Anti-aging agent composition, rubber composition and rubber article
By using an antioxidant composition of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine, N,N′-xylyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline polymer in a rubber composition, the shortcomings of existing antioxidants in dynamic fatigue resistance and thermo-oxidative aging heat generation are solved, thereby improving the flexural fatigue resistance of tires and reducing aging heat generation.
Patent Information
- Application Number
- PCT/CN2026/078603
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-02-11
- Publication Date
- 2026-11-12
AI Technical Summary
Existing antioxidants are not effective enough in improving the dynamic fatigue resistance of tire bead areas and reducing the heat generated by thermo-oxidative aging. Furthermore, some antioxidants, such as 6PPD, pose potential risks to the environment and human health.
An antioxidant composition of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine, N,N′-xylyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline polymer is used in rubber compositions to improve the flexural fatigue resistance of tires and reduce aging heat generation.
It significantly improves the flexural fatigue resistance of rubber products, reduces the flexural temperature rise after aging, extends tire service life, and enhances safety.
Smart Images

Figure PCTCN2026078603-FTAPPB-I100001 
Figure PCTCN2026078603-FTAPPB-I100002 
Figure PCTCN2026078603-FTAPPB-I100003
Abstract
Description
Antioxidant compositions, rubber compositions and rubber products Technical Field
[0001] This invention belongs to the field of rubber chemical industry, and specifically relates to an antioxidant composition, a rubber composition, and rubber products. Background Technology
[0002] During vehicle operation, the rim area experiences significant heat generation due to the pressure and cyclical forces exerted by the tire bead, coupled with the inherent hysteresis effect of the rubber. This heat can negatively impact tire safety and reduce its lifespan. With societal development and advancements in the automotive industry, the demands on tires are increasing. As a rubber product, tires undergo cyclical rolling during vehicle operation. During this rolling, the contact area between the tire bead and the tire experiences cyclical dynamic forces. Due to the tire's hysteresis effect, a large amount of heat rapidly accumulates in the bead area. After reaching high temperatures, the rubber material undergoes thermo-oxidative aging, reducing its strength and leading to problems such as bead cracking, delamination, and bulges. Therefore, it is necessary to improve the dynamic fatigue resistance and strength of the bead material components and reduce dynamic heat generation to mitigate the impact of heat generated by the tire's hysteresis effect on tire safety and lifespan. To this end, we need to add antioxidants to tires to improve their dynamic performance and reduce the impact of thermo-oxidative aging.
[0003] Existing comprehensive antioxidants offer relatively balanced protection across various properties, but they are not particularly effective in improving dynamic fatigue resistance and reducing heat generation after thermo-oxidative aging. Using aminopyridine antioxidants can effectively improve the dynamic fatigue resistance of tire rubber materials and reduce heat generation. Other properties, such as physical properties, can also be maintained in line with existing comprehensive antioxidants. This provides a significant improvement in addressing tire bead damage issues that occur during tire use.
[0004] 6PPD is a widely used antioxidant, but according to a 2021 article published in *Science*, the culprit behind the death of salmon is N-(1,3-dimethylbutyl)-N′-phenyl-p-phenylenediamine-quinone (6PPD-quinone), released from tire wear particles. 6PPD is a precursor to this substance. Previously, Professor Cai Zongwei's team at Hong Kong Baptist University published several articles reporting the widespread distribution of six emerging PPDs and their derivatives (6PPD-quinone) in Chinese cities, with a total detection rate as high as 81%. Furthermore, based on measured environmental concentrations, the annual intake of PPDs and 6PPD-quinone by adults is not low, indicating that long-term exposure to these pollutants may pose a significant risk to human health.
[0005] Therefore, there is an urgent need in this field to develop a new type of antioxidant. Summary of the Invention
[0006] The purpose of this invention is to provide an antioxidant composition, a rubber composition, and a rubber article.
