Solid-state battery cell, battery device, electric device, and positive electrode and preparation method therefor
By forming a coating layer on the surface of a lithium transition metal oxide substrate and doping it with elements, the interface problem between lithium transition metal oxide and sulfide electrolyte is solved, thereby improving the cycle performance and stability of solid-state battery cells.
Patent Information
- Application Number
- PCT/CN2026/071550
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-01-09
- Publication Date
- 2026-11-12
AI Technical Summary
In traditional solid-state battery cells, the interface problem between lithium transition metal oxides and sulfide electrolytes limits performance and affects cycle performance.
By forming a coating layer on the surface of a lithium transition metal oxide matrix and doping it with specific elements in a sulfide electrolyte, a Me-S covalent bond network is formed, reducing the possibility of element diffusion and improving interface stability.
It improves the cycle performance of solid-state battery cells, reduces interface impedance and polarization effect, enhances lithium-ion transport path, and extends battery life.
Smart Images

Figure PCTCN2026071550-FTAPPB-I100001 
Figure PCTCN2026071550-FTAPPB-I100002 
Figure PCTCN2026071550-FTAPPB-I100003
Abstract
Description
Solid-state battery cells, battery devices, electrical devices, positive electrodes and their preparation methods
[0001] Cross-reference to related applications
[0002] This application claims priority to Chinese Patent Application No. 202510591774.4, filed on May 8, 2025, entitled "Solid-state battery cell, battery device, power device, positive electrode and method thereof", the entire contents of which are incorporated herein by reference. Technical Field
[0003] This application relates to a solid-state battery cell, a battery device, an electrical device, a positive electrode, and a method for preparing the same. Background Technology
[0004] Compared to battery cells using liquid electrolytes, solid-state battery cells are less prone to combustion and explosion, offering high reliability and high energy density. Currently, traditional cathode active materials, such as lithium transition metal oxides, and solid electrolytes, such as sulfide electrolytes, have a solid-solid contact, which often leads to interface problems that affect the performance of solid-state battery cells. Summary of the Invention
[0005] This application provides a solid-state battery cell, a battery device, an electrical device, a positive electrode, and a method for preparing the same. The solid-state battery cell has good cycle performance.
[0006] In one aspect, embodiments of this application provide a solid-state battery cell, including a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is located between the positive and negative electrodes. The positive electrode includes a positive electrode film layer, which includes a positive electrode active material and a modified sulfide electrolyte. The positive electrode active material includes a substrate and a coating layer located on at least a portion of the surface of the substrate. The modified sulfide electrolyte includes a dopant element Me and a sulfide electrolyte. The substrate includes one or more of lithium transition metal oxides and lithium phosphates. The mismatch between the coating layer and the substrate is 0.5 to 3. The dopant element Me includes one or more of B, Si, Mo, and W. Me ions react with S ions in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol.
[0007] In some embodiments, based on the modified sulfide electrolyte, the mass percentage of dopant element M is 0.2% to 2%.
[0008] In some embodiments, the thickness of the coating layer is 1–20 nm.
[0009] In some embodiments, the coating layer includes one or more of LiAlO2 and Li3PO4.
[0010] In some embodiments, the coating layer is located on 90% to 100% of the substrate surface.
[0011] In some embodiments, the coating layer is located on 100% of the substrate surface.
[0012] In some embodiments, lithium transition metal oxides include those having the general formula Li a Ni b Co c M d O e D f One or more of the following materials, 0.8≤a≤1.2, 0.8≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Ge, Mo, Sn, Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and D includes one or more of N, F, S and Cl.
[0013] In some embodiments, lithium phosphates include those having the general formula Li z Fe (1-x) Mn x M y PO4 is one or more of the following materials; wherein x and y are natural numbers, with x ranging from 0 to 1 and y ranging from 0 to 0.1; z is from 0 to 1.1; M includes one or more metallic elements from Groups IVB, VB, VIII, IIA, IIIA, IVA and VA.
[0014] In some embodiments, sulfide electrolytes include those with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l The material, with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w Materials, Li 4-v Ge 1-v P vS4, one or more of Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from Se, Te, Cl, Br and I, 0<v<1, Me includes one or more elements selected from Si, Ge, Sn and Al.
[0015] In some embodiments, the positive electrode further comprises a positive electrode current collector, and the positive electrode film layer is located on at least one side of the positive electrode current collector.
[0016] In some embodiments, the positive electrode film layer further comprises a positive electrode conductive agent.
[0017] In some embodiments, the electrolyte layer comprises a sulfide electrolyte.
[0018] In some embodiments, the negative electrode comprises one or more of lithium, lithium alloys, natural graphite, artificial graphite, mesocarbon microbeads, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
[0019] In a second aspect, embodiments of the present application provide a battery device, comprising a plurality of the solid-state battery cells according to the first aspect.
[0020] In a third aspect, embodiments of the present application provide an electric device, comprising the solid-state battery cell according to the first aspect or the battery device according to the second aspect.
[0021] In a fourth aspect, embodiments of the present application provide a positive electrode, the positive electrode comprises a positive electrode film layer, the positive electrode film layer comprises a positive electrode active material and a modified sulfide electrolyte, the positive electrode active material comprises a matrix and a coating layer located on at least part of the surface of the matrix, the modified sulfide electrolyte comprises a doping element Me and a sulfide electrolyte; the matrix comprises one or more of lithium transition metal oxides and lithium-containing phosphates, the mismatch between the coating layer and the matrix is 0.5 to 3; the doping element Me comprises one or more of B, Si, Mo and W, and Me ions react with S in the sulfide electrolyte 2- to form a Me-S bond, and the bond energy of the Me-S bond is greater than 260 kJ / mol.
