally 0.60 wt. %or more, or optionally 0.80 wt. %or more, based on the total weight of the silicone composite. At the same time the content of the (C1) treating agent in the silicone composite may be 5.00 wt. %or less, optionally 3.50 wt. %or less, optionally 2.00 wt. %or less, or optionally 1.40 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the content of the (C1) treating agent in the silicone composite may be from 0.25 to 5.00 wt. %, optionally from 0.25 to 3.50 wt. %, optionally from 0.25 to 1.40 wt. %, optionally from 0.40 to 3.50 wt. %, optionally from 0.60 to 2.00 wt. %, or optionally from 0.80 to 1.40 wt. %, based on the total weight of the silicone composite. When the content of the (C1) treating agent is within the aforementioned range, it is possible to disperse the (B) TC filler (especially the (B2) TC filler) even better, and further improve the extrusion rate and mechanical properties such as elongation of the thermally-conductive composition.

[0056] The (C) treating agent may further include treating agents other than the (C1) treating agent. In some embodiments, the silicone composite may include (C2) a filler treating agent (hereinafter, also abbreviated as “ (C2) a treating agent” ) represented by the following formula (II) : SiR3m (OR3) 4-m       (II)

[0057] Each R3 may be same or different. R3 is an alkyl group, optionally alkyl group having from 1 to 20 carbon atoms, or optionally an alkyl group having from 1 to 10 carbon atoms.

[0058] Subscript “m” refers to the number of R3 directly bonded to the silicon atom and is integer from 1 to 3.

[0059] In some embodiments, the (C2) treating agent may be an alkyl trialkoxysilane. The alkyl trialkoxysilane may be represented by the formula SiR7 (OR8) 3, where each of R7 and R8 is independently an alkyl group having 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more even 11 or more carbon atoms while at the same time typically contains 20 or fewer, 18 or fewer, 16 or fewer, 14 or fewer, 12 or fewer, and can contain 10 or fewer carbon atoms. R8 is desirably a methyl group so as to form a methoxy group attached to the silicon atom. Non-limiting examples of the alkyl trialkoxysilane includes n-decyltrimethoxysilane.

[0060] The content of the (C2) treating agent in the silicone composite may be 0.02 wt. %or more, optionally 0.05 wt. %or more, optionally 0.10 wt. %or more, based on the total weight of the silicone composite. At the same time the content of the (C2) treating agent in the silicone composite may be 1.00 wt. %or less, optionally 0.70 wt. %or less, or optionally 0.30 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the content of the (C2) treating agent in the silicone composite may be from 0.02 to 1.00 wt. %, optionally from 0.05 to 1.00 wt. %, optionally from 0.10 to 0.70 wt. %, optionally from 0.10 to 0.30 wt. %, based on the total weight of the silicone composite.

[0061] In some embodiments, the total content of the (B) TC filler and the (C) treating agent may be 5.00 wt. %or more, optionally 30.00 wt. %or more, optionally 50.00 wt. %or more, or optionally 75.00 wt. %or more, based on the total weight of the silicone composite. At the same time the total content of the (B) TC filler and the (C) treating agent may be 99.00 wt. %or less, optionally 91.00 wt. %or less, optionally 87.00 wt. %or less, or optionally 84.00 wt. %or less, based on the total weight of the silicone composite. In some embodiments, the total content of the (B) TC filler and the (C) treating agent in the silicone composite may be from 5.00 to 99.00 wt.%, optionally from 30.00 to 91.00 wt. %, optionally from 50.00 to 87.00 wt. %, or optionally from 75.00 to 84.00 wt. %, based on the total weight of the silicone composite.

[0062] In some embodiments, the (B2) TC filler may be surface-treated with the (C1) treating agent. In some embodiments, the (B1) TC filler may be surface-treated with the (C1) treating agent and / or the (C2) treating agent.

