Glass-ceramic panel having rough surface, and preparation method therefor
By coating the surface of the microcrystalline glass panel with a colorless and transparent coating and controlling the surface roughness and morphology parameters, the problems of appearance, fingerprint resistance and scratch resistance of the microcrystalline glass panel are solved. The comprehensive optimization of black visual effect, fingerprint resistance and infrared transmittance is achieved, which is suitable for high-end display devices, kitchen appliances and decorative panels.
Patent Information
- Application Number
- PCT/CN2026/095904
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-12-26
- Filing Date
- 2026-05-09
- Publication Date
- 2026-11-12
AI Technical Summary
Existing microcrystalline glass panels suffer from poor appearance, are prone to fingerprints, are not scratch-resistant, and have low heating efficiency. In particular, it is difficult to improve fingerprint resistance and scratch resistance at the same time while maintaining a black visual effect and infrared transmittance.
A colorless and transparent coating is applied to the surface of the microcrystalline glass body. The coating surface has non-sharp protrusions. By controlling the surface roughness and morphology parameters, the microcrystalline glass panel has 0.5μm≤Ra≤2.5μm and 2.5≤Rc/Rq≤3.5. The coating does not contain colorants to maintain high infrared transmittance. Furthermore, the scratch resistance is improved by reasonably controlling the coating composition and surface structure.
It achieves a deeper and more uniform black visual effect, improves fingerprint resistance and scratch resistance, while maintaining high infrared transmittance, making it suitable for high-end display devices, kitchen appliances and decorative panels.
Smart Images

Figure CN2026095904_12112026_PF_FP_ABST
Abstract
Description
A microcrystalline glass panel with a rough surface and its preparation method
[0001] This application claims priority to Chinese Patent Application No. 202511995472.X, filed on December 26, 2025, entitled "A Microcrystalline Glass Panel with Rough Surface and a Method for Preparing the Same", the entire contents of which are incorporated herein by reference. Technical Field
[0002] This invention relates to the field of microcrystalline glass panels, specifically to a microcrystalline glass panel with a rough surface and its preparation method. Background Technology
[0003] Due to its high mechanical strength, good thermal stability, strong chemical inertness, and excellent optical uniformity in the visible light range, glass-ceramic has been widely used in high-end display devices, kitchen appliances, and decorative panels. To meet visual color rendering and functional requirements, a typical glass-ceramic panel consists of a glass-ceramic body and a surface coating.
[0004] However, existing microcrystalline glass technologies suffer from poor appearance, susceptibility to fingerprints and scratches, and low heating efficiency. Summary of the Invention
[0005] Based on the above issues, it is a pressing technical challenge to simultaneously ensure that microcrystalline glass panels possess excellent fingerprint resistance and scratch resistance while maintaining a black visual effect and without reducing infrared transmittance.
[0006] This invention provides a microcrystalline glass panel with a rough surface.
[0007] The microcrystalline glass panel includes a microcrystalline glass body and a coating applied to the surface of the microcrystalline glass body;
[0008] The microcrystalline glass body contains a colorant; the coating does not contain a colorant.
[0009] The CIELab color space coordinates of the microcrystalline glass panel are: L*≥24, -2.5≤b*≤0, -0.3≤a*≤0.5;
[0010] At least a portion of the surface of the microcrystalline glass panel has non-sharp protrusions, and the microcrystalline glass panel has a thickness of 0.5μm≤Ra≤2.5μm, and satisfies 2.5≤Rc / Rq≤3.5; where Ra is the arithmetic mean deviation of the profile, Rc is the average height of the profile unit, and Rq is the root mean square deviation of the profile.
[0011] The microcrystalline glass panel has a transmittance of ≥60% at 1600nm.
[0012] Preferably, the microcrystalline glass panel has an Rc ≤ 10 μm.
[0013] Preferably, the non-sharp protrusion has an arc-shaped or ellipsoidal peak structure.
[0014] Preferably, the Ra of the microcrystalline glass body is 0.005 to 2.2 μm.
[0015] Preferably, the coating comprises, by weight percentage:
[0016] The coating contains 7.2–9.8% Al2O3, 58.2–66.1% SiO2, 1.2–3.8% K2O, 2.3–4.9% Na2O, 15.2–19.3% B2O3, 1.7–2.1% BaO, 0.9–2.8% Li2O, 0.07–0.35% TiO2, and 1.3–3.6% ZrO2. It does not contain any colorants, especially PbO, Fe2O3, and ZnO. That is, PbO, Fe2O3, and ZnO exist only as unavoidable impurities in the coating. None of the three are present, and their mass percentage content is ≤0.05%. It also does not contain any other colorants.
[0017] Preferably, the microcrystalline glass panel has a Mohs hardness of not less than 6.
[0018] Preferably, the microcrystalline glass body comprises, by weight percentage:
[0019] SiO2 62-68%, Al2O3 19-23%, Li2O 2.8-4.3%, Na2O+K2O 0-1.2%, BaO 1-3%, CaO 0-1%, MgO+ZnO 0-4%, P2O5 0-2%, TiO2 2-4%, ZrO2 1-2%, clarifying agent 0.2-1.5%, coloring agent 0.02-1%;
[0020] The clarifying agent is any one or more of As2O3, Sb2O3, SnO2, and CeO2; the coloring agent is any one or more of V2O5, CoO, NiO, Cr2O3, MnO, and Fe2O3.
[0021] Preferably, the composition of the microcrystalline glass body, by mass percentage, is as follows:
[0022] When the clarifying agent is 0.6-1% As2O3, the colorant includes 0.2-0.4% V2O5, CoO+NiO+Cr2O3+MnO<0.1%, and Fe2O3<0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
[0023] Preferably, the composition of the microcrystalline glass body, by mass percentage, is as follows:
[0024] When the clarifying agent is SnO2 0.2-0.5%; the colorant includes V2O5 0.02-0.04%, CoO+NiO+Cr2O3+MnO<0.1%, Fe2O3<0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
[0025] Preferably, the average linear thermal expansion coefficient (40-700℃) of the microcrystalline glass body is <1.2ppm / K.
[0026] Preferably, it includes the following steps:
[0027] S100 melting: heating and melting the glass batch into a uniform molten glass;
[0028] S200 calendering: Flat green glass ribbons are produced by roll forming;
[0029] S300 crystallization: The green glass ribbon is heated in a gradient to 820-1050℃ and held for 20-120 minutes to induce crystallization inside the green glass ribbon and form a microcrystalline glass body.
[0030] S400 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, and then applied to at least a portion of the surface of the microcrystalline glass body by screen printing.
[0031] S500 heat treatment: After preliminary drying, the temperature is raised to the firing temperature at an average heating rate of 5-50K / min. The firing temperature is not lower than 800℃ and the firing time is 10-60min, so that the coating glass material is fully fused with the microcrystalline glass body. After cooling, a colorless and transparent coating is formed.
[0032] Preferably, the surface of the microcrystalline glass body is mechanically processed before the S400 coating is applied. Preferably, the mechanical processing includes one or more combinations of flat grinding, polishing, edge grinding and other conventional mechanical processing techniques.
[0033] Preferably, the S400 coating application further includes the following steps:
[0034] S401 coated glass material is mixed with organic additives according to the formula to form screen printing ink, wherein the particle size D50 of the coated glass material is <10μm;
[0035] The screen printing ink described in S402 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of not less than 400 mesh.
[0036] Preferably, the viscosity of the screen printing ink is 15,000 to 25,000 cP.
[0037] This invention also provides a method for preparing a microcrystalline glass panel with a rough surface, the method comprising the following steps:
[0038] A100 melting: heating and melting the glass batch into a uniform molten glass;
[0039] A200 calendering: Flat green glass ribbons are produced by roll forming;
[0040] A300 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, and then applied to at least a portion of the surface of the microcrystalline glass body using a screen printing method;
[0041] After the A400 is initially dried, it is gradually heated to the firing temperature, which is 820-1050℃, and the firing time is 20-60 minutes. This causes the raw glass to crystallize into the microcrystalline panel body, and the coating glass material is fully fused with the microcrystalline panel body. After cooling, a colorless and transparent coating is formed.
[0042] Preferably, the surface of the microcrystalline glass body is mechanically processed before the A300 coating is applied.
[0043] Preferably, the A400 coating application further includes the following steps:
[0044] A301 coated glass material is mixed with organic additives according to the formula to form screen printing ink, wherein the particle size D50 of the coated glass material is <10μm;
[0045] The screen printing ink described in A302 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of not less than 400 mesh.
