Positive electrode sheet for lithium-ion battery, lithium-ion battery, and electric device

By optimizing the material parameters of the inner and outer layers of the lithium-ion battery cathode, the thermal runaway risk and material coordination problem of high-nickel cathode materials were solved, achieving battery performance with high energy density, long cycle life and high safety.

WO2026233480A1PCT designated stage Publication Date: 2026-11-12CHERY AUTOMOBILE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2026/112724
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-01-29
Filing Date
2026-07-23
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials pose a risk of thermal runaway at high nickel content, and the electrochemical properties of materials in the bilayer composite structure are difficult to coordinate, resulting in insufficient safety and cycle life.

Method used

By controlling the relationship between the specific surface area, mass fraction, and median particle size of the inner lithium iron phosphate layer and the outer lithium nickel cobalt manganese oxide layer, the bilayer composite cathode structure is optimized, forming a stable conductive network and mechanical buffer layer, thereby synergistically improving battery performance.

Benefits of technology

While maintaining high energy density, it significantly improves the rate performance, cycle life, and thermal safety of lithium-ion batteries, ensuring the long-term stability and safety of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2026112724-FTAPPB-I100001
    Figure PCTCN2026112724-FTAPPB-I100001
  • Figure PCTCN2026112724-FTAPPB-I100002
    Figure PCTCN2026112724-FTAPPB-I100002
  • Figure PCTCN2026112724-FTAPPB-I100003
    Figure PCTCN2026112724-FTAPPB-I100003
Patent Text Reader

Abstract

Disclosed in the present application are a positive electrode sheet for a lithium-ion battery, a lithium-ion battery, and an electric device. The positive electrode sheet comprises a current collector, a first active material layer containing lithium iron phosphate, and a second active material layer containing lithium nickel manganese cobalt oxide. The positive electrode sheet satisfies: 0.5≤(SSA1×W1) / D50-1≤4, and 3%≤W1≤10%. In the present application, by means of the synergistic design of an inner lithium iron phosphate layer and an outer lithium nickel manganese cobalt oxide layer, the battery is ensured to have a high energy density and good rate performance, cycle life and thermal safety.
Need to check novelty before this filing date? Find Prior Art

Description

A positive electrode sheet for a lithium-ion battery, a lithium-ion battery, and an electrical device.

[0001] Cross-reference to related applications

[0002] This application claims priority to Chinese Patent Application No. 202610127809.3, filed on January 29, 2026, entitled "A Lithium-ion Battery Positive Electrode Sheet and a Lithium-ion Battery", the entire contents of which are incorporated herein by reference and constitute a part of this application for all purposes. Technical Field

[0003] This application belongs to the field of lithium-ion battery technology, and particularly relates to a positive electrode sheet for a lithium-ion battery, as well as a lithium-ion battery and an electrical device. Background Technology

[0004] The information disclosed in the background section of this invention is intended only to enhance the understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0005] The development of lithium-ion battery cathode material technology has always faced the challenge of synergistically optimizing multiple performance indicators such as energy density, safety, and cycle life. Layered transition metal oxides with high nickel content (such as lithium nickel cobalt manganese oxide) possess advantages in high specific capacity and high operating voltage, making them key materials for achieving high energy density in batteries. However, with increasing nickel content, the structural stability of the material decreases, making it prone to severe exothermic side reactions under thermal or electrical abuse conditions, posing a risk of thermal runaway. Its insufficient intrinsic safety has become a bottleneck restricting its widespread application in high-performance power batteries.

[0006] To improve the safety of high-nickel cathode systems, the industry typically considers incorporating olivine-type phosphate materials (such as lithium iron phosphate) with better thermal stability. Common composite strategies include bulk doping, surface coating, and physical mixing or bilayer structure design in the electrode layers. These methods improve the thermal safety of the system to some extent, but also introduce new technical problems: simple physical mixing may lead to the coupling of interfacial side reactions between the two materials in the electrolyte, which may exacerbate gas generation; while using methods such as bilayer coating to partition different materials, although theoretically functional separation can be achieved, improper matching can make it difficult to coordinate the electrochemical characteristics (such as operating voltage range, ionic / electronic conductivity) and kinetic behavior of the inner and outer layers, which may lead to obstruction of lithium-ion transport at the interlayer interface; or at high rates, the polarization difference may cause severe uneven reaction progress between the two layers; and additional side reactions may also be triggered, which may impair cycle life and interfacial stability.

