Semiconductor structure and preparation method therefor
By setting a groove structure and forming a doped layer on the upper electrode layer of the DRAM capacitor structure, the problem of easy peeling of the conductive layer is solved, the bonding and contact area are enhanced, and the device performance is improved.
Patent Information
- Application Number
- PCT/CN2026/093888
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-29
- Publication Date
- 2026-11-12
AI Technical Summary
In DRAM capacitor structures, the adhesion between the conductive layer and the semiconductor layer is poor, which makes the conductive layer easy to peel off from the semiconductor layer, affecting device performance.
A groove structure is formed on the upper electrode layer, and a doped layer is formed on the side and bottom of the groove structure. A conductive layer covers the groove structure to improve the bonding and increase the contact area.
This improves the bonding between the upper electrode layer and the conductive layer, prevents the conductive layer from peeling off, reduces contact resistance, avoids short circuits, and enhances device performance.
Smart Images

Figure CN2026093888_12112026_PF_FP_ABST
Abstract
Description
Semiconductor structure and its preparation method
[0001] This application claims priority to Chinese Patent Application No. 202510584956.9, filed on May 7, 2025, entitled "Semiconductor Structure and Preparation Method Thereof", the entire contents of which are incorporated herein by reference. Technical Field
[0002] This disclosure relates to the field of semiconductor technology, and in particular to a semiconductor structure and its fabrication method. Background Technology
[0003] DRAM (Dynamic Random Access Memory) is a volatile semiconductor memory mainly used in computers and other electronic devices as main memory. Each memory cell of DRAM consists of a transistor and a capacitor, and data is stored through the charge of the capacitor.
[0004] Currently, in the capacitor structure of DRAM, multiple capacitors are often connected in parallel using an electrode layer. In order to reduce the resistance of the electrode layer, the electrode layer adopts a stacked structure formed by a semiconductor layer and a conductive layer. However, due to the poor adhesion between the conductive layer and the semiconductor layer, the conductive layer is easy to peel off from the semiconductor layer under stress, which affects the performance of the device. Summary of the Invention
[0005] In view of this, a semiconductor structure and its fabrication method are provided. The semiconductor structure improves the bonding between the upper electrode layer and the conductive layer by setting a groove structure on the upper electrode layer, thereby preventing the conductive layer from peeling off from the upper electrode layer. At the same time, it can also increase the contact area between the upper electrode layer and the conductive layer, thereby reducing the contact resistance.
[0006] Other features and advantages of this disclosure will become apparent from the following detailed description, or may be learned in part from practice of this disclosure.
[0007] According to one aspect of this disclosure, a semiconductor structure is provided, the semiconductor structure comprising:
[0008] Substrate;
[0009] Multiple lower electrodes are spaced apart on the substrate;
[0010] A dielectric layer is disposed on the plurality of lower electrodes;
[0011] The upper electrode is disposed on the dielectric layer;
[0012] An upper electrode layer is disposed on the upper electrode and fills the gaps between the plurality of lower electrodes. At least one groove structure is formed on the upper electrode layer, and the depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding position of the groove structure.
[0013] A conductive layer is disposed on the upper electrode layer and fills the groove structure.
[0014] In one exemplary embodiment of this disclosure, a doped layer is disposed between the upper electrode layer and the conductive layer, the doped layer covering at least one of the first surface, the side surface of the groove structure, or the bottom surface of the groove structure; wherein, the first surface is the surface of the upper electrode layer away from the substrate.
[0015] In one exemplary embodiment of this disclosure, the doped layer includes a first doped layer and a second doped layer, wherein the first doped layer is located on the first surface; and the second doped layer is located on the bottom surface of the groove structure and / or the side surface of the groove structure.
[0016] In one exemplary embodiment of this disclosure, the doping dose of the second doped layer is greater than the doping dose of the first doped layer.
[0017] In one exemplary embodiment of this disclosure, the thickness of the second doped layer is less than the thickness of the first doped layer.
[0018] In one exemplary embodiment of this disclosure, the orthographic projection of the first doped layer on the surface of the substrate overlaps the orthographic projection of the first surface on the surface of the substrate.
[0019] According to another aspect of this disclosure, a method for fabricating a semiconductor structure is provided, the method comprising:
[0020] Provide substrate;
[0021] Multiple lower electrodes are formed on the substrate;
[0022] A dielectric layer is formed, the dielectric layer covering the plurality of lower electrodes;
[0023] An upper electrode is formed, which conformally covers the dielectric layer;
[0024] An upper electrode layer is formed on the upper electrode, the upper electrode layer fills the gaps between the plurality of lower electrodes, and the surface of the upper electrode layer is parallel to the surface of the substrate;
[0025] The upper electrode layer is etched along a first direction to form at least one groove structure on the upper electrode layer. The depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding position of the groove structure. The first direction is perpendicular to the substrate and points from the upper electrode layer to the substrate.
[0026] A conductive layer is formed, which covers the surface of the upper electrode layer and fills the groove structure.
[0027] In one exemplary embodiment of this disclosure, prior to etching the upper electrode layer along a first direction to form at least one groove structure within the upper electrode layer, the method includes:
[0028] The upper electrode layer is doped along the first direction to form a first doped layer on the side of the upper electrode layer away from the substrate.
[0029] In one exemplary embodiment of this disclosure, after forming the first doped layer on the side of the upper electrode layer away from the substrate, the process includes:
[0030] The first doped layer and the remaining upper electrode layer are etched along the first direction to form the groove structure; the bottom surface of the groove structure is lower than the side of the first doped layer closest to the substrate.
[0031] In one exemplary embodiment of this disclosure, the process of forming the groove structure and before forming the conductive layer includes:
[0032] The bottom surface and / or the side surface of the groove structure are doped to form a second doped layer on the bottom surface and / or the side surface of the groove structure.