[0046] Preferably, the viscosity of the screen printing ink is 15,000 to 25,000 cP. Beneficial effects:
[0047] This invention significantly improves the surface performance of microcrystalline glass panels by coating the surface with a colorless and transparent coating that has soft, non-sharp protrusions. Compared with existing technologies, this invention has the following beneficial technical effects:
[0048] 1. Enhanced black visual effect: A basic black appearance is provided by coating the surface of the colorant-containing microcrystalline glass body with a colorless and transparent coating, while avoiding infrared transmittance loss. The surface thickness of the microcrystalline glass panel is 0.5μm≤Ra≤2.5μm, and the non-sharp protrusions formed on the coating surface, 2.5≤Rc / Rq≤3.5, cause diffuse reflection of incident light on the panel surface, thus presenting a deeper and more uniform black visual effect;
[0049] 2. Improved fingerprint resistance: The coating surface has non-sharp protrusions, making the microcrystalline glass panel 0.5μm≤Ra≤2.5μm and satisfying 2.5≤Rc / Rq≤3.5, thereby avoiding the accumulation of grease on the surface, reducing fingerprint residue, and improving panel cleanliness and tactile experience;
[0050] 3. Improve scratch resistance: By rationally controlling the protrusion structure, the surface micro-stress distribution is made more uniform, and the density and hardness of the coating are improved by appropriately adjusting the glass material in the coating formula, thereby significantly enhancing the scratch resistance of the microcrystalline glass panel.
[0051] 4. Maintaining high infrared transmittance: Since the coating does not contain colorants and the protrusions are surface microstructures, they do not significantly scatter infrared light. The transmittance of the microcrystalline glass panel at 1600nm is ≥60%, ensuring the normal operation of functional modules that rely on infrared signals.
[0052] 5. Overall performance optimization: Through the coordinated design of microcrystalline glass body formula control, coating composition, non-sharp protrusions on the coating surface, and surface roughness parameters, this invention achieves a stable and repeatable comprehensive optimization effect between black appearance, infrared transmission, fingerprint resistance, and scratch resistance, making it suitable for mass production in high-end displays, home appliance panels, and functional integrated devices. Attached Figure Description
[0053] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0054] Figure 1 is an optical micrograph of the surface texture of Example 1;
[0055] Figure 2 shows the roughness evaluation profiles of Example 2 (top) and Comparative Example 3 (bottom). Detailed Implementation
[0056] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0057] The present invention will be further described below with reference to the accompanying drawings and embodiments, but the scope of protection of the present invention is not limited to the content.
[0058] The present invention provides a microcrystalline glass panel with a rough surface, the microcrystalline glass panel comprising a microcrystalline glass body and a coating applied to the surface of the microcrystalline glass body;
[0059] The microcrystalline glass body contains a colorant; the coating does not contain a colorant.
[0060] The CIELab color space coordinates of the microcrystalline glass panel are: L*≥24, -2.5≤b*≤0, -0.3≤a*≤0.5;
[0061] At least a portion of the surface of the microcrystalline glass panel has non-sharp protrusions, and the microcrystalline glass panel has a thickness of 0.5μm≤Ra≤2.5μm, and satisfies 2.5≤Rc / Rq≤3.5; where Ra is the arithmetic mean deviation of the profile, Rc is the average height of the profile unit, and Rq is the root mean square deviation of the profile.
[0062] The microcrystalline glass panel has a transmittance of ≥60% at 1600nm.
[0063] Preferably, the roughness Ra of the microcrystalline glass panel can be in the range of 0.6μm≤Ra≤2.4μm, 0.7μm≤Ra≤2.3μm, 0.6μm≤Ra≤2.2μm, 0.8μm≤Ra≤2.1μm, 0.9μm≤Ra≤2.0μm; Ra can be 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm.
[0064] Preferably, the ratio of the average height of the contour unit of the microcrystalline glass panel to the root mean square deviation of the contour, Rc / Rq, can be in the range of 2.6≤Rc / Rq≤3.4, 2.7≤Rc / Rq≤3.4, 2.8≤Rc / Rq≤3.3, 2.9≤Rc / Rq≤3.2, 2.8≤Rc / Rq≤3.1, 2.9≤Rc / Rq≤3.0, 2.9≤Rc / Rq≤3.3, etc.; the Rc / Rq value can be 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5.
[0065] For the appearance color, the b* value can be -0.1, -0.5, -0.7, -1.3, -1.7, -2.3, -2.5 to maintain a black appearance and avoid unpleasant colors such as gray or bluish tints; the L* value can be 24.0, 24.5, 25.0, 26.0, 27.0, 28.0, 30.0, 33.0, 35.0. If L* < 24, the microcrystalline panel with a rough surface will have insufficient reflectivity and a dull appearance. The dark color of the microcrystalline glass body also limits the L* value of the microcrystalline panel of this invention to no more than 35; a* should be as close to 0 as possible, and a* can be 0.45, 0.3, 0.2, 0.1, 0, -0.1, -0.2, -0.3 to maintain a black appearance and avoid unpleasant colors such as gray or reddish tints.
[0066] It should be noted that in this invention, "colorant-free coating" means that the coating composition does not contain any colorant components intentionally added for functional coloring purposes. The coating is allowed to contain unavoidable impurities from raw materials or processes, but the content of these impurities is strictly limited to a level that is insufficient to significantly affect the color appearance of the resulting coating, and is not used as a technical means to achieve any color rendering function. Generally, the mass percentage of a single colorant oxide component is ≤0.1%, preferably ≤0.05%, more preferably 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005%, or 0.001%. In this invention, colorant components are added to the microcrystalline glass body to give the microcrystalline glass panel a stable and uniform black base, while the coating applied to the surface of the microcrystalline glass body is a colorless and transparent coating, containing no colorant components that can be used for color rendering. Typical colorant components such as Fe, Ni, Mn, Cr, and Co exhibit significant infrared absorption. Applying them to coatings significantly reduces transmittance in the 1600nm band, leading to decreased performance or malfunction of infrared-dependent functional modules. Therefore, while adding black colorants to the coating can further deepen the black color, it sacrifices infrared transmittance, making it difficult to meet overall performance requirements. The colorless and transparent coating of this invention effectively avoids additional infrared absorption caused by colorants, thus ensuring that the transmittance of the microcrystalline glass panel at 1600nm is ≥60%, providing a reliable guarantee for the realization of infrared-related functions.
[0067] Building upon this foundation, the present invention further improves the black visual effect through the refined design of the coating surface morphology. Specifically, at least a portion of the surface of the microcrystalline glass panel involved in the present invention has non-sharp protrusions. These non-sharp protrusions have rounded peaks and gentle slopes. Under visible light illumination, the light undergoes diffuse reflection primarily at small angles, thereby effectively suppressing specular reflection and increasing the probability of incident light entering the microcrystalline glass body. The increased absorption of visible light by the substrate results in a deeper and more uniform black appearance. Since the protrusions are an adjustment of the surface micro-geometry rather than the introduction of light-absorbing components, the intrinsic light absorption characteristics of the material are not significantly altered while ensuring the transparency of the coating. This allows for maintaining high visible light black rendering performance while preserving high transmittance in the near-infrared band.
[0068] Furthermore, this invention defines surface morphology and roughness to achieve the aforementioned synergistic effect, and further defines the surface morphology parameters. In this invention, the roundness of the protrusion is defined using the Rc / Rq ratio, where Rc is the average height of the contour unit and Rq is the root mean square deviation of the contour. The ratio of Rc / Rq reflects whether the peak shape of the protrusion is sharp and steep. During the surface roughening process of the microcrystalline panel, Ra, Rq, and Rc generally change in the same direction; as Ra increases, Rq and Rc also increase synchronously. If the roughness is increased, it is only a proportional enlargement of the surface contour, then Ra, Rq, and Rc increase synchronously, and Rq / Ra and Rc / Rq will remain consistent. The surface texture's reflection behavior of light will not change significantly, that is, the Lab chromaticity coordinates remain stable. If, during the roughening process, the Rc / Rq ratio increases rapidly, that is, the height of the contour unit increases much faster than the increase of Rq, then the contour peak is steeper and sharper, which will significantly affect the optical reflection behavior of the surface texture, leading to a shift in chromaticity coordinates and a grayish or bluish tint. It is evident that a smooth-topped profile will have a higher Rq value than a sharp profile, i.e., a smooth profile, which has a higher Rq value and thus lower Rc / Rq value.
[0069] This invention surprisingly discovers that when Rc / Rq is limited to 3.5 or less, the surface forms non-sharp protrusions with rounded or ellipsoidal peaks. The height and slope distribution among the protrusions are relatively balanced, resulting in moderate diffuse reflection of visible light on the panel surface, which is beneficial for obtaining a uniform and deep black appearance. However, when Rc / Rq is limited to 3.5 or more, the protrusions are steep, and the surface will produce an excessively strong diffuse reflection effect. A large amount of light is scattered back on the coating surface and fails to enter the substrate for absorption, resulting in a grayish appearance and weakening the black effect. Through extensive experiments, the inventors found that this ratio cannot be further reduced. The surface texture formed under various process variations consistently has an Rc / Rq ratio of 2.5 or higher. Therefore, in this invention, the range of Rc / Rq is 2.5 to 3.5. Furthermore, regarding roughness, if the panel surface is too smooth, specular reflection dominates, easily leading to defects such as high gloss, whitening, or graying. When the surface roughness Ra > 2.5 μm, excessive surface roughness leads to excessive scattering, thereby weakening the effective absorption and uniform distribution of visible light. This causes the overall color of the panel to tend towards gray, which is not conducive to obtaining a deep black and uniform visual effect. At the same time, excessive Ra will cause the infrared light emitted by the heat source to be unconcentrated, reducing heating efficiency. Therefore, this invention simultaneously limits the protrusion morphology and surface roughness parameters to form a surface structure with non-sharp protrusions and moderate roughness. This allows visible light to have a moderate diffuse reflection effect on the surface of the microcrystalline glass panel, thereby achieving an excellent black appearance and good device performance for the microcrystalline glass panel.