[0007] Therefore, how to improve battery safety, rate performance and cycle life in a synergistic way by optimizing the structural design of the double-layer composite cathode while maintaining high energy density is an urgent problem to be solved. Summary of the Invention

[0008] To overcome the shortcomings of the prior art, this application provides a lithium-ion battery positive electrode sheet, a lithium-ion battery, and an electrical device. This application achieves synergistic optimization of the morphology, content, and function of the inner lithium iron phosphate layer and the outer lithium nickel cobalt manganese oxide layer, thereby synergistically improving the rate performance, cycle life, and thermal safety of the battery while ensuring high energy density.

[0009] To achieve the above objectives, one or more embodiments of this application provide the following technical solutions:

[0010] In a first aspect, this application provides a positive electrode sheet for a lithium-ion battery, including a current collector, a first active material layer disposed on at least one surface of the current collector, and a second active material layer disposed on the surface of the first active material layer.

[0011] The first active material layer includes lithium iron phosphate as the first positive electrode active material, and the second active material layer includes lithium nickel cobalt manganese oxide as the second positive electrode active material;

[0012] In the positive electrode of the lithium-ion battery, SSA1, W1 and D 50-1 The following relationship must be satisfied: 0.5 ≤ (SSA1 × W1) / D 50-1 ≤4;

[0013] Where SSA1 is the specific surface area of ​​lithium iron phosphate, in m². 2 / g; W1 is the mass fraction of the first active substance layer in the total mass of the first and second active substance layers, which satisfies 0.03≤W1≤0.1, i.e., 3%≤W1≤10%. When calculating the above relationship, W1 is substituted in decimal form; D 50-1 The median particle size of lithium iron phosphate is given in μm.

[0014] Optionally, W1 satisfies 0.05≤W1≤0.1.

[0015] Optionally, the specific surface area of ​​the lithium iron phosphate is 10–22 m². 2 / g.

[0016] Optionally, the median particle size of the lithium iron phosphate is 0.7–2 μm.

[0017] Optionally, the general chemical formula of the lithium nickel cobalt manganese oxide is LiNi. x Co y Mn 1-x-yO2, where 0.6 ≤ x ≤ 0.92, 0 <y<0.4,1-x-y> 0.

[0018] Optionally, the lithium nickel cobalt manganese oxide has a median particle size of 8–18 μm and a specific surface area of ​​0.3–1.0 m². 2 / g.

[0019] Optionally, the first active material layer further includes a first conductive agent and a first binder, and the mass ratio of the first positive electrode active material, the first conductive agent and the first binder is (94-97):(1-3):(2-4); the second active material layer further includes a second conductive agent and a second binder, and the mass ratio of the second positive electrode active material, the second conductive agent and the second binder is (96-98):(1-3):(1-2).

[0020] Optionally, the dry weight per unit area of ​​the first active material layer is 5–20 g / m². 2 The dry weight per unit area of ​​the second active material layer is 145–165 g / m². 2 .

[0021] Secondly, this application provides a lithium-ion battery, including the aforementioned lithium-ion battery positive electrode sheet.

[0022] Thirdly, this application provides an electrical device including the aforementioned lithium-ion battery.

[0023] The above one or more technical solutions have the following beneficial effects:

[0024] (1) This application correlates and controls the specific surface area (SSA1) of the inner lithium iron phosphate layer, the mass fraction (W1) of the first active material layer in the total mass of the first and second active material layers, and the median particle size (D) of the lithium iron phosphate. 50-1 The relationship between these three factors provides a precise quantitative basis for the design of bilayer composite cathode plates. This parameter effectively coordinates the functions of the inner lithium iron phosphate layer in constructing a conductive network, providing structural buffering, and stabilizing the electrochemical interface, solving the problem of the difficulty in systematically optimizing the material parameters and ratios of the functional layers in a bilayer structure.