[0022] Fifthly, embodiments of this application provide a method for preparing a positive electrode, comprising a matrix including one or more of lithium transition metal oxides and lithium phosphates, and a modified sulfide electrolyte including a dopant element Me and a sulfide electrolyte, wherein the dopant element Me includes one or more of B, Si, Mo, and W, and the Me ions react with S in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol; a coating layer is formed on at least part of the surface of the substrate by atomic layer deposition to obtain the positive electrode active material, and the mismatch between the coating layer and the substrate is 0.5 to 3; after mixing the modified sulfide electrolyte and the positive electrode active material, the positive electrode is obtained.
[0023] In some embodiments, the atomic layer deposition process includes the following steps: placing a substrate in a reaction chamber, alternately introducing lithium precursor gas, aluminum or phosphorus precursor gas and oxygen precursor gas, causing the lithium precursor gas, aluminum or phosphorus precursor gas and oxygen precursor gas to react on at least a portion of the substrate surface, and depositing the reaction products on at least a portion of the substrate surface to form a coating layer, the coating layer including one or more of LiAlO2 and Li3PO4.
[0024] In some embodiments, the lithium precursor comprises lithium tert-butoxide.
[0025] In some embodiments, the aluminum precursor includes trimethylaluminum.
[0026] In some embodiments, the phosphorus precursor includes one or more of trimethylphosphorus and phosphine.
[0027] In some embodiments, the oxygen precursor includes ozone.
[0028] In some embodiments, the deposition temperature of the atomic layer deposition process is 150–250°C.
[0029] In some embodiments, providing a modified sulfide electrolyte includes the following steps: mixing a sulfide electrolyte and a Me source and then annealing the mixture under an inactive atmosphere to obtain a modified sulfide electrolyte.
[0030] In some embodiments, the Me source includes one or more of Li3BO3, B2S3, Li3BS3, Li2SiO3, SiS2, MoS2, Li2MoO4, WS2, and Li2WO.
[0031] In some embodiments, the Me source accounts for 0.5% to 10.0% of the total mass based on the sulfide electrolyte.
[0032] In some embodiments, the annealing temperature is 90–150°C. Attached Figure Description
[0033] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments of this application will be briefly introduced below. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0034] Figure 1 shows a schematic diagram of a solid-state battery cell provided in some embodiments of this application.
[0035] Figure 2 shows a schematic diagram of an electrical device provided in some embodiments of this application.
[0036] The accompanying drawings are not necessarily drawn to scale. Detailed Implementation
[0037] To better understand the above-mentioned objectives, features, and advantages of this application, the solution of this application will be further described below. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.
[0038] Many specific details are set forth in the following description in order to provide a full understanding of this application, but this application may also be implemented in other ways different from those described herein; obviously, the embodiments in the specification are only some embodiments of this application, and not all embodiments.
[0039] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the solid-state battery cell, battery device, power-consuming device, positive electrode, and preparation method thereof. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0040] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0041] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.
[0042] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.
[0043] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0044] Unless otherwise specified, in this application, the terms "first," "second," etc., are used to distinguish different objects, rather than to describe a specific order or primary / secondary relationship.
[0045] In this application, the terms "multiple" or "various" refer to two or more kinds.
[0046] In the description of the embodiments of this application, unless otherwise specified, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0047] Unless otherwise stated, the test temperature for all parameters mentioned in this application is 25°C.
[0048] The solid-state battery cells mentioned in the embodiments of this application can independently perform charging and discharging functions. Solid-state battery cells can be cylindrical, cuboid, or other shapes, and the embodiments of this application are not limited in this respect. Figure 1 shows a cuboid solid-state battery cell 5 as an example.
[0049] The battery apparatus mentioned in the embodiments of this application may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple solid-state battery cells, which are connected in series, parallel, or mixed connections via busbars.
[0050] In some embodiments, a battery cell assembly is typically formed by arranging multiple solid-state battery cells.
[0051] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple solid-state battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple solid-state battery cells together with cable ties.
[0052] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.
[0053] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.
[0054] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple solid-state battery cells to the housing.
[0055] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.
[0056] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells.
[0057] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.
[0058] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use solid-state battery cells and battery devices, such as, but not limited to, mobile devices (e.g., mobile phones, tablets, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc. Solid-state battery cells and battery devices are used to store or provide electrical energy.
[0059] Figure 2 is a schematic diagram of an example electrical device. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc.
[0060] The solid-state battery cells in this application may include coin cells, molded cells, hard-case cells, pouch cells, etc.
[0061] During cycling, transition metal ions in the positive electrode active material diffuse into the electrolyte, while anions such as sulfur and oxygen in the electrolyte diffuse back into the lattice of the positive electrode active material, forming an interdiffusion layer and a space charge layer at the solid-solid interface between the positive electrode active material and the electrolyte. This causes a surge in impedance at the interface, a significant polarization effect, and blocks the lithium-ion transport path; it also reduces the capacity of the positive electrode active material and the ionic conductivity of the electrolyte; and the byproducts formed by diffusion accelerate the degradation of the solid-solid interface.
[0062] In view of this, embodiments of this application provide a solid-state battery cell, a battery device, an electrical device, a positive electrode, and a method for preparing the same, wherein the solid-state battery cell using the positive electrode has good cycle performance.
[0063] The solid-state battery cell provided in this application includes a positive electrode, an electrolyte layer, and a negative electrode, with the electrolyte layer located between the positive and negative electrodes.
[0064] The positive electrode provided in this application includes a positive electrode film layer, which comprises a positive electrode active material and a modified sulfide electrolyte. The positive electrode active material includes a substrate and a coating layer located on at least a portion of the surface of the substrate. The modified sulfide electrolyte includes a dopant element Me and a sulfide electrolyte. The substrate includes one or more of lithium transition metal oxides and lithium phosphates. The mismatch between the coating layer and the substrate is 0.5 to 3. The dopant element Me includes one or more of B, Si, Mo, and W. The Me ions react with S ions in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol.