[0070] On the other hand, fingerprint resistance is closely related to surface roughness. When the surface of the microcrystalline glass panel is too smooth, finger oils easily spread on the surface to form an oil film, leaving fingerprints. As the surface roughness increases, the surface microstructure disrupts the continuous spread of oils, causing them to be distributed in a discontinuous state, thereby reducing the visible contrast of fingerprints and reducing residue. However, when the surface roughness increases further, although oil spreading is suppressed, the rough structure forms deeper recessed areas, where oils and dirt tend to accumulate, making daily cleaning difficult and the surface feel rougher. Therefore, to achieve the fingerprint-resistant effect, this invention controls the surface roughness Ra to be between 0.5 and 2.5 μm.
[0071] Considering multiple performance requirements such as black appearance, infrared transmittance, and fingerprint resistance, this invention ultimately controls the roughness of the microcrystalline glass panel within the range of 0.5μm≤Ra≤2.5μm, and satisfies 2.5≤Rc / Rq≤3.5, ensuring that the surface exhibits a non-sharp protrusion. Under this parameter combination, the morphology of the rough structure and the optical scattering behavior work synergistically. The non-sharp protrusions and roughness bring a moderate diffuse reflection effect that enhances the black appearance, while the roughness ensures fingerprint resistance. Simultaneously, the microcrystalline glass panel of this invention also ensures infrared transmittance to meet functional requirements. Ultimately, this invention achieves synergistic optimization of multiple key performance aspects, ensuring the best overall balance between black visual appeal, fingerprint resistance, and excellent infrared transmittance.
[0072] Preferably, the microcrystalline glass panel has an Rc ≤ 10 μm.
[0073] More preferably, 1μm≤Rc≤9μm, 2μm≤Rc≤8μm.
[0074] In detail, the present invention further defines the range of the average height Rc of the microcrystalline glass panel contour unit, where Rc reflects the macroscopic level of the overall surface undulation.
[0075] By controlling the radius (Rc) to no more than 10μm, various adverse factors caused by excessive surface undulations can be effectively avoided. If Rc is too large, the height difference between surface protrusions and depressions increases significantly, easily leading to excessive multiple scattering of light on the surface. Some light is directly scattered back to the human eye without being absorbed by the microcrystalline glass body, thus weakening the black appearance and even causing a grayish phenomenon. At the same time, excessive contour height will also create obvious macroscopic unevenness on the surface, affecting the tactile feel and potentially accumulating oil, dust, and other contaminants, which is detrimental to panel cleaning and user experience.
[0076] Therefore, by limiting Rc to below 10μm, this invention ensures sufficient diffuse reflection capability of the surface configuration to improve the black appearance, while avoiding problems such as graying and fingerprint residue caused by excessive macroscopic fluctuations. Thus, in conjunction with parameters such as Ra and Rc / Rq, it achieves comprehensive optimization of visual effects, functional performance, and user experience.
[0077] Preferably, the non-sharp protrusion has an arc-shaped or ellipsoidal peak structure.
[0078] Referring to Figure 1, the non-sharp protrusions of this invention have arc-shaped or ellipsoidal peak structures. During the screen printing process, the coating ink is transferred in liquid form to the surface of the microcrystalline glass body or green glass ribbon. Under the action of surface tension, the ink droplets generate arc-shaped or ellipsoidal contours on the surface, thereby reconstructing the microstructure of the surface and ultimately forming arc-shaped or ellipsoidal peak structures. Compared with protrusions with sharp edges or flat tops, arc-shaped or ellipsoidal peaks can make the slope change of the protrusion top more continuous and gentle, thereby avoiding the formation of local high slope or sharp peak structures. When incident light comes into contact with the surface at the top of the protrusion, its reflection and scattering directions are continuously distributed, which is conducive to forming a stable and uniform diffuse reflection effect, further weakening specular reflection, avoiding the generation of highlights or bright spots due to local high reflection points, and helping to improve the uniformity and depth of the black appearance of the microcrystalline glass panel.
[0079] Meanwhile, the arc-shaped or ellipsoidal peak structure can effectively reduce the stress concentration at the top of the protrusion. During external force contact or friction, this type of peak morphology can disperse the contact stress along the curve, reducing the risk of local damage or microcrack initiation at the top of the protrusion, thereby improving scratch resistance. In addition, this peak structure is less likely to form narrow recessed areas with high aspect ratios, which helps to reduce fingerprint grease and dirt residue.
[0080] This invention achieves comprehensive optimization of black visual effect, fingerprint resistance, and scratch resistance by adjusting the microstructure of the coating surface.
[0081] Preferably, the Ra of the microcrystalline glass body is 0.005 to 2.2 μm.
[0082] The limitation of the surface roughness of the microcrystalline glass body in this invention is not based on the roughness itself as a functional parameter in the final use state, but as a basic condition for the subsequent coating formation and surface morphology controllability. During the preparation process, the microcrystalline glass body will retain some of its original texture and will also be treated by polishing, fine grinding and other methods. The surface roughness Ra is controlled in the range of 0.005 to 2.2 μm, which can ensure the flatness of the substrate surface and provide a stable surface state for the spreading, wetting and film formation of the coating.
[0083] When the Ra of the glass-ceramic substrate is within the range of 0.005–2.2 μm, macroscopic defects or sharp protrusions that do not affect the continuity of the coating will not affect its continuity. During screen printing and high-temperature firing, the coating material can flow and spread sufficiently, filling and reconstructing the surface undulations of the substrate, thus forming a continuous, dense, and firmly adhered coating structure. Therefore, the final surface morphology of the glass-ceramic panel is obtained through the combined effect of the original Ra of the glass-ceramic substrate and the reconstruction behavior of the coating during the high-temperature firing process.
[0084] Meanwhile, the initial surface roughness of the glass-ceramic substrate still has a boundary effect on the surface roughness of the final product. When the Ra value of the glass-ceramic substrate is large, although the coating has a certain leveling ability during the firing process, there is an upper limit to its correction of substrate undulations, which makes the Ra value of the final glass-ceramic panel generally show an increasing trend as the Ra value of the substrate increases.
[0085] Therefore, by reasonably limiting the Ra of the microcrystalline glass body to the range of 0.005 to 2.2 μm, the present invention achieves synergistic control between the surface state of the microcrystalline glass body and the sintering and forming of the coating, ensuring that the final microcrystalline glass panel obtains stable and controllable surface roughness, non-sharp protrusion structure and excellent comprehensive performance.
[0086] Preferably, the coating is prepared by screen printing ink, which includes a coating glass frit and organic additives, wherein the coating glass frit comprises, by weight percentage:
[0087] Al2O3 7.2–9.8%, SiO2 58.2–66.1%, K2O 1.2–3.8%, Na2O 2.3–4.9%, B2O3 15.2–19.3%, BaO 1.7–2.1%, Li2O 0.9–2.8%, TiO2 0.07–0.2%, ZrO2 2.65%, excluding PbO, Fe2O3, or ZnO.
[0088] Specifically, SiO2 is the main component of the coating, constructing the glass network structure and providing the coating with good acid and alkali resistance as well as high Mohs hardness, which is the basis for ensuring the long-term wear resistance and corrosion resistance of the coating. However, if the SiO2 content exceeds 66.1 wt%, it will significantly increase the melting temperature and melt viscosity, making it difficult for the coating to be fully wetted and integrated into the microcrystalline glass body during the firing process, resulting in insufficient interfacial bonding and affecting the coating adhesion.
[0089] Al2O3 and SiO2 together form a glass network structure, which further improves the chemical stability and surface hardness of the coating. If the Al2O3 content exceeds 9.8 wt%, it will significantly increase the firing difficulty of the coating, reduce the melt fluidity, and also make it difficult for the coating to form a dense bonding interface with the microcrystalline glass body during the firing process.
[0090] Therefore, SiO2 and Al2O3 coexist synergistically within the above-mentioned range, mainly to provide high hardness, low thermal expansion and excellent acid and alkali resistance, while also taking into account processability and coating adhesion during the firing process.
[0091] K₂O, Na₂O, BaO, Li₂O, and B₂O₃ are fluxing components in the coating system, used to adjust the degree of fracture of the glass network, reduce the melting temperature and melt viscosity of the raw materials, and promote the wetting and spreading of the coating melt on the surface of the microcrystalline glass substrate during firing, thereby achieving full fusion between the coating and the substrate. Among them, Li₂O not only has a fluxing effect, but can also form a crystalline phase with Si and Al with a low coefficient of thermal expansion, which helps to reduce the overall coefficient of thermal expansion of the coating, making it better match the low expansion characteristics of the microcrystalline glass body and reducing the risk of cracks caused by thermal stress during cooling.