[0007] In a first aspect, the present invention provides an antioxidant composition comprising 5-[(4-methylpentan-2-yl)amino]-2-(phenylamino)pyridine, N,N′-xylyl-p-phenylenediamine, and a 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
[0008] In one or more embodiments, the antioxidant composition contains 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine in a mass ratio of 1:(0.1-2) to N,N′-xylyl-p-phenylenediamine; and / or, the antioxidant composition contains 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine in a mass ratio of 1:(0.1-2) to 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
[0009] In a second aspect, the present invention provides a rubber composition comprising 100 parts by weight of a diene elastomer and 2-10 parts by weight of the antioxidant composition described in the first aspect of the present invention.
[0010] In one or more embodiments, the raw materials of the rubber composition include 3-5 parts by weight of the antioxidant composition.
[0011] In one or more embodiments, the diene elastomer is selected from one or more of natural rubber, butadiene rubber, styrene-butadiene rubber and polyisoprene; preferably, the diene elastomer is natural rubber.
[0012] In one or more embodiments, the raw materials of the rubber composition further include 10-70 parts by weight of reinforcing filler; preferably, the reinforcing filler is carbon black.
[0013] In one or more embodiments, the raw materials of the rubber composition further include 1-6 parts by weight of a crosslinking agent; preferably, the crosslinking agent is sulfur.
[0014] In one or more embodiments, the raw materials of the rubber composition further include 1-10 parts by weight of an activator; preferably, the activator is zinc oxide.
[0015] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of cobalt salt.
[0016] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of a tackifying resin.
[0017] In one or more embodiments, the raw materials of the rubber composition further include 0.1-6 parts by weight of a rubber binder; preferably, the rubber binder is a petroleum resin.
[0018] In one or more embodiments, the raw materials of the rubber composition further include 0.1-10 parts by weight of a softener; preferably, the softener is stearic acid and / or naphthenic oil.
[0019] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of an accelerator; preferably, the accelerator is N-tert-butyl-2-benzothiazole sulfenamide.
[0020] In one or more embodiments, the raw materials of the rubber composition further include 1-10 parts by weight of a plasticizer; preferably, the plasticizer is an environmentally friendly oil.
[0021] In a third aspect, the present invention provides a rubber article made from the rubber composition described in the second aspect of the present invention; preferably, the rubber article is a tire.
[0022] In a fourth aspect, the present invention provides a method for reducing the toxicity of rubber products, improving the flexural fatigue resistance of rubber products, reducing the heat generation during aging of rubber products, and / or improving the heat resistance of rubber products, the method comprising adding the antioxidant composition of the first aspect of the present invention to the raw materials of the rubber composition for preparing the rubber product; or the method comprising preparing the rubber product using the rubber composition of the second aspect of the present invention.
[0023] In one or more embodiments, the raw materials of the rubber composition include 100 parts by weight of a diene elastomer and 2-10 parts by weight of the antioxidant composition according to claim 1 or 2.
[0024] In one or more embodiments, the raw materials of the rubber composition include 3-5 parts by weight of the antioxidant composition.
[0025] In one or more embodiments, the diene elastomer is selected from one or more of natural rubber, butadiene rubber, styrene-butadiene rubber and polyisoprene; preferably, the diene elastomer is natural rubber.
[0026] In one or more embodiments, the raw materials of the rubber composition further include 10-70 parts by weight of reinforcing filler; preferably, the reinforcing filler is carbon black.
[0027] In one or more embodiments, the raw materials of the rubber composition further include 1-6 parts by weight of a crosslinking agent; preferably, the crosslinking agent is sulfur.
[0028] In one or more embodiments, the raw materials of the rubber composition further include 1-10 parts by weight of an activator; preferably, the activator is zinc oxide.
[0029] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of cobalt salt.
[0030] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of a tackifying resin.
[0031] In one or more embodiments, the raw materials of the rubber composition further include 0.1-6 parts by weight of a rubber binder; preferably, the rubber binder is a petroleum resin.
[0032] In one or more embodiments, the raw materials of the rubber composition further include 0.1-10 parts by weight of a softener; preferably, the softener is stearic acid and / or naphthenic oil.
[0033] In one or more embodiments, the raw materials of the rubber composition further include 0.1-3 parts by weight of an accelerator; preferably, the accelerator is N-tert-butyl-2-benzothiazole sulfenamide.
