Modified porous silicon composite negative electrode material, and preparation method therefor and use thereof

By preparing a porous silicon framework and using a composite conductive polymer coating and sulfide electrolyte filling method, the volume expansion and conductivity problems of silicon anodes in sulfide all-solid-state lithium batteries were solved, a stable electron/ion dual conduction network was constructed, and the cycle stability and rate performance of the battery were improved.

WO2026233071A1PCT designated stage Publication Date: 2026-11-12SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/090481
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-04-14
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Silicon anodes in sulfide-based all-solid-state lithium batteries suffer from issues such as volume expansion, low electronic/ionic conductivity, and poor interface stability, leading to deterioration in battery cycle performance.

Method used

A porous silicon framework was prepared by etching aluminum-silicon alloy with hydrochloric acid, and the modified porous silicon was coated with a composite conductive polymer of PEDOT:PSS and lithium polyethylene sulfonate. The pores were filled with sulfide electrolyte to construct an electron/ion dual conduction network.

Benefits of technology

It effectively alleviates volume expansion, improves electron transport efficiency and ion conduction pathways, enhances interface stability, and improves battery cycle stability and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2026090481_12112026_PF_FP_ABST
    Figure CN2026090481_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure relates to the technical field of all-solid-state batteries. Provided are a modified porous silicon composite negative electrode material, and a preparation method therefor and the use thereof. The preparation method comprises: mixing an aqueous PEDOT:PSS solution, an aqueous lithium polyethylene sulfonate solution and dimethyl sulfoxide to prepare a composite conductive polymer, and subjecting porous silicon prepared by means of a reaction under the conditions of an ice-water bath to coating modification to obtain a modified porous silicon material; and subjecting same and a sulfide electrolyte to ultrasonic mixing in a toluene solvent, and performing extraction to obtain a target material. In the obtained material, the volume expansion of a silicon-based negative electrode during charging and discharging is relieved by means of a porous structure, the electron conduction efficiency is improved by means of coating with the composite conductive polymer, the path of ion conduction is optimized by means of compounding with the sulfide electrolyte, and a stable interface buffer layer is formed to inhibit side reactions. The material can be used for preparing a negative electrode sheet which is used in combination with an NCM811 positive electrode sheet and a sulfide solid electrolyte sheet to form an all-solid-state battery, substantially improves the stability of a negative electrode interface, prolongs the cycle life of the battery, improves the rate capability of the battery, and has an important application value in the field of high-energy-density energy storage.
Need to check novelty before this filing date? Find Prior Art

Description

A modified porous silicon composite anode material, its preparation method and application

[0001] Cross-references to related applications

[0002] This disclosure claims priority to Chinese Patent Application No. 2025105783519, filed on May 7, 2025, entitled "A Modified Porous Silicon Composite Anode Material and Its Preparation Method and Application", the entire contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure relates to the field of all-solid-state battery technology, specifically to a modified porous silicon composite anode material, its preparation method, and its application. Background Technology

[0004] Sulfide-based all-solid-state lithium batteries have become an important development direction for next-generation batteries due to their high safety and high energy density potential. Traditional lithium-ion batteries use graphite anodes, but their theoretical specific capacity is low, making it difficult to meet future high-energy storage demands. Silicon, with its extremely high theoretical specific capacity and low delithiation potential, is considered a highly promising anode material. However, silicon exhibits severe volume expansion (~300%) during charge and discharge, leading to electrode structure damage, active material pulverization, and repeated rupture and regeneration of the solid electrolyte interface film, ultimately causing a sharp deterioration in battery cycle performance. To mitigate the volume expansion effect of silicon, researchers have proposed various strategies, such as nanostructuring, porous design, carbon coating, and alloying. Among these, porous silicon has attracted much attention because its internal pores can effectively buffer volume changes. Typically, porous silicon can be prepared by chemical etching, but the simple pore structure still cannot solve the problems of silicon's low intrinsic electronic conductivity and poor contact with the solid electrolyte interface. The application of silicon anodes in sulfide solid-state batteries still faces the following challenges: poor interfacial stability between silicon and sulfide electrolyte, which easily leads to side reactions; low electronic / ionic conductivity of silicon, resulting in severe polarization and poor rate performance; and volume expansion of silicon during charging and discharging, which can disrupt the tight contact between the solid electrolyte and the electrode and increase interfacial impedance.