[0092] Excessive K and Na content will lead to a significant increase in the coefficient of thermal expansion of the coating. The microcrystalline panel products and bodies of this invention have high temperature and low expansion characteristics and need to withstand repeated high and low temperature changes during use. If the coefficient of thermal expansion of the coating is too large, cracks are prone to occur under repeated thermal cycling or rapid heating and cooling conditions, reducing the thermal shock resistance of the coating. Excessive BaO and Li2O content may weaken the chemical stability of the coating and increase the risk of volatilization during high-temperature firing.
[0093] B2O3 can effectively reduce melt viscosity and improve film leveling within a certain range. However, when its content exceeds approximately 19.3%, the glass network structure is excessively weakened, which in turn affects the surface hardness and wear resistance of the coating. Furthermore, the coefficient of thermal expansion of the coating increases, making it prone to cracking during rapid temperature changes. When the B2O3 content is below 15.2%, the coating is difficult to fuse with the microcrystalline glass matrix, resulting in insufficient adhesion and causing the coating to peel off from the microcrystalline glass matrix under mechanical friction or thermal cycling.
[0094] Therefore, each fluxing component needs to be controlled in a coordinated manner within a limited range to achieve a balance between melt flowability, film quality, chemical stability and mechanical properties.
[0095] ZrO2 and TiO2 act as nucleating agents, providing crystallization sites during the coating firing process and promoting the formation of a uniformly distributed microcrystalline structure within the coating. They promote the formation of crystalline phases such as high-quartz solid solution or hydrothermal quartz solid solution, allowing the coefficient of thermal expansion to be controlled at a low level, thus improving the thermal stability of the coating. Through the synergistic effect of ZrO2 and TiO2, the coating achieves moderate microcrystallization while maintaining a certain degree of glass phase continuity. This results in a better match between the thermal expansion characteristics of the coating and the microcrystalline glass matrix, reducing interfacial residual stress and improving the long-term reliability of the coating.
[0096] The coating contains little or no Fe2O3 and ZnO, primarily used to regulate melting behavior, improve firing stability, and refine the microstructure. Because it contains no colorants, the coating is colorless and transparent, thus not obscuring the color of the microcrystalline glass substrate and avoiding any impact on infrared transmittance. Even with trace amounts of metal oxides, they can still contribute to optimizing the film uniformity and structural stability of the coating without significantly affecting its transparency and infrared transmittance.
[0097] Furthermore, the coating system described in this invention does not contain lead (Pb), avoiding the toxicity risks that may arise from traditional lead-containing glass or coating materials, and meeting the environmental and safety requirements of home appliances and consumer products. Under long-term use or high-temperature operating conditions, lead migration or volatilization will not adversely affect human health or the environment, making this microcrystalline glass panel more suitable for applications directly facing end users, such as electric ceramic cooktops and stoves.
[0098] Preferably, the microcrystalline glass panel has a Mohs hardness of not less than 6.
[0099] Specifically, the hardness of the microcrystalline glass panel of this invention mainly benefits from the dense silicon-aluminum-oxygen network structure mainly composed of SiO2 and Al2O3 in the coating, which provides a high surface hardness and wear resistance foundation for the coating. Simultaneously, B2O3 participates in the regulation of the network structure within a limited content range, ensuring the quality and adhesion of the fired film without significantly weakening the structural density of the coating, thus avoiding a decrease in surface hardness due to excessive softening. By rationally controlling the B2O3 content, a balance is achieved between the coating's processing performance and mechanical properties, ensuring that the final coating has both good film-forming stability and meets the requirements for scratch resistance and wear resistance in daily use.
[0100] Preferably, the glass batch material of the microcrystalline glass body comprises, by weight percentage:
[0101] SiO2 62-68%, Al2O3 19-23%, Li2O 2.8-4.3%, Na2O+K2O 0-1.2%, BaO 1-3%, CaO 0-1%, MgO+ZnO 0-4%, P2O5 0-2%, TiO2 2-4%, ZrO2 1-2%, clarifying agent 0.2-1.5%, coloring agent 0.02-1%;
[0102] The clarifying agent is any one or more of As2O3, Sb2O3, SnO2, and CeO2; the coloring agent is any one or more of V2O5, CoO, NiO, Cr2O3, MnO, and Fe2O3.
[0103] The oxides mentioned above do not represent the compound form of the metal element present in the product, but rather the mass percentage of the corresponding metal element in the product calculated in the form of the oxide.
[0104] The colorant primarily provides the black appearance of the microcrystalline glass body and adjusts the visible light transmittance of the microcrystalline panel. If the colorant content is too low, the visible light transmittance of the microcrystalline panel will be too high, making the electronic components below visible when the microcrystalline panel is assembled into a terminal appliance, affecting the user experience. If the colorant content is too high, the visible light transmittance of the microcrystalline panel will be too low, making it difficult to clearly identify light-emitting devices such as indicator lights below the panel, also affecting the user experience.
[0105] Preferably, the composition of the microcrystalline glass body, by mass percentage, is as follows:
[0106] When the clarifying agent is 0.6-1% As2O3, the colorant includes 0.2-0.4% V2O5, CoO+NiO+Cr2O3+MnO<0.1%, and Fe2O3<0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
[0107] Preferably, the composition of the microcrystalline glass body, by mass percentage, is as follows:
[0108] When the clarifying agent is SnO2 0.2-0.5%; the colorant includes V2O5 0.02-0.04%, CoO+NiO+Cr2O3+MnO<0.1%, Fe2O3<0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
[0109] Preferably, the coefficient of thermal expansion (40-700℃) of the microcrystalline glass body is <1.2ppm / K.
[0110] The microcrystalline glass body of the present invention is based on a SiO2-Al2O3-Li2O system, wherein SiO2 and Al2O3 together form a stable glass network framework, giving the substrate good chemical stability, heat resistance and mechanical strength; the introduction of Li2O within a limited range is beneficial to the formation of a low-expansion β-spodumene microcrystalline phase, thereby controlling the coefficient of thermal expansion of the microcrystalline glass panel to below 1.2ppm / K in the range of 40 to 700℃, meeting the dimensional stability requirements under high temperature conditions.
[0111] BaO, CaO, MgO, and ZnO serve as auxiliary modifying oxides, improving melting performance and crystallization controllability without significantly increasing the coefficient of thermal expansion. TiO2 and ZrO2 act as nucleating agents, promoting the uniform precipitation of microcrystals during crystallization and providing the basic conditions for obtaining a stable, fine, and uniformly distributed microcrystalline structure.
[0112] Under the premise of stable matrix composition, the present invention forms two technical routes: arsenic-containing plates and arsenic-free plates by differentiating the selection of clarifying agent system and coloring agent system.
[0113] When As₂O₃ is used as a clarifying agent and its content is controlled at 0.6–1%, the glass melt exhibits strong clarifying ability and a relatively stable redox environment. In this system, V₂O₅ is the main colorant, with an addition amount of 0.2–0.4%, while CoO, NiO, Cr₂O₃, MnO, and Fe₂O₃ are strictly limited to extremely low levels, existing only as unavoidable impurities.
[0114] In arsenic-containing systems, arsenic plays a regulatory role in the redox state of the system during melting and crystallization, allowing vanadium to coexist in multiple valence states within the glass-ceramic matrix and forming a stable, dark-colored light-absorbing characteristic overall. Although different valence states of vanadium compounds differ in their optical absorption characteristics, the valence transformation process of vanadium is constrained under the synergistic effect of As₂O₃, resulting in a stable and uniform black appearance for the obtained glass-ceramic panel, while maintaining a transmittance of no less than 60% at 1600 nm.
[0115] Meanwhile, this invention requires that the V2O5 be uniformly distributed within the microcrystalline glass body. The microcrystalline glass body has a volumetric coloring structure, where the colorant dissolves in the high-temperature glass melt during the glass melting stage and is distributed synergistically with the glass phase and crystalline phase during subsequent crystallization. This ensures that the colorant exists uniformly in the overall volume of the microcrystalline glass body in the form of ions or coordination structures, rather than as independent particles or locally enriched phases. This volumetric coloring method differs from the structural characteristics of colorants distributed in grain boundaries or intergranular spaces in ceramic sintering processes, effectively avoiding optical inhomogeneities caused by localized enrichment of colorants. This uniform distribution synergizes with the Ra roughness and Rc / Rq morphology parameters defined by the panel surface. The vanadium colorant provides stable light absorption within the substrate, and the non-sharp, rough surface structure reduces specular reflection and increases the probability of incident light entering the substrate, thereby further enhancing the black visual effect and avoiding color differences or graying problems caused by uneven local coloring.
[0116] In arsenic-free systems, SnO2 is used as a clarifying agent at a content of 0.2–0.5%, avoiding the use of arsenic and better meeting environmental protection and regulatory requirements. However, compared with As2O3, SnO2 has a different ability to regulate the redox state of the melt, resulting in a different overall chemical environment in the system.
