Method for determining parameter values for use in the manufacture of an electric melting zone of a glass furnace, method for manufacturing such a zone and a furnace, corresponding device and furnace

A method for determining parameter values optimizes the design of large glass furnaces by dividing the electric melting zone into modules with quadrature-supplied electrode groups, enhancing electrode and refractory integrity and energy efficiency, and addressing operational challenges like foaming and corrosion.

WO2026233710A1PCT designated stage Publication Date: 2026-11-12SAINT GOBAIN ISOVER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/061486
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-06
Filing Date
2026-04-21
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing methods for designing large electric glass furnaces face challenges in maintaining electrode and refractory integrity while ensuring homogeneous electric current distribution, particularly for tanks exceeding 80 m² in surface area, due to difficulties in satisfying operational constraints such as foaming, corrosion, temperature control, and electrical consumption.

Method used

A computer-implemented method for determining parameter values for an electric melting zone of a glass furnace, dividing the zone into modules with electrode groups supplied by alternating currents in quadrature, and optimizing parameters like electrode intensity, current limits, and module dimensions to ensure effective operation.

Benefits of technology

The method enables the design of large glass furnaces with improved electrode and refractory longevity, homogeneous current distribution, and optimized energy efficiency, addressing issues of foaming and corrosion, and reducing electrical consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2026061486_12112026_PF_FP_ABST
    Figure EP2026061486_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for determining parameter values for use in the manufacture of an electric melting zone of a glass furnace, said zone comprising a tank of surface area S and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups supplied by a two-phase alternating current, at least two single-phase groups being spaced apart by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said method comprising a determination of values of the parameters L[i], S and N, so as to optimize the operation of the furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Description Title of the invention: Method for determining parameter values ​​intended for use in the manufacture of an electric melting zone of a glass furnace, method for manufacturing such a zone and furnace, corresponding device and furnace Previous technique

[0001] The present invention relates to the general field of glass furnace manufacturing. More particularly, it relates to a method for determining parameter values ​​intended for use in manufacturing an electrical melting zone of a glass furnace. The invention also relates to methods for manufacturing such an electrical melting zone from at least one parameter thus determined and a glass furnace comprising this melting zone, as well as the electrical melting zone and the glass furnace respectively obtained by these manufacturing methods. The invention further relates, in particular, to a method for melting vitrifiable materials using said furnace.

[0002] In this description, "vitrifiable materials" or "raw materials" means all materials, natural ores or synthesized products, materials from recycling such as cullet, etc., which can be used in the composition to feed a glass furnace.

[0003] This includes silica sand, but also all additives (sodium carbonate, limestone, dolomite, alumina...), waste (including mineral fibers) which may come from the production of said fibers or from construction sites (construction or deconstruction), all possible liquid or solid fuels (plastic of composite material or not, organic matter, coals), and all types of cullet.

[0004] Also included are recyclable materials containing combustible (organic) elements such as, for example, coated mineral fibers with binder (of the type used in thermal or acoustic insulation or those used in the reinforcement of plastic material), laminated glazing with polyvinyl butyral type polymer sheets such as windshields, glass bottles (household cullet), or any type of "composite" material combining glass and plastic materials such as certain bottles.

[0005] Also recyclable are "glass-metal composites or metallic compounds" such as functionalized glazing with coatings containing metals.

[0006] In the description, the product of the fusion of these vitrifiable materials is called "fusion bath" (also called "bath of vitrifiable materials" or "glass bath" in the technical literature of the field).

[0007] Similarly, "glass" is understood to mean glass in the broadest sense, that is to say, encompassing any material with a vitreous matrix, glass-ceramic or ceramic.

[0008] Examples of glass furnace designs in which the melting process of glassable materials is carried out using electrical energy are known from the prior art. To achieve this, these glass furnaces are equipped with an electric melting zone comprising a vessel adapted to contain a molten bath and electrodes powered by an electric current. For example, patent EP0671116B1 describes an embodiment in which so-called "immersing" electrodes are used (i.e., electrodes immersed from the free surface of the molten bath). However, it is possible to use, in addition or as an alternative, electrodes completely immersed in the molten bath, for example, arranged vertically from the furnace floor or horizontally from the side walls of the vessel.

[0009] In order to design large electric furnaces, while avoiding premature wear of the electrodes and the refractories constituting the vessel, but also to improve the homogeneity of the distribution of electric current within the melting bath, it was proposed by patent application WO2024105247A1, in opposition to the traditional practice of using a three-phase supply, a solution consisting of positioning electrodes in a specific way and supplying them with a two-phase alternating current.

