Electronic device frame and manufacturing method therefor, and electronic device

By employing a composite structure of porous ceramic skeleton and plastic material in the electronic device frame, the problem of compatibility between frame strength and toughness was solved, achieving a high-strength, high-toughness, and lightweight design, which improved signal transmission and stability.

WO2026233046A1PCT designated stage Publication Date: 2026-11-12HUAWEI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/089704
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-09
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing electronic device frames struggle to combine strength, hardness, and toughness, making them susceptible to damage from mechanical impacts, and also presenting issues such as signal shielding and excessive weight.

Method used

A composite structure of porous ceramic skeleton and plastic material is adopted. By filling the pores of the porous ceramic skeleton with plastic material, an interlocking structure is formed. Combined with the internal and external structure, the strength, toughness and interfacial bonding strength of the frame are improved.

Benefits of technology

It achieves a high-strength, high-toughness, and lightweight frame design, reduces electromagnetic shielding, improves antenna signal transmission, and enhances the stability and versatility of the frame design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026089704_12112026_PF_FP_ABST
    Figure CN2026089704_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of electronic devices, and in particular to an electronic device frame and a manufacturing method therefor, and an electronic device. The electronic device frame comprises, from inside to outside, an internal structure, a composite framework structure, and an appearance structure that are sequentially fitted against one another. The composite framework structure comprises a porous ceramic framework and a plastic material filled in pores of the porous ceramic framework. By means of the combined effect of the composite framework structure, the internal structure and the appearance structure, the electronic device frame of the present application has high strength, high toughness, and high interface bonding strength and stability, and the frame is less prone to deformation and twisting, which is more conducive to realizing a lightweight design of the frame. Moreover, by means of the internal structure and the appearance structure, a diversified design of the electronic device frame can be realized, such that the frame better meets the application requirements of the electronic device. The problems of signal shielding and excessive weight of traditional metal frames are solved, and the brittleness defect of an all-ceramic frame is overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Electronic device frame and its preparation method, electronic device

[0001] This application claims priority to Chinese Patent Application No. 202510592029.1, filed with the State Intellectual Property Office of China on May 8, 2025, entitled "Electronic Device Frame and Preparation Method Thereof, Electronic Device", the entire contents of which are incorporated herein by reference. Technical Field

[0002] This application relates to the field of electronic equipment technology, and in particular to an electronic equipment frame and its manufacturing method, and an electronic equipment. Background Technology

[0003] Currently, the frames of electronic devices such as mobile terminals, watches, and virtual reality (VR) glasses, including battery covers and mid-frames, are primarily made of homogeneous materials. For example, mid-frames are mainly metal, while battery covers, due to signal requirements, are made of non-metallic materials, primarily ceramic or glass. These homogeneous material frames make it difficult to achieve a balance of strength, hardness, and toughness. For instance, while ceramic battery covers have sufficient hardness, ceramic is a brittle material. Brittle materials have poor impact resistance and are prone to cracking or complete rupture under mechanical impact (such as drops or compression), leading to battery exposure and potential short circuits, leaks, or safety hazards. Metal mid-frames, while possessing some toughness, lack sufficient hardness and are easily scratched. With the development of electronic devices, higher application requirements are being placed on their frames.

[0004] Therefore, it is particularly important to develop electronic device frames that combine hardness, strength, toughness, and a high-quality appearance to meet the development needs of electronic devices. Summary of the Invention

[0005] The purpose of this application is to provide an electronic device frame and its manufacturing method, as well as an electronic device, which aims to solve the problem that existing electronic device frames are difficult to possess compatible characteristics of strength, hardness and toughness.

[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:

[0007] The first aspect of this application provides an electronic device frame, which includes, from the inside out, an internal structure, a composite skeleton structure, and an external structure that are sequentially fitted together; wherein, the composite skeleton structure includes a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton.

[0008] In this application, the electronic device frame comprises a composite skeleton structure including a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton. On one hand, the porous ceramic skeleton possesses high strength, enhancing the rigidity of the electronic device frame; while the plastic material exhibits toughness, improving the toughness of the frame. Furthermore, the plastic material filling the pores of the porous ceramic skeleton forms an interlocking structure, thereby improving the stability of the electronic device frame. Simultaneously, the pores in the composite skeleton structure reduce the overall weight of the electronic device frame, facilitating lightweight design. On the other hand, the high thermal conductivity of the ceramic combined with the plastic material in the composite skeleton structure creates an efficient heat dissipation path, preventing heat accumulation. Moreover, compared to a metal skeleton, the discontinuous ceramic skeleton used in this application reduces electromagnetic shielding and improves antenna signal transmission (especially for 5G millimeter waves). Additionally, the internal and external structures are connected through the composite skeleton structure, and the ceramic pores and the plastic material filling them in the composite skeleton structure also contribute to improving the tightness and stability of the bond between the internal and external structures and the composite skeleton. Therefore, the electronic device frame of this application, through the combined effect of the composite skeleton structure, internal structure, and external structure, possesses high strength, high toughness, high interfacial bonding strength, and stability. The frame is not easily deformed or twisted, which is more conducive to achieving lightweight frame design. Furthermore, the internal and external structures allow for diversified design of the electronic device frame, enabling it to better meet the application requirements of electronic devices. It solves the signal shielding and excessive weight problems of traditional metal frames, while overcoming the brittleness of all-ceramic frames.

[0009] Some possible implementations involve using a porous ceramic framework where the ceramic material includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. In this case, the use of these ceramic materials as the porous ceramic framework is primarily based on their unique physical, chemical, and functional properties. By combining pore structure design (such as porosity and pore size distribution) with the filling of plastic materials, these materials can significantly improve the structural performance and functional characteristics of the electronic device frame.

[0010] In some possible implementations, the porosity of the porous ceramic framework is 15% to 80%. At this porosity, the strength and lightweight of the framework are well balanced.

[0011] In some possible implementations, the average size of the pores in the porous ceramic framework is 0.1 μm to 50 μm. This porosity ensures uniform impregnation of the plastic material, avoiding localized underfilling or overflow.

[0012] Some possible implementations include the use of at least one of a metallic material and a resin material as the plastic material. In this case, metal filling can enhance the thermal and electrical conductivity of the composite skeleton, which is beneficial for electromagnetic shielding or grounding design; resin filling can improve the shock absorption performance of the composite skeleton, making it suitable for frequent drop scenarios and more conducive to the lightweight design of electronic device frames.

[0013] In some possible implementations, the metal material in the plastic material includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy. These metal materials all possess excellent toughness, thermal conductivity, and electrical conductivity. When filled into the pores of the porous ceramic skeleton, the metal-filled network can optimize the heat transfer path, reduce the risk of local overheating, and significantly improve the thermal conductivity of the electronic device frame.

[0014] Some possible implementations include the use of at least one of the following resin materials in the plastic material: epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. These resin materials have a low modulus of elasticity, which can absorb mechanical vibration and impact energy, thus better improving the shock absorption performance of the composite skeleton.

[0015] Some possible implementations include using at least one of the following materials for the external structure: metal, resin, and ceramic. In this case, the external structure of the electronic device frame can be made of different materials such as metal, resin, and ceramic, depending on the specific application requirements.

[0016] Some possible implementations include using at least one of the following materials for the internal structure: metal, resin, and ceramic. In this case, the internal structure of the electronic device housing can be selected from different materials such as metal, resin, and ceramic, depending on the specific application requirements.

[0017] Some possible implementations include the use of at least one of the following metal materials in the exterior structure: aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, copper alloy, titanium, titanium alloy, stainless steel, steel-aluminum composite material, and titanium-aluminum composite material. In this case, these metal materials possess high rigidity, strong bending and compressive strength, and as an exterior structure, they can enhance the high strength and impact resistance of the electronic device frame.

[0018] Some possible implementations include the use of at least one of the following resin materials in the appearance structure: epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. In this case, these resins, as appearance structures, can improve the electronic device enclosure, enhancing its lightweight and cost advantages.

[0019] Some possible implementations include using a ceramic material in the outer structure that comprises at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. In this case, these ceramic materials possess high hardness and wear resistance, and as an outer structure, they can improve the scratch resistance of the electronic device frame, making it less prone to scratches over long-term use.

[0020] Some possible implementations include the use of at least one of the following metallic materials in the internal structure: aluminum, aluminum alloys, magnesium, magnesium alloys, gold, gold alloys, silver, silver alloys, copper, and copper alloys. In this case, these metallic materials have high thermal conductivity, allowing for optimized heat dissipation paths and rapid heat removal from the electronic device.

[0021] Some possible implementations include the use of at least one of the following resin materials in the internal structure: epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. In this case, these resin materials have low density and low elastic modulus, which is beneficial for lightweighting and complex molding of electronic device frames, while also absorbing vibration energy.

[0022] Some possible implementations include using at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond as the ceramic material in the internal structure. In this case, these ceramic materials possess high-temperature resistance properties, enabling them to maintain the structural stability of the electronic device frame under high-temperature environments.

[0023] In some possible implementations, the material of the internal structure and / or the material of the external structure is the same as the plastic material filling the pores of the composite skeleton structure. In this case, the same material has better compatibility, which can improve the bonding stability of the composite skeleton structure with the internal and external structures.

[0024] In some possible implementations, at least one functional layer selected from metal plating, polymer adhesive layer, and flux layer is further bonded between the composite skeleton structure and the outer structure and / or between the composite skeleton structure and the internal structure. In this case, by providing these functional layers between the composite skeleton structure and the outer / internal structure, it is beneficial to improve the bonding stability and tightness between the outer / internal structure and the composite skeleton structure.

[0025] One possible implementation involves forming an interlocking connection at the interface between the internal structure and the composite skeleton structure. In this case, increasing the contact area of ​​the interface creates a mechanical interlock, improving the bonding strength and tightness of the structures on both sides of the interface.