[0033] Wherein, the doping dose of the second doped layer is greater than that of the first doped layer, and the thickness of the second doped layer is less than that of the first doped layer.
[0034] In one exemplary embodiment of this disclosure, before forming the second doped layer on the bottom surface and / or the side surface of the groove structure, the following steps are included:
[0035] The sidewalls of the groove structure are etched using a wet etching process so that the orthogonal projection of the first doped layer on the surface of the substrate covers the orthogonal projection of the etched first surface on the surface of the substrate, wherein the first surface is the surface of the upper electrode layer away from the substrate.
[0036] The semiconductor structure disclosed herein includes at least one groove structure formed on the upper electrode layer, with a conductive layer disposed on the upper electrode layer and filling the groove structure. The groove structure improves the bonding between the upper electrode layer and the conductive layer, relieves contact stress, and prevents the conductive layer from peeling off from the upper electrode layer. It also increases the contact area between the upper electrode layer and the conductive layer, reducing contact resistance. Furthermore, the depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding location, preventing short circuits caused by contact between the conductive layer and structures below the upper electrode layer, thereby improving device performance. Attached Figure Description
[0037] Figure 1 is a schematic diagram of the structure of a capacitor in the prior art according to an exemplary embodiment of this disclosure.
[0038] Figure 2 is a flowchart of a method for fabricating a semiconductor structure in an exemplary embodiment of this disclosure.
[0039] Figure 3 is a schematic diagram of the semiconductor structure after the upper electrode layer is formed in an exemplary embodiment of the present disclosure.
[0040] Figure 4 is a schematic diagram of the structure of the semiconductor structure shown in Figure 2 after doping in an exemplary embodiment of this disclosure.
[0041] Figure 5 is a schematic diagram of the semiconductor structure after the groove structure is formed in an exemplary embodiment of the present disclosure.
[0042] Figure 6 is a top view of a semiconductor structure after etching of the groove structure in an exemplary embodiment of the present disclosure.
[0043] Figure 7 is a top view of another structure of the semiconductor structure after etching of the groove structure in the exemplary embodiment of this disclosure.
[0044] Figure 8 is an AA cross-sectional view of the semiconductor structure shown in Figures 6 and 7 in an exemplary embodiment of the present disclosure.
[0045] Figure 9 is a schematic diagram of a semiconductor structure forming a second doped layer in an exemplary embodiment of the present disclosure.
[0046] Figure 10 is a schematic diagram of another structure in which a semiconductor structure forms a second doped layer in an exemplary embodiment of the present disclosure.
[0047] Figure 11 is a schematic diagram of another structure in which a semiconductor structure forms a second doped layer in an exemplary embodiment of the present disclosure.
[0048] Figure 12 is a schematic diagram of a semiconductor structure in an exemplary embodiment of the present disclosure. Detailed Implementation
[0049] The technical solutions of this disclosure will be further described in detail below with reference to the accompanying drawings and embodiments. Although exemplary embodiments of this disclosure are shown in the drawings, it should be understood that this disclosure can be implemented in various forms and should not be limited to the embodiments described herein. Rather, these embodiments are provided to enable a more thorough understanding of this disclosure and to fully convey the scope of this disclosure to those skilled in the art.
[0050] The present disclosure is described in more detail below by way of example with reference to the accompanying drawings. The advantages and features of the present disclosure will become clearer from the following description and claims. It should be noted that the drawings are in a very simplified form and use non-precise proportions, and are only used to facilitate and clarify the illustration of the embodiments of the present disclosure.
[0051] It is understood that the meanings of “on”, “above” and “above” in this disclosure should be interpreted in the broadest sense, such that “on” means not only that it is “on” something without any intervening feature or layer (i.e., directly on something), but also that it is “on” something with an intervening feature or layer.
[0052] In the embodiments of this disclosure, the terms "first," "second," "third," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence.
[0053] In embodiments of this disclosure, the term "layer" refers to a portion of material comprising a region having thickness. A layer may extend over the entirety of a lower or upper structure, or may have a range smaller than that of the lower or upper structure. Furthermore, a layer may be a region of a homogeneous or heterogeneous continuous structure with a thickness less than the thickness of the continuous structure. For example, a layer may be located between the top and bottom surfaces of a continuous structure, or a layer may be located between any horizontal faces at the top and bottom surfaces of the continuous structure. A layer may extend horizontally, vertically, and / or along an inclined surface. A layer may include multiple sublayers.
[0054] It should be noted that the technical solutions described in the embodiments of this disclosure can be combined arbitrarily without conflict.
[0055] In related technologies, each memory cell of DRAM consists of a transistor and a capacitor, storing data through the capacitor's charge. As shown in Figure 1, the capacitor typically consists of a lower electrode 101, a dielectric layer 102, and an upper electrode 103. The dielectric layer 102 isolates the upper electrode 103 from the lower electrode 101. The upper electrode 103 is connected to the bit line via a transistor and directly participates in data reading and writing. Therefore, the structure of the upper electrode 103 determines the performance of the entire memory cell. Currently, in capacitor structures, a semiconductor layer 106 is generally used to connect the upper electrodes 103 of multiple memory cells in the array region in parallel. The semiconductor layer 106 is often made of silicon germanium (SiGe) film. To reduce the resistance of the semiconductor layer 106, a stacked structure of semiconductor layer 106 and conductive layer 105 is usually used instead of a single semiconductor layer 106. However, the bonding between the conductive layer 105 and the semiconductor layer 106 in this stacked structure is insufficient, and the conductive layer 105 is easily peeled off from the semiconductor layer 106, thus forming structural defects and affecting the overall performance of the device.
[0056] Based on this, the present disclosure provides a method for preparing a semiconductor structure, as shown in FIG2, the preparation method including: steps S10 to S70.
