Environmentally friendly leather made from recycled cowhide fibers, and production line and production process therefor

By using the structural design and composite process of recycled cowhide fiber environmentally friendly leather, the problems of low utilization rate of genuine leather and insufficient bonding strength have been solved, realizing high-strength composite and customized leather production.

WO2026232710A1PCT designated stage Publication Date: 2026-11-12FUJIAN YIHONG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/113810
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2025-08-11
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Traditional genuine leather suffers from irregularity, low utilization rate, and difficulty in customizing color and texture. Furthermore, the bonding strength between the base fabric and cowhide fibers is insufficient.

Method used

It adopts an environmentally friendly leather structure made of recycled cowhide fiber, including a cowhide fiber surface layer, a double-suede base layer and a cowhide fiber bottom layer. It is cross-linked with island yarn and high-shrinkage yarn, combined with temperature-sensitive hydrogel fiber to form a high-strength composite structure. The bonding strength is improved by oblique wire papermaking and hydroentanglement composite process.

Benefits of technology

It improves the tear strength, tensile properties, and durability of recycled cowhide fiber eco-friendly leather, allows for customization of colors and textures according to customer needs, enhances the cross-linking degree between the base fabric layer and cowhide fibers, and achieves high transverse tensile strength and longitudinal adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025113810_12112026_PF_FP_ABST
    Figure CN2025113810_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of fabrics, and particularly to an environmentally friendly leather made from recycled cowhide fibers, and a production line and a production process therefor. A cowhide fiber top layer and a cowhide fiber bottom layer mainly comprise recycled cowhide fibers. After hydroentangling, cowhide fibers are highly entangled with base fabric, thereby improving the durability of the environmentally friendly leather made from recycled cowhide fibers. The produced environmentally friendly leather made from recycled cowhide fibers has a hand feeling similar to that of genuine leather, and has good tear strength and tensile properties, thereby solving the problem of low utilization rate of conventional genuine leather caused by irregularity, piece size and natural limitations such as surface defects. The recycled leather can be provided in various lengths according to product requirements, and can be customized with various colors and textures according to customer requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Regenerated cowhide fiber eco-friendly leather and its production line and production process Technical Field

[0001] This invention relates to the field of fabric technology, specifically to environmentally friendly recycled cowhide fiber leather and its production line and production process. Background Technology

[0002] In the leather manufacturing industry, traditional genuine leather has long been widely used in many industries due to its excellent texture and performance. However, since genuine leather is mainly derived from animal hides, it faces several limitations. On the one hand, genuine leather is irregular and limited in size, and its surface is prone to natural defects such as wounds, resulting in low utilization. On the other hand, the color and texture of genuine leather are relatively fixed, making it difficult to customize according to diverse customer needs, which to some extent limits its application range. To solve these problems of traditional genuine leather, regenerated leather technology has emerged. Among the common regenerated leather technologies, some involve simple napping and defibering of cowhide waste, followed by compounding with other fibers or materials. Meanwhile, in terms of the selection and use of base fabric, ordinary woven base fabrics are more common. When these base fabrics are compounded with cowhide fibers, they mainly rely on simple physical bonding or a small amount of chemical cross-linking. Moreover, the base fabric usually adopts a single yarn structure, and the cross-linking and connection between yarns are relatively simple, making it difficult to form a high-strength bonding effect when compounded with cowhide fibers. The hydroentanglement cross-linking density is low, which affects the bonding strength and overall performance between the layers of leather. In view of this, this case arises. Summary of the Invention

[0003] One object of the present invention is to solve at least the above-mentioned problems through environmentally friendly leather made from recycled cowhide fibers, as well as its production line and production process.

[0004] To solve the above technical problems, the present invention adopts the following technical solution: the recycled cowhide fiber environmentally friendly leather includes, from top to bottom, a cowhide fiber surface layer, a double-suede base fabric layer and a cowhide fiber bottom layer. The double-suede base fabric layer has pile distributed on both the upper and lower surfaces. The cowhide fibers of the cowhide fiber surface layer and the cowhide fiber bottom layer are cross-linked with the yarn fibers and pile fibers of the double-suede base fabric layer.