[0010] The term "two-phase alternating current" refers to a system with two phases of the same frequency and amplitude that are in quadrature, that is, phase-shifted by 90° or π / 2 radians. The solution proposed by patent application WO2024105247A1 is particularly well-suited for electric furnaces with a chamber surface area of ​​approximately 80 m². 2However, it has been observed that this solution remains difficult to apply to the design of a tank whose surface area extends beyond 80 m². 2 , especially well beyond 80 m 2 (for example, up to 1000 m 2 ). This is due in particular to the fact that, for such large tank surfaces, it becomes much more difficult to understand and satisfy the constraints usually taken into consideration for proper furnace operation (examples of quantities / parameters / values ​​on which constraints can be considered: limitation of foaming, corrosion, temperature of the melting bath, electrical consumption, electrode life, safety with regard to the risk of exposure to electromagnetic fields, etc.). Description of the invention

[0011] The present invention aims to overcome all or part of the drawbacks of the prior art, particularly those described above, by proposing a solution that allows for the design of a glass furnace equipped with an electric melting zone, especially one of very large dimensions (for example, a tank surface area of ​​between 80 m²). 2 and 1000 m 2 ), much more effectively than state-of-the-art solutions.

[0012] To this end, and according to a first aspect, the invention relates to a computer-implemented method for determining parameter values ​​intended to be used for the manufacture of an electric melting zone of a glass furnace, said zone comprising a tank of surface area S in a theoretical horizontal plane, adapted to contain a melting bath and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank.

[0013] The said process is implemented by considering a set of given parameters, including: - an electrical fusion flux φ between the molten pool and a crust covering the molten pool, - a specific intensity for each group of electrodes, the specific intensity of a group of electrodes corresponding to the ratio between the electrical intensity supplying said group and the sum of the surfaces immersed in the molten pool of the electrodes of said group, - maximum and minimum current intensities of the electrical supply to the electrodes.

[0014] Furthermore, the said process includes a determination of the values ​​of the parameters L[i], S and N, such that, for each fusion module M[i], the following formula is satisfied: Or: ■ a1[i], b1[i] are coefficients taking into account the influence on L[i] of said maximum and specific intensities, and such that a1[i] x φ b1[i] is an upper bound of L[i], ■ a2[i], b2[i] are coefficients taking into account the influence on L[i] of said minimum and specific intensities, and such that a2[i] x φ b2[i] is a lower bound of L[i],

[0015] Thus, the determination method according to the invention makes it possible to identify possible values ​​(with regard to the preceding formula) of the parameters S, N, and L[i] for each of the melting modules. Ultimately, this amounts to identifying possible configurations of the melting zone, so as to ensure excellent operation of the glass furnace with regard to all the physical phenomena that occur in said zone Z and which are discussed in detail below.

[0016] In particular modes of implementation, the determination process may further include one or more of the following characteristics, taken individually or in all technically possible combinations.

[0017] In particular modes of implementation, a plurality of values ​​is determined for each of the parameters L[i], S and N, said process further comprising a selection, from said plurality of values ​​and in accordance with a determined selection criterion, of a value for each of said parameters.

[0018] In specific implementation modes, the electrical fusion flux φ is between 40 kW.m -2 and 80 kW.m -2 .

[0019] In specific implementation modes, the maximum electrical supply current to the electrodes is 10000 A.

[0020] In specific implementation modes, the minimum electrical supply current to the electrodes is 6000 A.

[0021] In certain implementation modes, the specific current of each electrode group is less than 2 A.cm -2 , preferably less than 1.6 A.cm -2and greater than 1 A.cm -2 , for example equal to 1.5 A.cm -2 .

[0022] In particular modes of implementation, for each fusion module M[i], the electrodes are arranged in a quadrilateral according to said theoretical horizontal plane, for example a rectangle, preferably a square.

[0023] In specific implementation methods: - the glass intended to be produced by the furnace is a transparent soda-lime glass, - the fusion modules are of the same square shape in said theoretical horizontal plane, - the parameter L[i] corresponds to the diagonal length of said square shape, - for each fusion module M[i], four groups of electrodes are respectively positioned at the ends of the two diagonals of said square shape, - the coefficients ai[i] and bi[i] are respectively equal to 1114.25 and -1.0149, - the coefficients a2[i] and b2[i] are respectively equal to 1533.54 and -1.2703.

[0024] In specific implementation methods: - the glass intended to be produced by the furnace is boron glass, - the fusion modules are of the same square shape in said theoretical horizontal plane, - the parameter L[i] corresponds to the diagonal length of said square shape, - for each fusion module M[i], four groups of electrodes are respectively positioned at the ends of the two diagonals of said square shape, - the coefficients al[i] and bl[i] are respectively equal to 1033.98 and -1.0318, - the coefficients a2[i] and b2[i] are respectively equal to 1701.18 and -1.3434.

[0025] In specific implementation methods, the surface area S of the tank is between 80 m 2 and 1000 m 2, preferably between 80 m 2 and 500 m 2 .

[0026] In particular implementation modes, the number N of fusion modules is between 1 and 7, preferably between 1 and 4.

[0027] According to another aspect, the invention relates to a computer program comprising instructions for implementing a method for determining parameter values ​​according to the invention when said computer program is executed by a computer.

[0028] This program can use any programming language, and be in the form of source code, object code, or code somewhere between source code and object code, such as in a partially compiled form, or in any other desirable form.

[0029] According to another aspect, the invention relates to a computer-readable information or recording medium on which a computer program according to the invention is recorded.