[0065] Modified sulfide electrolyte is a sulfide electrolyte used in the positive electrode of solid-state battery cells.
[0066] Mismatch refers to the difference in crystal structure parameters between the material in the coating layer and the matrix material.
[0067] This application, by providing a coating layer on at least a portion of the substrate surface and setting the mismatch between the coating layer and the substrate to 0.5–3, reduces dislocation accumulation at the interface between the coating layer and the substrate, thereby decreasing the likelihood of element diffusion along dislocation lines and consequently reducing the possibility of element diffusion into the sulfide electrolyte, thus improving the cycle performance of the solid-state battery cell. Simultaneously, by doping the sulfide electrolyte with specific elements, the application aims to improve the interaction between Me ions and S in the sulfide electrolyte. 2- It forms a strong Me-S covalent bond network, and the bond energy of the Me-S bond is greater than 260 kJ / mol, which can fix the S element in the sulfide electrolyte and reduce the possibility of S element diffusing into the matrix.
[0068] During cycling, certain elements incorporated into the sulfide electrolyte may diffuse into the substrate, which can reduce the cycle stability of solid-state battery cells. The coating layer designed in this application has a suitable mismatch with the substrate, reducing both the possibility of bulk elements in the sulfide electrolyte diffusing into the substrate and the possibility of dopant elements diffusing into the substrate, further improving the cycle performance of solid-state battery cells. Furthermore, the coating layer designed in this application has low affinity for specific dopant elements, reducing the possibility of interfacial byproducts forming between the coating layer and the dopant elements.
[0069] Therefore, the positive electrode active material and the modified sulfide electrolyte of this application can interact to jointly improve the cycle performance of solid-state battery cells.
[0070] The mismatch between the coating layer and the substrate can be tested using the following method:
[0071] The coated positive electrode active material was dispersed in anhydrous ethanol and observed under a high-resolution electron microscope (HRTEM). The lattice fringes of both the substrate and the coating layer were observed, and their lattice spacings were measured. The lattice mismatch degree between the two was then calculated using a formula: [Formula omitted for brevity] Where δ is the mismatch degree, d1 is the measured lattice spacing of the coating layer, and d2 is the measured lattice spacing of the matrix.
[0072] Optionally, the mismatch between the coating layer and the substrate is independently selected from any value of 0.5, 1.0, 1.5, 2.0, 2.5, 3.0 or a range between any two.
[0073] In some embodiments, based on the modified sulfide electrolyte, the mass percentage of dopant element M is 0.2% to 2%.
[0074] In this embodiment, by using appropriate doping amounts, a Me-S covalent bond network can be formed in the modified sulfide electrolyte, fixing the S element in the sulfide electrolyte and reducing the possibility of S element diffusing into the matrix; at the same time, it can reduce the possibility of doping elements blocking the ion transport channels in the modified sulfide electrolyte, thereby reducing the possibility of a decrease in the ionic conductivity of the modified sulfide electrolyte.
[0075] Optionally, the mass percentage of the dopant element M is independently selected from any value or a range between 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, and 2.0%.
[0076] In some embodiments, the thickness of the coating layer is 1–20 nm.
[0077] A coating layer of appropriate thickness can effectively isolate the sulfide electrolyte from direct contact with the substrate, reduce the possibility of side reactions at the interface, and has a certain mechanical strength to reduce the possibility of coating layer failure due to volume changes in the substrate during cycling; at the same time, it can also enable ions to have a lower migration path and improve the ionic conductivity of the positive electrode active material.
[0078] Optionally, the thickness of the coating layer is independently selected from any value or a range between 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, and 20nm.
[0079] In some embodiments, the coating layer includes one or more of LiAlO2 and Li3PO4.
[0080] Compared to coatings such as lithium niobate, the coating provided in this application has a lower mismatch degree with the substrate, which can result in less dislocation accumulation at the interface between the positive electrode active material and the modified sulfide electrolyte, thereby reducing the possibility of element diffusion along the dislocation line and further reducing interfacial side reactions between the substrate and the sulfide electrolyte, so as to improve the cycle performance of solid-state battery cells.
[0081] LiAlO2 has high oxidation stability and can withstand the high voltage environment of the positive electrode. As a coating layer, it can reduce the possibility of its own decomposition.
[0082] In some embodiments, the coating layer is located on 90% to 100% of the substrate surface.
[0083] Optionally, the coating layer is located on 95% to 100% of the substrate surface.
[0084] Alternatively, the coating layer may be located on 98% to 100% of the substrate surface.
[0085] In some embodiments, the coating layer is located on 100% of the substrate surface.
[0086] This can further reduce interfacial side reactions between the substrate and the sulfide electrolyte, reduce the decomposition of the sulfide electrolyte, and thus help to further improve the cycle performance of solid-state battery cells.
[0087] In some embodiments, lithium transition metal oxides include those having the general formula Li a Ni b Co c M d O e D f One or more of the following materials, 0.8≤a≤1.2, 0.8≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Ge, Mo, Sn, Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and D includes one or more of N, F, S and Cl.
[0088] As an example, lithium transition metal oxides may include, but are not limited to, LiNi. 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.80 Co 0.15 Al 0.05 O2, LiNi 0.9 Co 0.05 Mn 0.05O2(Ni90), LiNi 0.92 Co 0.04 Mn 0.04 O2(Ni92), LiNi 0.93 Co 0.035 Mn 0.035 O2(Ni93), LiNi 0.96 Co 0.02 Mn 0.02 One or more of O2 (Ni96).
[0089] In some embodiments, lithium phosphates include those having the general formula Li z Fe (1-x) Mn x M y PO4 is one or more of the following materials; wherein x and y are natural numbers, with x ranging from 0 to 1 and y ranging from 0 to 0.1; z is from 0 to 1.1; M includes one or more metallic elements from Groups IVB, VB, VIII, IIA, IIIA, IVA and VA.