[0057] Step S10: Provide a substrate;
[0058] Step S20: Form a plurality of lower electrodes on the substrate;
[0059] Step S30: Form a dielectric layer covering multiple lower electrodes;
[0060] Step S40: Form the upper electrode, which is conformally covered by the dielectric layer;
[0061] Step S50: An upper electrode layer is formed on the upper electrode, the upper electrode layer fills the gap between multiple lower electrodes, and the surface of the upper electrode layer is parallel to the surface of the substrate.
[0062] Step S60: Etch the upper electrode layer along the first direction to form at least one groove structure on the upper electrode layer. The depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding position of the groove structure. The first direction is perpendicular to the substrate and points from the upper electrode layer to the substrate.
[0063] Step S70: Form a conductive layer that covers the surface of the upper electrode layer and fills the groove structure.
[0064] The semiconductor structure fabrication method disclosed herein involves etching an upper electrode layer along a first direction to form at least one groove structure on the upper electrode layer. A conductive layer covers the surface of the upper electrode layer and fills the groove structure. The groove structure formed by this method can improve the bonding between the upper electrode layer and the conductive layer, prevent the conductive layer from peeling off from the upper electrode layer, and the fabrication method is simple and easy to operate. It can improve device performance without affecting the overall fabrication process of the device.
[0065] The following will describe in detail each step of the semiconductor structure fabrication method provided in the embodiments of this disclosure with reference to the accompanying drawings:
[0066] In the embodiments provided in this disclosure, referring to Figures 3 to 12, in step S10, a substrate 100 is provided.
[0067] The substrate 100 can be a semiconductor substrate, such as a silicon (Si) substrate, a germanium (Ge) substrate, a silicon-germanium (GeSi) substrate, SOI (Silicon on Insulator), or GOI (Germanium on Insulator). In some embodiments, the semiconductor substrate can also be a substrate including other elemental semiconductors or compound semiconductors, such as silicon carbide (SiC), indium phosphide (InP), or gallium arsenide (GaAs). The substrate 100 can be selected according to the actual design requirements of the semiconductor structure, and this disclosure does not impose specific limitations.
[0068] In the embodiments provided in this disclosure, in step S20, as shown in FIG3, a plurality of lower electrodes 101 are formed on the substrate 100.
[0069] Forming a plurality of lower electrodes 101 on a substrate 100 includes: forming a stacked structure on the substrate 100, the stacked structure including a plurality of insulating layers and a plurality of support layers sequentially and alternately deposited on the substrate 100; forming a plurality of capacitor holes within the stacked structure; filling the capacitor holes with a lower electrode material layer; and etching the lower electrode material layer so that the surface of the lower electrode material layer is flush with the surface of the stacked structure to form the lower electrodes 101.
[0070] The insulating layer can be formed using materials such as silicon oxide (SiO2), and can be formed using one or more methods such as physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), thermal oxidation, and sol-gel. The thickness of the insulating layer can be 5 nm to 20 nm. The number of insulating layers, thickness, material, and fabrication process can all be selected or adapted according to the structural parameters of the device, and this disclosure does not impose specific limitations.
[0071] The support layer can be made of silicon nitride (Si2N2) or similar materials. It can be formed using one or more methods such as low-pressure chemical vapor deposition (LPCVD), plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), and sputtering. After the lower electrode 101 is formed, the support layer can support the lower electrode 101 and prevent it from collapsing. Especially for deep trench capacitors with high aspect ratios, the support layer can improve the reliability of the structure. Of course, in some semiconductor structures, the support layer may not be required. The support layer can be adjusted according to the needs of the semiconductor structure.
[0072] Capacitor vias can be formed by etching the stacked structure using dry etching, wet etching, or a combination of both processes.
[0073] In the embodiments provided in this disclosure, in step S30, as shown in FIG3, a dielectric layer 102 is formed, which covers a plurality of lower electrodes 101.
[0074] After forming the lower electrode 101, the process includes: removing the insulating layer; and depositing a dielectric layer 102 on the lower electrode 101. The dielectric layer 102 can be formed from materials such as silicon oxide (SiO2), silicon nitride (Si2N2), hafnium oxide (HfO2), zirconium oxide (ZrO2), and barium strontium titanate (BaSrTiO2). The thickness of the dielectric layer 102 can be 1 nm to 10 nm. It can be formed using one or more methods such as physical vapor deposition (PVD), chemical vapor deposition (CVD), atomic layer deposition (ALD), thermal oxidation, and sol-gel. The thickness, material, and formation process of the dielectric layer 102 can be selected according to the actual process requirements of the device, and this disclosure does not impose specific limitations.
[0075] In the embodiments provided in this disclosure, in step S40, as shown in FIG3, an upper electrode 103 is formed, and the upper electrode 103 conformally covers the dielectric layer 102.
[0076] After forming the dielectric layer 102, the process includes forming an upper electrode 103 that conformally covers the dielectric layer 102. The upper electrode 103 can be one of titanium nitride (TiN), tantalum nitride (TaN), or ruthenium (Ru), or a multilayer structure formed from multiple of these materials. The thickness of the upper electrode 103 can be 3 nm to 20 nm. It can be formed using one or more processes, including physical vapor deposition (PVD), chemical vapor deposition (CVD), and atomic layer deposition (ALD). The material, thickness, and formation process of the upper electrode 103 can be selected according to the actual process requirements of the device, and this disclosure does not impose specific limitations.
[0077] In the embodiments provided in this disclosure, in step S50, as shown in FIG3, an upper electrode layer 104 is formed on the upper electrode 103. The upper electrode layer 104 fills the gap between the plurality of lower electrodes 101, and the surface of the upper electrode layer 104 is parallel to the surface of the substrate 100.