[0026] One possible implementation involves forming an interlocking connection at the interface between the composite skeleton structure and the outer appearance structure. In this case, increasing the contact area of ​​the interface creates a mechanical interlock, improving the bonding strength and tightness of the structures on both sides of the interface.

[0027] Some possible implementations include at least one of the following: a mobile terminal mid-frame, a mobile terminal cover, a watch housing, an earphone housing, an earphone case housing, a tablet computer frame, and a VR glasses mid-frame.

[0028] Secondly, this application provides a method for manufacturing an electronic device frame, comprising the following steps:

[0029] An internal structure, a composite skeleton structure, and an external structure are sequentially bonded together to form an electronic device frame. The composite skeleton structure includes a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton.

[0030] The method for fabricating an electronic device frame provided in this application involves preparing an internal structure, a composite skeleton structure, and an external structure that are sequentially bonded together. The composite skeleton structure is located between the internal and external structures and serves to connect them. The composite skeleton structure includes a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton. The porous ceramic skeleton has high strength, which improves the rigidity of the electronic device frame; while the plastic material has toughness, which improves the toughness of the electronic device frame. The plastic material filling the pores of the porous ceramic skeleton forms an interlocking structure, which is beneficial to improving the stability of the electronic device frame and facilitates its lightweight design. Through the combined action of the composite skeleton structure, the internal structure, and the external structure, the electronic device frame simultaneously possesses high strength, high toughness, high interfacial bonding strength, and stability.

[0031] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in a sequentially fitted manner. The steps include: after preparing the porous ceramic skeleton, filling the pores of the porous ceramic skeleton with the plastic material to form the composite skeleton structure. Simultaneously, the plastic material forms the internal structure and the external structure on the inner and outer surfaces of the composite skeleton structure, respectively. In this case, the plastic material overflows to the inner and outer surfaces of the porous ceramic skeleton while filling its internal pores, allowing the internal and external structures to be integrally formed during the filling process.

[0032] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in sequence, including the following steps: after preparing the porous ceramic skeleton, preparing the external structure on the outer surface of the porous ceramic skeleton; filling the inner surface of the porous ceramic skeleton with the plastic material to form the composite skeleton structure; and simultaneously, the plastic material forming the internal structure on the inner surface of the composite skeleton structure. In this case, preparing the external structure first on the outer surface of the porous ceramic skeleton facilitates diverse design options for the external structure.

[0033] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in a sequentially fitted manner. The steps include: after preparing the porous ceramic skeleton, preparing the internal structure on the inner surface of the porous ceramic skeleton; filling the outer surface of the porous ceramic skeleton with the plastic material to form the composite skeleton structure; and simultaneously, the plastic material forming the external structure on the outer surface of the composite skeleton structure. In this case, preparing the internal structure first on the inner surface of the porous ceramic skeleton facilitates diverse internal structure designs.

[0034] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in sequence, including the following steps: after preparing the porous ceramic skeleton, filling the pores of the porous ceramic skeleton with the plastic material to form the composite skeleton structure, while the plastic material forms the internal structure on the inner surface of the composite skeleton structure; preparing the external structure, and then attaching the external structure to the outer surface of the composite skeleton structure. In this case, preparing the external structure separately and then attaching it to the outer surface of the composite skeleton structure facilitates diversified design of the external structure.

[0035] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in sequence, with the steps including: after preparing the porous ceramic skeleton, filling the pores of the porous ceramic skeleton with the plastic material to form the composite skeleton structure, while the plastic material forms the external structure on the outer surface of the composite skeleton structure; preparing the internal structure, and then attaching the internal structure to the inner surface of the composite skeleton structure. In this case, it is beneficial for the diversified design of the internal structure and avoids affecting the filling effect of the plastic material in the composite skeleton structure during the preparation of the internal structure.

[0036] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in a sequentially fitted manner. The steps include: preparing a composite of the porous ceramic skeleton and the ceramic external structure; filling the inner surface of the porous ceramic skeleton with the plastic material to form the composite skeleton structure; and simultaneously, the plastic material forming the internal structure on the inner surface of the composite skeleton structure. In this case, the process is simplified, and the bonding tightness and stability between the ceramic external structure and the composite skeleton structure can be better improved.

[0037] Some possible implementations involve preparing the internal structure, composite skeleton structure, and external structure in a sequentially fitted manner. The steps include: preparing a composite of the porous ceramic skeleton and the internal ceramic structure; filling the outer surface of the porous ceramic skeleton with the plastic material to form the composite skeleton structure; and simultaneously, the plastic material forming the external structure on the outer surface of the composite skeleton structure. In this case, the process is simplified, and the bonding tightness and stability between the internal ceramic structure and the composite skeleton structure can be better improved.

[0038] Some possible implementations of the porous ceramic framework include ceramic powder sintering.

[0039] Some possible implementations include impregnation as a method of filling the plastic material.

[0040] Some possible implementations, whereby the internal structure is integrated into the inner surface of the composite skeleton structure and the external structure is integrated into the outer surface of the composite skeleton structure, include at least one of ceramic powder sintering, welding, hot isostatic pressing, die casting, and bonding. In the ceramic powder sintering process, the selected ceramic powder composition is the same as or similar to the chemical composition of the porous ceramic skeleton.

[0041] Thirdly, this application provides an electronic device comprising the above-described electronic device frame and / or an electronic device frame prepared by the above-described method.

[0042] The electronic device of this application includes an electronic device frame that possesses the aforementioned characteristics of high strength, high toughness, high interfacial bonding strength, and stability, thereby improving the stability, safety, and service life of the electronic device.

[0043] Some possible implementations include at least one of a mobile terminal, a watch, headphones, a tablet, and VR glasses.

[0044] The above description is merely an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it according to the contents of the specification, and to make the above and other objects, features and advantages of this application more apparent and understandable, the following are specific examples of this application. Detailed implementation method. Attached Figure Description

[0045] Figure 1 is a schematic diagram of the structure of the electronic device frame provided in an embodiment of this application;

[0046] Figure 2 is a schematic diagram of the structure of the electronic device provided in an embodiment of this application;

[0047] Figure 3 is a structural schematic diagram of the manufacturing process of the mobile phone mid-frame provided in Embodiment 1 of this application;

[0048] Figure 4 is a schematic diagram of the manufacturing process of the mobile phone mid-frame provided in Embodiments 2 and 11 of this application;

[0049] Figure 5 is a structural schematic diagram of the manufacturing process of the mobile phone mid-frame provided in Embodiment 3 of this application;

[0050] Figure 6 is a structural schematic diagram of the manufacturing process of the mobile phone mid-frame provided in Embodiment 4 of this application;

[0051] Figure 7 is a structural schematic diagram of the manufacturing process of the mobile phone back cover provided in Embodiment 5 of this application;

[0052] Figure 8 is a structural schematic diagram of the manufacturing process of the mobile phone back cover provided in Embodiment 6 of this application;

[0053] Figure 9 is a structural schematic diagram of the manufacturing process of the watch case provided in Embodiment 7 of this application;

[0054] Figure 10 is a structural schematic diagram of the manufacturing process of the watch bezel provided in Embodiment 8 of this application;

[0055] Figure 11 is a schematic diagram of the fabrication process of the composite skeleton of the electronic device frame provided in Embodiment 9 of this application;

[0056] Figure 12 is a structural schematic diagram of the electronic device frame provided in Embodiment 10 of this application;

[0057] In the figure, the following labels are used: 100—Mobile phone; 101—Mobile phone frame; 102—Mobile phone back cover; 103—Screen; 10—Composite skeleton structure; 11—Porous ceramic skeleton; 20—Exterior structure; 30—Internal structure; 40—Functional layer. Detailed Implementation

[0058] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0059] In this application, the term "and / or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0060] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0061] It should be understood that in the various embodiments of this application, the order of the above processes does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0062] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms “a,” “the,” and “the” used in the embodiments of this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.

[0063] The term "VR" refers to VR glasses, short for Virtual Reality. Also known as virtual reality glasses, these devices offer a completely new first-person perspective experience, allowing users to experience the life of a movie protagonist. VR glasses are a type of head-mounted display device that integrates simulation technology, computer graphics, machine interface technology, multimedia technology, sensing technology, and network technology. By simulating three-dimensional space and tracking the user's head movements, they provide an immersive experience, representing a novel human-computer interaction method.

[0064] Currently, judging from market trends, the frames of electronic devices such as mobile terminals, watches, headphones, tablets, and VR glasses, including battery covers and mid-frames, are primarily made of homogeneous materials. For example, mid-frames are mainly metal, while battery covers, due to signal requirements, are made of non-metallic materials, primarily ceramic or glass. These homogeneous material frames struggle to achieve a balance of strength, hardness, and toughness. For instance, while ceramic battery covers have sufficient hardness, ceramic is a brittle material. Brittle materials have poor impact resistance and are prone to cracking or complete rupture under mechanical impact (such as drops or compression), leading to battery exposure and potential short circuits, leaks, or safety hazards. Metal mid-frames, while possessing some toughness, lack sufficient hardness and are easily scratched. With the development of electronic devices, higher application requirements are being placed on their frames.

[0065] To address the challenge of achieving a balance of strength, hardness, and toughness in electronic device frames, research has revealed several technologies. One approach uses a ceramic frame or battery cover as the exterior, with internal connections to the metal frame structure achieved through adhesive bonding or back-adhesive methods. This method achieves a hard exterior while maintaining some internal flexibility, allowing for the fabrication of complex structures and thus providing both strength and toughness. However, this method suffers from weak interface strength, making it prone to cracking and separation upon impact. Furthermore, the assembly process introduces large tolerances, inevitably resulting in gaps and affecting overall refinement. Another approach uses a metal frame, with an integrated ceramic / plastic material injected into the outer surface via in-mold injection molding. While this method provides some plasticity and toughness, the bonding between the metal frame and the plastic / ceramic interface relies on surface treatments (such as anodizing, micro-arc oxidation, or sandblasting). Improper treatment can lead to delamination of the injection-molded layer, compromising structural integrity. Additionally, the metal frame offers significant electromagnetic shielding.