[0117] Under these conditions, if the high V₂O₅ content found in arsenic-containing plates is still used, it will result in excessively dark coloring or unstable optical properties. Therefore, this invention significantly reduces the amount of V₂O₅ added to an arsenic-free system, controlling it to only 0.02–0.04%, which is approximately one-tenth the amount used in arsenic-containing plate systems. In this way, the desired black appearance can still be obtained under arsenic-free conditions, while avoiding color deviations or unevenness caused by excessive vanadium content.
[0118] Similarly, in arsenic-free plates, the content of all transition metal oxides except V2O5 is limited to extremely low levels, ensuring a single and controllable source of coloring. The uniform distribution of vanadium colorant in the matrix, together with the surface roughness Ra and Rc / Rq parameters, allows the matrix light absorption and surface diffuse reflection to work together to achieve a stable black appearance.
[0119] On the other hand, the present invention provides a method for preparing a microcrystalline glass panel with a rough surface. By synergistically controlling the process parameters such as glass melting, forming, crystallization and coating sintering, the final microcrystalline glass panel is within a controllable range in terms of surface roughness, structural stability and optical performance, thereby meeting the comprehensive requirements of black appearance, fingerprint resistance, scratch resistance and high infrared transmittance.
[0120] Includes the following steps:
[0121] S100 melting: heating and melting the glass batch into a uniform molten glass to ensure that all components are fully mixed and form a melt with uniform composition and stability.
[0122] S200 calendering: Flat green glass ribbons are produced by roll forming;
[0123] S300 Crystallization: The green glass strip is gradually heated to a crystallization temperature of 820℃~1050℃ and held at this temperature for 20~120 minutes to induce crystallization within the green glass strip, forming a microcrystalline glass body. By controlling the crystallization temperature and holding time, the microcrystalline glass body can achieve a uniform crystal distribution and dense structure, thereby endowing the panel with high mechanical strength, thermal shock resistance, and a low coefficient of thermal expansion, providing structural protection for the bonding between the coating and the substrate during subsequent coating sintering. If the crystallization temperature is below 820℃, the crystallization efficiency is low, resulting in uneconomical production; if the crystallization temperature is too high, i.e., above 1050℃, it easily leads to excessively large precipitated crystals, causing the surface of the microcrystalline glass body to turn blue. If the crystallization temperature holding time is less than 20 minutes, insufficient crystallization will result in weakened microcrystalline panel strength, insufficient vanadium dyeing, and excessively high panel transmittance, affecting the black appearance; if the crystallization temperature holding time is higher than 120 minutes, excessive crystal growth will occur, causing the surface of the microcrystalline panel to turn blue.
[0124] S400 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, and then applied to at least a portion of the surface of the microcrystalline glass body by screen printing.
[0125] Preferably, the viscosity of the screen printing ink is 15,000 to 25,000 cP;
[0126] The ink viscosity should be controlled within the range of 15,000 to 25,000 cP. When the ink viscosity is too high, insufficient spreading or local accumulation is likely to occur during the coating process, affecting the uniformity of the coating surface. When the ink viscosity is too low, sagging or edge shrinkage is likely to occur, resulting in unstable coating thickness. By adjusting the screen printing ink viscosity within the above range, it is beneficial to ensure printing stability while providing conditions for the controllable evolution of the coating surface morphology during the subsequent sintering process.
[0127] S500 heat treatment: After preliminary drying, the temperature is raised to the firing temperature at an average heating rate of 5-50K / min. The firing temperature is not lower than 800℃ and held for 10-60 minutes to allow the coating glass material to fully fuse with the microcrystalline glass body and form a colorless and transparent coating.
[0128] With an average heating rate of 5K / min to 50K / min, a heating rate that is too low will cause the coating to remain in the low-temperature zone for too long, resulting in premature softening and localized flow of the glass frit. This is not conducive to forming a uniform coating thickness distribution and may amplify the original roughness of the substrate surface. On the other hand, a heating rate that is too high will cause the coating surface to densify rapidly, while the organic additives or gases remaining inside will have difficulty escaping in time. This will result in pinholes, bubbles, or localized loose structures during the sintering process, affecting the density, adhesion, and optical uniformity of the coating.
[0129] Before formal firing, drying or curing the screen printing ink can gradually remove solvents, resins, and other organic additives from the ink at a lower temperature, allowing the coated glass material to form a relatively stable inorganic framework structure before entering the high-temperature sintering stage. This pretreatment process effectively avoids the volume abrupt changes and gas evolution caused by the rapid decomposition of organic matter in the high-temperature range, thereby reducing the probability of internal defects in the coating and helping to achieve more uniform and controllable glass phase flow during subsequent firing.
[0130] Preferably, the firing temperature is 850–900°C. Within this temperature range, the coating glass phase has suitable fluidity, which can fill and reconstruct the rough structure on the surface of the microcrystalline glass body. Protrusions that originally had large slopes or sharp local features are gradually filled and reconstructed during the flow of the coating glass phase, forming a peak structure with a rounded or ellipsoidal top. At the same time, the coating components will not separate or the surface will become unstable due to excessive fluidity, which is conducive to obtaining a uniform and stable coating surface morphology.
[0131] Firing temperature and holding time significantly affect the flowability of the glass phase in the coating. Within the range of 850–900℃, appropriately extending the holding time helps the glass phase in the coating to flow fully and eliminate residual pores, thereby improving the density of the coating. It can also reduce steep peak morphology, lower the Rc / Rq ratio, and form a less sharp protrusion morphology. However, when the time exceeds 60 min, excessive heat treatment may lead to grain coarsening in the coating, increasing Ra, which is not conducive to the control of the final surface roughness.
[0132] Furthermore, the initial surface roughness of the glass-ceramic body will have a certain impact on the final coating roughness during the heat treatment process. The Ra value of the final glass-ceramic panel generally increases with the increase of the Ra of the glass-ceramic body. When the Ra of the glass-ceramic body is controlled within a reasonable range of 0.005 to 2.2 μm, the flow and reconstruction process of the coating during the firing process will further modify the surface morphology of the glass-ceramic product, so that the final coating surface has a stable and controllable roughness, thereby ensuring that the optical and functional properties of the glass-ceramic panel meet the requirements.
[0133] Therefore, by controlling the initial Ra of the microcrystalline glass body, the viscosity of the screen printing ink, the heat treatment temperature, and the holding time, it is possible to ensure full fusion between the coating and the substrate, while achieving a balance between coating densification and surface roughness control, ultimately producing a microcrystalline glass panel with a colorless and transparent coating, a non-sharp protrusion structure, and excellent overall performance.
[0134] Preferably, before the S400 coating is applied, the surface of the microcrystalline glass body is subjected to mechanical processing, including one or more combinations of flat grinding, polishing, edge grinding, and other conventional mechanical processing techniques.
[0135] After the microcrystalline glass body is crystallized, its surface retains the texture brought about by the calendering or crystallization process. The surface roughness and texture of the microcrystalline glass body obtained under different preparation conditions are somewhat different. For microcrystalline glass bodies that have not undergone mechanical processing, the original texture retained on the surface can be directly coated by screen printing. During the high-temperature firing process, the coated glass phase can reconstruct the original surface rough structure, thereby forming non-sharp protrusions with arc-shaped or ellipsoidal peak structures.
[0136] Furthermore, the inventors discovered that when the surface roughness of the microcrystalline glass body is low, the coated glass phase is more likely to form a stable and uniform surface microstructure at high temperatures. Therefore, in this invention, the microcrystalline glass body can be finely ground or polished before coating, which can reduce the surface roughness of the microcrystalline glass body and provide a good foundation for the uniform spreading, wetting and reconstruction of the subsequent coating during high-temperature firing.
[0137] Therefore, the final surface roughness and protrusion morphology of the microcrystalline glass panel are jointly determined by the roughness of the microcrystalline glass body and the screen printing process. When the roughness Ra of the microcrystalline glass body is 0.005 to 2.2 μm, after high-temperature heat treatment, secondary regulation can be achieved to form non-sharp protrusions, and the peak structure of the protrusions is arc-shaped or ellipsoidal, thereby achieving comprehensive optimization of black appearance, anti-fingerprint performance, scratch resistance and infrared transmittance.
[0138] Preferably, the S400 coating application further includes the following steps:
[0139] S401 coated glass material is mixed with organic additives according to the formula to form screen printing ink, wherein the particle size D50 of the coated glass material is <10μm;
[0140] The small and concentrated particle size of the coated glass frit helps improve the dispersion uniformity of screen printing inks and reduces local accumulation or surface defects caused by uneven particle size distribution. During the firing process, fine-particle glass frit is more likely to undergo uniform softening and viscous flow, thereby promoting coating densification and facilitating the formation of rounded, non-sharp surface microstructures.
[0141] The screen printing ink described in S402 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of not less than 400 mesh.
[0142] Using high mesh count screen printing allows for thinner and more uniform coating spread, avoiding localized excessive coating thickness that could lead to flow imbalance or increased surface roughness.