[0078] The upper electrode layer 104 can be a semiconductor layer, such as a germanium-silicon (SiGe) or boron-silicon (SiB) doped semiconductor layer. The upper electrode layer 104 is formed on the upper electrode 103, and the upper electrodes 103 of multiple capacitors can be connected through the upper electrode layer 104 to improve the performance of the device. Taking germanium-silicon (SiGe) as an example, the thickness of the upper electrode layer 104 can be 150nm to 250nm. The upper electrode layer 104 can be formed by one or more methods such as chemical vapor deposition (CVD), molecular beam epitaxy (MBE), and selective epitaxial growth (SEG). The material, thickness, and formation process of the upper electrode layer 104 can be selected according to the actual process requirements of the device, and this disclosure does not impose specific limitations.
[0079] In the embodiments provided in this disclosure, in step S60, as shown in FIG5, the upper electrode layer 104 is etched along the first direction X to form at least one groove structure 201 on the upper electrode layer 104. The depth of the groove structure 201 is less than the thickness of the upper electrode layer 104 at the corresponding position of the groove structure 201. The first direction X is a direction perpendicular to the substrate and pointing from the upper electrode layer 104 to the substrate 100.
[0080] As shown in Figure 4, before step S60, the process includes: doping the upper electrode layer 104 along the first direction X to form a first doped layer 301 on the side of the upper electrode layer 104 away from the substrate.
[0081] The upper electrode layer 104 can be doped with a Group III element, such as at least one of boron, gallium, indium, and thallium. This disclosure uses boron as an example for the doping process. When other doping elements are used, the doping process and conditions can be adjusted according to the type of doping element.
[0082] In some specific embodiments, the doping treatment of the upper electrode layer 104 along the first direction X can be performed by plasma doping (PLAD) to dope boron onto the surface of the upper electrode layer 104. The plasma doping can use a boron-containing gas, such as B₂H₂ or BH₃, and the doping dose can be 1 × 10⁻⁶. 16 ions / cm 2 (Number of ions per square centimeter) ~ 1×10 17 ions / cm 2 The doping process pressure is 5 mTorr to 20 mTorr.
[0083] The doping process may include: introducing a dopant gas onto the surface of the upper electrode layer 104, generating a plasma by radio frequency (RF) or microwave excitation to produce boron ions and free radicals; applying a bias voltage to the substrate 100, which can be 1kV to 10kV, and the ions are accelerated by the electric field to bombard the surface of the upper electrode layer 104; implanting boron ions into the surface layer of the upper electrode layer 104; and activating the doped atoms in the upper electrode layer 104 by an annealing process.
[0084] To avoid adverse effects of high-temperature annealing on the dielectric layer 102 within the structure, laser annealing can be used to activate boron ions in the upper electrode layer 104. The activation depth of the boron ions is less than or equal to 10 nm, so that the activated boron ions can form a high concentration of holes in the upper electrode layer 104. For example, the hole concentration can be greater than 1 × 10⁻⁶. 18 cm -3 When the subsequent conductive layer comes into contact with the upper electrode layer 104, the first doped layer 301 can reduce the contact resistance between the two, thereby improving the device performance.
[0085] As shown in Figure 5, after forming the first doped layer 301 on the side of the upper electrode layer 104 away from the substrate, the process includes etching the first doped layer 301 and the remaining upper electrode layer 104 along the first direction X to form a groove structure 201.
[0086] The number of groove structures 201 can be one, two, three, four, five, ten, fifty, one hundred, or even more. When there are multiple groove structures 201, they can be spaced apart in the upper electrode layer 104. In some embodiments, the spacing between the multiple groove structures 201 can be equal; in some embodiments, the spacing between some groove structures 201 is equal, while the spacing between some groove structures 201 is unequal; in some embodiments, the spacing between all groove structures 201 is unequal. In this disclosure, the number of groove structures 201 and the spacing between multiple groove structures 201 can be selected and adaptively adjusted according to actual design requirements, and this disclosure does not impose specific limitations.
[0087] The first doped layer 301 and the remaining upper electrode layer 104 can be etched using dry etching, wet etching, or a combination of both to form the groove structure 201. In some embodiments, the bottom surface 221 of the groove structure is flush with the side of the first doped layer 301 near the substrate 100; in other embodiments, the bottom surface 221 of the groove structure is lower than the side of the first doped layer 301 near the substrate 100. For example, when the thickness of the first doped layer 301 is 10 nm, the depth of the groove structure 201 formed at the corresponding location is at least 10 nm. Of course, depending on the thickness of the upper electrode layer 104 at different locations, the thickness of the corresponding first doped layer 301 can be different, and the depth of the formed groove structure 201 can also be different. Furthermore, to simplify the process, the depth of the groove structure 201 located at different positions of the upper electrode layer 104 can also be the same. In addition, the depth of each groove structure 201 must be less than the thickness of the upper electrode layer 104 at the corresponding position of the groove structure 201, so as to avoid the occurrence of device short circuit caused by the groove structure 201 penetrating the upper electrode layer 104.
[0088] Due to process limitations, when etching the first doped layer 301 and the remaining upper electrode layer 104, the angle between the side surface 211 of the formed groove structure 201 and the surface of the substrate 100 is within the range of 90°±10° due to the difference in the etch ratio. Furthermore, the side surface 211 and the bottom surface 212 of the groove structure 201 can be a strictly planar structure, an inclined structure, or a surface structure with wavy, sawtooth, or other similar structures.
[0089] In some embodiments, as shown in Figures 6, 7, and 8, in order to further increase the surface area of the groove structure 201, thereby increasing the contact area between the subsequent conductive layer 105 and the upper electrode layer 104 and reducing the contact resistance, after etching the first doped layer 301 and the remaining upper electrode layer 104 to form the groove structure 201, the method includes: etching the side surface 211 of the groove structure 201 using a wet etching process, so that the orthographic projection of the first doped layer 301 on the surface of the substrate 100 covers the orthographic projection of the etched first surface 114 on the surface of the substrate 100, wherein the first surface 114 is the surface of the upper electrode layer 104 away from the substrate 100. Meanwhile, in the direction Y parallel to the surface of the substrate 100, the first doped layer 301 has a large width, and both ends of the first doped layer 301 can extend above the groove structure 201. Thus, when the conductive layer 105 is deposited in the groove structure 201, the contact area between the conductive layer 105 and the upper electrode layer 104 can be increased, which is beneficial for the conductive layer 105 to release stress and thus can reduce the risk of the conductive layer 105 falling off.