[0025] (2) Through the above-mentioned quantitative design, this application has synergistically improved the overall performance of lithium-ion batteries while ensuring the high energy density dominated by lithium nickel cobalt manganese oxide with a high proportion. Specifically, the battery has both excellent high-rate discharge performance and long cycle life, which significantly alleviates the contradiction between the two in traditional designs; at the same time, the thermal stability and interface stability of the battery are enhanced, and the safety performance is fundamentally improved.

[0026] (3) The parameter relationship established in this application has clear process guidance, which is conducive to improving production consistency and yield, ensuring the controllability and consistency of battery product performance degradation throughout the entire life cycle, and meeting the stringent requirements of high-end power batteries for high safety, long life and reliability. Detailed Implementation

[0027] It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0028] In this application, the median particle size (D) 50 The particle size refers to the particle size at which the cumulative volume distribution percentage of particles reaches 50%, that is, the volume of particles below and above this particle size each accounts for 50%.

[0029] This application provides a positive electrode sheet for a lithium-ion battery, including a current collector, a first active material layer disposed on at least one surface of the current collector, and a second active material layer disposed on the surface of the first active material layer.

[0030] The first active material layer includes lithium iron phosphate as the first positive electrode active material, and the second active material layer includes lithium nickel cobalt manganese oxide as the second positive electrode active material;

[0031] In the positive electrode of the lithium-ion battery, SSA1, W1 and D 50-1 The following relationship must be satisfied: 0.5 ≤ (SSA1 × W1) / D 50-1 ≤4;

[0032] Where SSA1 is the specific surface area of ​​lithium iron phosphate, in m². 2 / g; W1 is the mass fraction of the first active substance layer in the total mass of the first and second active substance layers, which satisfies 0.03≤W1≤0.1, i.e., 3%≤W1≤10%. When calculating the above relationship, W1 is substituted in decimal form; for example, when W1 is 8%, it is substituted into the relationship as 0.08. D 50-1 The median particle size of lithium iron phosphate is given in μm.

[0033] The numerator term "SSA1×W1" in the relationship provided by the above-mentioned technical solution of this application comprehensively characterizes the total effective active interface contribution provided by lithium iron phosphate in the first active material layer. The specific surface area SSA1 determines the size of the reactive interface per unit mass of material, while the mass fraction W1 determines the relative content of the first active material layer in the overall electrode. Their product reflects the overall ability of the first active material layer to participate in charge transfer and interfacial reactions at the electrode scale. The denominator term D... 50-1This is related to the average diffusion path length of lithium ions within the solid phase of lithium iron phosphate particles. The larger the particle size, the greater the kinetic resistance to the migration of ions from the inside of the particle to the surface.

[0034] While existing technologies have explored the introduction of stabilizing materials such as lithium iron phosphate into bilayer composite cathodes to enhance safety, these approaches typically limit themselves to isolated adjustments or simple combinations of parameters for single or multiple materials. For example, optimizing the particle size or specific surface area of ​​lithium iron phosphate alone can control its processability or intrinsic reactivity. However, this application simultaneously constrains the aforementioned three key parameters, addressing the performance synergy challenges inherent in high-nickel systems.

[0035] When the value of the above relationship is below 0.5, it means that either the mass ratio of the first active material layer is too low, or the lithium iron phosphate particles in this layer are too coarse or have too small a specific surface area. These factors will prevent the first active material layer from forming a continuous and efficient electron / ion hybrid conductive network between the current collector and the high-activity layer, thus rendering its value as a functional layer unrealizable and contributing negligibly to the improvement of the overall rate performance of the battery. When the value of the above relationship is above 4, it usually corresponds to the use of excessively fine lithium iron phosphate nanoparticles or excessively high specific surface area. This will drastically increase the active sites on the surface of the lithium iron phosphate material and the contact area with the electrolyte, not only deteriorating the slurry processing performance but also triggering serious interfacial side reactions, leading to irreversible consumption of active lithium and electrolyte, which in turn damages the cycle life and long-term interfacial stability of the battery. When the value of the above relationship is within a specific range, the addition of a small amount of lithium iron phosphate can achieve three functions: first, to build a robust conductive path to ensure excellent rate performance; second, to form a stable initial interface to suppress side reactions; and third, to act as a mechanical and chemical buffer layer to improve overall safety. More preferably, 0.5 ≤ (SSA1 × W1) / D 50-1 ≤2.5, further, 0.5≤(SSA1×W1) / D 50-1 ≤2. It should be noted that, in the calculation, SSA1 and D... 50-1 All calculations are performed using unitless values, with the values ​​in meters. 2 The values ​​when / g and the values ​​when the unit is μm.