[0005] Preferably, the fabric structure of the double-pile base fabric layer is a double-layer structure with bonded warp. In the double-layer structure with bonded warp, the outer warp and outer weft are interwoven to form the base fabric outer layer, and the inner warp and inner weft are interwoven to form the base fabric inner layer. The bonded warp is interwoven with both the outer weft and the inner weft, so that the base fabric outer layer and the base fabric inner layer are connected to each other.

[0006] Preferably, in the double-layered weave structure, the outer weave is a two-up, two-down right-hand twill weave, the inner weave is a one-up, three-down right-hand twill weave, the warp yarn arrangement is one outer warp, one inner warp, and one weft yarn arrangement is one outer weft and one inner weft.

[0007] Preferably, the outer warp and inner warp are island-island yarns, which are composites of island-island yarns and high-shrinkage yarns through a web processing process. The island-island yarns are composite spinnings in which the island component is coated with the sea component. The sea component is low-viscosity PET, the island component is PBT / IPA copolymer, the high-shrinkage yarn is modified PET, the bonding warp is high-strength PA66 filament, and the outer weft and inner weft are modified PA6 staple fiber yarns.

[0008] Preferably, the raw materials of the island yarn include the following components by weight: 65-70 parts of low-viscosity PET, 35-40 parts of PBT / IPA copolymer, 30-35 parts of modified PET, and 0.6-0.8 parts of network oil.

[0009] Preferably, the slurry of the cowhide fiber surface layer and the cowhide fiber bottom layer comprises, by weight, the following components: 90-100 parts of regenerated cowhide fiber, 5-8 parts of plant fiber, 8-10 parts of thermosensitive hydrogel fiber, 3-5 parts of nanocellulose whiskers, and 5-8 parts of waterborne polyurethane.

[0010] The aforementioned production line for recycled cowhide fiber environmentally friendly leather includes an inclined wire paper machine, a base fabric unwinding machine, a base fabric belt conveyor, a composite belt conveyor, a hydroentangling device, and a drying device. There are two inclined wire paper machines. The base fabric unwinding machine is located at the front end of the base fabric belt conveyor. The hydroentangling device and the drying device are arranged sequentially at the rear end of the composite belt conveyor. A carding machine is located at the end of the base fabric belt conveyor. The carding machine is equipped with an upper carding roller and a lower carding roller arranged opposite each other. Following the carding machine are an upper air knife and a lower suction roller arranged opposite each other. Finally, an upper ionizing air bar and a lower ionizing air bar are arranged opposite each other.

[0011] The production process of the above-mentioned recycled cowhide fiber environmentally friendly leather includes the following steps:

[0012] Step a: Prepare the double-fleece base fabric;

[0013] Step b: The pulp is processed into kraft fiber material using a wire mesh papermaking machine;

[0014] Step c: The prefabricated double-fleece base fabric is unwound using a base fabric unwinding machine;

[0015] Step d: The double-pile base fabric is conveyed by the base fabric belt conveyor and sandwiched between the kraft fiber material produced by the two inclined wire paper machines. Finally, it is stacked on the composite belt conveyor to form a sandwich structure fabric.

[0016] Step e: The fabric enters the hydroentangling device, and the cowhide fiber surface layer, double-sleeved base fabric layer and cowhide fiber bottom layer are hydroentangled together by the hydroentangling machine;

[0017] Step f: The hydroentangled composite substrate is successively subjected to rolling drying, cylindrical drying, removal of harmful substances, and rotary screen drying, and finally rolled up.

[0018] Preferably, the preparation process of the double-fleece base fabric is as follows:

[0019] Step a: Prepare island-island yarn;

[0020] Step b: Weave a base fabric with a double-layer structure;

[0021] Step c, Alkali treatment: Alkali treatment is performed using 10% NaOH solution at a temperature of 90℃ for 30 minutes;

[0022] Step d, Double-sided texturing: Double-sided texturing is performed using a ceramic sand grinding disc at a speed of 1500 rpm and a pressure of 0.15 MPa.

[0023] Preferably, the preparation process of the island yarn is as follows: after melting the sea component slices and island component slices, the island yarn with a 16-island structure is formed by passing it through an island spinneret; the island yarn and high-shrinkage yarn are networked in proportion and synthesized into island yarn, and then treated with a polyether-type network oiling agent.