[0090] As an example, lithium phosphates may include, but are not limited to, one or more of LiFePO4 and LiMnPO4.
[0091] During the charging and discharging process, solid-state battery cells undergo Li insertion / extraction and consumption, resulting in varying Li molar content at different discharge states. In the examples of cathode active material matrices in this application, the Li molar content represents the initial state of the material, i.e., the state before material feeding. When the cathode active material is applied to a solid-state battery cell, the Li molar content changes after charge-discharge cycles. Similarly, in the examples of cathode active materials in this application, the O molar content is only a theoretical value. Lattice oxygen release causes changes in the O molar content, and the actual O molar content will also fluctuate.
[0092] This application also provides a method for preparing the above-mentioned positive electrode.
[0093] The method for preparing the positive electrode includes the following steps: providing a matrix comprising one or more of lithium transition metal oxides and lithium phosphates; providing a modified sulfide electrolyte comprising a dopant element Me and the sulfide electrolyte, wherein the dopant element Me comprises one or more of B, Si, Mo, and W; and the Me ions react with S in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol; a coating layer is formed on at least part of the surface of the substrate by atomic layer deposition to obtain the positive electrode active material, and the mismatch between the coating layer and the substrate is 0.5 to 3; after mixing the modified sulfide electrolyte and the positive electrode active material, the positive electrode is obtained.
[0094] Atomic layer deposition (ALD) technology can be used to form a thin and uniform coating layer on the substrate surface.
[0095] The thickness of the coating layer can also be easily adjusted by using a pulsed introduction of precursor gas in a cyclical manner.
[0096] In some embodiments, the atomic layer deposition process includes the following steps: placing a substrate in a reaction chamber, alternately introducing lithium precursor gas, aluminum or phosphorus precursor gas and oxygen precursor gas, causing the lithium precursor gas, aluminum or phosphorus precursor gas and oxygen precursor gas to react on at least a portion of the substrate surface, and depositing the reaction products on at least a portion of the substrate surface to form a coating layer, the coating layer including one or more of LiAlO2 and Li3PO4.
[0097] After each precursor gas has been introduced, an inert gas is introduced for purging to remove unreacted precursor gases and reaction byproducts. Optionally, the inert gas may include one or more of neon, argon, and helium.
[0098] In some embodiments, the lithium precursor includes lithium tert-butoxide (LiOtBU).
[0099] In some embodiments, the aluminum precursor includes trimethylaluminum (TMA).
[0100] In some embodiments, the phosphorus precursor includes one or more of trimethylphosphorus and phosphine.
[0101] In some embodiments, the oxygen precursor includes ozone.
[0102] In some embodiments, the deposition temperature of the atomic layer deposition process is 150 to 250°C, for example, it can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or any range of the above values.
[0103] Optionally, the deposition temperature of the atomic layer deposition process is 150–200°C.
[0104] Providing a modified sulfide electrolyte includes the following steps: mixing the sulfide electrolyte and the Me source and then annealing them under an inactive atmosphere to obtain the modified sulfide electrolyte.
[0105] Inactive atmospheres include nitrogen and inert gases.
[0106] Me can be incorporated into sulfide electrolytes by annealing in an inactive atmosphere.
[0107] In some embodiments, the Me source includes a B source, which includes one or more of lithium borate (Li3BO3), boron sulfide (B2S3), and lithium thioborate (Li3BS3).
[0108] In some embodiments, the Me source includes a Si source, which includes one or more of lithium silicate (Li2SiO3) and silicon sulfide (SiS2).
[0109] In some embodiments, the Me source includes a Mo source, which includes one or more of molybdenum sulfide (MoS2) and lithium molybdate (Li2MoO4).
[0110] In some embodiments, the Me source includes a W source, which includes one or more of tungsten sulfide (WS2) and lithium tungstate (Li2WO).
[0111] Me sources can reduce the possibility of introducing impurities while achieving doping modification.
[0112] In some embodiments, based on the sulfide electrolyte, the mass percentage of the Me source is 0.5% to 10.0%. For example, it can be 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, or any range of the above values.
[0113] In some embodiments, mixing the sulfide electrolyte and the Me source includes a ball milling process.
[0114] In some embodiments, the annealing temperature is 90–150°C. For example, it can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or any range of the above values.
[0115] [positive electrode]
[0116] The positive electrode provided in this application includes a positive electrode film layer, which includes the positive electrode active material and the modified sulfide electrolyte of this application.
[0117] In some embodiments, the mass percentage of the positive electrode active material in the positive electrode film layer can be ≥60%, for example, ≥61%, ≥62%, ≥63%, ≥64%, ≥65%, ≥66%, ≥67%, ≥68%, ≥69%, ≥70%, ≥71%, ≥72%, ≥73%, ≥74%, ≥75%, ≥76%, ≥77%, ≥78%, ≥79%, or ≥80%.
[0118] The positive electrode film layer includes a modified sulfide electrolyte, and the modified sulfide electrolyte includes a doping element Me and a sulfide electrolyte. In some embodiments, the sulfide electrolyte includes a molecular formula of Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l , and a material with a molecular formula of Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w , one or more of Li 4-v Ge 1-v P v S4, Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from Se, Te, Cl, Br and I, 0<v<1, and Me includes one or more elements selected from Si, Ge, Sn and Al.
[0119] Optionally, the sulfide electrolyte may include a molecular formula of Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l .
[0120] By way of example, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, Li6GaGe2S10 One or more of them.
[0121] Optionally, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, or Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 5.5 PS 4.5 Br 1.5 One or more of them.
[0122] In some embodiments, the mass percentage of the modified sulfide electrolyte in the positive electrode film can be 5%-35%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, or any range of the above values.