[0030] The information or recording medium can be any entity or device capable of storing the program. For example, the medium may include a storage means, such as a ROM, for example a CD-ROM or a microelectronic circuit ROM, or a magnetic recording means, for example a hard drive.

[0031] On the other hand, the information or recording medium can be a transmissible medium such as an electrical or optical signal, which can be transmitted via an electrical or optical cable, by radio, or by other means. The program according to the invention can, in particular, be uploaded to a network such as the Internet.

[0032] Alternatively, the information or recording medium may be an integrated circuit in which the program is incorporated, the circuit being adapted to execute or to be used in the execution of the process in question.

[0033] According to another aspect, the invention relates to a determination device comprising means configured to implement a method for determining parameter values ​​according to the invention.

[0034] For example, said determination device includes a computer program containing instructions for implementing said method of determining parameter values ​​when said computer program is executed by a computer.

[0035] According to another aspect, the invention relates to a manufacturing method, referred to as the "first manufacturing method", of an electric melting zone of a glass furnace, said zone comprising a tank of surface area S in a theoretical horizontal plane, adapted to contain a melting bath and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said manufacturing method being implemented from parameter values ​​L[i], S and N determined in accordance with a method for determining parameter values ​​according to the invention.

[0036] Correspondingly, the invention also relates to an electrical melting zone obtained by this first manufacturing process.

[0037] According to another aspect, the invention relates to a manufacturing process, called the "second manufacturing process", of a glass furnace comprising a manufacturing step of an electric melting zone in accordance with the first manufacturing process according to the invention.

[0038] In particular modes of implementation, the electric melting zone has a cold vault, and the glass furnace includes a corset linking the electric melting zone to a zone for refining and homogenizing the glass.

[0039] Preferably, the glass furnace (comprising a frame) has a tank with a surface area S between 200 m 2 and 500 m 2 .

[0040] In certain implementation configurations, the electric melting zone has a cold vault, and the glass furnace includes a groove connecting the electric melting zone to a forming unit. A working basin, for cooling and / or refining the glass, may be located between the electric melting zone and the forming unit.

[0041] Preferably, said glass furnace (comprising a groove) comprises a tank whose surface area S is between 80 m 2 and 200 m 2 .

[0042] Correspondingly, the invention also relates to a glass furnace obtained by this second manufacturing process.

[0043] According to another aspect, the invention relates to a process for melting vitrifiable materials implemented by means of a glass furnace obtained by the second manufacturing process according to the invention.

[0044] According to another aspect, the invention relates to a method for manufacturing glass wool, textile yarns and / or flat or hollow glass, said method implementing a process for melting vitrifiable materials according to the invention.

[0045] According to another aspect, the invention relates to a glass furnace comprising an electric melting zone having a tank of surface area S in a theoretical horizontal plane, adapted to contain a melting bath and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said furnace being manufactured by implementing a method for determining parameter values ​​according to the invention or by a method for manufacturing an electric melting zone of a glass furnace according to the invention.

[0046] According to another aspect, the invention relates to a glass product obtained by implementing a process of melting vitrifiable materials according to the invention or by implementing a furnace according to the invention. Brief description of the drawings

[0047] Other features and advantages of the present invention will become apparent from the description below, with reference to the accompanying drawings, which illustrate an example of an embodiment without being limiting in any way. In the figures: - [Fig. 1] schematically represents, from a top view, a particular embodiment of an electrical melting zone according to the invention; - [Fig. 2] represents, in the form of a flowchart, a particular method of implementing a process according to the invention to determine parameter values ​​intended to be used to manufacture an electric melting zone of a glass furnace; - [Fig. 3] is a graph representing an example of the evolution of corrosion of the tank of a melting zone as a function of the temperature of the melting bath in this tank; - [Fig. 4] is a graph representing an example of the evolution of the melt flow as a function of the temperature of the glass in the melting bath for a transparent soda-lime glass; - [Fig. 5] is a graph representing an example of the evolution of the temperature of the glass in the melting bath as a function of the specific draw for a transparent soda-lime glass with 40% cullet; - [Fig. 6] is a graph representing, for a transparent soda-lime glass with 40% cullet, an example of the evolution of specific electrical consumption as a function of the melting flux; - Figure 7 is a graph representing an example of the evolution of the total electrical intensity as a function of the side length of a melting modulus in the electrical melting zone for a transparent soda-lime glass with 40% cullet at a specific draw of 2.35 t / d / m 2 ; - Figure 8 is a table summarizing the results of a first simulation example; - Figure 9 is a table summarizing the results of a second simulation example - [Fig. 10] is a table grouping results from a third simulation example; - [Fig. 11] is a graph combining the results of the examples in Figures 8, 9 and 10; - [Fig. 12] is a table corresponding to a numerical application carried out at a specific fusion flux value; - [Fig. 13] represents, in the form of a flowchart, a particular method of implementing a process for manufacturing an electrical melting zone according to the invention; - [Fig. 14] represents, in the form of a flowchart, a particular method of implementing a process for manufacturing glass wool, textile yarns and / or flat or hollow glass according to the invention. Detailed description of the invention

[0048] The present invention relates in particular to a method for determining parameter values ​​intended for use in manufacturing an electrical melting zone (Z) in a glass furnace. Aspects relating to the implementation of this method are described in more detail later, and first, a specific embodiment of such a Z-zone, as manufactured using one or more of the parameters determined by this method, is presented.