[0024] As described above, the recycled cowhide fiber environmentally friendly leather, its production line, and production process provided by this invention have the following beneficial effects: Recycled cowhide fibers are obtained from cowhide waste through napping and defiberization. The recycled cowhide fibers constitute the main body of both the surface and bottom layers of the cowhide fibers. Therefore, the produced recycled cowhide fiber environmentally friendly leather has a feel close to genuine leather and possesses good tear strength and tensile properties. This solves the problem of low utilization rate caused by the irregularity, size, and surface damage inherent in traditional genuine leather. The recycled leather can be supplied in length according to product requirements and can be customized in various colors and textures according to customer needs. This material breaks through the limitations of genuine leather color and texture. The added temperature-sensitive hydrogel fiber can automatically adjust the gap between fiber layers according to the ambient humidity, giving the material self-regulating breathability. The base fabric has pile distributed on both the top and bottom sides. The evenly distributed pile structure can significantly improve the cross-linking degree between the base fabric layer and the cowhide fiber during hydroentangling, thereby improving the bonding strength of each layer of the composite fabric. The double pile base fabric layer combines the tensile strength of woven fabric and the strong cross-linking of non-woven fabric, so that the recycled cowhide fiber environmentally friendly leather has both high transverse tensile strength and longitudinal bonding strength, improving the durability of the recycled cowhide fiber environmentally friendly leather. Attached Figure Description

[0025] Figure 1 is a schematic diagram of the structure of environmentally friendly leather made from recycled cowhide fibers.

[0026] Figure 2 shows the fabric structure of the double-pile base fabric.

[0027] Figure 3 shows the warp cross-section of the double-fleece base fabric layer.

[0028] Figure 4 is a schematic diagram of the production line for recycled cowhide fiber environmentally friendly leather.

[0029] Figure 5 is a schematic diagram of the carding machine. Detailed Implementation

[0030] The present invention will be further described below through specific embodiments.

[0031] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.

[0032] As shown in Figure 1, the recycled cowhide fiber environmentally friendly leather of the present invention comprises, from top to bottom, a cowhide fiber surface layer 10, a double-sleeved base fabric layer 20, and a cowhide fiber bottom layer 30. Both the upper and lower surfaces of the double-sleeved base fabric layer 20 are covered with pile. The cowhide fibers of the cowhide fiber surface layer 10 and the cowhide fiber bottom layer 30 are cross-linked with the yarn fibers and pile fibers of the double-sleeved base fabric layer 20. The uniformly distributed pile structure on both the upper and lower surfaces of the base fabric introduced in this invention significantly improves the cross-linking degree between the base fabric layer and the cowhide fibers during hydroentangling lamination, thereby increasing the bonding strength of each layer of the composite fabric. The double-sleeved base fabric layer 20 combines the tensile strength of woven fabrics with the strong cross-linking properties of non-woven fabrics, enabling the recycled cowhide fiber environmentally friendly leather to simultaneously possess high transverse tensile strength and longitudinal bonding strength, thus improving the durability of the recycled cowhide fiber environmentally friendly leather.

[0033] The fabric structure of the double-pile base fabric layer 20 is a double-layer weave with interlocking warp. In this double-layer weave, the outer layer of the base fabric is formed by the interlacing of the outer warp and outer weft, and the inner layer is formed by the interlacing of the inner warp and inner weft. The interlocking warp interlaces with both the outer and inner weft, thus connecting the outer and inner layers of the base fabric. The double-pile base fabric layer 20 with this fabric structure has a double-layer fabric structure, ensuring sufficient strength while the base fabric is piled on both sides. Because the interlocking warp fiber material is different from the outer and inner warps, it will not dissolve in alkali. Moreover, the interlocking warp is hidden between the outer and inner layers, connecting them together, and will not undergo physical changes during the pile-drawing process, thus ensuring the connection strength between the outer and inner layers.