[0036] Through the aforementioned quantitative design, this application synergistically improves the overall performance of lithium-ion batteries while ensuring high energy density dominated by lithium nickel cobalt manganese oxide with a high proportion of lithium nickel cobalt manganese oxide. Specifically, the battery simultaneously possesses excellent high-rate discharge performance and long cycle life, significantly alleviating the contradiction between the two in traditional designs; at the same time, the battery's thermal stability and interface stability are enhanced, and safety performance is fundamentally improved.

[0037] In an optional embodiment of this application, W1 satisfies 0.05≤W1≤0.1. If W1 is too small, the lithium iron phosphate layer will be too thin, making it impossible to construct a continuous and effective three-dimensional conductive network and mechanical buffer layer between the current collector and the high-nickel layer; if W1 is too large, it will excessively crowd out the proportion of high-capacity nickel cobalt manganese oxide, significantly sacrificing the overall energy density of the battery.

[0038] In an optional embodiment of this application, the specific surface area of ​​the lithium iron phosphate is 10–22 m². 2 / g, more preferably 12-20m 2 / g. A suitable specific surface area of ​​lithium iron phosphate provides sufficient active surface area, facilitating close contact with the conductive agent and constructing an excellent electronic conductivity network. Simultaneously, the moderate specific surface area avoids the problems of severe agglomeration of nanomaterials, uncontrolled slurry viscosity, and exacerbated side reactions with the electrolyte caused by excessively high surface energy. Furthermore, it is beneficial to obtain a suitable pore structure after rolling, balancing ion transport and electrode strength. The specific surface area value described in this application was obtained by measuring using the BET nitrogen adsorption method.

[0039] The lithium iron phosphate used in this application can be an unmodified conventional material, or it can be carbon-coated and doped with metal ions (such as Mg). 2+ Ti 4+ Zr 4+ Materials modified with (etc.) to further improve their intrinsic electronic conductivity or structural stability. The morphology of lithium iron phosphate can be approximately spherical, plate-like, or other irregular polyhedra, and its primary particles can be single crystals or polycrystalline aggregates.

[0040] In an optional embodiment of this application, the median particle size of the lithium iron phosphate is 0.7–2 μm, more preferably 0.8–1.5 μm. While a smaller particle size is beneficial for shortening the lithium-ion diffusion path, it drastically increases the specific surface area and deteriorates the slurry rheology and electrode processability; a larger particle size significantly increases ion migration resistance, potentially leading to severe concentration polarization, especially during fast charging and discharging, thus limiting rate performance. The median particle size is measured using a laser particle size analyzer.

[0041] In an optional embodiment of this application, the general chemical formula of the lithium nickel cobalt manganese oxide is LiNi. x Co y Mn 1- x-y O2, where 0.6 ≤ x ≤ 0.92, 0 <y<0.4,1-x-y> 0. For example, you can choose medium-nickel systems such as NCM622 and NCM712 or high-nickel systems such as NCM811 and NCM9055.

[0042] In an optional embodiment of this application, the median particle size of the lithium nickel cobalt manganese oxide is 8–18 μm. A larger particle size is beneficial for obtaining high tap density and electrode compaction density, thereby increasing the volumetric energy density while reducing the total particle surface area. The specific surface area is 0.3–1.0 m². 2 / g; The lower specific surface area effectively limits the contact area between the material and the electrolyte, reducing interfacial side reactions and transition metal dissolution under high voltage, which is beneficial for improving long cycle life and high-temperature stability. The lithium nickel cobalt manganese oxide can be single crystal particles or polycrystalline secondary agglomerates.

[0043] In an optional embodiment of this application, the first active material layer further includes a first conductive agent and a first binder, and the mass ratio of the first positive electrode active material, the first conductive agent and the first binder is (94-97):(1-3):(2-4); the second active material layer further includes a second conductive agent and a second binder, and the mass ratio of the second positive electrode active material, the second conductive agent and the second binder is (96-98):(1-3):(1-2).