[0063] (D) Hydrosilylation reaction catalyst

[0064] In some embodiments, the silicone composite may include (D) a hydrosilylation reaction catalyst. The (D) hydrosilylation reaction catalysts are known in the art and are commercially available. In some embodiments, the (D) catalyst may include platinum group metal catalysts. Such catalysts can be (D-1) a metal selected from platinum, rhodium, ruthenium, palladium, osmium, and iridium. Alternatively, the (D) catalyst may be (D-2) a compound of such a metal, for example, chloridotris (triphenylphosphane) rhodium (I) (Wilkinson's Catalyst) , a rhodium diphosphine chelate such as [1, 2-bis (diphenylphosphino) ethane] dichlorodirhodium or [1, 2-bis (diethylphospino) ethane] dichlorodirhodium, chloroplatinic acid (Speier's Catalyst) , chloroplatinic acid hexahydrate, platinum dichloride. Alternatively, the (D) catalyst may be (D-3) a complex of the platinum group metal compound with a low molecular weight organopolysiloxane, or (D-4) the platinum group metal compound microencapsulated in a matrix or coreshell type structure. Non-limiting examples of the complexes of platinum with low molecular weight organopolysiloxanes include 1, 3-diethenyl-1, 1, 3, 3-tetramethyldisiloxane complexes with platinum (Karstedt's Catalyst) . Alternatively, the (D) catalyst may comprise (D-5) the complex microencapsulated in a resin matrix.

[0065] Exemplary hydrosilylation reaction catalysts are described in U.S. Patents 3,159,601; 3,220,972; 3,296,291; 3,419,593; 3,516,946; 3,814,730; 3,989,668; 4,784,879; 5,036,117; and 5,175,325; and EP 0 347 895 B. Microencapsulated hydrosilylation reaction catalysts and methods of preparing them are known in the art, as exemplified in U.S. Patents 4,766,176 and 5,017,654. Hydrosilylation reaction catalysts are commercially available, for example, SYL-OFFTM 4000 Catalyst and SYL-OFFTM 2700 are available from Dow Silicones Corporation of Midland, Michigan, USA.

[0066] The content of the (D) catalyst in the silicone composite will depend on various factors including the selection of the (A) organopolysiloxane, and its content of silicon bonded hydrogen atoms (Si-H) and / or alkenyl groups and the content of the platinum group metal in the catalyst selected, however, the content of the (D) catalyst is sufficient to catalyze hydrosilylation reaction of Si-H and alkenyl groups, optionally the amount of the (D) catalyst is sufficient to provide 1 ppm to 6,000 ppm of the platinum group metal based on the total weight of the silicone composite; optionally 1 ppm to 5,200 ppm, optionally 1 ppm to 1,000 ppm, optionally 1 ppm to 300 ppm, or optionally 1 ppm to 100 ppm, on the same basis. Optionally, the content of the (D) catalyst may be 0.01%to 5 wt. %based on the total weight of the silicone composite.

[0067] Other components

[0068] Other components are not specifically limited. Non-limiting examples of the other components include a cure inhibitor, a pigment, a reinforcing filler such as silica, and combinations thereof.

[0069] In some embodiments, the silicone composite does not simultaneously contain the (A1) organopolysiloxane having an alkenyl group, the (A2) organohydrogenpolysiloxane, and the (D) catalyst. For example, non-limiting examples of the embodiments of the silicone composite include: (i) containing the (A1) organopolysiloxane and the (A2) organohydrogenpolysiloxane, but not the (D) catalyst; (ii) containing the (A1) organopolysiloxane and the (D) catalyst, but not the (A2) organohydrogenpolysiloxane; or (iii) containing the (A2) organohydrogenpolysiloxane and the (D) catalyst, but not the (A1) organopolysiloxane.

[0070] <Method of producing a silicone composite>

[0071] The method of producing the silicone composite is not specifically limited. As non-limiting example of the method of producing the silicone composite, the following discloses the first and second methods. Note that the components used in the methods are the same as those described in the above section of “silicone composite” .