[0143] A method for preparing a microcrystalline glass panel with a rough surface, comprising the following steps:
[0144] A100 melting: heating and melting the glass batch into a uniform molten glass;
[0145] A200 calendering: Flat green glass ribbons are produced by roll forming;
[0146] A300 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, which is then applied to at least a portion of the surface of the green glass ribbon using a screen printing method;
[0147] A400 heat treatment: After initial drying, the temperature is gradually increased to the firing temperature, which is 820-1050℃, and the firing time is 20-60 minutes, so that the coating glass material and the green glass strip are fully fused. After cooling, a colorless and transparent coating is formed.
[0148] Specifically, this invention can also coat the green glass ribbon after calendering, achieving simultaneous crystallization and heat treatment sintering. The sintering temperature is controlled at 820–1050℃, and the sintering time is 20–60 minutes. This allows for the simultaneous crystallization of the green glass ribbon and the sintering of the coating film, ultimately forming a colorless and transparent coating upon cooling. Furthermore, this invention allows for mechanical processing of the green glass ribbon to impart an initial roughness. This initial roughness, combined with the coating effect, results in a sharp, protruding surface structure with arc-shaped or ellipsoidal peaks. The inspection method in this invention is as follows:
[0149] Surface roughness parameters Ra, Rq, Rc, Rsm, and Rdq were measured using a Mitutuyo SJ220, with λc = 0.8 mm, repeated 5 times. 1600 nm transmittance was measured using a PE lambda 1050+ with an integrating sphere. Appearance color was measured using a Hunterlab ColorQuestXE with the parameters "D65 light source, 10° observer".
[0150] In this invention, scratch resistance is evaluated by the following method:
[0151] Take quartz sand of 200 mesh or finer and spread it evenly on the surface of the microcrystalline panel. Place a 100mm × 100mm × 10mm wooden or plastic board on it, and place a 10kg object on the board. Move the board back and forth 5 times, counting each round trip as one round, with each one-way trip being 100mm. The surface scratches are graded as follows:
[0152] a. Poor, the surface has a large number of scratches, with more than 20 scratches;
[0153] b. Qualified, the surface has scratches, but there are no more than 3 scratches longer than 3cm;
[0154] c. Good, with scratches on the surface, which are short and shallow, and no scratches longer than 3cm;
[0155] d. Excellent, scratches longer than 1cm are difficult to observe on the surface.
[0156] In this invention, Mohs hardness is evaluated using the following method:
[0157] Holding a standard mineral, apply downward pressure (10±1) N and vertically and evenly scratch the surface of the specimen for about 2 cm along the cutting edge. Replace the standard mineral with different hardness values from low to high and compare the scratches. The hardness value of the standard mineral that just fails to produce obvious scratches on the surface of the specimen is the Mohs hardness value of the specimen.
[0158] The 1600nm transmittance includes direct light transmission and scattered light after passing through the sample, and was measured using a PELambada1050+ with an integrating sphere.
[0159] In this invention, the anti-fingerprint effect is evaluated using the following methods:
[0160] Touch the rough surface of a glass or ceramic object with your bare finger to create a fingerprint. Then place the surface under white light with a power of 300-400 lux and observe it at an angle of approximately 60°.
[0161] The visibility of oil stains, especially fingerprints, is assessed according to the following levels of severity:
[0162] a. Poor; the oil stains are immediately visible.
[0163] b. Qualified; oil stains should be visible after a few seconds of observation.
[0164] c. Good; the oil stains are visible upon continuous observation.
[0165] d. Excellent, oil stains are not visible.
[0166] Example 1
[0167] The glass batch composition of the microcrystalline glass body, by mass percentage, is: SiO2 64%, Al2O3 21%, Li2O 3%, Na2O+K2O 1%, BaO 2%, CaO 0%, MgO+ZnO 2%, P2O5 0.7%, TiO2 4%, ZrO2 1%, As2O3 1%, V2O5 0.3%;
[0168] The coated glass material, by weight percentage, includes:
[0169] Al2O3 9%, SiO2 61%, K2O 2%, Na2O 4%, B2O3 18%, BaO 1.5%, Li2O 2%, TiO2 0.3%, ZrO2 2.12%, PbO 0.02%, Fe2O3 0.04%, ZnO 0.02%.
[0170] Preparation methods include:
[0171] S100 melting: The glass batch prepared according to the composition of the microcrystalline glass body is heated and melted into a uniform glass liquid;
[0172] S200 calendering: Flat green glass ribbon with a thickness of 4mm is produced by roll forming;
[0173] S300 crystallization: The green glass ribbon is heated to the crystallization temperature of 930°C at a heating rate of 10K / min and held at the crystallization temperature for 30min to allow crystals to precipitate inside the green glass ribbon and form a microcrystalline glass body.
[0174] The microcrystalline glass body is cut, ground, and polished;
[0175] S400 coating application:
[0176] S401 coated glass material is mixed with organic additives according to the formula to form screen printing ink. The viscosity of the screen printing ink is 15000-20000 cP, and the particle size D50 of the coated glass material is 9.3 μm.
[0177] The screen printing ink described in S402 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of 420 mesh.
[0178] S500 heat treatment: After drying and curing at 120℃ for 30 minutes, the temperature is increased to 700℃ at an average heating rate of 15K / min, and then increased to 900℃ at an average heating rate of 5K / min. The firing time at 900℃ is 25 minutes to fully fuse the coating glass material with the microcrystalline glass body. After cooling, a colorless and transparent coating is formed.
[0179] Example 1 uses As₂O₃ as a clarifying agent and V₂O₅ for coloring. After crystallization, a microcrystalline glass substrate is obtained with an average linear thermal expansion coefficient (40-700℃) of 0.4ppm / K. The surface of the crystallized microcrystalline glass substrate is ground and polished to control the surface roughness Ra to 0.01μm. This results in a highly uniform substrate surface with low defects, while also reducing the interference of the rough surface on the subsequent coating flow and reconstruction behavior, creating favorable conditions for the coating during high-temperature firing. Based on this, a colorless and transparent coating without colorants is applied using a screen printing process. This coating only plays a role in surface morphology control and optical interface optimization during firing, without participating in color formation, thus avoiding the adverse effects of surface coloring on near-infrared transmittance. According to the test results, the microcrystalline glass panel obtained in Example 1 has Ra = 0.6 μm and Rc / Rq = 2.7. As shown in Figure 1, the protrusions on the surface of the microcrystalline glass panel are rounded and not sharp, and the protrusions have an ellipsoidal peak structure, which effectively suppresses excessive specular reflection and excessive diffuse reflection. In terms of optical performance, it has L* = 26, b* = -1.6, and a* = 0.1, exhibiting a stable and uniform deep black appearance. At the same time, the infrared transmittance at a wavelength of 1600 nm reaches 60.8%, proving that the surface morphology and colorless transparent coating structure, while ensuring the blackness of the appearance, do not cause significant scattering loss to near-infrared transmission, making it suitable for heating or sensing applications that rely on infrared radiation.
[0180] In terms of mechanics and durability, due to the adjustment of the B2O3 content in the coating, and the combination of SiO2 and Al2O3 as the main components, the resulting microcrystalline glass panel has a Mohs hardness of 6, exhibiting excellent scratch resistance; at the same time, the rounded protruding structure helps to reduce fingerprint residue and oil adhesion, and has good anti-fingerprint performance.
[0181] Thus, Example 1 achieves a good balance between black appearance, infrared transmittance, and mechanical properties.
[0182] Example 2
[0183] In Example 2, the microcrystalline glass body was crystallized, cut to the required size, and its surface was finely ground before a coating was applied. All other process conditions were the same as in Example 1. The fine grinding process was a conventional flat grinding process, using diamond abrasive. The surface roughness of the microcrystalline glass body was adjusted by controlling the grinding parameters. Compared to the polishing process in Example 1, the fine grinding process could moderately increase the initial surface roughness of the microcrystalline glass body, providing different initial morphological conditions for surface reconstruction during the subsequent coating sintering process.
[0184] In Example 2, based on the arsenic-containing system, the Ra of the microcrystalline glass substrate surface was increased to 0.4 μm through fine grinding. After applying a colorless transparent coating and sintering under this higher initial roughness condition, a black microcrystalline glass panel was obtained. The coating surface had Ra = 0.6 and Rc / Rq = 2.7. The surface protrusions remained non-sharp with rounded peaks, and no sharpening or strong diffuse reflection structures caused by increased substrate roughness were observed. Correspondingly, the panel exhibited an infrared transmittance of 61.2% at a wavelength of 1600 nm, maintaining good infrared transmittance performance. Simultaneously, it displayed a stable black appearance, excellent scratch resistance, a Mohs hardness of 6, and good fingerprint resistance.
[0185] Example 2 shows that even when the roughness of the microcrystalline glass body is significantly increased, as long as the roughness is controlled within a reasonable range, the coating firing process can still obtain the final surface morphology of the microcrystalline glass panel through its own reconstruction behavior, thereby ensuring a black appearance and infrared transmittance while achieving good mechanical and performance properties.