[0005] Public content

[0006] Therefore, the purpose of this disclosure is to provide a modified porous silicon composite anode material, its preparation method, and its application. A porous silicon framework is prepared by etching an aluminum-silicon alloy with hydrochloric acid to suppress silicon volume expansion. Then, a composite conductive polymer of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate (PEDOT:PSS) and lithium polyethylene sulfonate is used to coat the modified porous silicon in a mixed solvent of dimethyl sulfoxide and water to improve electronic conductivity. Finally, a sulfide electrolyte is deposited using a wet process to fill the pores of the modified porous silicon to optimize the ion conduction path and enhance ion transport.

[0007] The purpose of this disclosure is achieved through the following technical solution:

[0008] <First Aspect>

[0009] This disclosure provides a method for preparing a modified porous silicon composite anode material, comprising the following steps:

[0010] S1. Porous silicon is modified using a composite conductive polymer. The modified porous silicon material is obtained by extracting the reaction product and drying it. The composite conductive polymer is obtained by mixing and reacting PEDOT:PSS aqueous solution, lithium polyvinyl sulfonate aqueous solution and dimethyl sulfoxide.

[0011] S2. The modified porous silicon material, sulfide electrolyte, and organic solvent are mixed and reacted under sealed conditions. The reaction product is extracted and dried to obtain the modified porous silicon composite anode material.

[0012] As one implementation, the mass ratio of the PEDOT:PSS aqueous solution and the lithium polyvinyl sulfonate aqueous solution is (1-3):1.

[0013] As one embodiment, the mass ratio of the dimethyl sulfoxide and the PEDOT:PSS aqueous solution is (3-6):50.

[0014] In some embodiments, the mass ratio of the dimethyl sulfoxide and the PEDOT:PSS aqueous solution is (3.5–5.3):50.

[0015] As one embodiment, the concentration of the PEDOT:PSS aqueous solution is 0.8% to 2%.

[0016] In some embodiments, the concentration of the PEDOT:PSS aqueous solution is 1.5%.

[0017] As one embodiment, the mass ratio of PEDOT to PSS in the PEDOT:PSS aqueous solution is 1:(2-8).

[0018] In some embodiments, the mass ratio of PEDOT to PSS in the PEDOT:PSS aqueous solution is 1:6.

[0019] As one embodiment, the concentration of the lithium polyethylene sulfonate aqueous solution is 3.5–10.5 wt.%.

[0020] In some embodiments, the concentration of the lithium polyvinyl sulfonate aqueous solution is 7 wt.%.

[0021] As one embodiment, the method for preparing the lithium polyvinyl sulfonate aqueous solution is as follows: it is obtained by neutralizing the polyethylene sulfonate aqueous solution with a lithium-containing alkaline solution.

[0022] As one embodiment, the concentration of the polyethylene sulfonic acid aqueous solution is 4–13 wt.%.

[0023] In some embodiments, the concentration of the polyvinyl sulfonic acid aqueous solution is 8.3 wt.%.

[0024] As one implementation, the lithium-containing alkaline solution is selected as an aqueous solution of lithium hydroxide.

[0025] As one embodiment, the concentration of the lithium-containing alkaline solution is 4–10 wt.%.

[0026] As one embodiment, the method for preparing the aqueous solution of polyethylene sulfonate is as follows: sodium ions in the aqueous solution of sodium polyethylene sulfonate are exchanged for hydrogen ions using a hydrogen-form strong acid cation exchange resin.

[0027] As one embodiment, the concentration of the sodium polyvinyl sulfonate aqueous solution is 5–15 wt.%.

[0028] In some embodiments, the concentration of the sodium polyvinyl sulfonate aqueous solution is 10 wt.%.