[0072] The first method of producing a silicone composite comprises at least the following three steps: Step 1-1: surface-treating (B1) a thermally-conductive filler having a Dv50 of less than 5 μm  with at least one of (C1) a filler treating agent and (C2) a filler treating agent. Step 1-2: surface-treating (B2) a thermally-conductive filler having a Dv50 of 5 μm or more  with (C1) a filler treating agent. Step 1-3: mixing the surface-treated (B1) thermally conductive filler, the surface-treated (B2)  thermally conductive filler, and (A) an organopolysiloxane.

[0073] In Steps 1-1 and 1-2, the method of surface-treating the (B) TC filler with the (C) treating agent is not particularly limited (Hereinafter, this method may be referred to as the “ex-situ treatment” ) . Non-limiting examples of the ex-situ treatment include a method in which a water-based suspension containing the (B) TC filler and the (C) treating agent is refluxed, water is removed by filtration, and then further dried (Hereinafter, this approach may be referred to as the “water-based method” ) . In addition to the water-based method, known methods such as spray methods and solvent methods can also be employed for the ex-situ treatment.

[0074] In Step 1-3, the surface-treated (B1) TC filler obtained in Step 1-1, the surface-treated (B2) TC filler obtained in Step 1-2, and (A) an organopolysiloxane are mixed. The method of mixing is not particularly limited, and these components can be mixed all at once or sequentially. Compared with in-situ treatment, it is possible to suppress the dimerization of the (C) treating agent (especially, the (C1) treating agent) and the condensation between the formed methanol and the silanol group originating from the (A) organopolysiloxane, thereby suppressing the generation of alkoxy groups such as methoxy groups.

[0075] The second method of producing a silicone composite comprises at least the following two steps: Step 2-1: surface-treating (B1) a thermally-conductive filler having a Dv50 of less than 5 μm  with at least one of (C1) a filler treating agent and (C2) a filler treating agent. Step 2-2: mixing the surface-treated (B1) thermally-conductive filler, (B2) a thermally- conductive filler having a Dv50 of 5 μm or more, (C1) a filler treating agent, and (A) an organopolysiloxane.

[0076] The second method of producing a silicone composite includes the direct addition of the surface non-treated (B2) TC filler and the (C1) treating agent into (A) an organopolysiloxane, preferably under low-temperature conditions (hereinafter sometimes referred to as ″cold blending″ ) for the same reasons (suppressing the generation of alkoxy groups such as methoxy groups) stated above. The temperature for cold blending is not particularly limited, but may be at room temperature without extra heating, for example, from 0 to 50 ℃, or optionally from 10 to 30 ℃. In some embodiments, the surface-treatment of (B1) TC filler having may be carried out by the ex-situ treatment as stated in the first method, together with the (B2) TC filler surface-treated by the cold blending.

[0077] <Thermally-conductive composition>

[0078] The present disclosure provides a thermally-conductive composition including the silicone composite. In some embodiments, the thermally-conductive composition may comprise two components (i.e., a two-part composition including Part A and Part B) , with at least one of the components being the silicone composite described above.

[0079] In some embodiments, the thermally-conductive composition includes a silicone composite (part A) and a silicone composite (part B) . Regarding Part A and Part B, the following embodiments are provided as examples, but the thermally-conductive composition disclosed herein is not limited to these embodiments: · The silicone composite (Part A) includes (A1) an organopolysiloxane, (B) a TC filler, (C) a  treating agent, and (D) a catalyst, and does not include (A2) an organohydrogenpolysiloxane. · At the same time, the silicone composite (Part B) includes (A1) an organopolysiloxane, (A2)  an organohydrogenpolysiloxane, (B) a TC filler, and (C) a treating agent, and does not include (D) a catalyst.