[0049] Figure 1 schematically represents, from a top view, a particular embodiment of an electrical fusion zone Z according to the invention.

[0050] The melting zone Z is integrated into a glass furnace, that is, a furnace adapted for glass production. It should be noted that only zone Z is shown in Figure 1; the other elements / equipment / devices / arrangements of the glass furnace are known separately.

[0051] The term "glass manufacturing" includes the essential melting stage of the vitrifiable materials in the Z zone and, where appropriate, all subsequent / supplementary stages aimed at refining and homogenizing (for example by means of a hot vault refining and homogenizing zone with flame burners and connected to the Z zone, by a corset, or by a groove or any other means of connection depending on the intended application for the manufactured glass), or even conditioning the molten glass for its final shaping, in particular as flat glass (windows), hollow glass (flaps, bottles), glass in the form of mineral wool (in particular glass wool) used for its thermal or acoustic insulation properties, or even possibly glass in the form of so-called textile yarns used in reinforcement.

[0052] Conventionally, zone Z includes a suitable tank 10 (i made of suitable refractory materials) to contain the molten bath, and which, in the example of Figure 1, is rectangular in shape.

[0053] Preferably, zone Z is a cold-vaulted zone located above tank 10. There is no limitation on the surface area of ​​tank 10. For example, the surface area of ​​tank 10 is between 80 m² 2 and 1000 m 2 , preferably between 80 m 2 and 500 m 2 .

[0054] Preferably, the surface area S of tank 10 is between 200 m 2 and 500 m 2 in the case of a glass furnace intended for the manufacture of flat glass, typically soda-lime glass.

[0055] Preferably, the surface area S of tank 10 is between 80 m 2 and 200 m 2 in the case of a glass furnace intended for the manufacture of glass for glass wool, or textile yarns, typically boron glass.

[0056] It should be noted that the Z melting zone is entirely electric (i.e., glass melting is carried out solely using electrical energy). The operation of other parts of the furnace, for example, any refining and homogenizing and / or packaging zones, can be achieved using one or more types of energy (e.g., electrical energy and / or flame burners), according to any method known to those skilled in the art.

[0057] In the present embodiment, and as illustrated by Figure 1 by way of no limitation, the Z zone (and therefore a fortiori the tank 10) is divided into three fusion modules M[1], M[2], M[3] arranged one after the other.

[0058] It is important to note that considering three fusion modules M[1], M[2], M[3] does not limit the invention in any way. The number of fusion modules that can be considered results from considerations related to the execution of the determination method mentioned above, which is described in more detail later.

[0059] Each fusion module M[i] (i being an integer index between 1 and 3) corresponds to a virtual sub-part of the Z zone (i.e. there is no physical separation between two distinct fusion modules), this sub-part comprising a plurality of electrode groups.

[0060] More specifically, in the present embodiment, each fusion module M[i] comprises four electrode groups G[i, A], G[i, B], G[i, C], and G[i, D], each group consisting of three electrodes A[i,j], three electrodes B[i,j], three electrodes C[i,j], and three electrodes D[i,j] (where j is an integer index from 1 to 3). The use of three electrodes per electrode group is not a limitation of the invention; other numbers are possible. Furthermore, it is not precluded that at least one group may have a different number of electrodes than at least one other group.

[0061] For the sake of simplicity, only the reference signs corresponding to the electrodes A[1,j], B[1,j], C[1,j], D[1,j] of the fusion module M[1] are indicated in Figure 1. It is understood, however, that in the mode described here, the electrodes A[i,j], B[i,j], C[i,j], D[i,j] of the fusion module M[i], for i between 2 and 3, occupy positions similar to the respective positions of the electrodes A[1,j], B[1,j], C[1,j], D[1,j].

[0062] In this embodiment, the electrodes A[i,j], B[i,j], C[i,j], D[i,j] of each of the modules M[i] are immersion electrodes submerged from the free surface of the molten pool, for example with arms of square cross-section. As is known, the portion of an electrode in contact with the molten pool is composed of molybdenum.

[0063] It should be noted that the invention is not limited by the use of immersion electrodes, and nothing precludes, as a complement or alternative, the use of one or more electrodes completely immersed in the molten bath, for example, arranged vertically from the furnace floor or horizontally from the side walls of the vessel 10. Immersion electrodes, however, offer a number of advantages compared to completely immersed electrodes. First, they obviously avoid the difficulties associated with passing immersed electrodes through the refractory floor or side walls, and also the problems of replacing these electrodes when they are worn.They also help to minimize tank sealing problems 10 or refractory wear, particularly due to high temperatures which promote refractory attack and powerful convection currents which develop near the electrodes during operation.