[0029] As one implementation, the method for preparing the lithium polyethylene sulfonate aqueous solution is as follows: sodium ions in the sodium polyethylene sulfonate aqueous solution are exchanged for hydrogen ions using a hydrogen-form strong acid cation exchange resin to obtain an intermediate containing sulfonic acid groups, and then the hydrogen ions of the sulfonic acid groups are neutralized using a lithium hydroxide aqueous solution to obtain the lithium polyethylene sulfonate aqueous solution.

[0030] In some embodiments, 10g of sodium polyvinyl sulfonate is dissolved in 90g of deionized water, and the solution is passed through a column of a hydrogen-form strongly acidic cation exchange resin. The cations react with the H+ on the resin. + An exchange occurs, replacing the terminal group of the monomer from -SO3Na to -SO3H. The solution is then neutralized to pH 7 with a 7wt% lithium hydroxide aqueous solution to obtain an aqueous solution of lithium polyvinyl sulfonate.

[0031] As one embodiment, the mass ratio of the composite conductive polymer to porous silicon is (5-15):1.

[0032] In some embodiments, the mass ratio of the composite conductive polymer to porous silicon is 10:1.

[0033] As one implementation, the reaction time in the preparation process of the composite conductive polymer is 2 to 4 hours.

[0034] As one implementation, the reaction time for the modification treatment is 2 to 4 hours.

[0035] As one embodiment, the porous silicon is obtained by adding aluminum-silicon alloy powder to hydrochloric acid aqueous solution at 0°C and reacting for 4-10 hours, followed by washing, extracting the reaction product, and drying.

[0036] As one implementation, the mass ratio of aluminum to silicon in the aluminum-silicon alloy powder is (5-7):4.

[0037] In some embodiments, the mass ratio of aluminum to silicon in the aluminum-silicon alloy powder is 6:4.

[0038] As one embodiment, the concentration of the hydrochloric acid aqueous solution is 8–12 wt.%.

[0039] In some embodiments, the concentration of the hydrochloric acid aqueous solution is 10 wt.%.

[0040] As one implementation, the porous silicon is cleaned with deionized water after the reaction is complete.

[0041] As one implementation scheme, the mass ratio of the modified porous silicon to the sulfide electrolyte is (3-5):1.

[0042] In some embodiments, the mass ratio of the modified porous silicon to the sulfide electrolyte is 4:1.

[0043] As one implementation, the sulfide electrolyte is Li6PS5Cl.

[0044] As one implementation, the organic solvent is toluene.

[0045] As one embodiment, the ratio of the modified porous silica to the organic solvent is (0.8-1.2) g: 10 mL.

[0046] In some embodiments, the ratio of the modified porous silica to the organic solvent is 1 g: 10 mL.

[0047] As one implementation, in step S1, the modification treatment is carried out by magnetic stirring.

[0048] In one embodiment, the composite conductive polymer is mixed by magnetic stirring.

[0049] In one embodiment, the porous silicon is prepared by stirring and mixing using magnetic stirring.

[0050] In some embodiments, the magnetic stirring speed is 800 rpm.

[0051] As one implementation, in step S2, the modified porous silicon composite anode material is prepared by ultrasonic treatment to carry out the mixing reaction.

[0052] In some embodiments, the oscillation frequency of the ultrasonic treatment is 20 kHz.

[0053] As one implementation, the extraction of reaction products in step S1 and / or step S2 is performed by solid-liquid separation by centrifugation.

[0054] In some embodiments, the centrifugation speed is 5000 rpm and the time is 20 min.

[0055] As one implementation, the drying process described in step S1 and / or step S2 is performed using a vacuum drying method.

[0056] In some embodiments, the drying parameters are: vacuum degree 0.08 MPa and temperature 80°C.

[0057] <Second aspect>

[0058] This disclosure provides a modified porous silicon composite anode material, which is prepared by the above method.

[0059] <Third aspect>

[0060] This disclosure provides an application of a modified porous silicon composite anode material in all-solid-state lithium-ion batteries.

[0061] As one implementation, the negative electrode in the battery is obtained by pressing the modified porous silicon composite negative electrode material.

[0062] As one implementation, the positive electrode in the battery is formed by pressing together a mixture of ternary positive electrode material, sulfide solid electrolyte, and conductive agent.

[0063] As one implementation scheme, the ternary cathode material is selected from nickel-cobalt-manganese-lithium ternary materials.