[0080] <Cured product>

[0081] The cured product of the present disclose is obtainable by curing the thermally-conductive composition described above. In some embodiments, the cured product may be obtainable by curing the thermally-conductive composition through hydrosilylation reaction. The conditions for curing the thermally-conductive composition are not specifically limited and can be chosen depending on factors such as the type of each components described above. EXAMPLES

[0082] The silicone composite, the thermally-conductive composition, the cured product and the method of the present disclosure will now be described in detail using Inventive Examples (IE) and Comparative Examples (CE) . Note that in the formulas, ″Me″ indicates a methyl group and ″Vi″ indicates a vinyl group.

[0083] Extrusion rate, squeeze force, hardness, tensile strength, elongation, and thermal conductivity are measured as follows.

[0084] Extrusion rate

[0085] The extrusion rate is determined according to ASTM D2452. The sample is placed into the standard tube and extruded under a pressure of 621 kPa. The amount of sample extruded in one minute is measured. In the present disclosure, an extrusion rate of 80 g / min or higher is considered satisfactory.

[0086] Squeeze force

[0087] The sample is added to the dual-beam texture analyzer with the probe diameter of 40 mm. The initial gap thickness is set to 5.0 mm and the squeeze speed to 1.0 mm / s. During the squeezing process, the force is recorded. The squeeze force is the force data when gap is 0.5 mm. In the present disclosure, a squeeze force of 250 N or lower is considered satisfactory.

[0088] Hardness

[0089] The hardness (shore 00) is determined according to ASTM D2450 and JIS K6253. The cured sample is at least 1 / 4 inch (0.64 cm) thick, and the durometer needle is at least 1 / 2 inch (1.27 cm) from any edge for the reading to be meaningful. In the present disclosure, a hardness of 30 or higher is considered satisfactory. The cured samples used for evaluation of hardness, tensile strength, elongation, and thermal conductivity are obtained by mixing part A and part B with the weight ratio of 1: 1 in a speed mixer cup at 2,000 rpm for 30 seconds, heating to 100 ℃for 1 hour.

[0090] Tensile strength and elongation

[0091] The tensile strength and elongation are determined according to ASTM D412. In the present disclosure, a tensile strength of 0.1 MPa or higher is considered satisfactory, and an elongation of 200%or higher is considered satisfactory.

[0092] Thermal conductivity

[0093] The thermal conductivity is measured according to ISO 22007-2: 2022. The thermal conductivity of the cured sample with 29 mm wide, 29 mm long and 8 mm thick is measured by the hot disk method using a Hot Disk transient technology sensor C5501 from Hot Disk AB of Gothenburg, Sweden. In the present disclosure, a thermal conductivity 1.70 W / mK or higher is considered satisfactory.

[0094] The components used in the Inventive Examples and Comparative Examples are listed in Table 1 below.

[0095] Table 1

[0096] Preparation Example 1: (B1-1) TC filler surface-treated with (C1) treating agent

[0097] 100 g of the (B1-1) TC filler (small-size alumina) and 1.0 g of the (C1) treating agent are charged into a 1-L round-bottom flask containing 200 g of deionized water. The round flask, equipped with an agitator, a reflux condenser, and a thermometer, is heated. The aqueous solution (water-based suspension) is refiuxed at approximately 100 ℃ for 2 hours. The slurry of surface-treated (ex-situ treated) alumina is collected in a Buchner funnel by vacuum filtration. The slurry is then dried at 100 ℃ overnight to obtain a (C1) treating agent surface treated (B1-1) TC filler (hereinafter, also abbreviated as “ (B1-1) TC filler- (C1) treated” ) .

[0098] Preparation Example 2: (B1-1) TC filler surface-treated with (C2) treating agent

[0099] Except for using the (C2) treating agent instead of the (C1) treating agent, the same procedure as in Preparation Example 1 is followed to obtain a (C2) treating agent surface-treated (B1-1) TC filler (hereinafter also abbreviated as a “ (B1-1) TC filler- (C2) treated” ) .