[0066] Based on the above considerations, and to address the challenge of simultaneously achieving strength, hardness, and toughness in electronic device frames, this application proposes an electronic device frame that employs a composite skeleton structure comprising a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton, combined with internal and external structural features. This electronic device frame simultaneously possesses high strength, high toughness, and high interfacial bonding strength, thereby improving the overall drop resistance, scratch resistance, and other characteristics of the electronic device frame.

[0067] For ease of understanding, this application is specifically described through the following embodiments. It should be understood that the following embodiments are only used to illustrate the solution of this application and are not intended to limit the scope of this application.

[0068] In a first aspect, embodiments of this application provide an electronic device frame. In some embodiments, as shown in FIG1, the electronic device frame includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially fitted together; wherein, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and a plastic material filling the pores of the porous ceramic skeleton 11.

[0069] Thus, in the electronic device frame of this application embodiment, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and a plastic material filling the pores of the porous ceramic skeleton 11. On the one hand, the porous ceramic skeleton 11 has high strength, which can improve the high rigidity of the electronic device frame; while the plastic material has toughness, which can improve the toughness of the electronic device frame. Furthermore, the plastic material filling the pores of the porous ceramic skeleton 11 forms an interlocking structure, thereby improving the stability of the electronic device frame. At the same time, the pores in the composite skeleton structure 10 reduce the overall weight of the electronic device frame, which is beneficial to the lightweight design of the electronic device frame. On the other hand, the high thermal conductivity of the ceramic in the composite skeleton structure 10 combined with the plastic material can form an efficient heat dissipation path, avoiding heat accumulation. Moreover, compared with the metal skeleton, the discontinuous ceramic skeleton used in this application embodiment can reduce electromagnetic shielding and improve antenna signal transmission (especially 5G millimeter wave). In addition, the internal structure 30 and the external structure 20 are connected through the composite skeleton structure 10, and the plastic material filling the ceramic pores of the composite skeleton structure 10 also helps to improve the tightness and stability of the connection between the internal structure 30 and the external structure 20 and the composite skeleton. Therefore, the electronic device frame in this embodiment, through the combined effect of the composite skeleton structure 10, internal structure 30, and external structure 20, possesses high strength, high toughness, high interface bonding strength, and stability. The frame is not easily deformed or twisted, which is more conducive to achieving lightweight frame design. Furthermore, the internal structure 30 and external structure 20 allow for diversified design of the electronic device frame, enabling it to better meet the application requirements of electronic devices. This solves the signal shielding and excessive weight problems of traditional metal frames, while overcoming the brittleness of all-ceramic frames.

[0070] It should be noted that the electronic device frame provided in this application embodiment includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially fitted together. "From the inside out" refers to the frame from the application's inner / inner side to the application's outer / outer side. The external structure 20 refers to the structure that the user can directly observe after the electronic device frame is applied to the electronic device, i.e., the externally visible structure. Conversely, the internal structure 30 refers to the structure that is not externally visible after the electronic device frame is applied to the electronic device. As shown in Figure 2, the mobile phone 100 includes a screen 103, a mobile phone mid-frame 101, and a mobile phone back cover 102. For example, when the electronic frame is the mobile phone mid-frame 101, the mid-plate structure of the mid-frame is the application's inner / inner side, and the internal structure 30 includes the mid-plate; the four-sided border structure of the mid-frame is the application's outer / outer side, and the four-sided border is the external structure 20. When the electronic frame is the back cover 102 of a mobile phone, the surface of the back cover that contacts the mobile phone is the inner side / inner part of the application, and at this time the surface of the back cover that contacts the mobile phone is the internal structure 30. The surface of the back cover that is opposite to the mobile phone is the outer side / outer part of the application, and at this time the surface of the back cover that is opposite to the mobile phone is the outer structure 20.

[0071] In some possible implementations, the ceramic material in the porous ceramic framework 11 includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. In the design of the electronic device frame, embodiments of this application select materials such as silicon carbide (SiC), zirconium oxide (ZrO2), alumina (Al2O3), aluminum nitride (AlN), boron nitride (BN), boron carbide (B4C), and diamond as the porous ceramic framework 11, primarily based on their unique physical, chemical, and functional properties. These materials, through the combination of pore structure design (such as porosity and pore size distribution) and plastic material filling, can significantly improve the structural performance and functional performance of the electronic device frame. Among them, silicon carbide has high hardness, making it suitable for wear-resistant applications. Aluminum nitride has high thermal conductivity, making it suitable for high-power devices. Zirconia has high toughness and fracture resistance, making it suitable for devices with high drop resistance requirements. Boron nitride exhibits anisotropic thermal conductivity, allowing for the design of directional heat dissipation paths (such as in the hinge area of ​​foldable screens), making it suitable for high-frequency communication equipment frames, moving part support structures, and precision devices requiring directional heat dissipation. Boron carbide possesses ultra-high hardness, low density, high temperature resistance, and good chemical stability. Diamond ceramic materials refer to composite materials with diamond (C) as the matrix or reinforcing phase, exhibiting high hardness and high thermal conductivity.

[0072] In some possible implementations, the porosity of the porous ceramic framework 11 is 15% to 80%; exemplaryly, the porosity can be any typical but not limited point value or a range between any two points, such as 15%, 20%, 30%, 40%, 50%, 60%, 70%, 80%. At this porosity, the strength and lightweight of the framework are adequately balanced.

[0073] In some embodiments, different regions of the porous ceramic frame 11 can be configured with different porosities. By setting high and low porosities, the frame can better meet the application performance requirements of the electronic device. For example, a dense, low-porosity region (e.g., porosity of 15% to 40%) is provided in the porous ceramic frame 11 for the load-bearing area of ​​the electronic device, while a high-porosity region (e.g., porosity of 40% to 80%) is provided for the weight-reduction non-critical area of ​​the electronic device.

[0074] In some possible implementations, the average size of the pores in the porous ceramic framework 11 is 0.1 μm to 50 μm; exemplaryly, the average size of the pores in the porous ceramic framework 11 can be any typical but not limited point value or a range between any two point values, such as 0.1 μm, 0.3 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm. With this porosity, uniform impregnation of the plastic material can be ensured, avoiding localized insufficient filling or overflow.

[0075] In some possible implementations, the plastic material includes at least one of a metallic material and a resin material. The plastic material filling the pores of the composite skeleton in this application embodiment can be either a metallic material or a resin material. Metal filling enhances the thermal and electrical conductivity of the composite skeleton, facilitating electromagnetic shielding or grounding designs; resin filling improves the shock absorption performance of the composite skeleton, making it suitable for frequent drop scenarios (such as mobile phones), and is more conducive to lightweight design of electronic device frames.

[0076] In some possible implementations, the metal material in the plastic material includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy. These metal materials all possess excellent toughness, thermal conductivity, and electrical conductivity. When filled into the pores of the porous ceramic framework 11, the metal-filled network optimizes the heat transfer path, reduces the risk of localized overheating, and significantly improves the thermal conductivity of the electronic device frame, making it suitable for the heat dissipation needs of high-power electronic devices and enhancing device reliability. It forms a continuous conductive network, effectively shielding electromagnetic interference and meeting the EMC (electromagnetic compatibility) requirements of electronic devices. Furthermore, ceramics are relatively brittle, while the ductility of the metal can absorb impact energy, prevent crack propagation, and extend the service life of the electronic device frame. Moreover, porous ceramics are inherently lightweight, and even after being filled with metal, they can maintain a low weight while achieving high strength.

[0077] In some possible implementations, the resin material in the plastic material includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. These resin materials have a low modulus of elasticity, which allows them to absorb mechanical vibration and impact energy, thus improving the shock absorption performance of the composite frame. Furthermore, these resins have a density much lower than that of metallic materials (e.g., epoxy resin has a density of approximately 1.2 g / cm³). 3 After filling, the overall structure of the electronic device frame is lighter, which is more conducive to the lightweight design of the electronic device frame.

[0078] In some possible implementations, the material of the appearance structure 20 includes at least one of metal, resin, and ceramic materials. In this case, the appearance structure 20 of the electronic device frame can be made of different materials such as metal, resin, and ceramic according to specific application requirements. Alternatively, different materials can be used at different locations of the appearance structure 20 within the electronic device frame to better meet the application requirements of the electronic device.

[0079] In some embodiments, the appearance structure 20 can achieve different appearance effects through processing techniques such as CNC (computer-controlled precision machining) and polishing, or by adjusting the inherent properties of the material. This enables diversified design, allowing the electronic device frame to better meet the application requirements of the electronic device.

[0080] In some embodiments, the inner side of the outer structure 20 is connected to the outer side of the composite skeleton structure 10. The connection between the outer structure 20 and the composite skeleton can be a sintered connection, a mechanical connection, a welded connection, or an integral structure.

[0081] In some possible implementations, the metallic material in the outer structure 20 includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, copper alloy, titanium, titanium alloy, stainless steel, steel-aluminum composite material, and titanium-aluminum composite material. In this case, these metallic materials possess high rigidity, strong bending and compressive strength, and as the outer structure 20, they can enhance the strength and impact resistance of the electronic device frame. Furthermore, the metallic material has a high thermal conductivity, allowing for rapid dissipation of internal heat.

[0082] In some possible implementations, the resin material in the outer structure 20 includes at least one selected from epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. In this case, these resins, as the outer structure 20, can improve the electronic device frame, enhancing its lightweight and cost advantages. Furthermore, these resins have a low modulus of elasticity, which can absorb vibration energy and reduce the operating noise of the electronic device.