[0034] The raw materials of the rubber composition also include 1-10 parts by weight of a plasticizer; preferably, the plasticizer is an environmentally friendly oil.
[0035] The present invention has the following beneficial effects:
[0036] Rubber products made using the antioxidant composition or rubber composition of the present invention have significantly improved flexural fatigue resistance, and their flexural temperature rise after aging is also greatly reduced. Detailed Implementation
[0037] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0038] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0039] In this document, the terms “contains,” “includes,” “containing,” and similar terms encompass the meanings of “basically composed of” and “composed of.” For example, when this document discloses “A contains B and C,” “A is basically composed of B and C” and “A is composed of B and C” should be considered as having been disclosed in this document.
[0040] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0041] Unless otherwise specified, percentages refer to mass percentages and proportions refer to mass ratios in this article.
[0042] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples. Rather, all alternatives, modifications, and equivalents of the methods and materials described herein are covered within the scope defined by the claims.
[0043] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0044] The antioxidant compounds in the antioxidant compositions of the present invention have the structures shown in Table a below.
[0045] Table a
[0046] The antioxidant composition of the present invention includes the three antioxidant compounds shown in Table a. Rubber products made using the antioxidant composition of the present invention significantly improve the dynamic fatigue resistance of rubber materials and can reduce aging heat generation, thereby extending the service life of rubber products (such as tires) and improving the safety of rubber products (such as tires) during use.
[0047] The antioxidant composition of the present invention comprises 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine, N,N′-xylyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
[0048] In some embodiments, the antioxidant composition contains 5-[(4-methylpentan-2-yl)amino]-2-(phenylamino)pyridine in a mass ratio of 1:(0.1-2), for example 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.7, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, preferably 1:(0.1-1), 1:(0.1-0.8), 1:(0.1-0.7), 1:(0.1-0.6), 1:(0.1-0.5), 1:(0.2-0.5), 1:(0.3-0.4).
[0049] In some embodiments, the antioxidant composition contains 5-[(4-methylpentan-2-yl)amino]-2-(phenylamino)pyridine in a mass ratio of 1:(0.1-2) to the 2,2,4-trimethyl-1,2-dihydroquinoline polymer, for example, 1:0.1, 1:0.2, 1:0.3, 1:0.5, 1:0.7, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, preferably 1:(0.1-1), 1:(0.1-0.8), 1:(0.1-0.7), 1:(0.1-0.6), 1:(0.1-0.5), 1:(0.2-0.5), or 1:(0.3-0.4).
[0050] This invention provides a rubber composition. In some embodiments, the raw materials of the rubber composition include 100 parts by weight of a diene elastomer and 2-10 parts by weight of the antioxidant composition of this invention. Preferably, the raw materials of the rubber composition include 3-5 parts by weight of the antioxidant composition.
[0051] In this document, diene elastomers refer to elastomers whose monomers comprise dienes (such as butadiene or isoprene). Diene elastomers suitable for use in this invention can be various diene elastomers known in the art, including but not limited to one or more selected from natural rubber (NR), butadiene rubber (BR), isoprene rubber, styrene-butadiene rubber (SBR), chloroprene rubber (CR), nitrile rubber (NBR), polyisoprene, isoprene / butadiene copolymers, isoprene / styrene copolymers, and isoprene / butadiene / styrene copolymers. In some preferred embodiments, the diene elastomer comprises or is composed of natural rubber. Examples of natural rubber include SCR5.
[0052] The raw materials for the rubber composition of the present invention may further include reinforcing fillers. The amount of reinforcing filler in the raw materials of the rubber composition of the present invention may be 10-70 parts by weight, for example 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, or 70 parts by weight. The reinforcing fillers suitable for the present invention may be conventional reinforcing fillers used in rubber compositions, including but not limited to one or more selected from carbon black, silica, titanium dioxide, calcium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, clay, and talc. In some embodiments, the reinforcing filler comprises carbon black. Examples of carbon black include one or both of carbon black N326 and carbon black N330.