[0100] Preparation Example 3: (B1-2) TC filler surface-treated with the (C2) treating agent

[0101] 1.5 kg of the (B1-2) TC filler (small-size aluminum nitride) is highly sheared at 2,500 rpm in a 5-L reactor. 7.5 g of the (C2) treating agent is continuously sprayed over a period of 5 to 10 minutes. The powder is then heated to 100 ℃ and kept under vacuum for 1 hour to obtain a (C2) treating agent surface treated (B1-2) TC filler (hereinafter also abbreviated as a “ (B1-2) TC filler- (C2) treated” ) .

[0102] Preparation Example 4: (B2-1) TC filler surface-treated with (C1) treating agent

[0103] 100 g of the (B2-1) TC filler (large-size alumina) and 2.0 g of the (C1) treating agent are charged into a 1-L round-bottom flask containing 200 g of deionized water. The round flask, equipped with an agitator, a reflux condenser, and a thermometer, is heated. The aqueous solution (water-based suspension) is refluxed at approximately 100 ℃ for 2 hours. The slurry of surface-treated (ex-situ treated) alumina is collected in a Buchner funnel by vacuum filtration. The slurry is then dried at 100 ℃ overnight to obtain a (C1) treating agent surface treated (B2-1) TC filler (hereinafter also abbreviated as a “ (B2-1) TC filler- (C1) treated” ) .

[0104] Preparation Example 5: (B2-1) TC filler surface-treated with the (C2) treating agent

[0105] Except for using the (C2) treating agent instead of the (C1) treating agent, the same procedure as in Preparation Example 4 is followed to obtain a (C2) treating agent surface-treated (B2-1) TC filler (hereinafter also abbreviated as a “ (B2-1) TC filler- (C2) treated” ) .

[0106] The silicone composites (part A) containing the components shown in Tables 2 and 3, are prepared using the following procedure.

[0107] Inventive examples (IE) 1 to 6 and Comparative examples (CE) 2 to 7

[0108] The (B1) and / or (B2) TC fillers used (surface-treated or surface non-treated) are dried. The (B1) TC fillers are added into (A1-1) vinyl polymer and mixed at 1,500 rpm for 30 seconds to obtain a mixture (1a) . Half the amount of (B2) TC fillers are added to the mixture (1a) and mixed at 1,500 rpm for 30 seconds to obtain a mixture (2a) . Remaining half amount of (B2) TC fillers are added to the mixture (2a) and mixed at 1,500 rpm for 30 seconds twice under vacuum to obtain a mixture (3a) . Then, the masterbatch (1) , the (A1-2) vinyl polymer, the (D) catalyst, (C1) and / or (C2) treating agent if used are added to the mixture (3a) and mixed at room temperature (25 ℃) to obtain a silicone composite (part A) based on the ex-situ treatment.

[0109] Comparative example (CE) 1

[0110] The surface non-treated (B1-1) and (B2-1) fillers are dried. The surface non-treated (B1-1) TC fillers are added into (A1-1) vinyl polymer and mixed at 1,500 rpm for 30 seconds to obtain a mixture (1a) . Halfthe amount of the surface non-treated (B2-1) TC filler is added to the mixture (1a) and mixed at 1,500 rpm for 30 seconds to obtain a mixture (2a) . Remaining half amount of the surface non-treated (B2-1) TC filler is added to the mixture (2a) and mixed at 1,500 rpm for 30 seconds twice under vacuum to obtain a mixture (3a) . Then, the masterbatch (1) , the (A1-2) vinyl polymer, (C1) and (C2) treating agents to the mixture (3a) and mixed for 2 hours at 140 ℃ under vacuum to obtain a mixture (4a) . After cooling the mixture (4a) to below 60 ℃, the (D) catalyst is added to the mixture (4a) and mixed at room temperature (25 ℃) to obtain a silicone composite (part A) based on the in-situ treatment.