[0123] Optionally, the mass percentage of the modified sulfide electrolyte in the positive electrode film can be 10%-35%, 15%-35%, 10%-30%, or 15%-30%.
[0124] In some embodiments, the positive electrode film layer further includes a positive electrode conductive agent.
[0125] Optionally, the positive electrode conductive agent may be one or more of the following, including but not limited to superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes (CNTs), graphene, carbon nanofibers, and vapor-grown carbon fibers (VGCF).
[0126] In some embodiments, the positive electrode film layer includes a positive electrode conductive agent, and the mass percentage of the positive electrode conductive agent in the positive electrode film layer can be 1%-10%, for example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any range of the above values.
[0127] In some embodiments, the positive electrode film layer may or may not include a positive electrode binder, and can be adjusted according to the positive electrode composition and the preparation process of the solid-state battery cell.
[0128] Optionally, the positive electrode binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, cis-butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0129] In some embodiments, the positive electrode film layer includes a positive electrode binder, and the mass percentage of the positive electrode binder in the positive electrode film layer can be 1% to 3%.
[0130] In some embodiments, the positive electrode further includes a positive current collector, and the positive electrode film layer is located on at least one side of the positive current collector.
[0131] The positive electrode current collector has two surfaces opposite each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0132] In some embodiments, the positive current collector may be a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, such as, but not limited to, stainless steel foil, carbon-coated aluminum foil, or aluminum foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. As an example, the metal layer may include, but is not limited to, one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene.
[0133] In some embodiments, the positive electrode may not require an additional positive current collector; for example, the stainless steel sheet of the mold battery can be directly used as the positive current collector.
[0134] The positive electrode can be prepared by either a dry process or a wet process.
[0135] [Electrolyte layer]
[0136] In some embodiments, the electrolyte layer comprises a solid electrolyte.
[0137] Optionally, the solid electrolyte includes a sulfide electrolyte.
[0138] Optionally, the sulfide electrolyte may include Li 6+m+l P 1-m Mm S 5-n+l N n Y 1-l material, with the molecular formula being Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w material, Li 4-v Ge 1-v P v S4, one or more of Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from Se, Te, Cl, Br and I, 0<v<1, Me includes one or more elements selected from Si, Ge, Sn and Al.
[0139] Optionally, the sulfide electrolyte may include a material with the molecular formula being Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l material.
[0140] As an example, the sulfide electrolyte may include one or more of Li6PS5Cl, Li6PS5Br, Li6PS5I, Li6PS5Cl 0.5 Br 0.5 , Li 5.5 PS 4.5 Cl 1.5 , Li 5.5 PS 4.5 Br 1.5 , Li 10 GeP2S 12 , Li3PS4, Li7P3S 11 , Li 3.25 Ge 0.25 P 0.75 S4, Li6GaGe2S 10 .
[0141] Optionally, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, or Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 5.5 PS 4.5 Br 1.5 Li 10 GeP2S 12 One or more of them.
[0142] In some embodiments, the electrolyte layer may or may not include a binder, depending on the manufacturing process of the solid-state battery cell. Optionally, the binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0143] The electrolyte layer can be prepared by a dry process or a wet process.
[0144] [negative electrode]
[0145] In some embodiments, the negative electrode may include one or more of lithium, lithium alloy, natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
[0146] In some embodiments, the negative electrode can be a metal sheet, such as a lithium sheet or a lithium alloy sheet.
[0147] Optionally, other elements in the lithium alloy sheet may include, but are not limited to, one or more of In, Mg, Al, Zn, Sn, Ag, Au, Ga, Pt, and Fe.
[0148] Alternatively, the lithium alloy sheet may include, but is not limited to, InLi alloy sheet, Li-Mg alloy sheet, Li-Al alloy sheet, Li-Zn alloy sheet, Li-Fe alloy sheet, etc.
[0149] In some embodiments, the negative electrode may include a negative electrode current collector and a lithium-based metal layer located on at least one surface of the negative electrode current collector. The lithium-based metal layer may be metallic lithium or a lithium alloy. The negative electrode current collector has two surfaces opposite each other in its thickness direction, and the lithium-based metal layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0150] Optionally, other elements in the lithium alloy may include, but are not limited to, one or more of In, Mg, Al, Zn, Sn, Ag, Au, Ga, Pt, and Fe.
[0151] Alternatively, the lithium alloy may include, but is not limited to, InLi alloy, Li-Mg alloy, Li-Al alloy, Li-Zn alloy, Li-Fe alloy, etc.
[0152] In some embodiments, the negative electrode may include a negative electrode current collector and a negative electrode film layer located on at least one side of the negative electrode current collector, the negative electrode film layer including a negative electrode active material. The negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0153] Optionally, the negative electrode active material may include, but is not limited to, one or more of the following: natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
[0154] Optionally, the silicon-based material may include, but is not limited to, one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Optionally, the tin-based material may include, but is not limited to, one or more of elemental tin, tin oxide, and tin alloys. Optionally, the metal oxide may include, but is not limited to, one or more of TiO2, MoO2, In2O3, Al2O3, Cu2O, VO2, Ga2O3, Sb2O5, and Bi2O5.
[0155] In some embodiments, the negative electrode film layer may also include a negative electrode binder, or it may not include a negative electrode binder, which can be adjusted according to the negative electrode composition and the preparation process of the solid-state battery cell.
[0156] Optionally, the negative electrode binder may include, but is not limited to, one or more of the following: styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, polyacrylic acid, polymethacrylic acid, sodium polyacrylate, polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), carboxymethyl chitosan (CMCS), methyl vinyl silicone rubber, nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), thermoplastic styrene-butadiene rubber (SBS), isoprene rubber, cis-butadiene rubber (BR), ethyl cellulose, fluororubber, and acrylate rubber.