[0053] The raw materials of the rubber composition of the present invention may further include a crosslinking agent, such as sulfur. The sulfur is preferably insoluble sulfur. In the raw materials of the rubber composition of the present invention, the amount of sulfur can be 1-6 parts by weight, preferably 4-6 parts by weight, for example 4.5 parts by weight, 4.6 parts by weight, or 5 parts by weight.
[0054] The raw materials for the rubber composition of the present invention may also include other components that can be used in the rubber composition, including but not limited to one or more selected from activators, cobalt salts, plasticizers, tackifying resins, rubber adhesives, softeners and accelerators.
[0055] Activators can accelerate vulcanization, improve the thermal conductivity, abrasion resistance, and tear resistance of rubber products. The raw materials of the rubber composition of the present invention preferably include activators. Examples of activators include ZnO. In the raw materials of the rubber composition of the present invention, the amount of activator can be 1-10 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, or 10 parts by weight. In some preferred embodiments, the activator includes ZnO, or the activator is ZnO. In some preferred embodiments, the amount of ZnO in the raw materials of the rubber composition of the present invention is 7-9 parts by weight or 1-3 parts by weight, for example, 3 parts by weight or 8 parts by weight.
[0056] Cobalt salts can effectively promote the adhesion of rubber to steel cords. When used as a tire belt layer compound, the raw materials of the rubber composition of the present invention preferably include cobalt salts. Cobalt salts that can be used in the present invention include, but are not limited to, cobalt borylate and cobalt neodecanoate. In the raw materials of the rubber composition of the present invention, the amount of cobalt salt can be 0.1-3 parts by weight, preferably 0.1-1 parts by weight, for example, 0.2 parts by weight, 0.5 parts by weight, or 0.8 parts by weight.
[0057] The tackifying resin is used to enhance the adhesion between the rubber and the steel cord. When used as a tire belt layer compound, the raw materials of the rubber composition of the present invention preferably include a tackifying resin. Suitable tackifying resins include resorcinol donors, such as resorcinol-80. The mass fraction of resorcinol-80 is ≥80%. In the raw materials of the rubber composition of the present invention, the amount of tackifying resin can be 0.1-3 parts by mass, preferably 0.5-2.5 parts by mass, for example 1 part by mass, 1.5 parts by mass, 1.9 parts by mass, or 2 parts by mass.
[0058] Rubber adhesives are substances that can improve the tackiness of rubber materials. The raw materials of the rubber composition of the present invention preferably include a rubber adhesive, which is preferably a petroleum resin, such as C9 resin. The amount of rubber adhesive used in the raw materials of the rubber composition of the present invention can be 0.1 to 6 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, or 6 parts by weight.
[0059] Softeners can be used to improve the processing properties of rubber compositions. Softeners may include petroleum-based softeners, such as naphthenic oils, aromatic oils, processing oils, lubricating oils, paraffin wax, liquid paraffin wax, petroleum asphalt, petroleum jelly, etc., and may also include fatty oil softeners, such as stearic acid, castor oil, linseed oil, rapeseed oil, coconut oil, waxes (such as beeswax, carnauba wax, and lanolin), tall oil, linoleic acid, palmitic acid, lauric acid, etc. In this invention, the softener is optionally added. When the raw materials of the rubber composition of this invention include a softener, the amount of softener can be 0.1 to 10 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, and 10 parts by weight. In some embodiments, stearic acid and / or naphthenic oil are used as softeners.
[0060] The accelerator is typically a vulcanization accelerator, and may be one or more selected from sulfonamide vulcanization accelerators, thiazole vulcanization accelerators, thiuram vulcanization accelerators, guanidine vulcanization accelerators, dithiocarbamate vulcanization accelerators, aldehyde-amine vulcanization accelerators, aldehyde-amine vulcanization accelerators, imidazoline vulcanization accelerators, and xanthic acid vulcanization accelerators. In the raw materials of the rubber composition of the present invention, the amount of accelerator may be 0.1-3 parts by weight, preferably 1-2 parts by weight, for example 1.2 parts by weight, 1.4 parts by weight, 1.6 parts by weight, or 1.8 parts by weight. In some preferred embodiments, the accelerator is accelerator DZ (N,N′-dicyclohexyl-2-benzothiazole sulfinamide). In some preferred embodiments, the accelerator is accelerator NS (N-tert-butyl-2-benzothiazole sulfinamide).