[0111] In Tables 2 and 3, under the column “NMR peak from 3.30 to 3.80 ppm” , “No” means that when a silicone composite (part A) is extracted with n-hexane and the 1H-NMR of the obtained extract is measured (standard substance: tetramethyl silane) , no peaks are observed in the region of 3.30 to 3.80 ppm or very small peaks (with an integral value of 0.003%or less of the integral value of the peaks in the region of-0.3 ppm to 0.5 ppm) are observed in the region. “Yes” also means that at least one peak (with an integral value exceeding 0.003%of the integral value of the peaks in the region of-0.3 ppm to 0.5 ppm) is observed in the region of 3.30 to 3.80 ppm.

[0112] Table 2

[0113] Table 3

[0114] The silicone composites (part B) containing the components shown in Table 4, are prepared using the following procedure.

[0115] Liquid materials (a (A1-1) vinyl polymer, a (A2-1) SiH polymer, a (A2-2) SiH polymer, a (C2) treating agent, and a masterbatch (1) and a masterbatch (2) ) are mixed at 1,500 rpm for 30 seconds to obtain a mixture (1b) . The (B1) TC fillers are added into the mixture (1b) and mixed at 1,500 rpm for 30 seconds to obtain a mixture (2b) . Halfthe amount of (B2) TC fillers are added to the mixture (2b) and mixed at 1,500 rpm for 30 seconds to obtain a mixture (3b) . Remaining half amount of (B2) TC fillers are added to the mixture (3b) and mixed at 1,500 rpm for 30 seconds to obtain a mixture (4b) . The mixture (4b) is heated at 140 ℃ for 2 hours under vacuum (base heating) . The heated mixture (4b) is cooled to room temperature. Then, the pigments (1) and (2) are added into the cooled mixture (4b) to obtain a silicone composite (part B) .

[0116] Table 4

[0117] The silicone composite (part A) and the silicone composite (part B) with the weight ratio 1: 1 in a speed mixer cup at 2,000 rpm for 30 seconds, heating to 100 ℃ for 1 hour. Then, the various evaluations mentioned above are conducted. The results are shown in Tables 5 and 6 below.

[0118] Table 5

[0119] Table 6

[0120] As shown in Tables 5 and 6, the thermally-conductive compositions including the silicone composite (Part A) of IEs 1 to 6, all exhibit high extrusion rate (≥ 80 g / min) and high elongation (≥ 200%) . Further, the thermally-conductive compositions of IEs 1 to 6, all exhibit low squeeze force (≤ 250 N) , high hardness (≥ 30) , high tensile strength (≥ 0.1 MPa) , and high thermal conductivity (≥1.7 W / mK) .

[0121] In CE1, which uses a silicone composite (part A) where the NMR peaks are observed in the region, the thermally-conductive composition exhibits a low extrusion rate (< 80 g / min) and low mechanical property such as low elongation (< 200%) . In CE2 to CE7, which use a silicone composite (part A) which does not contain the (C1) treating agent, the thermally-conductive compositions exhibit low extrusion rate and / or low mechanical property such as low elongation.INDUSTRIAL APPLICABILITY

[0122] According to the present disclosure, it is possible to provide a silicone composite that can be used to prepare a thermally-conductive composition capable of exhibiting high extrusion rate and excellent elongation.