[0157] In some embodiments, the negative electrode film layer may further include a negative electrode conductive agent, or may not include a negative electrode conductive agent.
[0158] Optionally, the negative electrode conductive agent may include, but is not limited to, one or more of super conductive carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes (CNT), graphene, carbon nanofibers, and vapor grown carbon fibers (VGCF).
[0159] In some embodiments, the negative electrode film layer may further include a solid electrolyte, or may not include a solid electrolyte.
[0160] Optionally, the solid electrolyte may include a sulfide electrolyte.
[0161] Optionally, the sulfide electrolyte may include a material with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l , a material with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w , one or more of Li 4-v Ge 1-v P v S4, Li2S-P2S5 based materials, Li2S-SiS2 based materials, Li2S-MeS-P2S5 based materials, and LiGeGaS based materials, where 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from Se, Te, Cl, Br and I, 0<v<1, and Me includes one or more selected from Si, Ge, Sn and Al.
[0162] Optionally, the sulfide electrolyte may include a material with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l .
[0163] As an example, sulfide electrolytes may include Li6PS5Cl, Li6PS5Br, Li6PS5I, and Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 5.5 PS 4.5 Br 1.5 Li 10 GeP2S 12 Li3PS4, Li7P3S 11 Li 3.25 Ge 0.25 P 0.75 S4, Li6GaGe2S 10 One or more of them.
[0164] Optionally, the sulfide electrolyte may include Li6PS5Cl, Li6PS5Br, Li6PS5I, or Li6PS5Cl. 0.5 Br 0.5 Li 5.5 PS 4.5 Cl 1.5 Li 5.5 PS 4.5 Br 1.5 Li 10 GeP2S 12 One or more of them.
[0165] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. The metal foil may be a pure metal, an alloy, or a surface-treated metal, such as, but not limited to, stainless steel foil, copper foil, and nickel foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. As an example, the metal layer may include, but is not limited to, one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymer substrate may include, but is not limited to, one or more of polypropylene, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene, and polyethylene.
[0166] The negative electrode does not require an additional negative current collector; for example, the stainless steel sheet of a mold battery can be used directly as the negative current collector.
[0167] The negative electrode can be prepared by either a dry process or a wet process.
[0168] In some embodiments, the solid-state battery cell may further include an outer packaging for accommodating the electrode assembly formed by assembling the negative electrode, electrolyte layer, and positive electrode. The outer packaging may be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging may also be a flexible package, such as a pouch. The material of the flexible package may be plastic, such as one or more of aluminum-plastic film, polypropylene, polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0169] The methods for preparing solid-state battery cells are well known. For example, the assembly methods of solid-state battery cells include, but are not limited to, coin cells, molded cells, hard-case cells, and pouch cells.
[0170] Example
[0171] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on mass, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0172] Example 1
[0173] Preparation of positive electrode active materials
[0174] Atomic layer deposition process was used on LiNi substrate. 0.8 Co 0.1 Mn 0.1 A LiAlO2 coating layer is formed on the O2 surface.
[0175] LiNi matrix 0.8 Co 0.1 Mn 0.1 O2 was placed in the reaction chamber, and trimethylaluminum gas, lithium tert-butoxide (LiOtBU) gas, and ozone gas were alternately introduced to react on the substrate surface, causing the reaction products to deposit on the substrate surface to form a LiAlO2 coating layer. After each precursor gas was introduced, nitrogen gas was introduced for purging to remove unreacted precursor gases and reaction byproducts. The deposition temperature was 180℃. The coating layer thickness was adjusted to 2 nm using a pulsed, cyclical introduction of precursor gases.
[0176] Preparation of modified sulfide electrolytes
[0177] The sulfide electrolyte Li7P3S 11 The mixture was ball-milled with source B, Li3BS3, and the mass of source B, Li7P3S, was used as the sulfide electrolyte. 11The mixture was 1% by mass, ball-milled at 400 rpm for 12 hours. It was then annealed at 110℃ under an argon atmosphere to obtain a modified sulfide electrolyte doped with boron ions.
[0178] Preparation of solid-state battery cells
[0179] The above-prepared positive electrode active material, modified sulfide electrolyte doped with B ions, and vapor-grown carbon fiber (VGCF) positive electrode conductive agent were mixed at a mass ratio of 70:27:3; then 1% of the total mass of the positive electrode active material and modified sulfide electrolyte doped with B ions as binder polytetrafluoroethylene (PTFE) was added, and the positive electrode film was formed using a roll forming machine.
[0180] Solid-state battery cells are assembled using a 10mm diameter solid-state battery cell mold: 100mg of sulfide electrolyte Li6PS5Cl is added to the solid-state battery cell mold and flattened to form an electrolyte layer; then 100mg of a mixture of Li6PS5Cl and indium powder in a mass ratio of 70:30 is added to one side of the electrolyte layer, flattened, and then a layer of lithium foil is applied and pressed together; then the prepared positive electrode film layer is installed on the other side of the electrolyte layer, and finally the solid-state battery cell mold is pressurized to obtain the solid-state battery cell.
[0181] Performance testing
[0182] Cyclic performance was tested using the Xinwei Battery Testing System.
[0183] At 25°C, the solid-state battery cell was charged to 4.3V (vs. Li+ / Li) at a current density of 0.1C, left to stand for 10 minutes, and then discharged to 2.6V (vs. Li+ / Li) at a current density of 0.1C.
[0184] The initial discharge specific capacity at 0.1C current density (mAh / g) = the initial discharge capacity at 0.1C current density C1 / the mass of the positive electrode active material.