[0090] Wet etching can be used to etch one side of the groove structure 201 or to etch both sides of the groove structure 201 simultaneously, both of which can increase the surface area of the groove structure 201. Of course, given the etching process, wet etching is usually used to etch both sides of the groove structure 201 simultaneously.
[0091] After etching the side surface 211 of the groove structure, as shown in Figures 6 and 7, the orthographic projection of the first doped layer 301 on the surface of the substrate 100 covers the orthographic projection of the etched first surface 114 on the surface of the substrate 100. The ratio between the orthographic projection of the etched first surface 114 on the surface of the substrate 100 and the orthographic projection of the first doped layer 301 on the surface of the substrate 100 can be 50% to 95%. This ensures both an increase in the surface area of the groove structure 201 and the support of the upper electrode layer 104 for the first doped layer 301.
[0092] As shown in Figures 9, 10 and 11, after etching the side surface 211 of the groove structure 201 using a wet etching process and before forming the conductive layer 105, the process includes: doping the bottom surface 221 and / or the side surface 211 of the groove structure 201 to form a second doped layer 302 on the bottom surface 221 and / or the side surface 211 of the groove structure 201.
[0093] In some embodiments, as shown in FIG9, only the bottom surface 221 of the groove structure 201 may be doped to form a second doped layer 302 on the bottom surface 221 of the groove structure. When the second doped layer 302 is formed only on the bottom surface 221 of the groove structure 201, a patterned mask layer (not shown in the figure) may be used to cover the side surface 211 of the groove structure 201 before the bottom surface 221 of the groove structure 201 is doped. After the second doped layer 302 is formed on the bottom surface 221 of the groove structure 201, the patterned mask layer is removed to expose the side surface 211 of the groove structure 201.
[0094] In some embodiments, as shown in FIG10, the bottom surface 221 and the side surface 211 of the groove structure 201 can be doped simultaneously to form a second doped layer 302 on the bottom surface 221 and the side surface 211 of the groove structure 201.
[0095] In some embodiments, as shown in FIG11, only the side surface 211 of the groove structure 201 may be doped to form a second doped layer 302 on the side surface 211 of the groove structure 201. When the second doped layer 302 is formed only on the side surface 211 of the groove structure 201, a patterned mask layer (not shown in the figure) may be used to cover the bottom surface 221 of the groove structure 201 before the side surface 211 of the groove structure 201 is doped. After the second doped layer 302 is formed on the side surface 211 of the groove structure 201, the patterned mask layer is removed to expose the bottom surface 221 of the groove structure 201.
[0096] In the above embodiments, the formation process of the second doped layer 302 is the same as or similar to the formation process of the first doped layer 301, and will not be repeated here.
[0097] Since the second doped layer is formed within the groove structure 201, in order to ensure the formation quality of the second doped layer, the doping dose of the second doped layer 302 is greater than that of the first doped layer 301, so as to ensure that the second doped layer 302 with a high concentration of doped ions is formed within the groove structure 201, thereby reducing the resistance of the second doped layer 302.
[0098] In order to prevent dopant elements (such as boron ions) from diffusing into the capacitor structure and causing a short circuit, the thickness of the second doped layer 302 is smaller than the thickness of the first doped layer 301. This prevents short circuits caused by the diffusion of dopant ions into the capacitor structure and improves the overall performance of the device.
[0099] In the embodiments provided in this disclosure, as shown in FIG12, in step S70, a conductive layer 105 is formed, which covers the surface of the upper electrode layer 104 and fills the groove structure 201. The conductive layer 105 may be made of a metallic material, such as tungsten (W) or tungsten nitride (WN), and its thickness may be 50 nm to 150 nm. The conductive layer 105 may be formed using one or more processes selected from chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD). The material, thickness, and formation process of the conductive layer 105 can be selected according to the actual process requirements of the device, and this disclosure does not impose specific limitations.
[0100] The semiconductor structure fabrication method disclosed herein increases the contact area between the upper electrode layer 104 and the conductive layer 105 by forming a groove structure 201 on the upper electrode layer 104, thereby reducing the contact resistance of the structure and improving the device performance. The fabrication process of the groove structure 201 is relatively simple and will not affect the overall process flow.
[0101] This fabrication method can be used to fabricate capacitor structures in DRAM devices. Of course, the application of this fabrication method to other types of semiconductor structures and the adaptive modifications of this fabrication method are all within the scope of protection of this disclosure.
[0102] It should be noted that although the steps of the semiconductor structure fabrication method in this disclosure are described in a specific order in the accompanying drawings, this does not require or imply that these steps must be performed in that specific order, or that all the steps shown must be performed to achieve the desired result. Additional or alternative steps may be omitted, multiple steps may be combined into one step, and / or one step may be broken down into multiple steps.
[0103] This disclosure provides a semiconductor structure, as shown in FIG12, and in conjunction with FIGS. 3 to 11, the semiconductor structure includes: a substrate 100, a plurality of lower electrodes 101, a dielectric layer 102, an upper electrode 103, an upper electrode layer 104, and a conductive layer 105.
[0104] In this configuration, multiple lower electrodes 101 are spaced apart on the substrate 100; a dielectric layer 102 is disposed on the multiple lower electrodes 101; an upper electrode 103 is disposed on the dielectric layer 102; an upper electrode layer 104 is disposed on the upper electrode 103 and fills the gaps between the multiple lower electrodes 101; at least one groove structure 201 is formed on the upper electrode layer 104, and the depth of the groove structure 201 is less than the thickness of the upper electrode layer 104 at the corresponding position of the groove structure 201; a conductive layer 105 is disposed on the upper electrode layer 104 and fills the groove structure 201.