[0061] Plasticizers are commonly used additives in rubber products to improve the processing performance of rubber. They reduce the intermolecular forces in rubber, thereby lowering the glass transition temperature of rubber, increasing its plasticity and flowability, and facilitating subsequent molding operations. Plasticizers can also improve the mechanical properties of vulcanized rubber, enhancing the elasticity, lubricity, and flexibility of the compound. In this article, the plasticizer is an environmentally friendly oil. In some embodiments, the amount of plasticizer in the raw materials of the rubber composition of the present invention is 1-10 parts by weight, 1-3 parts by weight, or 3-10 parts by weight, for example, 3 parts by weight, 5 parts by weight, or 8 parts by weight.
[0062] In some preferred embodiments, the raw materials of the rubber composition of the present invention include: 100 parts by weight of diene elastomer, 1-6 parts by weight (e.g., 1.5 parts by weight) of sulfur, 0.1-7 parts by weight (e.g., 5 parts by weight) of the antioxidant composition of the present invention, 10-70 parts by weight (e.g., 60 parts by weight) of carbon black, 1-10 parts by weight (e.g., 3 parts by weight) of ZnO, 1-10 parts by weight (e.g., 3 parts by weight) of environmentally friendly oil, 0.1-6 parts by weight (e.g., 0.8 parts by weight) of rubber adhesive, 0.1-10 parts by weight (e.g., 2 parts by weight) of softener and 0.1-3 parts by weight (e.g., 0.75 parts by weight) of accelerator, or a mixture of the above components.
[0063] The uncured rubber of the present invention can be prepared using conventional rubber mixing methods, such as a two-stage mixing process: a first-stage thermomechanical (e.g., internal mixer) mixing, in which rubber composition raw materials other than crosslinking agents and accelerators are mixed and kneaded until the entire mixture reaches a maximum temperature between 110°C and 190°C to obtain a first-stage rubber; and a second-stage thermomechanical (e.g., open mill) mixing, in which the first-stage rubber is cooled to below 100°C, crosslinking agents and accelerators are added, and the first-stage rubber is kneaded with the crosslinking agents and accelerators until the maximum temperature below 110°C to obtain a second-stage rubber, i.e., the uncured rubber.
[0064] Uncured rubber is vulcanized (cured) to obtain vulcanized rubber. The vulcanization temperature is usually 130℃-200℃, such as 140-160℃ or 150±5℃; the vulcanization time depends on the vulcanization temperature, vulcanization system and vulcanization kinetics, and is usually 15-60 minutes, such as 20-40 minutes or 30±5 minutes.
[0065] Compared to rubber products prepared using other antioxidants or antioxidant compositions, or other rubber compositions, rubber products prepared using the antioxidant compositions or rubber compositions of the present invention (e.g., tires, especially tire belt layers and carcasses) exhibit significantly improved flexural fatigue resistance, and their flexural temperature rise after aging is also greatly reduced. Therefore, the present invention also provides a rubber product made from the rubber composition of the present invention. The rubber product can be a tire, rubber shoe, sealing strip, sound insulation panel, vibration damping pad, etc. The rubber product is preferably a tire, such as a tire belt layer and carcass. The method for preparing the rubber product from the rubber composition is the vulcanization (curing) method described herein, as described in any embodiment herein.
[0066] This invention also provides methods for reducing the toxicity of rubber products, improving the flexural fatigue resistance of rubber products, reducing the heat generation during aging of rubber products, and / or improving the heat resistance of rubber products. The methods include adding the antioxidant composition of this invention to the raw materials of a rubber composition for preparing the rubber product; or the methods include preparing the rubber product using the rubber composition of this invention. The antioxidant composition of this invention, the rubber composition of this invention, the raw materials of the rubber composition of this invention, and the rubber product of this invention are as described in any embodiment herein.