Claims

1.A silicone composite comprising:(A) an organopolysiloxane;(B) a thermally-conductive filler; and(C) a filler treating agent;wherein the (B) thermally-conductive filler includes;(B1) a thermally-conductive filler having a Dv50 of less than 5 μm, and(B2) a thermally-conductive filler having a Dv50 of 5 μm or more;wherein the (C) filler treating agent includes (C1) a filler treating agent represented by the following formula (I) :R13SiO- (R22SiO) n-SiR13   (I)where R1 is each independently an alkyl group or an alkoxy group, provided that at least one R1 is an alkoxy group, R2 is each independently an alkyl group or an aryl group, and n is the average number of (R22SiO) units and has a value of 10 or more and 400 or less; andwherein the silicone composite has a 1H-NMR spectrum, using deuterated benzene as the solvent, that substantially lacks a peak within a range of 3.30 ppm and 3.80 ppm.2.The silicone composite according to claim 1, wherein the (C) filler treating agent further includes (C2) a filler treating agent represented by the following formula (II) : SiR3m (OR3) 4-m     (II)where R3 is each independently an alkyl group, and m is an integer from 1 to 3.3.The silicone composite according to claim 1, wherein the (B2) thermally-conductive filler is surface-treated with the (C1) filler treating agent.4.The silicone composite according to claim 1, wherein the (B1) thermally-conductive filler is surface-treated with the (C1) filler treating agent.5.The silicone composite according to claim 2, wherein the (B1) thermally-conductive filler is surface-treated with the (C2) filler treating agent.6.The silicone composite according to claim 1, wherein the (B1) thermally-conductive filler and the (B2) thermally-conductive filler are each independently selected from the group consisting of aluminum trihydrate, alumina, aluminum nitride, zinc oxide, magnesium hydroxide, and glass beads.7.The silicone composite according to claim 1, wherein the content of the (A) organopolysiloxane is from 1.00 to 95.00 wt%, based on the total weight of the silicone composite, and the total content of the (B) thermally-conductive and the (C) filler treating agent is from 5.00 to 99.00 wt%, based on the total weight of the silicone composite.8.The silicone composite according to claim 1, wherein the (A) organopolysiloxane includes at least one of (A1) an organopolysiloxane having an alkenyl group and (A2) an organohydrogenpolysiloxane.9.The silicone composite according to claim 1, further comprising (D) a hydrosilylation reaction catalyst.10.A thermally-conductive composition comprising two components, wherein at least one of the two components is the silicone composite according to any one of claims 1 to 9.11.A cured product obtainable by curing the thermally-conductive composition according to claim 10.12.A method of producing a silicone composite, comprising:surface-treating (B1) a thermally-conductive filler having a Dv50 of less than 5 μm with at least one of (C1) a filler treating agent represented by the following formula (I) and (C2) a filler treating agent represented by the following formula (II) :R13SiO- (R22SiO) n-SiR13    (I)where R1 is each independently an alkyl group or an alkoxy group, provided that at least one R1 is an alkoxy group, R2 is each independently an alkyl group or an aryl group, and n is the average number of (R22SiO) units and has a value of 10 or more and 400 or less,SiR3m (OR3) 4-m    (II)where R3 is each independently an alkyl group, and m is an integer from 1 to 3;surface-treating (B2) a thermally-conductive filler having a Dv50 of 5 μm or more with the (C1) filler treating agent; andmixing the surface-treated (B1) thermally conductive filler, the surface-treated (B2) thermally conductive filler, and (A) an organopolysiloxane.13.A method of producing a silicone composite, comprising:surface-treating (B1) a thermally-conductive filler having a Dy50 of less than 5 μm with at least one of (C1) a filler treating agent represented by the following formula (I) and (C2) a filler treating agent represented by the following formula (II) :R13SiO- (R22SiO) n-SiR13  (I)where R1 is each independently an alkyl group or an alkoxy group, provided that at least one R1 is an alkoxy group, R2 is each independently an alkyl group or an aryl group, and n is the average number of (R22SiO) units and has a value of 10 or more and 400 or less,SiR3m (OR3) 4-m     (II)where R3 is each independently an alkyl group, and m is an integer from 1 to 3; andmixing the surface-treated (B1) thermally-conductive filler, (B2) a thermally-conductive filler having a Dv50 of 5 μm or more, the (C1) filler treating agent, and (A) an organopolysiloxane.