[0064] Conventionally, each electrode A[i,j], B[i,j], C[i,j], D[i,j] is separated from the wall of the tank 10 by a minimum distance (measured along the normal to the wall nearest the electrode), for example, greater than 450 mm, preferably greater than 600 mm, preferably greater than 800 mm, preferably greater than 950 mm, preferably greater than 1075 mm, preferably greater than 1500 mm. Achieving such a minimum distance helps to limit premature wear (due to corrosion) of the wall of the tank 10.

[0065] Furthermore, in the present embodiment, and as illustrated by Figure 1 by way of no limitation, the fusion modules M[1], M[2], M[3] are of the same square shape in a theoretical horizontal plane (i.e. a theoretical plane parallel to the bottom of the tank 10)

[0066] It should be noted that, for a modulus M[i], a shape of a defined type is defined as the shape of said type located closest to the electrodes A[i,j], B[i,j], C[i,j], D[i,j]. In particular, in the example in Figure 1, the edges of said square shape pass through the electrodes A[i,j], B[i,j], C[i,j], D[i,j] for j taking the values ​​1 and 3.

[0067] The four electrode groups G[i, A], G[i, B], G[i, C], and G[i, D] of each module M[i] are positioned respectively at the ends of the two diagonals of the square shape, as illustrated in Figure 1, which is not intended to be limiting. These diagonals are shown in Figure 1 for illustrative purposes only, to symbolize the principal current directions for electrical exchange between the electrodes of each group.

[0068] More specifically, from the point of view of power supply, we have: - groups G[i, A] and G[i, B] are supplied by an alternating current of the same phase PH[i, A, B] (i.e. they are single-phase), - the groups G[i, C] and G[i, D] are supplied by an alternating current of the same phase PH[i, C, D], - the phase PH[i, A, B] is in quadrature with the phase PH[i, C, D].

[0069] In general, with regard to aspects relating to the realization of an electrical installation capable of supplying the electrodes A[i,j], B[i,j], C[i,j], D[i,j] of each module M[i], so as to obtain a quadrature of phase between the groups G[i, A], G[i, B], G[i, C], G[i, D], the document WO2024105247A1 already mentioned above can be consulted.

[0070] It follows from this configuration that, for each melting module M[i], the single-phase groups (i.e., groups G[i, A] and G[i, B] on the one hand, and groups G[i, C] and G[i, D] on the other) are separated by a length L[i] corresponding to the diagonal length of the square shape. This length L[i] is characteristic of the extent of the melting module M[i] in the tank 10.

[0071] It is important to note that considering electrodes arranged in this way (i.e., in a square) along a theoretical horizontal plane does not constitute a limitation of the invention. Thus, the electrodes of a fusion module M[i] can be arranged in any shape within such a theoretical horizontal plane (e.g., a quadrilateral, for example, a rectangle), provided that at least two single-phase groups are separated by a length L[i] characteristic of the extent of the fusion module M[i] in the cell 10.

[0072] In general, the only constraint imposed in terms of the configuration of a melting module M[i] is that at least two single-phase groups are separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank 10. It follows from this single constraint that the respective shapes of the tank 10 and of the melting module(s) M[i] are not limiting of the invention.

[0073] For example, nothing prevents us from considering a tank 10 of rectangular, square, circular, etc. shape in the theoretical horizontal plane.

[0074] As a complement or alternative, nothing excludes considering a fusion module M[i] of square, rectangular, circular, etc. shape in the theoretical horizontal plane.

[0075] For example, if the shape of a fusion module M[i] is a trapezoid in the theoretical horizontal plane, said distance L[i] characteristic of the extent of said module M[i] in the tank 10 corresponds to the largest diagonal of the trapezoidal shape.

[0076] For example, if the shape of a fusion module M[i] is rectangular in the theoretical horizontal plane, said distance L[i] characteristic of the extent of said module M[i] in the tank 10 corresponds to the diagonal of said rectangular shape.

[0077] According to another example, if the shape of a fusion module M[i] is circular in the theoretical horizontal plane, said distance L[i] characteristic of the extent of said module M[i] in the tank 10 corresponds to the diameter of said circular shape.

[0078] Nothing also excludes the possibility that two fusion modules arranged within tank 10 are of distinct shapes in the theoretical horizontal plane.

[0079] As a consequence of these considerations regarding the respective shapes of the tank 10 and the fusion modules, said fusion modules may partition the tank 10, i.e., partition the internal space of the tank 10, taking into account the minimum electrode-tank distance mentioned above (this is the case in the example illustrated in Figure 1). Alternatively, a fusion module may occupy only a fraction of the space allocated to it in the tank 10 (example: a circular module with a square space allocated to it in the tank 10).

[0080] It is therefore understood from the above that from the moment the respective general shapes of the tank 10 and the fusion modules are chosen, the said distance L[i] of each of the said fusion modules plays a fundamental role in terms of parameter to configure the Z zone.

[0081] Therefore, the purpose of the determination process mentioned above is to allow the identification, in particular, of possible values ​​of said parameter L[i] for each of the melting modules (which ultimately amounts to identifying possible configurations of the Z zone), so as to ensure excellent operation of the glass furnace with regard to all the physical phenomena which take place at the level of the Z zone.