[0034] In the double weave with binding warp stitching, the face weave is a two-over two-under right twill, the back weave is a one-over three-under right twill, the arrangement sequence of warp yarns is one face warp, one back warp, and one binding warp, and the arrangement sequence of weft yarns is one face weft and one back weft. As shown in Figure 2, it is the looming draft of the fabric weave, in which Chinese numerals one, two, three, four denote face warps and face wefts, Roman numerals Ⅰ, Ⅱ, Ⅲ, Ⅳ denote back warps and back wefts, letters a, b, c, d denote binding warps, the interlacing points of face warps and face wefts are marked with the face weave symbol "★", the interlacing points of back warps and back wefts are marked with the back weave symbol "☆", the binding symbol is "Δ", the heald lifting symbol is "〇", and "□" indicates that the face warp is not lifted when the back weft is inserted. As shown in Figure 3, it is the warp-wise cross-sectional view, the binding warp a interlaces with face weft two and back weft Ⅲ respectively, and is composed of two systems of yarns; the binding warp is hidden between the face layer and the back layer to connect the two layers together, which gives a stable structure and prolongs the service life of the fabric; as shown in Figure 3, fluff is formed on the warp floats on both the inner and outer sides after alkali treatment and sanding.

[0035] The outer and inner warp are island-island yarns, which are composite yarns made by web processing of island-island yarns and high-shrinkage yarns. The island-island yarns are made by coating the island components with the island components through composite spinning. The island component is low-viscosity PET, the island component is PBT / IPA copolymer, the high-shrinkage yarn is modified PET, the bonding warp is high-strength PA66 filament, and the outer and inner wefts are modified PA6 staple fiber yarns. The low-viscosity PET used in the island component has excellent alkali solubility, with an intrinsic viscosity of 0.60 dL / g. As a continuous phase, it coats the island component, forming fluff gaps after dissolution. The solubility is ≥98% at 10% NaOH, 90℃, and 30 min. The island component uses PBT / IPA... The copolymer is alkali-resistant to hydrolysis, retaining ≥95% of its strength after alkali treatment. It forms 16-lobed radial ultrafine fibers with a diameter of 1-2 μm and a specific surface area of ​​6-8 m² / g, enhancing the anchoring points of the hydroentangled crosslinking. The high-shrinkage yarn uses modified PET, preferably modified polyethylene terephthalate copolymer. 8% isophthalic acid is added to the PET matrix as a comonomer to improve the shrinkage rate. 0.5% triphenyl phosphite is added as a heat stabilizer to inhibit thermal oxidative degradation during high-temperature shrinkage treatment. 1% nano-silica is added as an alkali auxiliary agent, dispersed in the PET matrix to form an alkali-resistant barrier and improve alkali resistance. After copolymer modification, it is impregnated with 0.3% fluorocarbon resin solution to form an alkali-resistant coating, reducing alkali adsorption by 40%. All percentages mentioned above refer to weight percentages. The single filament fineness is 75 dtex / 36f, with a circular cross-section and a boiling water shrinkage rate of 38%. During shrinkage, it pulls the floating length of the island yarn. The bending process provides mechanical tension for pile formation and also exhibits good alkali resistance. The island yarn floats on the upper and lower surfaces of the base fabric as a float. After alkaline treatment, the shape of the high-shrinkage yarn is broken, resulting in shrinkage. Subsequently, the sea component of the island yarn dissolves as a continuous phase, while the island fibers loosely wrap around the high-shrinkage yarn. These island fibers are composed of ultrafine fibers with extremely fine diameters. After napping, they break, forming numerous delicate and uniform pile clusters on the inner and outer surfaces of the base fabric. The pile clusters effectively enhance the bonding strength with the cowhide fibers. According to tests, the recycled cowhide fiber environmentally friendly leather made from double-pile base fabric has a pile density of 3000 fibers / cm². Compared with recycled cowhide fiber leather made from ordinary fabric base fabrics, such as plain weave or twill weave base fabrics, this significantly increases the hydroentangling crosslinking points. SEM cross-sectional observation shows that the hydroentangling crosslinking depth doubles, the interlayer peel strength increases by 30-40%, and the interlayer peel strength is ≥80N / cm. The bonding is hidden between the two layers of base fabric to reduce contact with alkaline solutions. Both the high-strength PA66 filament and the modified PA6 staple yarn are impregnated with fluorocarbon resin solution to form an alkali-resistant coating, which reduces the amount of alkali absorbed and improves alkali resistance.

[0036] The raw materials for island-type yarn, by weight, include the following components: 65-70 parts low-viscosity PET, 35-40 parts PBT / IPA copolymer, 30-35 parts modified PET, and 0.6-0.8 parts network oil. The network oil is a polyether-type network agent with a molecular weight of 5000 and a friction coefficient ≤0.25, which enhances the cohesion between island-type yarn and high-shrinkage yarn, prevents fiber slippage during napping, and imparts antistatic properties.