[0185] Then, the solid-state battery cell is charged to 4.3V (vs. Li+ / Li) at a current density of 0.1C, left to stand for 10 minutes, and then discharged to 2.6V (vs. Li+ / Li) at a current density of 0.1C. The discharge capacity at this point is recorded as the first discharge capacity at a current density of 0.1C. The first coulombic efficiency (%) at a current density of 0.1C = the first discharge capacity at a current density of 0.1C / the first charge capacity at a current density of 0.1C. The solid-state battery cell is then cycled through a current density of 0.1C according to the above charge and discharge process.
[0186] The capacity retention rate of a solid-state battery cell after 200 cycles at a current density of 0.3C = discharge capacity after 200 cycles at a current density of 0.3C / initial discharge capacity at a current density of 0.3C × 100%. The higher this value, the better the cycle performance of the solid-state battery cell.
[0187] Methods for testing mismatch:
[0188] The coated positive electrode active material was dispersed in anhydrous ethanol and observed under a high-resolution electron microscope (HRTEM). The lattice fringes of both the substrate and the coating layer were observed, and their lattice spacings were measured. The lattice mismatch degree between the two was then calculated using a formula: [Formula omitted for brevity] Where δ is the mismatch degree, d1 is the measured lattice spacing of the coating layer, and d2 is the measured lattice spacing of the matrix.
[0189] Examples 2-9
[0190] The preparation methods for the positive electrode active material, the modified sulfide electrolyte, the solid-state battery cell, and the performance testing methods are the same as in Example 1, with the only differences being the thickness of the coating layer and the amount of B-source Li3BS3 added. See Table 1 for details.
[0191] Comparative Example 1
[0192] The preparation and performance testing of the solid-state battery cells were the same as in Example 1, except that the substrate LiNi was not used. 0.8 Co 0.1 Mn 0.1 O2 coating does not affect the sulfide electrolyte Li7P3S 11 Doping modification is performed.
[0193] Comparative Example 2
[0194] The preparation of the modified sulfide electrolyte, the preparation of the solid-state battery cell, and the performance testing were the same as in Example 1, except that the substrate LiNi was not used. 0.8 Co 0.1 Mn 0.1 O2 is used for coating.
[0195] Comparative Example 3
[0196] The preparation of the positive electrode active material, the preparation of the solid-state battery cell, and the performance testing were the same as in Example 1, except that the sulfide electrolyte Li7P3S was not used. 11 Doping modification is performed.
[0197] Table 1
[0198] Examples 1-9 disclose the use of LiAlO2 to treat LiNi matrix 0.8 Co 0.1 Mn 0.1 After coating with O2, a positive electrode active material is obtained, and then the sulfide electrolyte Li7P3S is applied. 11 Modified sulfide electrolytes were obtained by boron doping; while Comparative Example 1 disclosed a LiNi matrix without coating modification. 0.8 Co 0.1 Mn 0.1 O2 and undoped sulfide electrolyte Li7P3S 11 Comparative Example 2 discloses a LiNi matrix without coating modification. 0.8 Co 0.1 Mn 0.1 O2 and the sulfide electrolyte Li7P3S 11 Modified sulfide electrolytes were obtained by boron doping; Comparative Example 3 discloses the use of LiAlO2 to modify the LiNi matrix. 0.8 Co 0.1 Mn 0.1 After O2 coating, a positive electrode active material and an unmodified sulfide electrolyte Li7P3S are obtained. 11 As shown in Table 1, the positive electrode active materials and modified sulfide electrolytes disclosed in Examples 1-9 can interact with each other to jointly improve the cycle performance of solid-state battery cells.
[0199] Example 10, Comparative Examples 4-5
[0200] The preparation and performance testing methods for solid-state battery cells are the same as in Example 1, with the differences being in the preparation of the positive electrode active material and the modified sulfide electrolyte. The only differences are in the type of coating layer and the types of doping elements. See Table 2 for details.
[0201] Table 2
[0202] In Examples 1 and 10, LiAlO2 was used to treat the LiNi matrix. 0.8 Co 0.1 Mn 0.1 After coating with O2, a positive electrode active material is obtained, and then the sulfide electrolyte Li7P3S is applied. 11 Modified sulfide electrolytes were obtained by doping with B and Mo respectively; while Comparative Example 4 discloses the use of LiAlO2 to modify the LiNi matrix. 0.8 Co 0.1 Mn 0.1 O2 is coated, and then the sulfide electrolyte Li7P3S is... 11 Sb doping modification was performed separately; Comparative Example 5 discloses the use of Al2O3 to modify the LiNi matrix.0.8 Co 0.1 Mn 0.1 O2 is coated, and then the sulfide electrolyte Li7P3S is... 11 Boron doping was performed separately. Table 2 shows that in Comparative Example 4, the Sb-S bond energy formed between the dopant element and S in the sulfide electrolyte is low, allowing S to easily diffuse into the positive electrode active material; while in Comparative Example 5, the coating layer is Al2O3, which, along with the LiNi matrix, forms a bond with low energy. 0.8 Co 0.1 Mn 0.1 O2 has a high degree of mismatch, and the element will diffuse along the mismatch line, thereby reducing the good cycle performance of solid-state battery cells.
[0203] The above description is merely a specific implementation of this application. Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the specific working processes of the systems, modules, and units described above can be referred to the corresponding processes in the foregoing method embodiments, and will not be repeated here. It should be understood that the protection scope of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be covered within the protection scope of this application.
Claims
1. A solid-state battery cell, comprising a positive electrode, an electrolyte layer, and a negative electrode, wherein the electrolyte layer is located between the positive electrode and the negative electrode. The positive electrode includes a positive electrode film layer, the positive electrode film layer includes a positive electrode active material and a modified sulfide electrolyte, the positive electrode active material includes a substrate and a coating layer located on at least a portion of the surface of the substrate, and the modified sulfide electrolyte includes a dopant element Me and a sulfide electrolyte. The substrate comprises one or more of lithium transition metal oxides and lithium phosphates, and the mismatch between the coating layer and the substrate is 0.5 to 3. The doping element Me includes one or more of B, Si, Mo, and W, and the Me ions react with S in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol.