[0064] As one implementation, the nickel-cobalt-manganese-lithium ternary material is one or more of NCM811, NCM622, and NCM523.

[0065] In some embodiments, the conductive agent is VGCF.

[0066] In some embodiments, the mass ratio of NCM811, sulfide solid electrolyte, and conductive agent is 80:15:5.

[0067] As one implementation, the electrolyte sheet in the battery is made of sulfide electrolyte material.

[0068] In some embodiments, the sulfide electrolyte is Li6PS5Cl.

[0069] Compared with the prior art, this disclosure has the following beneficial effects:

[0070] The modified porous silicon composite anode material preparation method disclosed herein, through a multi-scale synergistic modification strategy, simultaneously solves key challenges of silicon-based anodes in solid-state batteries, such as volume expansion, interfacial impedance, and ion conduction. It constructs a highly efficient and stable electron / ion dual conduction network, demonstrating significant technical advantages in improving the cycle stability and rate performance of silicon-based anodes in all-solid-state batteries. Specifically:

[0071] (1) Alleviate volume expansion and improve structural stability

[0072] A silicon-based material with a uniform porous structure was prepared by reacting aluminum-silicon alloy powder with hydrochloric acid in an ice-water bath process, and then vacuum-dried to form a stable pore structure. This porous structure provides ample expansion buffer space for silicon during charge and discharge, effectively suppressing particle breakage and structural pulverization, ensuring the integrity of the electrode structure during cycling, and improving electrochemical performance.

[0073] (2) Conductive coating layer to enhance electron transport efficiency

[0074] A continuous conductive network is formed using PEDOT:PSS. Lithium polyethylene sulfonate introduces lithium-affinity groups to enhance the chemical bonding between the polymer and the silicon surface. After coating, the material is vacuum dried to form an elastic conductive layer, which has both electronic conduction and mechanical buffering functions.

[0075] (3) Optimize ion conduction pathways and construct an electron / ion dual conduction network.

[0076] The lithium sulfonate groups on the modified porous silicon surface form a lithium-ion conductive interface layer with the sulfide electrolyte. This structure constructs a continuous dual conduction network of porous silicon framework electron conduction / sulfide electrolyte ion conduction, which significantly improves the electrochemical performance of the negative electrode.

[0077] (4) Interface buffer layer to suppress side reactions

[0078] The composite conductive polymer coating layer and the sulfide electrolyte work synergistically to form a three-layer interface protection structure:

[0079] The inner layer, with its porous silicon pore walls, provides physical support to resist volume expansion stress;

[0080] The intermediate layer, a conductive polymer elastic layer, absorbs mechanical stress and at the same time blocks direct contact between silicon and electrolyte, suppressing the side reaction of lithium ion reduction to form SEI film.

[0081] On the outer side, the sulfide electrolyte and the lithium-affinity groups of the polymer layer form a stable interface, reducing the risk of lithium ion enrichment and dendrite growth at the interface.

[0082] (5) The process is highly controllable and suitable for large-scale production.

[0083] The preparation method employs mature industrial technologies, which are easy to scale up and control, providing a reliable process foundation for industrial production. Attached Figure Description

[0084] Other features, objects, and advantages of this disclosure will become more apparent from the following detailed description of non-limiting embodiments with reference to the accompanying drawings:

[0085] Figure 1 is a flowchart of the preparation method of the modified porous silicon composite anode material provided in this disclosure;

[0086] Figure 2 is a SEM image of the porous silicon material prepared in Example 1 of this disclosure, magnified by 2000.

[0087] Figure 3 is a SEM image of the porous silicon material prepared in Example 1 of this disclosure, magnified by 10000. Detailed Implementation

[0088] The present disclosure will now be described in detail with reference to the embodiments. These embodiments will help those skilled in the art to further understand the present disclosure, but do not limit the present disclosure in any way. It should be noted that those skilled in the art can make several adjustments and improvements without departing from the concept of the present disclosure. These all fall within the protection scope of the present disclosure.