[0037] The pulp of the cowhide fiber surface layer 10 and the cowhide fiber bottom layer 30, by weight, includes the following components: 90-100 parts recycled cowhide fiber, 5-8 parts plant fiber, 8-10 parts thermosensitive hydrogel fiber, 3-5 parts nanocellulose whiskers, and 5-8 parts waterborne polyurethane. Among these components, recycled cowhide fiber is obtained from waste cowhide through napping and defiberization. Recycled cowhide fiber is the main component in the cowhide fiber surface layer 10 and the cowhide fiber bottom layer 30. Therefore, the produced recycled cowhide fiber environmentally friendly leather has a feel close to genuine leather and possesses good tear strength and tensile properties. This solves the problem of low utilization rate caused by the irregularity, size, and surface damage of traditional genuine leather. Recycled leather can be supplied in length according to product requirements and can be customized in various colors and textures according to customer needs, breaking through the limitations of genuine leather in terms of color and texture. The plant fiber uses bamboo pulp fiber to enhance flexibility and breathability; nanocellulose whiskers improve cross-linking density and tear resistance; waterborne polyurethane enhances interlayer bonding; and thermosensitive water... The gel fiber comprises the following raw materials in parts by weight: 80-90 parts of N-isopropylacrylamide, 1-3 parts of crosslinking agent, 5-10 parts of hydrophilic modifying monomer, and 0.5-2 parts of dispersant. N-isopropylacrylamide (NIPAM) contains both hydrophobic (isopropyl) and hydrophilic (amide) groups, which can induce swelling or shrinkage through changes in environmental humidity, thereby adjusting the porosity of the fiber layer. The crosslinking agent is N,N'-methylenebisacrylamide (MBA), which constructs a three-dimensional network structure to enhance the mechanical strength and shape stability of the fiber. The hydrophilic modifying monomer is acrylamide (AM) or hydroxyethyl methacrylate (HEMA), which adjusts the moisture absorption properties and improves hydrophilicity and swelling degree. The dispersant is polyvinyl alcohol (PVA). The raw materials for thermosensitive hydrogel fibers are prepared by polymerization reaction to obtain PNIPAM prepolymer, in which PNIPAM (poly-N-isopropylacrylamide) molecular chain is the main molecular chain of PNIPAM prepolymer. Then, through wet spinning or electrospinning process, it is solidified into fiber by coagulation bath (such as ethanol aqueous solution), and then stretched and dried to obtain thermosensitive hydrogel fiber. The added thermosensitive hydrogel fibers can automatically adjust the gaps between fiber layers according to the ambient humidity, giving the material self-regulating breathability and a dynamically responsive composite layer to the fabric. Due to its swelling-shrinkage characteristics, the thermosensitive hydrogel fibers can achieve a 200% range of breathability adjustment. Under low humidity (<40% RH): the hydrophobic groups of the PNIPAM molecular chain dominate the fiber shrinkage, reducing the volume by 25%-30%, and the porosity of the fiber layer decreases from 60% to 30%, increasing airflow resistance. Under high humidity (>60% RH): water molecules form hydrogen bonds with the hydrophilic groups (-CONH-) of PNIPAM, causing the fiber to swell, increasing the volume by 40%-50%, and increasing the porosity to 70%-80%, significantly improving breathability. Because the pile clusters on the surface of the double-pile base fabric form three-dimensional air-guiding channels, the gap change effect of the thermosensitive fibers is amplified, thus improving the overall breathability adjustment.