[0105] The semiconductor structure provided in this disclosure, by forming at least one groove structure 201 on the upper electrode layer 104, and disposing a conductive layer 105 on the upper electrode layer 104 and filling the groove structure 201, can improve the bonding between the upper electrode layer 104 and the conductive layer 105, release contact stress, and prevent the conductive layer 105 from peeling off from the upper electrode layer 103. Furthermore, it can increase the contact area between the upper electrode layer 104 and the conductive layer 105, reducing contact resistance. Thirdly, the depth of the groove structure 201 is less than the thickness of the upper electrode layer 104 at the corresponding position, which can prevent the conductive layer 105 from contacting structures located below the upper electrode layer 104, thus preventing short circuits and improving device performance.
[0106] The various parts of the semiconductor structure provided in the embodiments of this disclosure will now be described in detail with reference to the accompanying drawings:
[0107] In the embodiments provided in this disclosure, as shown in Figures 3 to 12, the substrate 100 can be a semiconductor substrate, such as a silicon (Si) substrate, a germanium (Ge) substrate, a silicon-germanium (GeSi) substrate, SOI (Silicon on Insulator), or GOI (Germanium on Insulator). In some embodiments, the semiconductor substrate can also be a substrate including other elemental semiconductors or compound semiconductors, such as silicon carbide (SiC), indium phosphide (InP), or gallium arsenide (GaAs). The substrate 100 can be selected according to the actual design requirements of the semiconductor structure, and this disclosure does not impose specific limitations.
[0108] The substrate 100 provided in this disclosure may also include other device structures for forming memory cells, such as transistors, word line structures, and shallow trench isolation structures. Although the embodiments provided in this disclosure do not describe in detail the other device structures on the substrate 100, it should be understood that the semiconductor structures of this disclosure include other device structures for forming memory.
[0109] In the embodiments provided in this disclosure, as shown in FIG12, a plurality of lower electrodes 101 are disposed at intervals on the substrate 100. The plurality of lower electrodes 101 can be arranged in an array at intervals on the substrate 100. Each lower electrode 101 can be formed of a conductive material or a metal-containing material, for example, the conductive material can be doped polycrystalline silicon, and the metal-containing material can be titanium nitride, etc. The material of each lower electrode 101 can be selected and adapted according to actual process and structural requirements, and this disclosure does not impose specific limitations. Each lower electrode 101 can have a columnar or quasi-columnar shape, for example, a cylindrical shape.
[0110] In the embodiments provided in this disclosure, as shown in FIG12, a dielectric layer 102 is disposed on a plurality of lower electrodes 101. The dielectric layer 102 may cover the sidewalls and top surface of each lower electrode 101. In subsequent processes, the dielectric layer 102 may be used to isolate the upper electrode 103 and the lower electrode 101 to ensure electrical isolation between the upper and lower electrodes 101.
[0111] The dielectric layer 102 can be formed of materials such as silicon oxide (SiO2), silicon nitride (Si2N2), hafnium oxide (HfO2), zirconium oxide (ZrO2), and barium strontium titanate (BaSrTiO2). The thickness of the dielectric layer 102 can be 1nm to 10nm. The thickness and material of the dielectric layer 102 can be selected according to actual process requirements. The above embodiments are only illustrative. With the development of the miniaturization process of the process structure, the material of the dielectric layer 102 can be other insulating materials, and the thickness of the dielectric layer 102 can be thinner. The dielectric layer 102 in the semiconductor structure of this disclosure can be changed accordingly, all of which are within the protection scope of this disclosure.
[0112] In the embodiments provided in this disclosure, as shown in FIG12, the upper electrode 103 is disposed on the dielectric layer 102, and the upper electrode 103 conformally covers the dielectric layer 102. The upper electrode 103 can be one of the materials such as titanium nitride (TiN), tantalum nitride (TaN), or ruthenium (Ru), or a multilayer structure formed by multiple of the above materials. In this disclosure, titanium nitride is used as an example for the upper electrode 103, but upper electrodes 103 formed of other materials are still within the scope of protection of this disclosure. The thickness of the upper electrode 103 can be 3nm to 20nm. With the development of miniaturization of process structures, the material of the upper electrode 103 can be other materials, and the thickness of the upper electrode 103 can be thinner. The upper electrode 103 in the semiconductor structure of this disclosure can vary accordingly, all of which are within the scope of protection of this disclosure.
[0113] In the embodiments provided in this disclosure, as shown in FIG12, an upper electrode layer 104 is disposed on the upper electrode 103 and fills the gaps between multiple lower electrodes 101. The upper electrode layer 104 can be a semiconductor layer, such as a germanium-silicon (SiGe) or boron-silicon (SiB) doped semiconductor layer. The upper electrode layer 104 is formed on the upper electrode 103, and the upper electrodes 103 of multiple capacitors can be connected through the upper electrode layer 104 to improve the performance of the device. The embodiments of this disclosure are described using germanium-silicon (SiGe) as an example of the upper electrode layer 104. When other materials are used for the upper electrode layer 104, its thickness and other parameters will change with the material of the upper electrode layer 104.
[0114] The thickness of the upper electrode layer 104 can be 150nm to 250nm, for example, it can be 150nm, 180nm, 200nm, 220nm, 250nm, etc. The thickness of the upper electrode layer 104 can refer to the minimum distance between the surface of the upper electrode layer 104 and the surface of the upper electrode 103.