[0082] It should be noted that the determination method is implemented by a determination device according to the invention (not shown in the figures). Said determination device comprises, for example, a processing circuit including one or more processors and storage means (magnetic hard drive, electronic memory, optical disc, etc.) in which data and a computer program product are stored, in the form of a set of program code instructions to be executed to implement all or part of the steps of the determination method.

[0083] Alternatively or in addition, the processing circuit includes one or more programmable logic circuits (FPGA, PLD, etc.), and / or one or more specialized integrated circuits (ASIC), and / or a set of discrete electronic components, etc., adapted to implement all or part of the steps of the determination process.

[0084] In other words, the processing circuit corresponds to a set of means configured by software (specific computer program product) and / or hardware (FPGA, PLD, ASIC, etc.) to implement the different stages of the determination process.

[0085] Figure 2 represents, in the form of a flowchart, a particular method of implementing the determination process according to the invention.

[0086] The determination process is implemented by considering a set of given parameters, including: - an electrical fusion flux φ, - a specific intensity for each group of electrodes, the specific intensity of a group of electrodes corresponding to the ratio between the electrical intensity supplying the electrodes of said group and the sum of the surfaces immersed in the melting bath of the electrodes of said group, - maximum and minimum current intensities of the electrical supply to the electrodes.

[0087] It is known that the electrical melting of glassable materials is achieved by energy transfer between the hot molten glass in the vat 10 and the "cold" crust composed of the glassable materials introduced onto the top of the melting bath, which are not yet melted. This energy transfer is proportional to the temperature of the hot molten glass in the vat 10. The melting flux corresponds to the power required to melt the glassable materials and heat the glass to the hot temperature, expressed per unit area S of the vat 10. Put another way, this is the energy required to produce the glass per unit area of ​​the vat 10 (unit: kW.m-2).

[0088] Therefore, and as illustrated by Figure 2, the determination process includes a step S10 of determining the values ​​of the parameters L[i], S and N, so that, for each fusion modulus M[i], the following formula (F) is satisfied: Or: - a₁[i], b₁[i] are coefficients taking into account the influence on L[i] of said maximum and specific intensities, and such that (a₁[i] × φ b₁[i] ) is an upper bound of L[i], ■ a2[i], b2[i] are coefficients taking into account the influence on L[i] of said minimum and specific intensities, and such that (a2[i] x <p b2[ ' ] ) is a lower bound of L[i].

[0089] To understand the origin of the preceding formula (F), the technical considerations relevant to the implementation of this determination method will now be described. To this end, the physical phenomena that must be taken into account to guarantee excellent furnace operation will be detailed, and the extent to which each of these physical phenomena leads to one or more constraints impacting the sizing and configuration of zone Z, such that, to satisfy these constraints, the preceding inequality must be verified.

[0090] The physical phenomena taken into account in the implementation of the determination process are as follows.

[0091] A) Foaming

[0092] During glass melting, the decarbonation-dehydration reactions and the decomposition of sulfates are of particular importance for crust stability. The emitted gases can then escape through the granular porous medium into the atmosphere, dissolve in the glass matrix up to their solubility limit, or form bubbles and, through coalescence, foam. The reaction kinetics are temperature-dependent; a high temperature can lead to significant foaming, to the point of creating a substantial insulating layer of gas between the hot glass and the raw material crust. This gaseous layer acts as a thermal barrier, impacting the melting capacity of the raw materials and potentially causing the furnace to overflow.

[0093] Consequently, to ensure proper melting and prevent excessive foaming, it is best to limit the temperature of the molten glass. Experiments show, for example, that for soda-lime glass used in the production of flat glass, a molten glass temperature below 1500 °C, preferably below 1450 °C, helps to limit the impact of foaming phenomena, and for boron-containing glass used in the production of insulation fibers, a molten glass temperature below 1400 °C, preferably below 1350 °C, helps to limit the impact of foaming phenomena.

[0094] B) Corrosion

[0095] As is well known, the higher the temperature of the molten glass, the more the furnace materials in contact with this molten glass are subject to corrosion. This is particularly true for the refractory materials used in the construction of the furnace 10.

[0096] Consequently, to ensure a good furnace lifespan, it is best to limit the temperature of the molten glass. Experiments show, for example, that for soda-lime glass used in the production of flat glass, a molten glass temperature below 1500 °C, preferably below 1450 °C, helps to limit the impact of corrosion, or for boron-containing glass intended for the production of insulation fiber, a molten glass temperature below 1400 °C, preferably below 1350 °C, helps to limit the impact of corrosion.

[0097] This principle is illustrated, for example, by Figure 3, which is a graph representing the evolution of corrosion in tank 10 (millimeters per year: mm / year) as a function of the melt pool temperature (degrees Celsius: °C). More specifically, in Figure 3, this evolution is represented by curve C3a. A dashed curve C3b is also shown, representing a limiting temperature set to restrict the impact of corrosion.

[0098] C) Drawn from the glass

[0099] The melting flux φ is directly proportional to the temperature of the glass. Experimentally, it has been shown that the melting flux φ can be approximated by the following formula:

[0100] φ = α × Tf γ + β

[0101] In this formula, the parameter Tf represents the temperature of the molten glass (i.e. the temperature of the glass in the melting bath) when the furnace is in nominal operation.