[0089] To facilitate understanding, the abbreviations or nouns mentioned below will be explained first:

[0090] PEDOT:PSS aqueous solution: CAS No.: 155090-83-8, Product No.: P191136, 1.5% aqueous solution, PEDOT:PSS = 1:6, purchased from Aladdin Chemical Reagent Platform;

[0091] Hydrogen-form strong acid cation exchange resin: Model IR-120(H), CAS No.: 9002-23-7, purchased from Aladdin Chemical Reagent Platform;

[0092] Aluminum-silicon alloy powder: composed of 60% aluminum and 40% silicon by mass, with a particle size of 6-8μm;

[0093] VGCF: Carbon nanofiber conductive agent, VGCF-H, purchased from Kejingzhida Technology Co., Ltd.

[0094] This specific embodiment provides a method for preparing a modified porous silicon composite anode material, the steps of which are shown in Figure 1.

[0095] (1) Porous silicon materials and composite conductive polymers were prepared separately, specifically as follows:

[0096] Preparation of porous silicon material: Silicon-aluminum alloy powder is etched in hydrochloric acid aqueous solution, then washed with deionized water, and centrifuged and dried to obtain porous silicon material.

[0097] Preparation of composite conductive polymers:

[0098] Sodium polyvinyl sulfonate aqueous solution was passed through a cation exchange resin to obtain polyvinyl sulfonic acid, which was then lithiumized to obtain lithium polyvinyl sulfonate.

[0099] A composite conductive polymer was prepared by mixing and stirring PEDOT:PSS aqueous solution, lithium polyvinyl sulfonate aqueous solution, and dimethyl sulfoxide.

[0100] (2) Modifying porous silicon using composite conductive polymers, specifically:

[0101] Modified porous silicon was coated with a composite conductive polymer and then centrifuged and dried to obtain the modified porous silicon material.

[0102] (3) The sulfide solid electrolyte is deposited in the pores of the modified porous silicon by ultrasonic treatment, and then centrifuged and dried to obtain the modified porous silicon composite anode material.

[0103] The method will be described in detail below through examples.

[0104] Example 1

[0105] This embodiment provides a method for preparing a modified porous silicon composite anode material, the steps of which are as follows:

[0106] S1. Modified porous silicon material is obtained by modifying porous silicon with composite conductive polymer.

[0107] S11. Mix 5g of PEDOT:PSS aqueous solution, 5g of lithium polyvinyl sulfonate aqueous solution, and 0.526g of dimethyl sulfoxide, and stir magnetically for 2h to obtain a composite conductive polymer.

[0108] S12. Add 1g of porous silicon material to 10g of composite conductive polymer, stir magnetically for 2h, then separate the solid and liquid by centrifugation, and then dry in vacuum at 80℃ for 10h to obtain modified porous silicon material.

[0109] The preparation method for lithium polyvinyl sulfonate aqueous solution is as follows: Dissolve 10g of sodium polyvinyl sulfonate in 90g of deionized water, and pass the solution through a column of hydrogen-form strong acid cation exchange resin. The cations react with the H+ on the resin. + An exchange occurs, replacing the terminal group of the monomer from -SO3Na to -SO3H. The solution is then neutralized to pH 7 with a 7wt% lithium hydroxide aqueous solution to obtain an aqueous solution of lithium polyvinyl sulfonate with a terminal group of -SO3Li.

[0110] It should be noted that, according to calculations, the concentration of polystyrene sulfonate is approximately 8.3 wt.%, and the concentration of lithium polystyrene sulfonate is approximately 7 wt.%.

[0111] The preparation method of porous silicon materials is as follows:

[0112] 3g of aluminum-silicon alloy powder was added to 15mL of 10wt.% hydrochloric acid aqueous solution. The reaction system was placed in an ice-water bath and stirred continuously with a magnetic stirrer. After etching for 10h, the reaction product was washed three times with deionized water, centrifuged, and then vacuum dried at 80℃ for 10h to obtain porous silicon material, as shown in Figures 2 and 3.

[0113] To ensure a stable reaction, in this embodiment, aluminum-silicon alloy powder is added to hydrochloric acid in batches to avoid heat accumulation caused by the exothermic reaction and to maintain the system temperature relative to the ambient temperature.