[0044] In optional embodiments of this application, the first conductive agent and the second conductive agent may be independently selected from one or more of conductive carbon black (such as Super P, Ketjen black), carbon nanotubes, graphene, and carbon fibers. Preferably, a composite system of conductive carbon black and carbon nanotubes is used to construct a point-line combined three-dimensional conductive network.

[0045] In optional embodiments of this application, the first adhesive and the second adhesive may each be independently selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, sodium carboxymethyl cellulose, polyacrylic acid, and their salts. Polyvinylidene fluoride is preferred because it has excellent chemical stability and bonding strength under high voltage.

[0046] In an optional embodiment of this application, the dry weight per unit area of ​​the first active material layer is 5–20 g / m². 2 More preferably 8-15 g / m 2 The dry weight per unit area of ​​the second active material layer is 145–165 g / m². 2 More preferably 150-160 g / m 2 In this application, unless otherwise stated, the dry weight per unit area of ​​the first active material layer and the second active material layer refers to the dry weight per unit area of ​​a single side.

[0047] This application does not impose any special restrictions on the preparation method of the above-mentioned lithium-ion battery positive electrode sheet, but preferably includes the following steps:

[0048] Slurry preparation: The first positive electrode active material, the second positive electrode active material, and the corresponding conductive agent and binder are mixed at high speed in a solvent according to the specified proportions until a uniform and stable slurry is formed. The solid content of the slurry can be 40-80%.

[0049] Double-layer coating: The slurry is uniformly coated onto the current collector (such as aluminum foil or carbon-coated aluminum foil with a thickness of 8-12μm) using a double-layer coating machine to form a double-layer structure;

[0050] Drying and rolling: The solvent is thoroughly dried in an oven at 80℃~130℃, followed by rolling at room temperature. The rolled electrodes can be cut to the required size as needed.

[0051] This application also provides a lithium-ion battery, including the aforementioned positive electrode. The lithium-ion battery further includes a negative electrode, a separator, an electrolyte, and outer packaging.

[0052] The negative electrode sheet may include graphite, silicon-based materials, soft / hard carbon, and other negative electrode active materials, coated onto a copper foil current collector. The separator may be a polyethylene, polypropylene microporous membrane, or a ceramic-coated composite membrane thereof. The electrolyte contains lithium salts (such as LiPF6) and organic solvents (such as a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate), and may contain film-forming additives, flame-retardant additives, etc.

[0053] This application also provides an electrical device including the aforementioned lithium-ion battery.

[0054] The electrical device provided in this application refers to any equipment, system, or vehicle that uses the aforementioned lithium-ion battery as its power supply source or energy storage core unit.

[0055] The technical solution of this application will be further described below with reference to specific embodiments. This application does not have any special restrictions on the source of reagents used in the following embodiments; commercially available products well known to those skilled in the art can be used. In the following embodiments, the specific surface area value was measured by the BET nitrogen adsorption method, and the particle size value was measured by a Malvern 2000 laser particle size analyzer.

[0056] Example 1

[0057] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0058] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 0.8 μm and the specific surface area (SSA1) is 20 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0059] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0060] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 8% of the total mass of the two active material layers.

[0061] Example 2

[0062] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0063] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 1.0 μm and the specific surface area (SSA1) is 14 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0064] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0065] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 8% of the total mass of the two active material layers.

[0066] Example 3

[0067] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0068] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 1.2 μm and the specific surface area (SSA1) is 12 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0069] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0070] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 8% of the total mass of the two active material layers.

[0071] Example 4

[0072] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0073] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 0.8 μm and the specific surface area (SSA1) is 20 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0074] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0075] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 8.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on top of it have a single-sided dry weight of 157.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 5% of the total mass of the two active material layers.

[0076] Example 5

[0077] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0078] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 1.0 μm and the specific surface area (SSA1) is 14 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0079] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0080] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 8.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on top of it have a single-sided dry weight of 157.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 5% of the total mass of the two active material layers.

[0081] Example 6

[0082] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0083] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 1.2 μm and the specific surface area (SSA1) is 12 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0084] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0085] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 8.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on top of it have a single-sided dry weight of 157.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 5% of the total mass of the two active material layers.

[0086] Example 7

[0087] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0088] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 0.8 μm and the specific surface area (SSA1) is 20 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0089] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0090] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 10% of the total mass of the two active material layers.