[0083] In some possible implementations, the ceramic material in the outer structure 20 includes at least one selected from silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. In this case, these ceramic materials possess high hardness and wear resistance, and as the outer structure 20, they can improve the scratch resistance of the electronic device frame, making it less prone to scratches over long-term use. Furthermore, these ceramic materials also possess high-temperature resistance and chemical stability, and as the outer structure 20, they can improve the oxidation resistance and acid / alkali resistance of the electronic device frame.

[0084] In some possible implementations, the material in the internal structure 30 includes at least one of metal, resin, and ceramic materials. In this case, the internal structure 30 of the electronic device frame can be selected from different materials such as metal, resin, and ceramic according to specific application requirements. Alternatively, different materials can be used at different locations within the internal structure 30 of the electronic device frame to better meet the application requirements of the electronic device.

[0085] In some possible implementations, the metallic material in the internal structure 30 includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy. In this case, these metallic materials have high thermal conductivity, optimizing the heat dissipation path and rapidly dissipating heat from the electronic device. Furthermore, these metallic materials also possess high rigidity and high ductility, enabling the internal structure 30 to support precision components and improve the bending and compressive strength of the electronic device. Simultaneously, they absorb impact energy, preventing damage to the internal components of the electronic device.

[0086] In some possible implementations, the resin material in the internal structure 30 includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. In this case, these resin materials have low density and low elastic modulus, which is beneficial for lightweighting and complex molding of the electronic device frame as the internal structure 30, while also absorbing vibration energy.

[0087] In some possible implementations, the ceramic material in the internal structure 30 includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. In this case, these ceramic materials possess high-temperature resistance, enabling them to maintain the structural stability of the electronic device chassis under high-temperature conditions. Simultaneously, these ceramic materials exhibit high resistivity and low dielectric loss, making them suitable for high-frequency, high-voltage insulation applications.

[0088] In some possible implementations, the material of the internal structure 30 and / or the material of the external structure 20 is the same as the plastic material filling the pores of the composite skeleton structure 10. In this case, the same material has better compatibility, which can improve the bonding stability between the composite skeleton structure 10 and the internal structure 30 and the external structure 20.

[0089] In some possible implementations, at least one functional layer 40, selected from a metal plating layer, a polymer adhesive layer, and a flux layer, is further bonded between the composite skeleton structure 10 and the outer structure 20 and / or between the composite skeleton structure 10 and the inner structure 30. In this case, by providing these functional layers 40 between the composite skeleton structure 10 and the outer / inner structure 20, the bonding stability and tightness between the outer / inner structure 30 and the composite skeleton structure 10 are improved. The polymer adhesive layer (such as polyurethane) can also mitigate the difference in thermal expansion between ceramic and metal, preventing cracking. The metal plating layer forms a metal reinforcement layer on the brittle ceramic material surface of the composite skeleton structure 10 through electroplating or chemical plating, improving impact resistance and surface hardness. It also forms a continuous conductive path on the surface of non-conductive materials (such as ceramic or resin), enabling electrical connections (such as grounding or signal transmission) between different structures. The flux layer improves the reliability of the solder joints.

[0090] In some possible implementations, an interlocking connection is formed at the interface between the internal structure 30 and the composite skeleton structure 10. In some possible implementations, an interlocking connection is formed at the interface between the composite skeleton structure 10 and the external structure 20. In this case, by forming an interlocking connection at the interface between the composite skeleton structure 10 and the internal structure 30 / external structure 20, for example, by providing a concave-convex interlocking structure at the interface, the contact area of ​​the interface is increased, a mechanical interlock is formed, and the bonding strength and tightness of the structures on both sides of the interface are improved.

[0091] In some possible implementations, the electronic device frame includes at least one of a mobile terminal mid-frame, a mobile terminal cover plate, a watch case, an earphone case, an earphone box case, a tablet computer frame, and a VR glasses mid-frame. The electronic device frame in this application is applied to structural components of consumer electronics such as mobile terminals, watches, earphones, tablet computers, and VR glasses. A mobile terminal refers to a computer device that can be used while in motion, exemplarily including a mobile phone 100, a laptop, a tablet computer, a POS machine, and even an in-vehicle computer. The mid-frame refers to the middle part of the mobile terminal's outer shell, mainly used to fix core components such as the screen 103, battery, and motherboard, while also providing structural support and aesthetic design. The cover plate includes a battery back cover. In some embodiments, the electronic device frame includes a mobile phone mid-frame 101, a mobile phone back cover plate 102, a watch case, a tablet mid-frame, a tablet back cover, and a VR glasses mid-frame.

[0092] The electronic device frame of the above embodiments of this application can be obtained by the following methods.

[0093] Secondly, embodiments of this application provide a method for manufacturing an electronic device frame, comprising the following steps:

[0094] An internal structure 30, a composite skeleton structure 10, and an external structure 20 are sequentially bonded together to form an electronic device frame. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and a plastic material filling the pores of the porous ceramic skeleton 11.

[0095] The method for fabricating an electronic device frame provided in this application involves preparing an internal structure 30, a composite skeleton structure 10, and an external structure 20 that are sequentially bonded together. The composite skeleton structure 10 is located between the internal structure 30 and the external structure 20, serving to connect them. The composite skeleton structure includes a porous ceramic skeleton 11 and a plastic material filling the pores of the porous ceramic skeleton 11. The porous ceramic skeleton 11 has high strength, which improves the rigidity of the electronic device frame; while the plastic material has toughness, which improves the toughness of the electronic device frame. The plastic material filling the pores of the porous ceramic skeleton 11 forms an interlocking structure, which is beneficial to improving the stability of the electronic device frame and facilitates lightweight design. Through the combined action of the composite skeleton structure 10, the internal structure 30, and the external structure 20, the electronic device frame simultaneously possesses high strength, high toughness, high interfacial bonding strength, and stability.

[0096] In some possible implementations, the steps of preparing the sequentially fitted internal structure 30, composite skeleton structure 10, and external structure 20 include: preparing a porous ceramic skeleton 11, filling the pores of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10, preparing the internal structure 30 and external structure 20 respectively, and bonding the internal structure 30 and external structure 20 to the inner and outer surfaces of the composite skeleton structure 10 respectively. In this case, preparing the composite skeleton structure 10, internal structure 30, and external structure 20 separately, and then combining the three, can improve the design versatility of the internal structure 30 and external structure 20.

[0097] In some possible implementations, the steps of preparing the sequentially fitted internal structure 30, composite skeleton structure 10, and external structure 20 include: after preparing a porous ceramic skeleton 11, filling the pores of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10, while the plastic material forms the internal structure 30 and external structure 20 on the inner and outer surfaces of the composite skeleton structure 10, respectively. In this case, the plastic material overflows to the inner and outer surfaces of the porous ceramic skeleton 11 while filling the pores, so that the internal structure 30 and external structure 20 are integrally formed during the filling process of the porous ceramic skeleton 11. At this time, the materials of the internal structure 30 and external structure 20 are the same as the plastic material filled in the porous ceramic skeleton 11, which is beneficial to improving the bonding strength and stability between the composite skeleton structure 10 and the internal structure 30 and external structure 20. Furthermore, combining the filling step of the porous ceramic skeleton 11 with the processing steps of the internal structure 30 and external structure 20 into one process saves processing steps and reduces shell costs.

[0098] For example, the manufacturing steps of this application embodiment, regarding the mid-frame structure, can achieve a one-piece ceramic mid-frame effect without antenna seams. Regarding the ceramic back cover, a stepped ceramic design from the outside to the inside can be achieved, which is beneficial for reducing the weight of the ceramic back cover and increasing its rigidity.

[0099] In some possible implementations, the steps of preparing the sequentially bonded internal structure 30, composite skeleton structure 10, and external structure 20 include: after preparing a porous ceramic skeleton 11, preparing the external structure 20 on the outer surface of the porous ceramic skeleton 11; filling the inner surface of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10; and simultaneously, the plastic material forming the internal structure 30 on the inner surface of the composite skeleton structure 10. In this case, preparing the external structure 20 first on the outer surface of the porous ceramic skeleton 11 facilitates diversified design of the external structure 20. Then, filling the inner surface of the porous ceramic skeleton 11 with a plastic material, while the plastic material overflows to the inner surface of the composite skeleton structure 10 to form the internal structure 30, thus obtaining the composite skeleton structure 10 and the internal structure 30, simplifies the preparation process and improves the bonding stability and tightness between the internal structure 30 and the composite ceramic skeleton.

[0100] In some possible implementations, the steps of preparing the sequentially bonded internal structure 30, composite skeleton structure 10, and external structure 20 include: after preparing a porous ceramic skeleton 11, preparing the internal structure 30 on the inner surface of the porous ceramic skeleton 11, filling the outer surface of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10, and simultaneously forming the external structure 20 on the outer surface of the composite skeleton structure 10 with the plastic material. In this case, preparing the internal structure 30 first on the inner surface of the porous ceramic skeleton 11 facilitates diversified design of the internal structure 30. Then, filling the outer surface of the porous ceramic skeleton 11 with a plastic material, while the plastic material overflows to the outer surface of the composite skeleton structure 10 to form the external structure 20, thus obtaining the composite skeleton structure 10 and the external structure 20, simplifies the preparation process and improves the bonding stability and tightness between the external structure 20 and the composite ceramic skeleton.

[0101] In some possible implementations, the steps of preparing the sequentially bonded internal structure 30, composite skeleton structure 10, and external structure 20 include: after preparing a porous ceramic skeleton 11, filling the pores of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10, while the plastic material forms the internal structure 30 on the inner surface of the composite skeleton structure 10; preparing the external structure 20, and then bonding the external structure 20 to the outer surface of the composite skeleton structure 10. In this case, preparing the external structure 20 separately and then bonding it to the outer surface of the composite skeleton structure 10 facilitates the diversified design of the external structure 20 and avoids affecting the filling effect of the plastic material in the composite skeleton structure 10 during the preparation of the external structure 20.