[0114] S2. Preparation of modified porous silicon composite anode materials

[0115] In an argon glove box, 0.25g of D... 50 A sulfide electrolyte (Li6PS5Cl) with a diameter of 5 μm, 1 g of modified porous silicon, and 10 mL of toluene were added to a reaction flask and sealed. The flask was then subjected to ultrasonic treatment for 3 h (ultrasonic oscillation frequency of 20 kHz). The reaction product was then extracted by solid-liquid separation by centrifugation. Finally, the flask was vacuum dried at 80 °C for 10 h to obtain the modified porous silicon composite anode material.

[0116] In this embodiment, the magnetic stirrer used rotates at 800 rpm; the centrifugation parameters are: 5000 rpm rotation speed and 20 min time; vacuum drying is performed at a vacuum level of 0.08 MPa and a temperature of 80°C.

[0117] Example 2

[0118] This embodiment provides a method for preparing a modified porous silicon composite anode material, the steps of which are as follows:

[0119] S1. Modified porous silicon material is obtained by modifying porous silicon with composite conductive polymer.

[0120] S11. Mix 15g of PEDOT:PSS aqueous solution, 5g of lithium polyvinyl sulfonate aqueous solution, and 1.05g of dimethyl sulfoxide, and stir magnetically for 2h to obtain a composite conductive polymer.

[0121] S12. Add 1g of porous silicon material to 10g of composite conductive polymer, stir magnetically for 2h, then separate the solid and liquid by centrifugation, and then dry in vacuum at 80℃ for 10h to obtain modified porous silicon material.

[0122] The preparation method for lithium polyvinyl sulfonate aqueous solution is as follows: Dissolve 10g of sodium polyvinyl sulfonate in 90g of deionized water, and pass the solution through a column of hydrogen-form strong acid cation exchange resin. The cations react with the H+ on the resin. + An exchange process occurs, replacing the terminal group of the monomer from -SO3Na to -SO3H. The mixture is then neutralized to pH 7 with a 7wt% aqueous solution of lithium hydroxide to obtain lithium polyvinyl sulfonate with a terminal group of -SO3Li.

[0123] The preparation method of porous silicon materials is as follows:

[0124] 3g of aluminum-silicon alloy powder was added to 15mL of 10wt.% hydrochloric acid aqueous solution. The reaction system was placed in an ice-water bath and stirred continuously with a magnetic stirrer. After reacting for 5 hours, the reaction product was washed three times with deionized water, centrifuged, and then vacuum dried at 80℃ for 10 hours to obtain porous silicon material.

[0125] To ensure a stable reaction, in this embodiment, aluminum-silicon alloy powder is added to hydrochloric acid in batches to avoid heat accumulation caused by the exothermic reaction and to maintain the system temperature relative to the ambient temperature.

[0126] S2. Preparation of modified porous silicon composite anode materials

[0127] In an argon glove box, 0.25 g of sulfide electrolyte (Li6PS5Cl), 1 g of modified porous silicon, and 10 mL of toluene were added to a reaction flask and sealed. The flask was then sonicated for 3 h (ultrasonic oscillation frequency of 20 kHz). The reaction product was then extracted by solid-liquid separation by centrifugation. Finally, the flask was vacuum dried at 80 °C for 10 h to obtain the modified porous silicon composite anode material.

[0128] In this embodiment, the magnetic stirrer used rotates at 800 rpm; the centrifugation parameters are: 5000 rpm rotation speed and 20 min time; vacuum drying is performed at a vacuum level of 0.08 MPa and a temperature of 80°C.

[0129] Comparative Example 1

[0130] This comparative example provides a method for preparing a composite anode material, the steps of which are basically the same as those in Example 1, the difference being:

[0131] Instead of using porous silicon materials, aluminum-silicon alloy powder is used for coating modification, that is, the porous silicon material in step S12 is replaced with aluminum-silicon alloy powder to prepare modified silicon materials.

[0132] Comparative Example 2

[0133] This comparative example provides a method for preparing a composite anode material, the steps of which are basically the same as those in Example 1, the difference being:

[0134] Instead of using a composite conductive polymer to encapsulate the modified porous silicon material, the modified porous silicon is directly replaced with porous silicon material in step S2.