[0067] This invention also provides the application of the antioxidant composition and rubber composition of this invention in reducing the toxicity of rubber products, improving the flexural fatigue resistance of rubber products, reducing the heat generation during aging of rubber products, and / or improving the heat resistance of rubber products. The application includes adding the antioxidant composition of this invention to the raw materials of the rubber composition used to prepare the rubber product; or the application includes preparing the rubber product using the rubber composition of this invention. The antioxidant composition, rubber composition, and rubber product of this invention are as described in any embodiment herein.
[0068] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Experimental methods in the following embodiments, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. Percentages and parts are by weight unless otherwise stated.
[0069] Preparation of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine
[0070] (1) Add 400g (3mol) of aniline and 182g (0.5mol) of 25wt% tetramethylammonium hydroxide (TMAH) aqueous solution to a 1L four-necked flask, stir and heat to 40-55℃, then distill under reduced pressure to dehydrate, allowing TMAH to form a salt with aniline. During this process, the reaction solution gradually changes from yellow to dark red. Gradually heat to 72℃, and when the fraction reaches 46mL, add 63.5g (0.5mol) of 3-nitropyridine dropwise while distilling under reduced pressure (-0.098MPa) at 72℃. The addition is carried out for 3 hours, and after the addition is complete, keep warm for 1 hour. LC monitoring detects the presence of 3-nitropyridine. The pyridine reaction was completed, yielding a condensate. The condensate was transferred to a 500 mL stainless steel reactor, and 100 g of deionized water and 80 g of nickel catalyst were added. The reactor was purged with hydrogen three times, heated to 75 °C, and hydrogen was introduced at 1.5 MPa for hydrogenation reduction. LC monitoring showed that the nitro and nitroso compounds were completely reduced. The reactor was then filtered and separated. The organic phase was washed with water and distilled under reduced pressure (-0.1 MPa, 160 °C) to remove aniline and light byproducts. Finally, 47.4 g of the reduced product was distilled off, cooled, and solidified into a yellow solid with a yield of approximately 51%. GC analysis showed a content >99%.
[0071] (2) 37.1 g (0.2 mol) of reduction product, 280.6 g (2.8 mol) of 4-methyl-2-pentanone and 0.5 g of Pt / C catalyst were added to the reactor. The reactor was purged with hydrogen three times, heated to 70 °C, and hydrogen was introduced to 1.5 MPa for reaction. The reaction was detected by GC. When the content of reduction product was <0.1%, the reaction was stopped. The temperature was lowered, the catalyst was removed by filtration, and the light components were removed by vacuum distillation (-0.1 MPa, 180 °C) to obtain 53.3 g of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine (yield of about 99%). The content was >98% by GC. After cooling and solidification, it was a light brown solid.
[0072] The obtained 5-[(4-methylpentan-2-yl)amino]-2-(phenylamino)pyridine was subjected to NMR analysis, and the results were as follows: 1H NMR: δ 8.86 (1H), 7.54 (2H), 7.44 (1H), 7.35 (1H), 7.31 (2H), 6.93 (1H), 5.53 (2H), 3.33 (1H), 1.90 (2H), 1.62 (1H), 1.24 (3H), 0.89 (6H).
[0073] The sources and specifications of the raw materials used in the examples are as follows:
[0074] Natural rubber SCR5: Xishuangbanna Sinochem Rubber Co., Ltd.;
[0075] Carbon Black N330: Shanghai Cabot Carbon Black Co., Ltd.;
[0076] ZnO: Yonghua Chemical Technology (Jiangsu) Co., Ltd.;
[0077] Stearic acid: Sinopharm Chemical Reagent Co., Ltd.;
[0078] Environmentally friendly oil: Hansheng Petrochemical (Ningbo) Co., Ltd., grade 4010;
[0079] C9 resin: ExxonMobil, grade 5600;
[0080] Sulfur S: Sinopharm Chemical Reagent Co., Ltd.;
[0081] Accelerator NS: Weilin New Materials Technology Co., Ltd.;
[0082] Antioxidant 6PPD: Sheng'ao Chemical Technology Co., Ltd.;
[0083] Anti-aging agent RD: Sunon Chemical Technology Co., Ltd.;
[0084] Anti-aging agent DTPD: Sheng'ao Chemical Technology Co., Ltd.