[0102] In some possible implementations, the steps of preparing the sequentially attached internal structure 30, composite skeleton structure 10, and external structure 20 include: after preparing a porous ceramic skeleton 11, filling the pores of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10, while the plastic material forms the external structure 20 on the outer surface of the composite skeleton structure 10; preparing the internal structure 30, and then bonding the internal structure 30 to the inner surface of the composite skeleton structure 10. In this case, preparing the internal structure 30 separately and then bonding it to the inner surface of the composite skeleton structure 10 facilitates the diversified design of the internal structure 30 and avoids affecting the filling effect of the plastic material in the composite skeleton structure 10 during the preparation of the internal structure 30.

[0103] In some possible implementations, the steps of preparing the sequentially bonded internal structure 30, composite skeleton structure 10, and external structure 20 include: preparing a composite of a porous ceramic skeleton 11 and a ceramic external structure 20; filling the inner surface of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10; and simultaneously, the plastic material forms the internal structure 30 on the inner surface of the composite skeleton structure 10. In this case, the external structure 20 is a dense ceramic. By controlling the size of the ceramic powder particles, the porous ceramic skeleton 11 and the dense ceramic external structure 20 can be prepared simultaneously, simplifying the process and improving the bonding tightness and stability between the ceramic external structure 20 and the composite skeleton structure 10. Then, the inner surface of the porous ceramic skeleton 11 is filled with a plastic material to form the composite skeleton structure 10, and simultaneously, the plastic material overflows onto the inner surface of the composite skeleton structure 10 to form the internal structure 30.

[0104] For example, the porous ceramic framework 11 uses micron-sized large-particle ceramic powder, and the external structure 20 uses nano-sized small-particle ceramic powder. After pressing to obtain a ceramic green body of the porous ceramic framework 11 and the external structure 20, a high-porosity porous ceramic framework 11 and a dense ceramic external structure 20 are obtained by sintering. A composite framework structure 10 is formed by filling the inner surface of the porous ceramic framework 11 with plastic material, and at the same time, the plastic material forms an internal structure 30 on the inner surface of the composite framework structure 10.

[0105] In some possible implementations, the steps of preparing the sequentially bonded internal structure 30, composite skeleton structure 10, and external structure 20 include: preparing a composite of a porous ceramic skeleton 11 and the ceramic internal structure 30; filling the outer surface of the porous ceramic skeleton 11 with a plastic material to form the composite skeleton structure 10; and simultaneously, the plastic material forms the external structure 20 on the outer surface of the composite skeleton structure 10. In this case, the internal structure 30 is a dense ceramic. By controlling the size of the ceramic powder particles, the porous ceramic skeleton 11 and the dense ceramic internal structure 30 can be prepared simultaneously, simplifying the process and improving the bonding tightness and stability between the ceramic internal structure 30 and the composite skeleton structure 10. Then, the outer surface of the porous ceramic skeleton 11 is filled with a plastic material to form the composite skeleton structure 10, and simultaneously, the plastic material overflows onto the outer surface of the composite skeleton structure 10 to form the external structure 20.

[0106] In some possible implementations, the method for preparing the porous ceramic framework 11 includes sintering the ceramic powder. In some embodiments, the sintering temperature is 800°C to 1500°C. Exemplarily, it can be any typical but not limited point value or a range between any two point values, such as 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C.

[0107] In some possible implementations, the method for preparing the porous ceramic framework 11 and / or the appearance structure 20 as dense ceramic includes ceramic injection molding (CIM). This involves mixing ceramic powder with a thermoplastic binder (such as paraffin wax or polyethylene) to form a "feed," which is then injected into a mold using an injection molding machine. The resulting material is then debonded and sintered to obtain a high-precision ceramic part. Key steps include: 1. Feed preparation: Ceramic powder (50%–60%) is mixed with a binder to ensure uniformity and flowability. 2. Injection molding: The feed is heated and melted at high temperature and injected into the mold. After cooling, it is demolded to obtain a "green body." 3. Debonding: The binder is removed through solvent extraction, thermal decomposition, or catalytic debonding (this process is the most time-consuming and prone to defects). 4. Sintering: Densification is performed at high temperature to obtain the final ceramic part.

[0108] In some possible implementations, the method for preparing the porous ceramic framework 11 and / or the appearance structure 20 as dense ceramic includes the dry pressing method, the core of which is to press ceramic powder into shape in a mold under high pressure, and then sinter it to obtain a dense ceramic body. This method is suitable for producing ceramic parts with simple shapes and high dimensional accuracy requirements. The dry pressing process includes: 1. Powder preparation: Selecting high-purity ceramic powders (silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, diamond, etc.), and controlling the powder particle size (usually 100nm~50um) and distribution uniformity through ball milling, spray drying, etc. Adding binders (such as polyvinyl alcohol PVA, in small amounts, 1-5wt%) improves powder flowability and formability. 2. Granulation: The mixed powder is granulated by spray granulation or mechanical granulation to form particles with good flowability (particle size approximately 50-200μm), reducing friction during pressing and improving filling uniformity. 3. Loading Method: Vibration or mechanical feeding ensures uniform powder filling of the mold cavity, avoiding density gradients. 4. Pressing: Uniaxial pressing, typically 50-200 MPa, adjusted according to ceramic type and shape. Pressure is usually maintained for 5-30 seconds to promote particle rearrangement and elastic deformation recovery. 5. Demolding: After slowly releasing pressure, the green body is removed from the mold using an ejector mechanism to prevent cracking due to elastic aftereffects. 6. Debinding and Sintering: Slow heating at 300-600℃ removes binders and lubricants to prevent cracking. The temperature is selected according to the ceramic type; pressureless sintering or hot pressing is commonly used.

[0109] In some possible implementations, methods for preparing porous ceramic framework 11 and / or appearance structure 20 as dense ceramics include cold isostatic pressing (CIP). CIP is a molding technique that applies isotropic high pressure (typically 100-600 MPa) to ceramic powder at room temperature using a liquid medium (such as water or oil) to uniformly densify the powder. Its core advantage lies in eliminating the density gradient in traditional unidirectional pressing, making it suitable for the fabrication of complex shapes or large-sized parts. Key steps include: 1. Powder pretreatment: The ceramic powder needs to have good flowability and uniformity, and a small amount of binder (such as PVA) may be added. 2. Loading and sealing: The powder is loaded into an elastic mold (such as rubber or plastic), vacuumed, and then sealed. 3. Pressure molding: The powder is placed in a high-pressure container, and pressure is transmitted through a liquid medium to uniformly compress the powder. Demolding and subsequent processing: After demolding, drying and sintering processes are required. Isotropic pressure ensures a consistent material density distribution and reduces sintering deformation. Suitable for high-hardness ceramics (such as alumina and silicon carbide), large-sized or irregularly shaped parts (such as crucibles and nozzles).

[0110] In some possible implementations, the method for preparing the porous ceramic framework 11 and / or the appearance structure 20 as dense ceramic includes casting molding. The casting molding process mainly includes several steps: slurry preparation, casting molding, green body drying, debinding, and sintering. First, ceramic powder and dispersant are added to a solvent (water or organic solvent), and the particle agglomeration is broken up by ball milling or ultrasonic vibration, and the solvent wets the powder. Then, binder and plasticizer are added, and a stable and uniform slurry is obtained by secondary ball milling. The slurry is then molded on a casting machine to obtain a green body. Then, it is dried to evaporate the solvent, and the binder forms a network structure between the ceramic powders to obtain a green body film. Next, the green body film is machined to obtain the desired specific shape. Finally, the desired finished product is obtained through debinding and sintering.

[0111] In some possible implementations, methods for preparing porous ceramic framework 11 and / or appearance structure 20 as dense ceramics include thermostatic isostatic pressing (TIP), a molding technique where the mold temperature is kept constant at a certain temperature (50℃~300℃), and isotropic high pressure (typically 100MPa-600MPa) is applied to the ceramic powder through a liquid medium (such as water or oil) to uniformly densify the powder. Its core advantage lies in eliminating the density gradient in traditional unidirectional pressing, making it suitable for the fabrication of complex shapes or large-sized parts. Key steps include: 1. Powder pretreatment: The ceramic powder needs to have good flowability and uniformity, and a small amount of binder (such as PVA) may be added. 2. Loading and sealing: The powder is loaded into an elastic mold (such as rubber or plastic), vacuumed, and then sealed. 3. Pressure molding: The powder is placed in a high-pressure container, and pressure is transmitted through a liquid medium to uniformly compress the powder. Demolding and subsequent processing: After demolding, drying and sintering processes are required. Isotropic pressure ensures a consistent material density distribution and reduces sintering deformation. Suitable for high-hardness ceramics (such as alumina and silicon carbide), large-sized or irregularly shaped parts (such as crucibles and nozzles).

[0112] In some possible implementations, the filling method for the plastic material includes impregnation. In this case, the pores in the porous ceramic framework 11 are fully filled by an impregnation process (such as vacuum pressure impregnation), avoiding porosity defects.

[0113] In some possible implementations, the methods for bonding the internal structure 30 to the inner surface of the composite skeleton structure 10 and the external structure 20 to the outer surface of the composite skeleton structure 10 include at least one of ceramic powder sintering, welding, hot isostatic pressing, die casting, and bonding. The welding, hot isostatic pressing, and die casting methods in this application are mainly applicable when the internal structure 30 and the external structure 20 are made of metallic materials. Welding refers to a process that connects metal frame components in a molten or plastic state by local heating or pressurization. Hot isostatic pressing refers to treating the metal frame under isotropic pressure in a high-temperature (typically 800-2000℃) and high-pressure (100-200MPa) inert gas (such as argon) environment to eliminate internal defects and improve material properties. Die casting refers to a process that rapidly forms metal frame components by injecting molten metal under high pressure into a mold, suitable for mass production of complex shapes. The bonding method of ceramic powder sintering is mainly applicable when the internal structure 30 and the external structure 20 are ceramic materials. The ceramic powder sintering process is used, and the selected ceramic powder composition is the same as or similar to the chemical composition of the porous ceramic framework 11. Bonding refers to the direct bonding of two homogeneous or heterogeneous semiconductor materials with clean, atomically flat surfaces after surface cleaning and activation treatment, under certain conditions. This bonding is achieved through van der Waals forces, molecular forces, or even atomic forces, uniting the two structures into one.