[0038] As shown in Figure 4, the production line for recycled cowhide fiber environmentally friendly leather includes an inclined wire paper machine 1, a base fabric unwinding machine 2, a base fabric belt conveyor 3, a composite belt conveyor 4, a hydroentangling device, and a drying device. There are two inclined wire paper machines 1. The base fabric unwinding machine 2 is located at the front end of the base fabric belt conveyor 3. The hydroentangling device and the drying device are arranged sequentially at the rear end of the composite belt conveyor 4. A carding machine 5 is located at the end of the base fabric belt conveyor 3. The base fabric after being carded by the carding machine 5 is combined with the cowhide fiber material produced by the two inclined wire paper machines 1 and then enters the composite belt conveyor 4. The carding machine 5 is equipped with an upper carding roller 51 and a lower carding roller 52 arranged opposite to each other. After that, there is an upper air knife 53 and a lower suction roller 54 arranged opposite to each other. Finally, there is an upper ionizing air bar 55 and a lower ionizing air bar 56 arranged opposite to each other. The base fabric passes sequentially through the gaps between the upper and lower comb rollers 51 and 52, the gap between the upper air knife 53 and the lower suction roller 54, and the gap between the upper and lower ionizing air bars 55 and 56. The upper and lower comb rollers 51 and 52 comb the pile, transforming the pile from clustered aggregation to single-fiber dispersion. The upper air knife 53 blows open the surface pile, and the lower suction roller 54 adsorbs and straightens the bottom pile, forming a symmetrical three-dimensional pile structure. The upper and lower ionizing air bars 55 and 56 eliminate static electricity in the pile, preventing fiber agglomeration due to static electricity. By adding a three-stage treatment system of double-sided comb roller group, dual airflow dispersion, and electrostatic activation at the rear end of the base fabric conveyor belt 3, efficient dispersion and orientation of the pile on the upper and lower surfaces of the double-pile base fabric are achieved, solving the problems of pile agglomeration and low penetration rate, and improving the hydroentanglement crosslinking density.

[0039] The production process of recycled cowhide fiber eco-friendly leather includes the following steps:

[0040] Step a: Prepare the double-fleece base fabric;

[0041] Step b: The pulp is processed into kraft fiber material through inclined wire paper machine 1;

[0042] Step c: The prefabricated double-fleece base fabric is unwound by the base fabric unwinding machine 2;

[0043] Step d: The double-pile base fabric is conveyed by the base fabric belt conveyor 3 and sandwiched between the cowhide fiber material produced by the two inclined wire paper machines 1, and finally stacked on the composite belt conveyor 4 to form a sandwich structure fabric.

[0044] Step e: The fabric enters the hydroentangling device, and the cowhide fiber surface layer 10, the double-sleeved base fabric layer 20 and the cowhide fiber bottom layer 30 are hydroentangled together by the hydroentangling machine.

[0045] Step f: The hydroentangled composite substrate is successively subjected to rolling drying, cylindrical drying, removal of harmful substances, and rotary screen drying, and finally rolled up.

[0046] The preparation process of double-fleece base fabric is as follows:

[0047] Step a: Prepare island-island yarn;

[0048] Step b: Weave a base fabric with a double-layer structure;

[0049] Step c, Alkali treatment: Alkali treatment is performed using 10% NaOH solution at a temperature of 90℃ for 30 minutes;

[0050] Step d, Double-sided texturing: Double-sided texturing is performed using a ceramic sand grinding disc at a speed of 1500 rpm and a pressure of 0.15 MPa.

[0051] The preparation process of island-island yarn is as follows: Island component chips and sea-island component chips are melted and then passed through an island-island spinneret to form 16-island structured island-island yarns. These island-island yarns are then networked with high-shrinkage yarns in a specific ratio and synthesized into island-island yarns, which are then treated with a polyether-type network oil. The network nozzle pressure is 0.6 MPa, the polyether-type network oil concentration is 0.8%, and the coating speed is 20 m / min, ensuring that the fiber surface friction coefficient is ≤0.25.

[0052] The above are merely some specific embodiments of the present invention, but the design concept of the present invention is not limited thereto. Any non-substantial modifications made to the present invention using this concept shall be considered as infringing upon the protection scope of the present invention.

[0053]

Claims

1. Regenerated cowhide fiber environmentally friendly leather, characterized by: From top to bottom, it includes a cowhide fiber surface layer, a double-sleeved base fabric layer, and a cowhide fiber bottom layer. Both the top and bottom surfaces of the double-sleeved base fabric layer are covered with pile. The cowhide fibers in the cowhide fiber surface layer and the cowhide fiber bottom layer are cross-linked with the yarn fibers and pile fibers of the double-sleeved base fabric layer.

2. The environmentally friendly recycled cowhide fiber leather according to claim 1, characterized in that: The fabric structure of the double-pile base fabric layer is a double-layer structure with bonded warp. In the double-layer structure with bonded warp, the outer warp and outer weft are interwoven to form the base fabric outer layer, and the inner warp and inner weft are interwoven to form the base fabric inner layer. The bonded warp is interwoven with both the outer weft and the inner weft, so that the base fabric outer layer and the base fabric inner layer are connected to each other.