[0186] Example 3
[0187] The composition of the microcrystalline glass body, by mass percentage, is: SiO2 65%, Al2O3 20%, Li2O 4%, Na2O+K2O 1%, BaO 1.7%, CaO 0%, MgO+ZnO 2.9%, P2O5 0.7%, TiO2 3.3%, ZrO2 1%, SnO2 0.3%, V2O5 0.04%, and other impurities 0.06%; the average linear thermal expansion coefficient (40-700℃) of the microcrystalline glass body is 0.4ppm / K.
[0188] In Example 3, the clarifying agent As2O3 was replaced with SnO2 to construct an arsenic-free system, while the amount of V2O5 added was significantly reduced. Under this arsenic-free system, volume coloring effect can still be achieved by reasonably controlling the amount of V2O5, so that the microcrystalline glass body presents a stable black tone.
[0189] In terms of forming and surface treatment, Example 3 retains the naturally formed surface rough texture during the calendering process, only cutting it to the required size without further machining. The calendering process uses a two-roll or three-roll calendering process, with the pressure roller Ra of the rough texture surface being 1.8 μm, and the rough texture Ra formed on the surface of the microcrystalline glass body being 0.9 μm. Under the above-mentioned relatively large initial roughness conditions, Example 3 uses the same colorless transparent coating system and firing process as Example 1. During the high-temperature sintering process, the coating redistributes and reconstructs the original calendering texture through glass phase viscosity flow and surface tension, making the surface protrusion morphology tend to be rounded. Test results show that the surface roughness Ra of the microcrystalline glass panel obtained after coating sintering is 0.9 μm, Rc / Rq = 2.9, the coating surface still has a non-sharp, rounded peak structure of protrusions, and the transmittance at 1600 nm reaches 61.0%, which is basically equivalent to Example 1. Its appearance parameters are L*=25, b*=-1.5, a*=0.2, exhibiting a deep black appearance and excellent anti-fingerprint and anti-scratch effects.
[0190] Example 3 shows that even without polishing, while retaining the rough texture of calendering, this example can still achieve effective control of surface morphology and roughness by reconstructing the coating during the coating firing process, so as to generate protrusions with non-sharp, rounded peak structures, while maintaining a deep black appearance, high infrared transmittance and good mechanical durability.
[0191] Example 4
[0192] In Example 4, the surface roughness of the rough texture roller used for calendering was increased to Ra = 2.5 μm, resulting in a rough texture Ra of 2.0 μm on the surface of the microcrystalline glass body. The surface of the resulting microcrystalline glass body was not further polished or finely ground, and a screen printing coating was directly applied. The remaining process conditions were the same as in Example 3.
[0193] Under these relatively high initial roughness conditions, after coating sintering, the surface roughness of the resulting microcrystalline glass panel is Ra = 2.0 μm, Rc / Rq = 2.8. It can be seen that although the roughness of the microcrystalline glass body is significantly higher than that of Examples 1-3, the high-temperature firing of the coating results in a non-sharp protrusion structure on the final coating surface, with rounded peaks and no steep peaks. In terms of performance, Example 4 achieves an infrared transmittance of 60.5% at a wavelength of 1600 nm. Simultaneously, its appearance parameters L* = 27, b* = -2.2, a* = 0.4, exhibiting a stable black appearance. In terms of usability, the panel still demonstrates excellent fingerprint resistance and scratch resistance.
[0194] As can be seen, in Example 4, even if a large rough texture is introduced on the surface of the microcrystalline glass body through the rolling process, a non-sharp protrusion can still be obtained through the coating sintering process, and an arc-shaped peak can be formed. This can maintain the black appearance and high infrared transmittance while taking into account comprehensive performance such as fingerprint resistance and scratch resistance.
[0195] Example 5
[0196] The S500 heat treatment process involves a heat treatment temperature of 890°C and a holding time of 35 minutes, with other conditions the same as in Example 4.
[0197] By lowering the peak firing temperature and appropriately extending the holding time, the glass phase in the coating maintains sufficient fluidity while promoting a more complete and controlled crystal growth process within the coating. This allows for the refinement and adjustment of the coating surface morphology without introducing sharp protrusions. This firing regime makes the coating's reconstruction behavior smoother, which is conducive to the formation of a stable and uniform microstructure.
[0198] Test results show that the surface roughness of the microcrystalline glass panel obtained in Example 5 is Ra = 2.0 μm, Rc / Rq = 2.8. Its protrusion morphology remains predominantly rounded with ellipsoidal peaks, without high aspect ratios or sharp peaks. In terms of optical performance, the transmittance at 1600 nm is 60.5%. The appearance parameters are L* = 27, b* = -2.1, a* = 0.3, exhibiting a stable black appearance. Furthermore, this panel demonstrates excellent scratch resistance and fingerprint resistance.
[0199] As can be seen from Example 5, under the condition of high microcrystalline glass body roughness, by reasonably selecting the firing temperature and holding time, the surface morphology and comprehensive performance of the final panel can be kept in a stable and controllable state. The selection of firing process parameters is the key parameter for adjusting the roughness and surface morphology of the microcrystalline glass panel, which plays an important role in the final appearance, feel and functional performance.
[0200] Example 6
[0201] The difference between Example 6 and Example 1 is:
[0202] The preparation method includes the following steps:
[0203] A100 melting: The glass batch prepared according to the composition of the microcrystalline glass body is heated and melted into a uniform glass liquid;
[0204] A200 calendering: Through roll forming, a flat green glass ribbon with a thickness of 4mm is produced;
[0205] A300 coating application:
[0206] A301 coated glass material is mixed with organic additives according to the formula to form screen printing ink. The viscosity of the screen printing ink is 15,000 to 20,000 cP, and the particle size D50 of the coated glass material is 9.3 μm.
[0207] The screen printing ink described in A302 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of 420 mesh.
[0208] A400 heat treatment: After initial drying, the temperature is gradually increased to 930℃ and the firing time is 25 minutes, so that the raw glass strip crystallizes into the microcrystalline panel body, and the coating glass material is fully fused with the microcrystalline panel body. After cooling, a colorless and transparent coating is formed.
[0209] Test results show that after simultaneous processing, the surface roughness of the resulting microcrystalline glass panel is Ra = 0.6 μm, Rc / Rq = 2.8, indicating that the protrusions formed on the coating surface are still rounded and non-sharp, forming an ellipsoidal peak structure. Its 1600nm transmittance is 60.8%, indicating that simultaneous processing did not introduce additional infrared scattering loss. The appearance parameters L* = 26, b* = -1.6, a* = 0.0, exhibiting a stable and uniform deep black appearance. Simultaneously, the microcrystalline glass panel maintains excellent Mohs hardness and scratch resistance, and good fingerprint resistance. Its overall performance is not significantly degraded compared to the embodiment where crystallization was followed by independent coating and sintering.
[0210] As can be seen from Example 6, under the condition that the crystallization process and coating heat treatment are carried out simultaneously in this invention, the coating can still undergo flow and reconstruction processes at high temperatures and then stably solidify during the subsequent cooling process, thereby obtaining the expected surface morphology and stable comprehensive performance. This not only broadens the process implementation path but also provides a feasible solution for simplifying the heat treatment process and improving production efficiency.
[0211] Comparative Example 1
[0212] The pressure roller inside the rough roller is processed to Ra 3.0 μm, and the surface Ra value of the microcrystalline glass body obtained by calendering is 2.6 μm. It is then directly screen printed, and other conditions are the same as in Example 3.
[0213] In Comparative Example 1, the test results showed that the surface roughness of the microcrystalline glass panel was Ra = 2.7 μm and Rc / Rq = 3.6. Ra is greater than 2.5 μm, and Rc / Rq exceeds 3.5, indicating that the coating surface formed a highly steep, sharp protrusion structure with significant peak-to-valley differences. According to the measurement results, Rc increased significantly, reaching 12.0 μm. In this case, the height of the protrusions in the surface profile increased, but the overall height distribution increased only slightly, indicating the formation of tall protrusion structures. Compared with the smooth and rounded protrusion morphology of Example 3 (Rc / Rq < 3.0), the surface profile in Comparative Example 1 exhibited obvious sharp-peaked characteristics.
[0214] In terms of optical performance, in Comparative Example 1, L* = 28, b* = -2.8, and a* = 0.2, the overall visual effect is grayed out, and the black rendering performance is significantly worse. This is because the sharp protrusions and large surface roughness lead to an excessively strong diffuse reflection effect. A large amount of incident light is directly scattered back on the coating surface and has difficulty penetrating into the interior of the microcrystalline glass body to be absorbed, thus weakening the depth of the black rendering.
[0215] In terms of performance, Comparative Example 1 maintains excellent scratch resistance, thanks to its larger surface undulations and higher overall roughness, which improves its mechanical damage resistance to some extent. However, the sharp protrusions and greater roughness make it prone to leaving grease on the surface, significantly reducing its fingerprint resistance and failing to meet the requirements for the appearance and user experience of a high-end black panel.