[0115] As shown in Figures 5, 8 to 11, at least one groove structure 201 is formed on the upper electrode layer 104. For example, the number of groove structures 201 can be one, two, three, four, five, ten, fifty, one hundred, or even more. When there are multiple groove structures 201, they can be spaced apart in the upper electrode layer 104. In some embodiments, the spacing between the multiple groove structures 201 can be equal; in some embodiments, the spacing between some groove structures 201 is equal, while the spacing between some groove structures 201 is unequal; in some embodiments, the spacing between all groove structures 201 is unequal. In this disclosure, the number of groove structures 201 and the spacing between multiple groove structures 201 can be selected and adaptively adjusted according to actual design requirements, and this disclosure does not impose specific limitations.
[0116] In each groove structure 201, the depth must be less than the thickness of the upper electrode layer 104 at the corresponding position to avoid short circuits caused by the groove structure 201 penetrating the upper electrode layer 104. The ratio of the depth of the groove structure 201 to the thickness of the upper electrode layer 104 at the corresponding position can be 5% to 80%, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, or 80%. In some specific embodiments, when the thickness of the upper electrode layer 104 is 200 nm, the depth of the groove structure 201 at the corresponding position can be 20 nm; in some specific embodiments, when the thickness of the upper electrode layer 104 is 100 nm, the depth of the groove structure 201 at the corresponding position can be 10 nm.
[0117] The present invention provides a groove structure 201 in the upper electrode layer 104, which can increase the contact area between the upper electrode layer 104 and the subsequent film layer and reduce the contact resistance. Due to the setting of the groove structure 201, the bonding between the upper electrode layer 104 and the subsequent film layer can be improved and the contact stress can be reduced, thereby avoiding the subsequent film layer from peeling off on the upper electrode layer 104 and causing structural defects.
[0118] It should be noted that the side surface 211 of the groove structure 201 provided in this disclosure can be perpendicular to the surface of the substrate 100. The side surface 211 of the groove structure 201 and the surface of the substrate 100 can be strictly perpendicular to each other, i.e., the angle between them is 90°. However, in actual manufacturing processes, due to process errors, the angle between the side surface 211 of the groove structure 201 and the surface of the substrate 100 can be 90° ± 10°, all of which are understood to be within the protection scope of this disclosure. Furthermore, due to different fabrication processes, the side surface 211 and bottom surface 221 of the groove structure 201 can be strictly planar, inclined, or have wavy, sawtooth, or other surface structures, all of which fall under the protection of the groove structure 201 of this disclosure.
[0119] In the embodiments provided in this disclosure, as shown in FIG12 and in conjunction with FIG9, a conductive layer 105 is disposed on the upper electrode layer 104 and fills the groove structure 201. The conductive layer 105 may be made of a metallic material, such as tungsten (W) or tungsten nitride (WN). The thickness of the conductive layer 105 may be 50 nm to 150 nm, for example, 50 nm, 80 nm, 100 nm, 120 nm, 150 nm, etc. The thickness of the conductive layer 105 may refer to the minimum distance between the surface of the conductive layer 105 and the surface of the upper electrode layer 104.
[0120] In this disclosure, since the conductive layer 105 extends into the groove structure 201, the contact area between the upper electrode layer 104 and the conductive layer 105 can be increased through the groove structure 201, reducing the contact stress. Furthermore, the groove structure 201 also has a certain fixing effect on the conductive layer 105 in the direction parallel to the surface of the substrate, thereby preventing the conductive layer 105 from peeling off from the upper electrode layer 104.
[0121] In some embodiments, a doped layer is provided between the upper electrode layer 104 and the conductive layer 105. By providing a doped layer between the upper electrode layer 104 and the conductive layer 105, the contact resistance between the upper electrode layer 104 and the conductive layer 105 is reduced, thereby further improving the performance of the device.
[0122] The doped layer can be a semiconductor film layer containing doped elements. Furthermore, to improve the simplicity of the doped layer fabrication process and the compatibility between the doped layer and the upper electrode layer 104, the doped layer can typically use the upper electrode layer 104 as a substrate, and be doped on the surface of the upper electrode layer 104 to form the doped layer. That is, the elements present in the doped layer are at least partially the same as those present in the upper electrode layer 104. Taking germanium-silicon (SiGe) as an example, the doped layer also contains germanium-silicon. In addition, the doped layer contains doped elements, which are Group III elements. For example, the doped element can be at least one of boron, gallium, indium, and thallium. By doping the upper electrode layer 104, a high concentration of holes can be generated within the upper electrode layer 104, thereby reducing the resistance of the upper electrode layer 104 and improving its processing performance. The hole concentration in the doped layer can be greater than 1 × 10⁻⁶. 18 cm -3 This is to improve the performance of the upper electrode layer 104.
[0123] The doped layer can cover at least one of the first surface 114, the side surface 211 of the groove structure 201, or the bottom surface 221 of the groove structure 201. The first surface 114 is the surface of the upper electrode layer 104 away from the substrate 100.
[0124] In some embodiments, the doped layer may cover only one of the first surface 114, the side surface 211 of the groove structure 201, or the bottom surface 221 of the groove structure 201; in some embodiments, the doped layer may cover two of the first surface 114, the side surface 211 of the groove structure, or the bottom surface 221 of the groove structure; in some embodiments, the doped layer may cover the surface formed by the first surface 114, the side surface 211 of the groove structure, or the bottom surface 221 of the groove structure. The doped layer may consist of multiple discontinuously distributed film layers or a single continuously distributed film layer. The distribution position of the doped layer can be selected and adaptively adjusted according to the actual design and process requirements of the semiconductor structure, and this disclosure does not impose specific limitations.
[0125] In some embodiments, as shown in FIG12, the doped layer may include a first doped layer 301 and a second doped layer 302, wherein the first doped layer 301 is located on the first surface 114, and the second doped layer 302 is located on the bottom surface 221 and / or the side surface 211 of the groove structure 201.
[0126] In some specific embodiments, as shown in FIG9, the second doped layer 302 is located only on the bottom surface 221 of the groove structure 201. In some specific embodiments, as shown in FIG10, the second doped layer 302 is located on both the bottom surface 221 and the side surface 211 of the groove structure 201. In some specific embodiments, as shown in FIG11, the second doped layer 302 is located only on the side surface 211 of the groove structure 201. The process of forming the second doped layer 302 within the groove structure 201 can be found in the above-described preparation method section, and will not be repeated here.