[0091] Example 8

[0092] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0093] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 2.0 μm and the specific surface area (SSA1) is 10 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0094] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0095] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 10% of the total mass of the two active material layers.

[0096] Example 9

[0097] This embodiment provides a positive electrode sheet for a lithium-ion battery, the preparation method of which is as follows:

[0098] (1) Preparation of the first active material layer slurry: The median particle size (D) was selected. 50-1 The micrometer diameter is 0.7 μm and the specific surface area (SSA1) is 22 m². 2Lithium iron phosphate (LFP) was used as the first positive electrode active material. Lithium iron phosphate, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 900) were mixed at a mass ratio of 95:1.5:0.5:3. N-methylpyrrolidone (NMP) solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a first active material slurry with a solid content of 65%.

[0099] (2) Preparation of the second active material layer slurry: A median particle size of 15 μm and a specific surface area of ​​0.5 m² were selected. 2 / g single-crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) was used as the second positive electrode active material. NCM811, conductive carbon black (Super P), carbon nanotubes, and polyvinylidene fluoride (PVDF, model 5130) were mixed at a mass ratio of 96.8:1.5:0.5:1.2. NMP solvent was added to a high-speed mixer, and the mixture was homogeneously mixed to form a second active material slurry with a solid content of 70%.

[0100] (3) Double-layer coating and electrode preparation: Using precision double-layer coating technology, the slurry prepared in steps (1) and (2) is coated onto one surface of a carbon-coated aluminum foil current collector with a thickness of 12 μm and 2 μm coatings on both sides. By controlling the coating process parameters, a single-sided unit area dry weight of 13.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 152.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer) is then applied. After drying, the same double-layer coating process is performed on the other side of the carbon-coated aluminum foil current collector, followed by drying. Then, a compaction density of 3.45 g / cm³ is achieved. 3 The material is rolled to obtain the positive electrode sheet. The first active material layer has a mass fraction (W1) of 10% of the total mass of the two active material layers.

[0101] Comparative Example 1

[0102] The difference between this comparative example and Example 4 is that the median particle size (D) of lithium iron phosphate in this comparative example is... 50-1 The surface area is 3 μm, and the specific surface area (SSA1) is 8 m². 2 / g.

[0103] Comparative Example 2

[0104] The difference between this comparative example and Example 4 is that the median particle size (D) of lithium iron phosphate in this comparative example is... 50-1 The micrometer diameter (SSA1) is 0.58 μm, and the specific surface area (SSA1) is 25 m². 2 / g, and the mass fraction W1 of the first active material layer in this comparative example is 10% of the total mass of the two active material layers. That is, by controlling the coating process parameters, a single-sided unit area dry weight of 16.6g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the dry weight per unit area on one side directly stacked thereon are 149.6 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer).

[0105] Comparative Example 3

[0106] The difference between this comparative example and Example 5 is that the mass fraction W1 of the first active material layer in this comparative example is 2% of the total mass of the two active material layers. That is, by controlling the coating process parameters, a single-sided unit area dry weight of 3.3 g / m² is achieved. 2 The first active material layer (lithium iron phosphate layer) and the layer directly stacked on it have a single-sided dry weight of 162.9 g / m². 2 The second active material layer (lithium nickel cobalt manganese oxide layer).

[0107] Comparative Example 4

[0108] The difference between this comparative example and Example 4 is that this comparative example does not contain a lithium iron phosphate layer, but only a single layer of lithium nickel cobalt manganese oxide is coated. The dry weight per unit area of ​​the lithium nickel cobalt manganese oxide layer is 166.2 g / m². 2 .

[0109] The parameter values ​​and the relationship (SSA1×W1) / D of Examples 1-6 and Comparative Examples 1-4 50-1 The calculated values ​​are summarized in Table 1.

[0110] Table 1. Parameter values ​​and calculation results for the examples and comparative examples.