[0216] In summary, Comparative Example 1 shows that in an arsenic-free system, if the surface roughness of the glass-ceramic substrate is further increased, exceeding Ra by more than 2.5 μm and Rc / Rq by more than 3.5, even with the application of a coating and high-temperature sintering, the flow and reconstruction capabilities of the coating are insufficient to eliminate the steep undulations introduced by the substrate, ultimately resulting in sharp protruding structures. While this type of surface morphology is beneficial for scratch resistance, it significantly degrades the black appearance and fingerprint resistance.
[0217] Comparative Example 2
[0218] Compared to Example 2, the difference is that 0.2% Fe2O3 was added to the coating composition, and the transmittance at 1600nm was 52%.
[0219] Test results show that the surface morphology parameters of the microcrystalline glass panel obtained in Comparative Example 2 are Ra = 0.6 μm and Rc / Rq = 2.7, indicating that the coating still forms a non-sharp protrusion structure. In terms of appearance, it has L* = 24, b* = -1.7, and a* = 0.2, exhibiting a black appearance, and possesses excellent scratch resistance and good anti-fingerprint effect.
[0220] In terms of infrared optical performance, Comparative Example 2 showed significant degradation, with a transmittance of only 52% at 1600 nm. This indicates that although the addition of Fe2O3 helps to enhance the black appearance, the introduction of colorant into the coating will result in additional infrared absorption in the coating, leading to a decrease in infrared light transmittance and affecting the performance of the device.
[0221] Therefore, Comparative Example 2 shows that introducing a colorant into the coating can produce a black appearance, but at the expense of near-infrared transmittance.
[0222] Comparative Example 3
[0223] Compared to Example 2, the difference is that after crystallization, the calendered textured surface is finely ground without applying a coating.
[0224] Test results show that the Ra of the microcrystalline glass panel in Comparative Example 3 is 0.4 μm, and Rc / Rq is 3.6, indicating that the surface of the microcrystalline glass panel is relatively smooth overall but has relatively sharp peaks. As can be seen from Figure 1, the contour of Example 2 is more rounded, while the surface protrusions of Comparative Example 3 are sharper due to the lack of coating reconstruction, resulting in uneven visible light scattering and a gray appearance rather than a deep black color.
[0225] Furthermore, due to the lack of a coating, the panel in Comparative Example 3 performed poorly in terms of scratch resistance and fingerprint resistance.
[0226] Thus, Comparative Example 3 shows that the presence of the coating plays a key role in the reconstruction of the surface morphology of the microcrystalline glass panel and the rounding of protrusions. Without the coating, Rc / Rq becomes too high and sharp protrusions increase, thereby causing graying of the appearance and a decrease in scratch resistance and fingerprint resistance.
[0227] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A microcrystalline glass panel with a rough surface, characterized in that, The microcrystalline glass panel includes a microcrystalline glass body and a coating applied to the surface of the microcrystalline glass body; The microcrystalline glass body contains a colorant; the coating does not contain a colorant. The CIELab color space coordinates of the microcrystalline glass panel are: L*≥24, -2.5≤b*≤0, -0.3≤a*≤0.5; At least a portion of the surface of the microcrystalline glass panel has non-sharp protrusions, and the microcrystalline glass panel has a thickness of 0.5μm≤Ra≤2.5μm, and satisfies 2.5≤Rc / Rq≤3.5; where Ra is the arithmetic mean deviation of the profile, Rc is the average height of the profile unit, and Rq is the root mean square deviation of the profile. The microcrystalline glass panel has a transmittance of ≥60% at 1600nm.
2. The microcrystalline glass panel according to claim 1, characterized in that, The microcrystalline glass panel has a diameter of Rc≤10μm.
3. The microcrystalline glass panel according to claim 1, characterized in that, The non-sharp protrusions have an arc-shaped or ellipsoidal peak structure.
4. The microcrystalline glass panel according to claim 1, characterized in that, The Ra of the microcrystalline glass body is 0.005 to 2.2 μm.
5. The microcrystalline glass panel according to claim 1, characterized in that, The coating is prepared by screen printing ink, which includes a coating glass frit and organic additives, wherein the coating glass frit comprises, by mass percentage: Al2O3 7.2–9.8%, SiO2 58.2–66.1%, K2O 1.2–3.8%, Na2O 2.3–4.9%, B2O3 15.2–19.3%, BaO 1.7–2.1%, Li2O 0.9–2.8%, TiO2 0.07–0.35%, ZrO2 1.3–3.6%, excluding PbO, Fe2O3, or ZnO.
6. The microcrystalline glass panel according to claim 5, characterized in that, The microcrystalline glass panel has a Mohs hardness of not less than 6.
7. The microcrystalline glass panel according to claim 1, characterized in that, The glass batch material of the microcrystalline glass body comprises, by mass percentage: SiO2 62-68%, Al2O3 19-23%, Li2O 2.8-4.3%, Na2O+K2O 0-1.2%, BaO 1-3%, CaO 0-1%, MgO+ZnO 0-4%, P2O5 0-2%, TiO2 2-4%, ZrO2 1-2%, clarifying agent 0.2-1.5%, coloring agent 0.02-1%; The clarifying agent is any one or more of As2O3, Sb2O3, SnO2, and CeO2; the coloring agent is any one or more of V2O5, CoO, NiO, Cr2O3, MnO, and Fe2O3.
8. The microcrystalline glass panel according to claim 7, characterized in that, The glass batch material of the microcrystalline glass body comprises, by mass percentage: When the clarifying agent is 0.6-1% As2O3, the colorant includes 0.2-0.4% V2O5, CoO+NiO+Cr2O3+MnO<0.1%, and Fe2O3<0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
9. The microcrystalline glass panel according to claim 7, characterized in that, The glass batch material of the microcrystalline glass body comprises, by weight percentage: When the clarifying agent is SnO2 0.2-0.5%; the colorant includes V2O5 0.02-0.04%, CoO+NiO+Cr2O3+MnO <0.1%, Fe2O3 <0.1%, and the colorant is uniformly distributed in the microcrystalline glass body.
10. The microcrystalline glass panel according to claim 1, characterized in that, The average linear thermal expansion coefficient (40–700 °C) of the microcrystalline glass body is <1.2 ppm / K.
11. A method for preparing a microcrystalline glass panel with a rough surface, comprising preparing a microcrystalline glass panel as described in any one of claims 1 to 10, characterized in that, Includes the following steps: S100 melting: heating and melting the glass batch into a uniform molten glass; S200 calendering: Flat green glass ribbons are produced by roll forming; S300 crystallization: The green glass ribbon is heated in a gradient to 820-1050℃ and held for 20-120 minutes to induce crystallization inside the green glass ribbon and form a microcrystalline glass body. S400 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, and then applied to at least a portion of the surface of the microcrystalline glass body by screen printing. S500 heat treatment: After preliminary drying, the temperature is raised to the firing temperature at an average heating rate of 5-50K / min. The firing temperature is not lower than 800℃ and the firing time is 10-60min, so that the coating glass material is fully fused with the microcrystalline glass body. After cooling, a colorless and transparent coating is formed.
12. The preparation method according to claim 11, characterized in that, Before applying the S400 coating, the surface of the microcrystalline glass body is mechanically processed.
13. The preparation method according to claim 11, characterized in that, The S400 coating application also includes the following steps: S401 coated glass material is mixed with organic additives according to the formula to form screen printing ink, wherein the particle size D50 of the coated glass material is <10μm; The screen printing ink described in S402 is applied to at least a portion of the surface of the microcrystalline glass body by screen printing, with a screen mesh count of not less than 400 mesh.
14. The preparation method according to claim 11, characterized in that, The viscosity of the screen printing ink is 15,000 to 25,000 cP.
15. A method for preparing a microcrystalline glass panel with a rough surface, comprising preparing a microcrystalline glass panel as described in any one of claims 1 to 10, characterized in that, Includes the following steps: A100 melting: heating and melting the glass batch into a uniform molten glass; A200 calendering: Flat green glass ribbons are produced by roll forming; A300 Coating Application: The coating glass material is mixed with organic additives to form screen printing ink, which is then applied to at least a portion of the surface of the green glass ribbon using a screen printing method; A400 Crystallization: After initial drying, the temperature is gradually increased to the firing temperature, which is 820-1050℃, and the firing time is 20-60 minutes, so that the raw glass strip crystallizes into the microcrystalline panel body, and the coating glass material is fully fused with the microcrystalline panel body. After cooling, a colorless and transparent coating is formed.
16. The preparation method according to claim 15, characterized in that, Before applying the A300 coating, the surface of the green glass strip is mechanically processed.
17. The preparation method according to claim 15, characterized in that, The A400 coating application also includes the following steps: A301 coated glass material is mixed with organic additives according to the formula to form screen printing ink, wherein the particle size D50 of the coated glass material is <10μm; The screen printing ink described in A302 is applied to at least a portion of the surface of a raw glass ribbon by screen printing, with a screen mesh count of not less than 400 mesh.