[0102] The coefficients α, β, and γ depend on the type of glass. As a non-limiting example, for a transparent soda-lime glass (e.g., Fe2O3 content less than 1000 ppm) intended for the manufacture of flat glass, the coefficients α, β, and γ can be taken to be 0.3024, -379.31, and 1.0, respectively.

[0103] It should be noted that the coefficients α, β, and γ typically depend on the composition of the vitrifiable materials used for the glass to be produced (flat glass, bottle glass, fiber, etc.), the desired color of the glass (if applicable), the thermal conductivity of the glass, and so on. These aspects are well known to those skilled in the art and are therefore not described in further detail here.

[0104] It therefore follows from the previous formula that the melt flow φ is directly proportional to the temperature of the glass. Consequently, the glass yield, i.e., the quantity of glass produced over time, is also proportional to the temperature of the glass. This can be expressed as follows:

[0105] φ = (δ × Δ) / S = α × Tf γ + β

[0106] Here, the parameter δ represents the furnace draft (unit: kg.s -1 ), the parameter S represents the surface area of ​​the tank 10 in the theoretical horizontal plane parallel to the sole (unit: m² 2 The parameter Δ represents the energy required to melt and heat 1 kg of glass to the temperature Tf, also known as the "processing energy" (unit kJ.kg). -1 ).

[0107] It should be noted that, in the preceding formula, the quantity δ / S corresponds to a so-called "specific" draw, that is to say, a draw per unit area of ​​the tank 10 in the theoretical horizontal plane kg.s -1 .m -2 .

[0108] It is therefore clear that to determine the relationship between the glass pull δ and the temperature Tf of the glass, it is necessary to know the glass production energy Δ. As is known, this production energy Δ depends in particular on the composition of the vitrifiable raw materials and the cullet content used.

[0109] As a non-limiting example, based on a first example given for a transparent soda-lime glass, it is possible to thermodynamically evaluate the energy Δ required to melt one kg of glass at the calcine rate c (expressed as a number between 0 and 1) and heat it to the temperature Tf using the formula:

[0110] Δ = 1.42 × Tf – 847.5 × c + 631.

[0111] Similarly, according to a second example given for a boron fiber insulation glass, the energy Δ required to melt one kg of glass at the calcine rate c (expressed as a number between 0 and 1) and heat it to the temperature Tf using the formula:

[0112] Δ = 1.22 × Tf – 831 × c + 822.

[0113] Figure 4 is a graph representing the evolution of the temperature Tf (degrees Celsius: °C) as a function of the melting flux φ for a transparent soda-lime glass.

[0114] Figure 5 is a graph representing the evolution of the temperature Tf (degrees Celsius: °C) as a function of the specific gravity ô / S (here expressed in tonnes per day per unit area: t.j'Lnr 2 ) for a transparent soda-lime glass with 40% calcin (i.e. calcin content = 0.4).

[0115] Therefore, taking into account the considerations in sections A) and B) above concerning the temperature Tf, namely, for a transparent soda-lime glass, preferably limiting Tf to an upper limit of 1500°C, or even 1450°C, or for a boron fiber insulating glass, preferably limiting Tf to an upper limit of 1400°C, or even 1350°C, to limit corrosion and avoid foaming and destabilization of the fusion crust, we deduce from Figures 4 and 5 that, in order to comply with these constraints on the temperature Tf, it is preferable to: - limit the fusion flux φ to an upper limit of 80 kW.m -2 , either - limit the specific draw to 3.0 tj -1 .m -2 , or even 2.8 tj -1 .m -2 , or even 2.4 tj -1 .m -2 , or even 2.2 tj -1 .m -2 for a 40% decalcin soda-lime glass or - limit the specific draw to 3.0 tj -1 .m -2, or even 2.8 tj^.m' 2 , or even 2.4 tj^.m' 2 , or even 2.2 tj^.m' 2 for a boron fiber insulation glass with 40% cullet.

[0116] D) Electricity consumption

[0117] In addition to the electrical energy consumed to heat and melt the glass so that it reaches the temperature Tf, electrical energy may also be consumed to compensate for heat losses occurring when the furnace is in operation.

[0118] Examples of such heat losses include: - thermal losses via the base of tank 10. These losses are proportional to the surface area S of tank 10; - heat losses through the walls of tank 10. These losses are proportional to the perimeter of tank 10; - Heat losses through the electrodes located in the melt pool, particularly when these electrodes are immersed. These losses are proportional to the number of electrodes used, which is itself related to the number of melting modules and their respective sizes; - Heat losses through the "cold" composition crust located on the surface of the melt pool. These losses are proportional to the surface area S of the tank 10.

[0119] In view of the detailed formulas above in section C) concerning the draft of the glass, it is understood that the thermal losses related to the surface S of the tank 10 are also related to the specific draft ô / S or to the melting flux q>.

[0120] In particular, the higher the specific draw ô / S or the melt flow q>, the lower the proportion of heat losses described above relative to the energy contribution for glass production.