3. The environmentally friendly recycled cowhide fiber leather according to claim 2, characterized in that: In the double-layered weave structure, the outer weave is a two-up, two-down right-hand twill weave, and the inner weave is a one-up, three-down right-hand twill weave. The warp yarns are arranged in the order of one outer warp, one inner warp, and one weft yarn, and the weft yarns are arranged in the order of one outer weft and one inner weft.

4. The environmentally friendly recycled cowhide fiber leather according to claim 3, characterized in that: The outer and inner warp are island-island yarns, which are made by combining island-island yarns and high-shrinkage yarns through a web processing process. The island-island yarns are made by coating the island component with the sea component and spinning them together. The sea component is low-viscosity PET, the island component is PBT / IPA copolymer, the high-shrinkage yarn is modified PET, the bonding warp is high-strength PA66 filament, and the outer and inner weft are modified PA6 staple fiber yarns.

5. The environmentally friendly recycled cowhide fiber leather according to claim 4, characterized in that: The raw materials of the island yarn include the following components by weight: 65-70 parts of low-viscosity PET, 35-40 parts of PBT / IPA copolymer, 30-35 parts of modified PET, and 0.6-0.8 parts of network oil.

6. The environmentally friendly recycled cowhide fiber leather according to claim 1, characterized in that: The slurry for the cowhide fiber surface layer and the cowhide fiber bottom layer comprises, by weight, the following components: 90-100 parts of regenerated cowhide fiber, 5-8 parts of plant fiber, 8-10 parts of thermosensitive hydrogel fiber, 3-5 parts of nanocellulose whiskers, and 5-8 parts of waterborne polyurethane.

7. The production line for recycled cowhide fiber environmentally friendly leather according to any one of claims 1-6, characterized in that: The system includes an inclined wire paper machine, a base fabric unwinder, a base fabric belt conveyor, a composite belt conveyor, a hydroentangling device, and a drying device. There are two inclined wire paper machines. The base fabric unwinder is located at the front end of the base fabric belt conveyor. The hydroentangling device and the drying device are arranged sequentially at the rear end of the composite belt conveyor. A carding machine is located at the end of the base fabric belt conveyor. The carding machine has an upper carding roller and a lower carding roller arranged opposite each other. Following the carding machine are an upper air knife and a lower suction roller arranged opposite each other. Finally, there are upper and lower ionizing air bars arranged opposite each other.

8. The production process of recycled cowhide fiber environmentally friendly leather according to any one of claims 1-6, characterized in that: Includes the following steps: Step a: Prepare the double-fleece base fabric; Step b: The pulp is processed into kraft fiber material using a wire mesh papermaking machine; Step c: The prefabricated double-fleece base fabric is unwound using a base fabric unwinding machine; Step d: The double-pile base fabric is conveyed by the base fabric belt conveyor and sandwiched between the kraft fiber material produced by the two inclined wire paper machines. Finally, it is stacked on the composite belt conveyor to form a sandwich structure fabric. Step e: The fabric enters the hydroentangling device, and the cowhide fiber surface layer, double-sleeved base fabric layer and cowhide fiber bottom layer are hydroentangled together by the hydroentangling machine; Step f: The hydroentangled composite substrate is successively subjected to rolling drying, cylindrical drying, removal of harmful substances, and rotary screen drying, and finally rolled up.

9. The production process of recycled cowhide fiber environmentally friendly leather according to claim 8, characterized in that: The preparation process of the double-fleece base fabric is as follows: Step a: Prepare island-island yarn; Step b: Weave a base fabric with a double-layer structure; Step c, Alkali treatment: Alkali treatment is performed using 10% NaOH solution at a temperature of 90℃ for 30 minutes; Step d, Double-sided texturing: Double-sided texturing is performed using a ceramic sand grinding disc at a speed of 1500 rpm and a pressure of 0.15 MPa.

10. The production process of recycled cowhide fiber environmentally friendly leather according to claim 9, characterized in that: The preparation process of the island yarn is as follows: after melting the sea component chips and island component chips, the island yarn with a 16-island structure is formed by passing it through an island spinneret; the island yarn is networked with high-shrinkage yarn in a certain proportion and synthesized into island yarn, and then treated with a polyether-type network oiling agent.