2. The solid-state battery cell according to claim 1, wherein, Based on the modified sulfide electrolyte, the mass percentage of the dopant element M is 0.2% to 2%.
3. The solid-state battery cell according to claim 1 or 2, wherein, The thickness of the coating layer is 1–20 nm.
4. The solid-state battery cell according to any one of claims 1-3, wherein, The coating layer includes one or more of LiAlO2 and Li3PO4.
5. The solid-state battery cell according to any one of claims 1-4, wherein, The coating layer is located on 90% to 100% of the surface of the substrate.
6. The solid-state battery cell according to any one of claims 1-5, wherein, The coating layer is located on 100% of the surface of the substrate.
7. The solid-state battery cell according to any one of claims 1-6, wherein, The lithium transition metal oxide includes those having the general formula Li a Ni b Co c M d O e D f One or more of the following materials, 0.8≤a≤1.2, 0.8≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more of Ge, Mo, Sn, Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, D includes one or more of N, F, S and Cl; and / or, The lithium-containing phosphate includes those having the general formula Li z Fe (1-x) Mn x M y One or more of the following materials containing PO4; wherein x and y are natural numbers, with x ranging from 0 to 1 and y ranging from 0 to 0.1; z ranging from 0 to 1.1; M including one or more metallic elements from Groups IVB, VB, VIII, IIA, IIIA, IVA, and VA; and / or, The sulfide electrolyte includes a material with the molecular formula Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l , a material with the molecular formula Li 10±δ Ge 1-g G g P 2-q Q q S 12-w W w , one or more of Li 4-v Ge 1-v P v S4, Li2S-P2S5-based materials, Li2S-SiS2-based materials, Li2S-MeS-P2S5-based materials, and LiGeGaS-based materials, where 0≤m<1, 0≤n<1, -1<l<1, M includes one or more elements selected from Ge, Si, Sn, Al, Zr and Sb, N includes one or more elements selected from Se and Te, Y includes one or more elements selected from Cl, Br and I, 0≤δ<1, 0≤g≤1, 0≤q≤2, 0≤w<1, G includes one or two elements selected from Si and Sn, Q includes Sb, W includes one or more elements selected from Se, Te, Cl, Br and I, 0<v<1, and Me includes one or more elements selected from Si, Ge, Sn and Al.
8. The solid-state battery cell according to any one of claims 1-7, wherein, The positive electrode further includes a positive electrode current collector, and the positive electrode film layer is located on at least one side of the positive electrode current collector; and / or, The positive electrode film layer further includes a positive electrode conductive agent; and / or, The electrolyte layer includes a sulfide electrolyte; and / or, The negative electrode includes one or more of lithium, lithium alloy, natural graphite, artificial graphite, mesophase micro carbon spheres, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, and metal oxides.
9. A battery device comprising a plurality of solid-state battery cells according to any one of claims 1-8.
10. An electrical device comprising a solid-state battery cell according to any one of claims 1-8 or a battery device according to claim 9.
11. A positive electrode, The positive electrode includes a positive electrode film layer, the positive electrode film layer includes a positive electrode active material and a modified sulfide electrolyte, the positive electrode active material includes a substrate and a coating layer located on at least a portion of the surface of the substrate, and the modified sulfide electrolyte includes a dopant element Me and a sulfide electrolyte. The substrate comprises one or more of lithium transition metal oxides and lithium phosphates, and the mismatch between the coating layer and the substrate is 0.5 to 3. The doping element Me includes one or more of B, Si, Mo, and W, and the Me ions react with S in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol.
12. A method for preparing a positive electrode, A matrix is provided, the matrix comprising one or more of lithium transition metal oxides and lithium-containing phosphates. A modified sulfide electrolyte is provided, the modified sulfide electrolyte comprising a dopant element Me and a sulfide electrolyte, wherein the dopant element Me comprises one or more of B, Si, Mo, and W, and the Me ions react with S in the sulfide electrolyte. 2- Me-S bonds are formed, and the bond energy of the Me-S bonds is greater than 260 kJ / mol; A coating layer is formed on at least a portion of the surface of the substrate by atomic layer deposition to obtain a positive electrode active material, wherein the mismatch between the coating layer and the substrate is 0.5 to 3. The modified sulfide electrolyte and the positive electrode active material are mixed to obtain the positive electrode.
13. The preparation method according to claim 12, wherein, The atomic layer deposition process includes the following steps: The substrate is placed in a reaction chamber, and lithium precursor gas, aluminum or phosphorus precursor gas and oxygen precursor gas are alternately introduced to react with at least a portion of the surface of the substrate, and the reaction products are deposited on at least a portion of the surface of the substrate to form a coating layer, the coating layer comprising one or more of LiAlO2 and Li3PO4.
14. The preparation method according to claim 13, wherein, The lithium precursor includes lithium tert-butoxide; and / or The aluminum precursor includes trimethylaluminum; and / or, The phosphorus precursor includes one or more of trimethylphosphine and phosphine; and / or, The oxygen precursor includes ozone; and / or, The deposition temperature of the atomic layer deposition process is 150–250°C.
15. The preparation method according to any one of claims 12-14, wherein, Providing a modified sulfide electrolyte includes the following steps: The modified sulfide electrolyte was obtained by mixing the sulfide electrolyte and the Me source and then annealing it under an inactive atmosphere.
16. The preparation method according to claim 15, wherein, Me sources include one or more of Li3BO3, B2S3, Li3BS3, Li2SiO3, SiS2, MoS2, Li2MoO4, WS2, and Li2WO; and / or, Based on the sulfide electrolyte, the Me source comprises 0.5% to 10.0% by mass; and / or, The annealing temperature is 90–150℃.