[0135] Comparative Example 3

[0136] This comparative example provides a method for preparing a composite anode material, the steps of which are basically the same as those in Example 1, the difference being:

[0137] The modified porous silicon material is used directly as the negative electrode material, without performing the S2 step.

[0138] Comparative Example 4

[0139] This comparative example provides a method for preparing a composite anode material, the steps of which are basically the same as those in Example 1, the difference being:

[0140] Porous silicon was modified using only PEDOT:PSS aqueous solution without using composite conductive polymers.

[0141] Detection and Analysis

[0142] (1) Pressure cell assembly

[0143] The composite anode materials prepared in the above embodiments and comparative examples were respectively assembled into pressure cells for testing. The steps are as follows:

[0144] In an argon glove box, 30 mg of sulfide electrolyte (Li6PS5Cl) powder was placed in a pressure cell mold with a diameter of 10 mm, and pressed into tablets on a tablet press. A pressure of 1 ton was applied and the pressure was held for 1 min to obtain electrolyte tablets.

[0145] 30mg of composite positive electrode material is spread evenly on the surface of the electrolyte sheet, and then 1 ton of pressure is applied again and held for 1 minute to compress it into a sheet;

[0146] 10 mg of composite negative electrode material was spread evenly on the other side of the electrolyte tablet, and then compressed into tablets by applying 1 ton of pressure and holding the pressure for 1 minute on a tablet press.

[0147] A 15μm thick, 10mm diameter aluminum foil is placed on the surface of the composite positive electrode sheet as the positive current collector, and a 15μm thick copper foil is placed on the other side as the negative current collector. After assembly, a pressure of 1 ton is applied and held for 1 minute to obtain a sulfide all-solid-state lithium-ion battery.

[0148] The preparation steps of the composite cathode are as follows: 80 mg of NCM811 powder, 15 mg of Li6PS5Cl sulfide solid electrolyte, and 5 mg of conductive agent VGCF powder are placed in a mortar and ground for 30 min to obtain the composite cathode material.

[0149] (2) Performance Testing

[0150] The Xinwei Battery Testing System, model CT-4000, was used to conduct charge and discharge tests on the all-solid-state batteries. The charge and discharge cycle was 0.2C-0.5C. Specifically, the charge and discharge method was as follows: first, 3 cycles of 0.2C charge and discharge, then jump to 0.5C cycle. The voltage range was 4.3-2.5V, and the temperature was 28℃. The discharge capacity of the sulfide all-solid-state batteries was tested, and the test results are shown in Table 1.

[0151] Table 1. Battery performance data of sulfide-based all-solid-state lithium batteries

[0152] Table 1 shows that the batteries in Examples 1 and 2 exhibit significantly higher discharge capacity, coulombic efficiency, and cycle stability after 30 cycles compared to Comparative Examples 1 to 4 at 0.2C and 0.5C, respectively. The composite anode system provided in this disclosure constructs a continuous electron / ion dual conduction network, improves the anode interface stability, and significantly enhances the electrochemical performance of the silicon anode in sulfide all-solid-state batteries. This is mainly reflected in the following aspects:

[0153] (1) Porous structure buffers volume expansion:

[0154] The porous silicon structure formed by etching aluminum-silicon alloy with hydrochloric acid provides space for silicon volume expansion at the mesoscale. During battery charging and discharging, silicon undergoes significant volume changes, and the porous structure can accommodate the expanded silicon, preventing silicon particle breakage and electrode structure damage caused by excessive volume expansion, thus ensuring the integrity and stability of the electrode.

[0155] (2) Optimization of interface interaction performance:

[0156] Lithium polyvinyl sulfonate is a lithium-containing polyelectrolyte. Its flexible polymer chains can encapsulate porous silicon, suppressing structural damage caused by volume expansion, and the Li in the sulfonic acid groups... + It provides an ion transport pathway and improves interfacial ion conductivity. After the composite conductive polymer is coated with porous silicon, the conductive polymer can better adhere to the surface of the porous silicon at the interface, further enhancing electron transport. Then, it is subjected to wet ultrasonic treatment with sulfide electrolyte to construct an ion exchange pathway between electrolyte and modified porous silicon, promote ion transport, and improve the electrochemical performance of the entire system.