[0111] Test case

[0112] Preparation of lithium-ion batteries: Artificial graphite, conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 93:2:2:1.5:1.5. Deionized water was added and stirred to prepare a slurry with a solid content of 48%. This slurry was uniformly coated on both sides of an 8 μm thick copper foil. After drying and rolling, a coating weight of 104.29 g / m² was obtained. 2The negative electrode sheet was prepared. The positive electrode sheets from Examples 1-6 and Comparative Examples 1-4, along with the aforementioned negative electrode sheets, were cut and welded with tabs, and wound together with a polyethylene-based ceramic-coated separator to form a battery cell. The battery cell was placed in an aluminum-plastic film packaging bag, and an EC / EMC / DMC electrolyte (volume ratio 3:5:2) containing 1.0 M LiPF6 was injected. After vacuum sealing, settling, formation (0.1C constant current charging to 3.6V), shaping, and capacity testing, a soft-pack lithium-ion battery with a rated capacity of 5 Ah was obtained.

[0113] The testing method is as follows:

[0114] 1. Energy density test:

[0115] At 25°C, the battery was charged at a constant current of 0.2C to 4.2V, then switched to constant voltage charging until the current dropped to 0.05C. After resting for 30 minutes, it was discharged at a constant current of 0.2C to 2.8V, and the discharge capacity was recorded. Based on the cell's mass and volume, its gravimetric energy density (Wh / kg) and volumetric energy density (Wh / L) were calculated.

[0116] 2. High-rate long-cycle test:

[0117] At 25°C, the battery was charged at a constant current of 1C to 4.2V, then switched to constant voltage charging until the current dropped to 0.05C, and immediately discharged at a constant current of 3C to 2.8V. This constitutes one cycle. The discharge capacity (C0) of the first cycle was recorded. This "1C charge / 3C discharge" cycle was repeated, and the discharge capacity (C0) of the 500th cycle was recorded. 500 ), and according to the formula "Capacity retention rate = (C 500 The capacity retention rate after high-rate cycling is calculated using " / C0)×100%".

[0118] 3. DC internal resistance (DCR) growth rate test:

[0119] At 25°C, charge the battery to 50% state of charge (SOC). Test the initial DC internal resistance (DCR0): Apply a 10-second 3C discharge pulse and record the voltage drop (ΔV) at the start of the pulse. Calculate the DC internal resistance using ΔV / ΔI. After completing the 300th "1C charge / 3C discharge" cycle (refer to "2. High-rate long-cycle test" in the test method), adjust the battery to 50% SOC again and test the DC internal resistance (DCR0) after the cycle using the same method. 300 The DCR growth rate is calculated using the formula "[(DCR) 300 The calculation is performed using the formula: -DCR0) / DCR0]×100%.

[0120] 4. Thermal stability test:

[0121] Disassemble the batteries that have not undergone cycling, as well as those that have completed 500 high-rate long-cycle tests (refer to "2. High-rate long-cycle test" in the test method). Remove the positive electrode, wash it with dimethyl carbonate (DMC), and dry it. Take an appropriate amount of the positive electrode material after these cycles and test it using a differential scanning calorimeter (DSC). The test conditions are: under an inert atmosphere (such as argon), heat from 50°C to 350°C at a heating rate of 5°C / min, and record the peak temperature of the exothermic reaction. The higher the peak temperature, the better the thermal stability of the material after long-term cycling.

[0122] The test results are summarized in Tables 2 and 3.

[0123] Table 2. Electrochemical test results of lithium-ion batteries in the examples and comparative examples.

[0124] Table 3. Thermal stability test results of lithium-ion batteries in the examples and comparative examples. Note: The "DSC peak temperature before cycling" data in Table 3 are the average test values ​​of brand-new, uncycled batteries prepared in the same batch as each example / comparative example; the "DSC peak temperature after 500 cycles" data are the average test values ​​of batteries in the same batch after completing 500 high-rate cycles. The two sets of data are from different battery samples to ensure the consistency of the initial state of the batteries.

[0125] As can be seen from the experimental results in Tables 2 and 3, using Examples 1 to 6 of this application (where the parameters satisfy 0.5 ≤ (SSA1 × W1) / D) 50-1 The lithium-ion batteries prepared by ≤4) achieve excellent synergy and balance in terms of energy density, high-rate cycle life, power retention rate and long-term thermal stability.