[0114] In some possible embodiments, the ceramic material in the porous ceramic framework 11 includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond; the porosity of the porous ceramic framework 11 is 15% to 80%; and the average size of the pores in the porous ceramic framework 11 is 0.1 μm to 50 μm.

[0115] In some possible embodiments, the plastic material includes at least one of a metallic material and a resin material. The metallic material includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy; the resin material includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether.

[0116] In some possible embodiments, the material in the appearance structure 20 includes at least one of metallic materials, resin materials, and ceramic materials; wherein, the metallic material in the appearance structure 20 includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, copper alloy, titanium, titanium alloy, stainless steel, steel-aluminum composite material, and titanium-aluminum composite material; the resin material in the appearance structure 20 includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether; the ceramic material in the appearance structure 20 includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond.

[0117] In some possible embodiments, the material in the internal structure 30 includes at least one of a metallic material, a resin material, and a ceramic material. Specifically, the metallic material in the internal structure 30 includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy; the resin material in the internal structure 30 includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether; and the ceramic material in the internal structure 30 includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond.

[0118] In some possible implementations, at least one functional layer 40 selected from metal plating, polymer adhesive layer, and flux layer is further bonded between the composite skeleton structure 10 and the outer structure 20 and / or between the composite skeleton structure 10 and the inner structure 30.

[0119] In some possible implementations, an interlocking connection is formed at the interface between the internal structure 30 and the composite skeleton structure 10; an interlocking connection is formed at the interface between the composite skeleton structure 10 and the external structure 20.

[0120] The beneficial effects of the above embodiments of this application have been discussed in detail above, and will not be repeated here.

[0121] In some possible implementations, the preparation of the electronic device frame also includes processing techniques such as injection molding, CNC machining, polishing, and surface treatment, to process it into finished structural components such as the middle frame or cover plate of the electronic product.

[0122] In some possible implementations, the electronic device frame includes at least one of a mobile terminal mid-frame, a mobile terminal cover, a watch casing, and a VR glasses mid-frame.

[0123] In some possible implementations, after assembling the electronic device frame with components such as camera modules, batteries, screen modules, and chips, the entire device can be assembled into a complete electronic device such as a mobile terminal, watch, earphones, tablet computer, or VR glasses.

[0124] Thirdly, embodiments of this application provide an electronic device, which includes the electronic device frame described above and / or the electronic device frame prepared by the above method.

[0125] The electronic device in this application embodiment includes an electronic device frame that possesses the above-mentioned characteristics such as high strength, high toughness, high interfacial bonding strength, and stability, thereby improving the stability, safety, and service life of the electronic device.

[0126] In some possible implementations, the electronic device includes at least one of a mobile terminal, a watch, headphones, a tablet computer, VR glasses, etc.

[0127] In some embodiments, a mobile terminal, or mobile communication terminal, refers to a computer device that can be used while on the move, including mobile phones, laptops, tablets, POS machines, and even in-vehicle computers. The mid-frame and cover of the mobile terminal can adopt the aforementioned electronic device frame. The case and back cover of a watch can also adopt the aforementioned electronic device frame. The mid-frame of VR glasses can also adopt the aforementioned electronic device frame.

[0128] Example

[0129] The following description uses specific embodiments. These embodiments are exemplary and are only used to explain this application, and should not be construed as limiting the application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all commercially available conventional products.

[0130] Example 1

[0131] This application provides a mobile phone mid-frame 101, as shown in Figure 1, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal or resin filling the pores of the porous ceramic skeleton 11. The external structure 20 is a dense ceramic. Its preparation includes the following steps:

[0132] 1. A porous ceramic framework 11 is formed by sintering ceramic powder, as shown in Figure 3(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The particle size of the ceramic powder ranges from 100 nm to 20 μm. The porous ceramic framework 11 formed by sintering at a temperature of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, and the average size of the pores is 0.1 μm to 50 μm.

[0133] 2. Dense ceramic powder is dry-pressed around the porous ceramic framework 11 and sintered together to form the external structure 20, as shown in Figure 3(b). The ceramic material used in this process can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond, and its material can be the same as the framework material in step 1. The process of dry-pressing the dense ceramic powder is as follows: the ceramic powder is first spray-granulated and then filled into a mold, and dry-pressed green body is obtained after a certain pressure and time. Then, the green body is cold isostatically pressed to obtain a dry-pressed green body with uniform stress.

[0134] 3. On the inner surface of the porous ceramic skeleton 11 of the above structure, metal or resin is filled by pressure impregnation, so that the metal / resin fills the through holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. At the same time, the metal / resin fills the interior of the frame formed by the porous ceramic skeleton 11 to form an internal structure 30, as shown in Figure 3(c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process is as follows: the metal is heated to the corresponding melting point range to obtain a liquid metal flow, and the impregnation pressure range is 0.05MPa-1MPa. The vacuum degree range matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0135] 4. Perform CNC machining on the above-mentioned structural blank to obtain the mobile phone mid-frame 101, as shown in Figure 3(d).

[0136] As can be seen, the embodiments of this application achieve the effect of an integrated ceramic frame with no antenna gaps.

[0137] Example 2

[0138] This application provides a mobile phone mid-frame 101, as shown in Figure 4, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal or resin filling the pores of the porous ceramic skeleton 11. The external structure 20 is a dense ceramic. Its preparation includes the following steps:

[0139] 1. Ceramic powders with particle sizes ranging from 50 nm to 500 nm and 1 μm to 20 μm are respectively filled into a mold and dry-pressed into a green body with micron-sized particles inside and nano-sized particles outside. The green body is then sintered at 800℃ to 1500℃ to obtain a ceramic structure with a dense exterior and a porous interior, resulting in a composite of a porous ceramic framework 11 and a dense ceramic exterior structure 20, as shown in Figures 4(a) and (b). The ceramic powder material can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond; the porosity of the porous ceramic framework 11 is approximately 15% to 80%, and the average pore size is 0.1 μm to 50 μm.

[0140] 2. On the inner surface of the porous ceramic skeleton 11 of the above structure, metal or resin is filled by pressure impregnation, so that the metal / resin fills the through holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. At the same time, the metal / resin fills the interior of the frame surrounded by the porous ceramic skeleton 11 to form an internal structure 30, as shown in Figure 4(c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process is as follows: the metal is heated to the corresponding melting point range to obtain a liquid metal flow, and the impregnation pressure range is 0.05MPa-1MPa. The vacuum degree range matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0141] 3. The above-mentioned structural blank is CNC machined to obtain the mobile phone mid-frame 101, as shown in Figure 4(d).

[0142] As can be seen, the embodiments of this application achieve the same effect as Embodiment 1, but the processing steps of the porous ceramic skeleton 11 and the dense ceramic appearance structure 20 are combined into one, saving processing steps and reducing shell cost.

[0143] Example 3

[0144] This application provides a mobile phone mid-frame 101, as shown in Figure 5, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together; wherein, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal or resin filling the pores of the porous ceramic skeleton 11; the external structure 20 and the internal structure 30 are both filling materials. Its preparation includes the following steps:

[0145] 1. A porous ceramic framework 11 is formed by sintering ceramic powder, as shown in Figure 5(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The particle size of the ceramic powder ranges from 100 nm to 50 μm. The porous ceramic framework 11 formed by sintering at a temperature of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, and the average size of the pores is 0.1 μm to 50 μm.

[0146] 2. Within and outside the porous ceramic skeleton 11 described above, metal or resin is pressure-impregnated and filled, causing the metal / resin to fill the through-holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. Simultaneously, the metal / resin surrounds the outer surface of the composite skeleton structure 10 to form an external structure 20, and fills the interior of the frame formed by the porous ceramic skeleton 11 to form an internal structure 30, as shown in Figures 5(b) and (c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process involves heating the metal to a corresponding melting point range to obtain a liquid metal flow, with the applied impregnation pressure ranging from 0.05 MPa to 1 MPa. The vacuum range for pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0147] 3. The above-mentioned structural blank is CNC machined to obtain the mobile phone mid-frame 101, as shown in Figure 5(d).

[0148] As can be seen, in the embodiment of this application, the internal structure 30 and the external structure 20 are formed simultaneously during the pore filling process of the porous ceramic skeleton 11, and a metal / resin external structure 20 and internal structure 30 mid-frame are obtained. Compared with conventional metal / plastic mid-frames, this solution contains a high-rigidity porous ceramic skeleton 11, which makes the overall rigidity of the structural component high, not easy to be twisted and deformed, and also conducive to shell thinning.

[0149] Example 4

[0150] This application provides a mobile phone mid-frame 101, as shown in Figure 6, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially attached to each other; wherein, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal filling the pores of the porous ceramic skeleton 11; the external structure 20 and the internal structure 30 are both made of metal. Its preparation includes the following steps:

[0151] 1. A porous ceramic framework 11 is formed by sintering ceramic powder, as shown in Figure 6(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The particle size of the ceramic powder ranges from 100 nm to 50 μm. The porous ceramic framework 11 formed by sintering at a temperature of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, and the average size of the pores is 0.1 μm to 50 μm.