[0085] Examples 1-5, Comparative Examples 1-5
[0086] The rubber compounds of Examples 1-5 and Comparative Examples 1-5 were prepared according to the following methods and the contents of each component in Tables 1-1 and 1-2.
[0087] 1. The first stage of mixing is carried out in an internal mixer with a rotor speed of 55 r / min. -1 The rotor's temperature control water temperature is 60℃, and the filler factor is 0.75. When the internal mixer chamber temperature reaches 60℃, mixing begins. The mixing process is as follows: add raw rubber SCR5, add 2 / 3 of the total filler (carbon black N330) and all minor components (ZnO, stearic acid, antioxidant, and C9 resin) at 30s, add the remaining filler at 60s, add environmentally friendly oil when the internal mixer temperature rises to 110℃, raise and lower the pressure roller once when the internal mixer temperature rises to 130℃, clean, and discharge the glue when the internal mixer temperature rises to 150℃.
[0088] 2. The second stage of mixing is carried out on a two-roll mill. The rolling temperature of the two-roll mill is set to 50℃. The mixing process is as follows: add the first stage of mixed rubber, mix evenly, add sulfur S and accelerator NS, cut left and right 3 times each, manually alternate rolling and triangular wrapping 5 times each, and then sheet out. After standing at room temperature for 24 hours, the rubber composition is obtained.
[0089] 3. The rubber composition obtained in step 2 is vulcanized at 150°C for 30 minutes to obtain the rubber compound.
[0090] Table 1-1: Comparative Rubber Compound Components
[0091] Table 1-2: Rubber Components in Examples
[0092] Test Example 1: Flexion Crack Test
[0093] The flexural resistance of the rubber compound was tested according to GB / T 13934-2006 "Determination of flexural cracking and crack growth of vulcanized rubber or thermoplastic rubber (Demercia type)".
[0094] The rating criteria for the flexural crack test are shown in Table 2.
[0095] The experimental results of the flexural crack test are shown in Table 3.
[0096] Table 2
[0097] Table 3
[0098] As shown in Table 3, the rubber compounds of Examples 1-5 prepared using the antioxidant composition of the present invention have flexural properties comparable to those of the rubber compound of Comparative Example 3 prepared using 6PPD, and the flexural properties of the rubber compounds of Examples 1-5 are superior to those of Comparative Examples 1-2 and 4-5.
[0099] Test Example 2: Flexural Temperature Rise Test
[0100] The flexural temperature rise test of the rubber compound was conducted in accordance with GB / T 15584 "Determination of temperature rise and fatigue resistance of vulcanized rubber in flexural test - Part 1: Basic principle" and GB / T 1687 "Determination of temperature rise and fatigue resistance of vulcanized rubber in flexural test - Part 2: Test procedure".
[0101] The hot air aging test was conducted in accordance with GB / T 3512-2014 "Accelerated aging and heat resistance test of vulcanized rubber or thermoplastic rubber in hot air".
[0102] Test conditions: The specimen was subjected to a prestress of 1.0 MPa, the temperature of the constant temperature chamber was 55℃, the preheating time was 30 min, and the test time was 25 min.
[0103] The experimental results of the flexural temperature rise test are shown in Tables 4-1 and 4-2.
[0104] Table 4-1
[0105] Table 4-2
[0106] As shown in Table 5, the heat resistance of the rubber compounds prepared in Examples 1-5 is comparable to that of Comparative Examples 1-5.
Claims
1. An antioxidant composition, characterized in that, The antioxidant composition comprises 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine, N,N′-xylyl-p-phenylenediamine, and 2,2,4-trimethyl-1,2-dihydroquinoline polymer.
2. The antioxidant composition according to claim 1, characterized in that, In the antioxidant composition, the mass ratio of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine to N,N′-xylyl-p-phenylenediamine is 1:(0.1-2); and / or, in the antioxidant composition, the mass ratio of 5-[(4-methylpent-2-yl)amino]-2-(phenylamino)pyridine to 2,2,4-trimethyl-1,2-dihydroquinoline polymer is 1:(0.1-2).