[0126] All embodiments exhibited a capacity retention of over 80% and a DC internal resistance growth rate of less than 50% after 500 cycles of a demanding 1C charge / 3C discharge cycle. This demonstrates that, within the parameter range of this application, the inner lithium iron phosphate layer effectively constructs a stable conductive network and mechanical buffer layer, mitigating the degradation of the high-nickel layer structure and interfacial side reactions during repeated fast charge and discharge cycles, thereby simultaneously resolving the contradiction between high rate capability and long cycle life.

[0127] Comparative Examples 1 and 3, due to insufficient contribution from the lithium iron phosphate layer (overly coarse particles or too low proportion), failed to form an effective buffer, resulting in significantly worse high-rate cycling performance and internal resistance growth compared to the examples. Comparative Example 2, due to the use of excessively fine, high-specific-surface-area lithium iron phosphate with an excessively high proportion, although initially exhibiting low internal resistance, triggered severe interfacial side reactions during cycling, leading to a sharp capacity decay and a surge in internal resistance. Comparative Example 4 (pure ternary system), lacking functional layer protection, showed the most severe degradation in high-rate cycling performance and interfacial deterioration.

[0128] As can be seen, this application successfully designed a bilayer composite cathode by precisely controlling the quantitative relationship between the specific surface area, mass fraction, and median particle size of the inner lithium iron phosphate layer. This design, while preserving the high energy density of the high-nickel system to the greatest extent, endows the battery with excellent high-rate cycle performance, a slow power decay rate, and outstanding long-cycle thermal stability, achieving a synergistic improvement in high safety, long lifespan, and fast charge / discharge performance.

[0129] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. A positive electrode sheet for a lithium-ion battery, comprising a current collector, a first active material layer disposed on at least one surface of the current collector, and a second active material layer disposed on the surface of the first active material layer, characterized in that, The first active material layer includes lithium iron phosphate as the first positive electrode active material, and the second active material layer includes lithium nickel cobalt manganese oxide as the second positive electrode active material; In the positive electrode of the lithium-ion battery, SSA1, W1 and D 50-1 The following relationship must be satisfied: 0.5 ≤ (SSA1 × W1) / D 50-1 ≤4; Where SSA1 is the specific surface area of ​​lithium iron phosphate, in m². 2 / g; W1 is the mass fraction of the first active substance layer in the total mass of the first and second active substance layers, which satisfies 0.03≤W1≤0.1, i.e., 3%≤W1≤10%. When calculating the above relationship, W1 is substituted in decimal form; D 50-1 The median particle size of lithium iron phosphate is given in μm.

2. The lithium-ion battery positive electrode sheet as described in claim 1, characterized in that, The W1 satisfies 0.05≤W1≤0.

1.

3. The lithium-ion battery positive electrode sheet as described in claim 1, characterized in that, The specific surface area of ​​the lithium iron phosphate is 10–22 m². 2 / g.

4. The positive electrode of a lithium-ion battery as described in claim 1, characterized in that, The median particle size of the lithium iron phosphate is 0.7–2 μm.

5. The positive electrode of a lithium-ion battery as described in claim 1, characterized in that, The general chemical formula of the lithium nickel cobalt manganese oxide is LiNi x Co y Mn 1-x-y O2, where 0.6 ≤ x ≤ 0.92, 0 <y<0.4,1-x-y> 0.

6. The positive electrode of a lithium-ion battery as described in claim 1, characterized in that, The median particle size of the lithium nickel cobalt manganese oxide is 8–18 μm, and the specific surface area is 0.3–1.0 m². 2 / g.

7. The lithium-ion battery positive electrode sheet as described in claim 1, characterized in that, The first active material layer further includes a first conductive agent and a first binder, and the mass ratio of the first positive electrode active material, the first conductive agent and the first binder is (94-97):(1-3):(2-4); the second active material layer further includes a second conductive agent and a second binder, and the mass ratio of the second positive electrode active material, the second conductive agent and the second binder is (96-98):(1-3):(1-2).

8. The positive electrode of a lithium-ion battery as described in claim 1, characterized in that, The dry weight per unit area of ​​the first active material layer is 5-20 g / m². 2 The dry weight per unit area of ​​the second active material layer is 145–165 g / m². 2 .

9. A lithium-ion battery, characterized in that, Including the positive electrode sheet of a lithium-ion battery as described in any one of claims 1 to 8.

10. An electrical appliance, characterized in that, Including the lithium-ion battery as described in claim 9.