[0152] 2. A metal is pressure-impregnated into and filled with the porous ceramic skeleton 11 described above, forming a composite skeleton structure 10 by filling the through-holes within the porous ceramic skeleton 11 with the metal. Simultaneously, the metal fills the interior of the frame formed by the porous ceramic skeleton 11, forming an internal metal structure 30, and surrounds the outer surface of the composite skeleton structure 10, as shown in Figure 6(b). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The pressure impregnation process involves heating the metal to a corresponding melting point range to obtain a liquid metal flow, with an impregnation pressure range of 0.05 MPa to 1 MPa. The vacuum level matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0153] 3. A U-shaped or multi-segmented metal profile is fabricated to form the external structure 20 of the metal profile. The metal profile includes, but is not limited to, aluminum alloy, stainless steel, pure titanium, titanium alloy, steel-aluminum composite material, titanium-aluminum composite material, and amorphous materials. The composite structure obtained in step 2 is bonded to the external structure 20 of the metal profile. The outer surface of the composite skeleton structure 10 is connected to the inner wall metal of the external structure 20 by pressure impregnation of metal, forming a completed structural blank, as shown in Figure 6(c). The welding can be performed using friction stir welding or laser welding.

[0154] 4. Perform CNC machining on the above-mentioned structural blank to obtain the mobile phone mid-frame 101, as shown in Figure 6(d).

[0155] As can be seen, compared with the metal appearance structure 20 in Embodiment 3, the metal profile appearance structure 20 in this application embodiment has better control over its refinement, and the metal profile outer frame can use different metal types from the internal pressure-impregnated metal. For example, lightweight magnesium alloy or aluminum alloy can be used for pressure impregnation to form the middle frame filling material and internal structure 30; while the external profile structure can use profile aluminum alloy with better viewing effect, or stainless steel, or pure titanium, or titanium alloy. By welding the overflow of the internal pressure-impregnated metal of the porous ceramic skeleton 11 to the inner side of the external profile structure, a composite metal middle frame can be formed, achieving a lightweight, high-aesthetic, and drop-resistant product effect.

[0156] Example 5

[0157] This application provides a mobile phone back cover 102, as shown in Figure 7, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal / resin filling the pores of the porous ceramic skeleton 11. The external structure 20 is dense ceramic, and the internal structure 30 is metal / resin. Its preparation includes the following steps:

[0158] 1. Ceramic powder is sintered to form a porous ceramic framework 11, thus forming the porous ceramic framework 11 structure of the box-shaped mobile phone back cover 102, as shown in Figure 7(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond; the particle size of the ceramic powder ranges from 100 nm to 50 μm; and the porous ceramic framework 11 formed by sintering at a temperature of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, with an average pore size of 0.1 μm to 50 μm.

[0159] 2. Dry-pressed dense ceramic powder is applied to the outer surface of the porous ceramic skeleton 11 structure of the aforementioned box-shaped mobile phone back cover 102 and sintered together to form the external structure 20, as shown in Figure 7(b). The ceramic material used in this process can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond, and its material can be the same as the skeleton material in step 1. The dry-pressed dense ceramic powder process is as follows: the ceramic powder is first spray-granulated and then filled into a mold, and a dry-pressed green body is obtained after a certain pressure and time. The green body is then subjected to cold isostatic pressing to obtain a dry-pressed green body with uniform stress.

[0160] 3. Inside the porous ceramic skeleton 11 of the above structure, metal or resin is filled by pressure impregnation, so that the metal / resin fills the through holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. At the same time, the metal / resin fills the interior of the frame surrounded by the porous ceramic skeleton 11 to form a metal internal structure 30, as shown in Figure 7(c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process is as follows: the metal is heated to the corresponding melting point range to obtain a liquid metal flow, and the impregnation pressure range is 0.05MPa-1MPa. The vacuum degree range matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0161] 4. The above-mentioned structural blank is subjected to CNC machining to obtain the mobile phone back cover 102, as shown in Figure 7(d).

[0162] As can be seen, the embodiments of this application achieve the effect of an integrated mobile phone back cover 102, with no antenna gaps on the appearance surface, a larger ceramic skeleton in the mobile phone back cover 102, and better overall rigidity of the mobile phone back cover 102.

[0163] Example 6

[0164] This application provides a mobile phone back cover 102, as shown in Figure 8, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal / resin filling the pores of the porous ceramic skeleton 11. The external structure 20 is dense ceramic, and the internal structure 30 is metal / resin. Its preparation includes the following steps:

[0165] 1. Ceramic powder is sintered to form a porous ceramic framework 11, resulting in a porous ceramic framework 11 structure with a complex structure for the mobile phone back cover 102, as shown in Figure 8(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond; the particle size of the ceramic powder ranges from 100 nm to 50 μm; and the porous ceramic framework 11 formed by sintering at temperatures of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, with an average pore size of 0.1 μm to 50 μm.

[0166] 2. Dry-pressed dense ceramic powder is applied to the outer surface of the porous ceramic skeleton 11 structure of the aforementioned complex-structured mobile phone back cover 102, and sintered together to form the external structure 20, as shown in Figure 8(b). The ceramic material used in this process can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond, and its material can be the same as the skeleton material in step 1. The dry-pressed dense ceramic powder process is as follows: the ceramic powder is first spray-granulated and then filled into a mold, and a dry-pressed green body is obtained after a certain pressure and time. The green body is then subjected to cold isostatic pressing to obtain a dry-pressed green body with uniform stress.

[0167] 3. Inside the porous ceramic skeleton 11 of the above structure, metal or resin is filled by pressure impregnation, so that the metal / resin fills the through holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. At the same time, the metal / resin fills the interior of the frame surrounded by the porous ceramic skeleton 11 to form a metal internal structure 30, as shown in Figure 8(c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process involves heating the metal to the corresponding melting point range to obtain a liquid metal flow, with the applied impregnation pressure range being 0.05 MPa-1 MPa. The vacuum degree range matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0168] 4. The above-mentioned structural blank is subjected to CNC machining to obtain a mobile phone back cover 102 with a complex structure, as shown in Figure 8(d).

[0169] As can be seen, the porous ceramic skeleton 11 structure of the mobile phone back cover 102 with a complex structure in this application embodiment can simplify the post-CNC machining process and improve the manufacturing efficiency.

[0170] Example 7

[0171] This application provides a watch case, as shown in Figure 9, comprising, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially fitted together; wherein, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal / resin filling the pores of the porous ceramic skeleton 11; the external structure 20 is dense ceramic, and the internal structure 30 is precious metal. Its preparation includes the following steps:

[0172] 1. A porous ceramic framework 11 for the watch case is formed by sintering ceramic powder, as shown in Figure 9(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The particle size of the ceramic powder ranges from 100 nm to 50 μm. The porous ceramic framework 11 formed by sintering at a temperature of 800℃ to 1500℃ has a porosity of approximately 15% to 80%, and the average size of the pores is 0.1 μm to 50 μm.

[0173] 2. Dense ceramic powder is dry-pressed onto the outer surface of the porous ceramic skeleton 11 of the aforementioned casing and sintered together to form the external structure 20, as shown in Figure 9(b). The ceramic material used in this process can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond, and its material can be the same as the skeleton material in step 1. The process of dry-pressing dense ceramic powder is as follows: the ceramic powder is first spray-granulated and then filled into a mold, and dry-pressed green body is obtained after a certain pressure and time. Then, the green body is subjected to cold isostatic pressing to obtain a dry-pressed green body with uniform stress.

[0174] 3. Inside the porous ceramic skeleton 11 of the aforementioned case, metal, particularly precious metals such as pure gold, 18K gold, or rose gold, is pressure impregnated and filled. This fills the through-holes in the porous ceramic skeleton 11, forming a composite skeleton structure 10. Simultaneously, the metal surrounds the frame structure formed by the porous ceramic skeleton 11, forming an internal metal structure 30, as shown in Figures 9(c) and (d). The pressure impregnation process involves heating the metal to a suitable melting point range to obtain a liquid metal flow. The applied impregnation pressure range is 0.05 MPa to 1 MPa. The vacuum level matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0175] 4. The above-mentioned structural blank is CNC machined to obtain the watch case, as shown in Figure 9(e).

[0176] As can be seen, the embodiments of this application achieve the appearance effect of fusion between precious metal and ceramic in the watch case, and the precious metal part on the watch case is not easy to fall off.

[0177] Example 8

[0178] This application provides a bezel frame, as shown in Figure 10, comprising, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially fitted together; wherein, the composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal / resin filling the pores of the porous ceramic skeleton 11; the external structure 20 is a precious metal, and the internal structure 30 is ceramic. Its preparation includes the following steps:

[0179] 1. Ceramic powders with particle sizes ranging from 20 nm to 500 nm and 1 μm to 10 μm are respectively filled into a mold and dry-pressed into a green body with micron-sized particles on the outside and nano-sized particles on the inside. The green body is then sintered at 800℃ to 1500℃ to obtain a ceramic structure with a dense interior and a porous exterior, resulting in a composite of a porous ceramic framework 11 and a dense ceramic internal structure 30, as shown in Figures 10(a) and (b). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The porosity of the porous ceramic framework 11 is approximately 15% to 80%, and the average pore size is 0.1 μm to 50 μm.

[0180] 2. On the outside of the porous ceramic skeleton 11 of the aforementioned bezel, metal, especially precious metals such as pure gold, 18K gold, or rose gold, is pressure impregnated to fill the through-holes in the porous ceramic skeleton 11, forming a composite skeleton structure 10. Simultaneously, the metal surrounds the frame structure formed by the porous ceramic skeleton 11, forming a metallic appearance structure 20, as shown in Figures 10(c) and (d). The pressure impregnation process involves heating the metal to a corresponding melting point range to obtain a liquid metal flow, with the applied impregnation pressure ranging from 0.05 MPa to 1 MPa. The vacuum level matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0181] As can be seen, the embodiments of this application achieve the effect of fusing precious metals and ceramics inside the bezel, and the precious metal parts on the watch case are not easy to fall off.