3. A rubber composition, characterized in that, The raw materials of the rubber composition include 100 parts by weight of diene elastomer and 2-10 parts by weight of the antioxidant composition according to claim 1 or 2.
4. The rubber composition according to claim 3, characterized in that, The raw materials for the rubber composition include 3-5 parts by weight of the antioxidant composition.
5. The rubber composition according to claim 3, characterized in that, The rubber composition has one or more of the following characteristics: The diene elastomer is selected from one or more of natural rubber, butadiene rubber, styrene-butadiene rubber, and polyisoprene; preferably, the diene elastomer is natural rubber. The raw materials of the rubber composition also include 10-70 parts by weight of reinforcing filler; preferably, the reinforcing filler is carbon black; The raw materials of the rubber composition further include 1-6 parts by weight of a crosslinking agent; preferably, the crosslinking agent is sulfur; The raw materials of the rubber composition further include 1-10 parts by weight of an activator; preferably, the activator is zinc oxide; The raw materials of the rubber composition also include 0.1-3 parts by weight of cobalt salt; The raw materials of the rubber composition also include 0.1-3 parts by weight of tackifying resin; The raw materials of the rubber composition also include 0.1-6 parts by weight of a rubber binder; preferably, the rubber binder is a petroleum resin; The raw materials of the rubber composition further include 0.1-10 parts by weight of a softener; preferably, the softener is stearic acid and / or naphthenic oil; The raw materials of the rubber composition further include 0.1-3 parts by weight of an accelerator; preferably, the accelerator is N-tert-butyl-2-benzothiazole sulfenamide; The raw materials of the rubber composition also include 1-10 parts by weight of a plasticizer; preferably, the plasticizer is an environmentally friendly oil.
6. A rubber article made from the rubber composition according to any one of claims 3-5; preferably, the rubber article is a tire.
7. A method for reducing the toxicity of rubber products, improving the flexural fatigue resistance of rubber products, reducing the heat generation during aging of rubber products, and / or improving the heat resistance of rubber products, characterized in that: The method includes adding the antioxidant composition of claim 1 or 2 to the raw materials of the rubber composition for preparing rubber articles; or The method includes preparing the rubber article using the rubber composition of any one of claims 3-5.
8. The method as described in claim 7, characterized in that, The raw materials of the rubber composition include 100 parts by weight of diene elastomer and 2-10 parts by weight of the antioxidant composition according to claim 1 or 2.
9. The method as described in claim 7, characterized in that, The raw materials for the rubber composition include 3-5 parts by weight of the antioxidant composition.
10. The method as described in claim 7, characterized in that, The rubber composition has one or more of the following characteristics: The diene elastomer is selected from one or more of natural rubber, butadiene rubber, styrene-butadiene rubber, and polyisoprene; preferably, the diene elastomer is natural rubber. The raw materials of the rubber composition also include 10-70 parts by weight of reinforcing filler; preferably, the reinforcing filler is carbon black; The raw materials of the rubber composition further include 1-6 parts by weight of a crosslinking agent; preferably, the crosslinking agent is sulfur; The raw materials of the rubber composition further include 1-10 parts by weight of an activator; preferably, the activator is zinc oxide; The raw materials of the rubber composition also include 0.1-3 parts by weight of cobalt salt; The raw materials of the rubber composition also include 0.1-3 parts by weight of tackifying resin; The raw materials of the rubber composition also include 0.1-6 parts by weight of a rubber binder; preferably, the rubber binder is a petroleum resin; The raw materials of the rubber composition further include 0.1-10 parts by weight of a softener; preferably, the softener is stearic acid and / or naphthenic oil; The raw materials of the rubber composition further include 0.1-3 parts by weight of an accelerator; preferably, the accelerator is N-tert-butyl-2-benzothiazole sulfenamide; The raw materials of the rubber composition also include 1-10 parts by weight of a plasticizer; preferably, the plasticizer is an environmentally friendly oil.