[0127] By using different process steps and sequences, doped layers with different properties can be formed at different locations on the upper electrode layer 104 to meet the performance requirements of the structure.
[0128] In some embodiments, as shown in Figures 6 and 7, the orthographic projection of the first doped layer 301 on the surface of the substrate 100 overlaps the orthographic projection of the first surface 114 on the surface of the substrate 100. Simultaneously, in the direction Y parallel to the surface of the substrate 100, the first doped layer 301 has a large width, and both ends of the first doped layer 301 can extend above the groove structure 201. This increases the contact area between the conductive layer 105 and the upper electrode layer 104 when the conductive layer 105 is deposited in the groove structure 201, which helps release stress in the conductive layer 105 and reduces the risk of the conductive layer 105 detaching.
[0129] Since the second doped layer is formed within the groove structure 201, in order to ensure the formation quality of the second doped layer, the doping dose of the second doped layer 302 is greater than that of the first doped layer 301, so as to ensure that the second doped layer 302 with a high concentration of doped ions is formed within the groove structure 201, thereby reducing the resistance of the second doped layer 302.
[0130] In order to prevent dopant elements (such as boron ions) from diffusing into the capacitor structure and causing a short circuit, the thickness of the second doped layer 302 is smaller than the thickness of the first doped layer 301. This prevents short circuits caused by the diffusion of dopant ions into the capacitor structure and improves the overall performance of the device.
[0131] It should be noted that the semiconductor structure provided in this disclosure can be fabricated using the semiconductor structure fabrication method provided in the above embodiments. This semiconductor structure can be a capacitor structure in a DRAM device; of course, the semiconductor structure provided in this disclosure can also be other types of devices or device structures, and this disclosure does not impose any specific limitations.
[0132] The above description is merely a specific embodiment of this disclosure, but the scope of protection of this disclosure is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this disclosure should be included within the scope of protection of this disclosure. Therefore, the scope of protection of this disclosure should be determined by the scope of the claims.
Claims
1. A semiconductor structure, characterized in that, include: Substrate; Multiple lower electrodes are spaced apart on the substrate; A dielectric layer is disposed on the plurality of lower electrodes; The upper electrode is disposed on the dielectric layer; An upper electrode layer is disposed on the upper electrode and fills the gaps between the plurality of lower electrodes. At least one groove structure is formed on the upper electrode layer, and the depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding position of the groove structure. A conductive layer is disposed on the upper electrode layer and fills the groove structure.
2. The semiconductor structure according to claim 1, characterized in that, A doped layer is disposed between the upper electrode layer and the conductive layer, and the doped layer covers at least one of the first surface, the side surface of the groove structure, or the bottom surface of the groove structure; wherein, the first surface is the surface of the upper electrode layer away from the substrate.
3. The semiconductor structure according to claim 2, characterized in that, The doped layer includes a first doped layer and a second doped layer, wherein the first doped layer is located on the first surface; and the second doped layer is located on the bottom surface of the groove structure and / or the side surface of the groove structure.
4. The semiconductor structure according to claim 3, characterized in that, The doping dose of the second doped layer is greater than that of the first doped layer.
5. The semiconductor structure according to claim 3, characterized in that, The thickness of the second doped layer is less than the thickness of the first doped layer.
6. The semiconductor structure according to any one of claims 3-5, characterized in that, The orthographic projection of the first doped layer on the surface of the substrate overlaps the orthographic projection of the first surface on the surface of the substrate.
7. A method for fabricating a semiconductor structure, characterized in that, include: Provide substrate; Multiple lower electrodes are formed on the substrate; A dielectric layer is formed, the dielectric layer covering the plurality of lower electrodes; An upper electrode is formed, which conformally covers the dielectric layer; An upper electrode layer is formed on the upper electrode, the upper electrode layer fills the gaps between the plurality of lower electrodes, and the surface of the upper electrode layer is parallel to the surface of the substrate; The upper electrode layer is etched along a first direction to form at least one groove structure on the upper electrode layer. The depth of the groove structure is less than the thickness of the upper electrode layer at the corresponding position of the groove structure. The first direction is perpendicular to the substrate and points from the upper electrode layer to the substrate. A conductive layer is formed, which covers the surface of the upper electrode layer and fills the groove structure.
8. The method for preparing a semiconductor structure according to claim 7, characterized in that, Before etching the upper electrode layer along the first direction to form at least one groove structure within the upper electrode layer, the process includes: The upper electrode layer is doped along the first direction to form a first doped layer on the side of the upper electrode layer away from the substrate.
9. The method for preparing a semiconductor structure according to claim 8, characterized in that, After forming the first doped layer on the side of the upper electrode layer away from the substrate, the process includes: The first doped layer and the remaining upper electrode layer are etched along the first direction to form the groove structure; the bottom surface of the groove structure is lower than the side of the first doped layer closest to the substrate.
10. The method for preparing a semiconductor structure according to claim 9, characterized in that, The process after forming the groove structure and before forming the conductive layer includes: The bottom surface and / or the side surface of the groove structure are doped to form a second doped layer on the bottom surface and / or the side surface of the groove structure. Wherein, the doping dose of the second doped layer is greater than that of the first doped layer, and the thickness of the second doped layer is less than that of the first doped layer.
11. The method for preparing a semiconductor structure according to claim 10, characterized in that, Before forming the second doped layer on the bottom surface and / or the side surface of the groove structure, the process includes: The sidewalls of the groove structure are etched using a wet etching process so that the orthogonal projection of the first doped layer on the surface of the substrate covers the orthogonal projection of the etched first surface on the surface of the substrate, wherein the first surface is the surface of the upper electrode layer away from the substrate.