[0157] The specific embodiments of this disclosure have been described above. It should be understood that this disclosure is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the substantive content of this disclosure. Industrial applicability

[0158] The modified porous silicon composite anode material disclosed herein alleviates the volume expansion of silicon-based anodes during charging and discharging through its porous structure, enhances electron conduction efficiency through coating with a composite conductive polymer, optimizes ion conduction pathways through composite with a sulfide electrolyte, and forms a stable interface buffer layer to suppress side reactions. This material can be used to prepare anode sheets, which, when combined with NCM811 cathode sheets and sulfide solid electrolyte sheets, form all-solid-state batteries. This significantly improves the stability of the anode interface, enhances battery cycle life and rate performance, and has important application value in the field of high-energy-density energy storage.

Claims

1. A method for preparing a modified porous silicon composite anode material, characterized in that, Includes the following steps: S1. Porous silicon is modified using a composite conductive polymer. The modified porous silicon material is obtained by extracting the reaction product and drying it. The composite conductive polymer is obtained by mixing and reacting PEDOT:PSS aqueous solution, lithium polyvinyl sulfonate aqueous solution and dimethyl sulfoxide. S2. The modified porous silicon material, sulfide electrolyte, and organic solvent are mixed and reacted under sealed conditions. The reaction product is extracted and dried to obtain the modified porous silicon composite anode material.

2. The method according to claim 1, characterized in that, It also includes one or more of the following technical features: A. The mass ratio of the PEDOT:PSS aqueous solution and the lithium polyvinyl sulfonate aqueous solution is (1-3):1; B. The mass ratio of the dimethyl sulfoxide and the PEDOT:PSS aqueous solution is (3-6):50; C. The mass ratio of the composite conductive polymer to porous silicon is (5-15):1; D. The mass ratio of PEDOT to PSS in the PEDOT:PSS aqueous solution is 1:(2-8); E. The concentration of the PEDOT:PSS aqueous solution is 0.8-2%; F. The concentration of the lithium polyvinyl sulfonate aqueous solution is 3.5–10.5 wt.%.

3. The method according to claim 1, characterized in that, The porous silicon was obtained by adding aluminum-silicon alloy powder to hydrochloric acid aqueous solution at 0°C and reacting for 4-10 hours, followed by washing, extraction of the reaction product and drying.

4. The method according to claim 3, characterized in that, It also includes one or more of the following technical features: A. The mass ratio of aluminum to silicon in the aluminum-silicon alloy powder is (5-7):4; B. The concentration of the hydrochloric acid aqueous solution is 8–12 wt.%.

5. The method according to claim 1, characterized in that, It also includes one or more of the following technical features: A. The mass ratio of the modified porous silicon to the sulfide electrolyte is (3-5):1; B. The ratio of the modified porous silica to the organic solvent is (0.8-1.2) g: 10 mL.

6. The method according to claim 1, characterized in that, It also includes one or more of the following technical features: A. The sulfide electrolyte is Li6PS5Cl; B. The organic solvent used is toluene.

7. The method according to claim 1, characterized in that, It also includes one or more of the following technical features: In steps A and S1, the modification treatment is carried out by magnetic stirring. B. The composite conductive polymer is mixed by magnetic stirring. C. The porous silicon is prepared by stirring and mixing using magnetic stirring. In steps D and S2, the modified porous silicon composite anode material is prepared by ultrasonic treatment to carry out the mixing reaction.

8. A modified porous silicon composite anode material, characterized in that, It is prepared by the method according to any one of claims 1 to 7.

9. An application of the modified porous silicon composite anode material according to claim 8.

10. The application according to claim 9, characterized in that, It also includes one or more of the following technical features: A. The negative electrode sheet in the battery is obtained by pressing the modified porous silicon composite negative electrode material; B. The positive electrode in the battery is formed by pressing together a mixture of ternary positive electrode material, sulfide solid electrolyte and conductive agent; C. The electrolyte sheet in the battery is made of sulfide electrolyte material.