[0182] Example 9

[0183] This application provides a composite skeleton structure 10 for an electronic device frame, as shown in Figure 11. It utilizes ceramic powder and sintersects a porous ceramic skeleton 11, half of which is dense ceramic and half is porous ceramic, as shown in Figure 11(a). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond; the particle size ranges from 100 nm to 50 μm, forming a porous ceramic skeleton 11 with a porosity of approximately 15% to 80% and an average pore size of 0.1 μm to 50 μm under conditions of 800℃ to 1500℃. Then, metal or resin is filled into the porous ceramic skeleton 11 to form the composite skeleton structure 10. Simultaneously, the metal / resin can also form an external metal or resin structure 20 and an internal structure 30 on the surface of the composite skeleton structure 10, as shown in Figure 11(b).

[0184] As can be seen, the embodiments of this application can realize a composite form in which the frame is made of porous ceramic and other materials, so that different parts of the frame can meet the different application requirements of electronic devices.

[0185] Example 10

[0186] This application provides a composite skeleton structure 10 for an electronic device frame, as shown in Figure 12. In order to improve the bonding force between the appearance structure 20 and the composite skeleton structure 10, a functional layer 40 can be added to the bonding surface between the appearance structure 20 and the porous ceramic skeleton 11, such as a metal plating layer, a polymer adhesive, a flux (whose components are metals such as silver, copper, and tin or non-metallic materials such as silicates).

[0187] Example 11

[0188] This application provides a mobile phone mid-frame 101, as shown in Figure 4, which includes, from the inside out, an internal structure 30, a composite skeleton structure 10, and an external structure 20 sequentially bonded together. The composite skeleton structure 10 includes a porous ceramic skeleton 11 and metal or resin filling the pores of the porous ceramic skeleton 11. The external structure 20 is a dense ceramic. Its preparation includes the following steps:

[0189] 1. Ceramic powders with particle sizes ranging from 50 nm to 500 nm and 1 μm to 20 μm are separately prepared into cast and dried green bodies, which are then layered and pressed together to form a composite green body. The composite green body is then pressed in a mold using warm isostatic pressing to form a green body with micron-sized particles inside and nano-sized particles outside. Sintering at 800℃ to 1500℃ yields a ceramic structure with a dense exterior and a porous interior, resulting in a composite of a porous ceramic framework 11 and a dense ceramic exterior structure 20, as shown in Figures 4(a) and (b). The ceramic powder can be one or more of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. The porosity of the porous ceramic framework 11 is approximately 15% to 80%, and the average pore size is 0.1 μm to 50 μm.

[0190] 2. On the inner surface of the porous ceramic skeleton 11 of the above structure, metal or resin is filled by pressure impregnation, so that the metal / resin fills the through holes in the porous ceramic skeleton 11 to form a composite skeleton structure 10. At the same time, the metal / resin fills the interior of the frame surrounded by the porous ceramic skeleton 11 to form an internal structure 30, as shown in Figure 4(c). The metal material can be one or more of aluminum alloy, magnesium alloy, pure gold, gold alloy, pure silver, silver alloy, and copper alloy. The resin includes one or more of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. The pressure impregnation process is as follows: the metal is heated to the corresponding melting point range to obtain a liquid metal flow, and the impregnation pressure range is 0.05MPa-1MPa. The vacuum degree range matching the pressure impregnation is 10. -1 Pa-10 -4 Pa.

[0191] 3. The above-mentioned structural blank is CNC machined to obtain the mobile phone mid-frame 101, as shown in Figure 4(d).

[0192] As can be seen, the embodiments of this application achieve the same effect as Embodiment 1, but the processing steps of the porous ceramic skeleton 11 and the dense ceramic appearance structure 20 are combined into one, saving processing steps and reducing the manufacturing cost of the mobile phone frame.

[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. The protection scope of this application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims. Therefore, the protection scope of this application should be determined by the protection scope of the claims.

Claims

1. An electronic device frame, characterized in that, The electronic device frame comprises, from the inside out, an internal structure, a composite skeleton structure, and an external structure that are sequentially fitted together; wherein, the composite skeleton structure includes a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton.

2. The electronic device frame as described in claim 1, characterized in that, The ceramic material in the porous ceramic framework includes at least one of silicon carbide, zirconium oxide, alumina, aluminum nitride, boron nitride, boron carbide, and diamond. And / or, the porosity of the porous ceramic framework is 15% to 80%; And / or, the average size of the pores in the porous ceramic framework is 0.1 μm to 50 μm.

3. The electronic device frame as described in claim 1 or 2, characterized in that, The plastic material includes at least one of metal materials and resin materials.

4. The electronic device frame as described in claim 3, characterized in that, The ductile material includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy. And / or, in the plastic material, the resin material includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether.

5. The electronic device frame as described in any one of claims 1 to 4, characterized in that, The material used in the exterior structure includes at least one of the following: metal, resin, and ceramic. And / or, the materials in the internal structure include at least one of metallic materials, resin materials, and ceramic materials.

6. The electronic device frame as described in claim 5, characterized in that, The metallic material in the aforementioned external structure includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, copper alloy, titanium, titanium alloy, stainless steel, steel-aluminum composite material, and titanium-aluminum composite material. And / or, the resin material in the appearance structure includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. And / or, the ceramic material in the appearance structure includes at least one of silicon carbide, zirconium oxide, aluminum oxide, aluminum nitride, boron nitride, boron carbide, and diamond; And / or, the metallic material in the internal structure includes at least one of aluminum, aluminum alloy, magnesium, magnesium alloy, gold, gold alloy, silver, silver alloy, copper, and copper alloy; And / or, the resin material in the internal structure includes at least one of epoxy resin, polycarbonate, polyphenolic resin, polyester, unsaturated polyester, silicone ether resin, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, polysulfone, polyphenylene ether, and chlorinated polyether. And / or, the ceramic material in the internal structure includes at least one of silicon carbide, zirconium oxide, aluminum oxide, aluminum nitride, boron nitride, boron carbide, and diamond.

7. The electronic device frame as described in any one of claims 1 to 6, characterized in that, The material of the internal structure and / or the material of the external structure is the same as the plastic material filling the pores of the composite skeleton structure.

8. The electronic device frame as described in any one of claims 1 to 7, characterized in that, At least one functional layer selected from metal plating, polymer adhesive layer, and flux layer is further bonded between the composite skeleton structure and the outer structure and / or between the composite skeleton structure and the internal structure.

9. The electronic device frame as described in any one of claims 1 to 8, characterized in that, An interlocking connection is formed at the interface between the internal structure and the composite skeleton structure; And / or, an interlocking connection is formed at the interface between the composite skeleton structure and the appearance structure.

10. The electronic device frame as described in any one of claims 1 to 9, characterized in that, The electronic device frame includes at least one of the following: a mobile terminal mid-frame, a mobile terminal cover, a watch casing, an earphone casing, an earphone case casing, a tablet computer frame, and a VR glasses mid-frame.

11. A method for manufacturing an electronic device frame, characterized in that, Includes the following steps: An internal structure, a composite skeleton structure, and an external structure are sequentially bonded together to form an electronic device frame. The composite skeleton structure includes a porous ceramic skeleton and a plastic material filling the pores of the porous ceramic skeleton.

12. The method for manufacturing an electronic device frame as described in claim 11, characterized in that, The steps of preparing the sequentially attached internal structure, the composite skeleton structure, and the external structure include: After preparing the porous ceramic skeleton, the pores in the porous ceramic skeleton are filled with the plastic material to form the composite skeleton structure. At the same time, the plastic material forms the internal structure and the external structure on the inner and outer sides of the composite skeleton structure, respectively. Alternatively, after preparing the porous ceramic skeleton, the external structure is prepared on the outer surface of the porous ceramic skeleton, and the plastic material is filled on the inner surface of the porous ceramic skeleton to form the composite skeleton structure. At the same time, the plastic material forms the internal structure on the inner surface of the composite skeleton structure. Alternatively, after preparing the porous ceramic skeleton, the internal structure is prepared on the inner side of the porous ceramic skeleton, and the plastic material is filled on the outer side of the porous ceramic skeleton to form the composite skeleton structure. At the same time, the plastic material forms the external structure on the outer side of the composite skeleton structure. Alternatively, after preparing the porous ceramic skeleton, the pores in the porous ceramic skeleton are filled with the plastic material to form the composite skeleton structure, and the plastic material forms the internal structure on the inner side of the composite skeleton structure; the external structure is prepared and the external structure is combined with the outer side of the composite skeleton structure. Alternatively, after preparing the porous ceramic skeleton, the pores in the porous ceramic skeleton are filled with the plastic material to form the composite skeleton structure, and the plastic material forms the appearance structure on the outer surface of the composite skeleton structure; the internal structure is prepared and the internal structure is combined with the inner surface of the composite skeleton structure. Alternatively, a composite of the porous ceramic skeleton and the ceramic appearance structure can be prepared, and the composite skeleton structure can be formed by filling the inner surface of the porous ceramic skeleton with the plastic material, while the plastic material forms the internal structure on the inner surface of the composite skeleton structure. Alternatively, a composite of the porous ceramic skeleton and the internal ceramic structure can be prepared, and the composite skeleton structure can be formed by filling the outer surface of the porous ceramic skeleton with the plastic material, while the plastic material forms the appearance structure on the outer surface of the composite skeleton structure.

13. The method for manufacturing the electronic device frame as described in claim 12, characterized in that, The method for preparing the porous ceramic framework includes ceramic powder sintering; And / or, the filling method of the plastic material includes impregnation; And / or, the method of attaching the internal structure to the inner side of the composite skeleton structure and the method of attaching the external structure to the outer side of the composite skeleton structure includes at least one of ceramic powder sintering, welding, hot isostatic pressing, die casting bonding, and bonding.

14. An electronic device, characterized in that, The electronic device includes an electronic device frame as described in any one of claims 1 to 10 and / or an electronic device frame prepared by the method described in any one of claims 11 to 13.

15. The electronic device as claimed in claim 14, characterized in that, The electronic device includes at least one of a mobile terminal, a watch, headphones, a tablet computer, and VR glasses.