[0121] Ultimately, the specific electrical consumption (i.e., the electrical consumption relative to the weight of molten glass) will therefore generally decrease with the increase in specific draw ô / S or the melting flux q>, eventually stabilizing.

[0122] This principle is illustrated, for example, by Figure 6, which is a graph showing the evolution of specific electrical consumption (here in kilowatt-hours per tonne: kWh / t) for a transparent soda-lime glass with 40% cullet. -1 ) as a function of the fusion flux q> (unit: kW.m -2 ). More specifically, in Figure 6, different curves of this evolution are illustrated, each curve corresponding to a square-shaped fusion modulus M[i] in the theoretical horizontal plane: - curve C6a (curve with cross): fusion modulus M[i] whose side length is equal to 14 m; - curve C6b (curve equipped with squares): fusion modulus M[i] whose side length is equal to 12 m; - C6c curve (curve equipped with triangles): fusion modulus M[i] whose side length is equal to 10 m; - C6d curve (curve equipped with circles): fusion modulus M [i] whose side length is equal to 8 m; - curve C6e (curve equipped with rhombuses): fusion modulus M[i] whose side length is equal to 6 m.

[0123] In this example in Figure 6, and considering the evolution of curves C6a, C6b, C6c, C6d, and C6e, it might be possible, for example, to limit the fusion flux q to a lower value of 40 kW.m². -2 (i.e., a specific draw ô / S greater than ~1.5 tj -1 .m -2 (from figures 4 and 5) to reduce the oven's electrical consumption.

[0124] As for other heat losses not directly related to the surface area S of the tank 10, these will depend in particular on the configuration of zone Z in terms of the number and configuration of the fusion modules used. Generally speaking, the fewer fusion modules present in zone Z, the lower these other heat losses.

[0125] For example, the number of fusion modules can be between 1 and 7, preferably between 1 and 4.

[0126] E) Electric intensity

[0127] As is known, the smaller the surface area of ​​an electrode, the greater the electrical current that must be passed through said electrode to achieve electrical power.

[0128] It is also known that the wear rate of an electrode depends on the specific current applied to it, said specific current corresponding to the electrical current supplying a unit area immersed in the melting bath of said electrode.

[0129] Preferably, it may also be considered to limit the specific current of each electrode group to a higher level. For example, the specific current of each electrode group may be set below 2 A.cm -2 , preferably less than 1.6 A.cm -2 , for example equal to 1.5 A.cm -2 .

[0130] Preferably, it may also be considered to limit the specific current of each electrode group to a lower value. For example, the specific current of each electrode group may be set above 1 A.cm -2 .

[0131] It should be noted that these values ​​are set for the initial commissioning of the furnace. Indeed, the inevitable wear of the electrodes over time means that these values ​​will increase.

[0132] According to another aspect, it can be observed that the total electrical intensity required to maintain a given fusion flux q> increases when the extent of a fusion modulus M[i] in the tank 10 increases.

[0133] This principle is illustrated, for example, by Figure 7, which is a graph representing, for a transparent soda-lime glass with 40% cullet and a melting flux q fixed at 65 kW.m -2 and a specific draw fixed at 2.35 tj -1 .m -2The evolution of the total electric current (here in amperes: A) as a function of the side length (here in meters: m) of a fusion modulus M[i]. More specifically, in Figure 7, different curves of this evolution are illustrated, each curve corresponding to a fixed specific current value: - curve C7a (curve with diamonds): specific current equal to 1 A.cm -2 ; - curve C7b (curve with squares): specific intensity equal to 1.5 A.cnr 2 ; - curve C7c (curve with circles): specific intensity equal to 2 A.cnr 2 .

[0134] From yet another perspective, it is known that the higher the electrical current used, the stronger the electromagnetic field generated by the current flow. Consequently, any conductive element of the furnace located within this generated electromagnetic field is likely to generate induced currents.

[0135] For example, it has been observed that above 8000 A, metallic elements near the furnace (example: furnace support structure) can heat up to the point of becoming red-hot.

[0136] All of these induced currents will therefore reduce the energy efficiency of the oven and increase the risk of staff exposure to the electromagnetic field.

[0137] For these reasons, it may be possible to limit the current supplied to the electrodes. For example, the maximum current supplied to the electrodes could be 10,000 A.

[0138] Finally, as seen above in section D) concerning power consumption, it is advantageous to limit the number of fusion modules to minimize heat losses not directly related to the surface area S of the cell 10. Therefore, as shown in Figure 7, the current supplied to the electrodes of a fusion module depends on the size of that module; consequently, it may be possible to limit this current to a lower value. For example, a minimum current supplying the electrodes could be 6000 A.

[0139] The rest of the description concerns three examples of numerical simulation, noted below as "example no. 1", "example no. 2" and "example no. 3".

[0140] More specifically, in these three examples, numerical simulation software is used, modeling the operation of a glass furnace with an electrical melting zone (Z). This software is notably capable of solving the electric field and evaluating the current flowing through the electrodes. For each phase, the power (P) is related to the current (I) and the voltage (U) by the equation P = U x I, and the voltage is related to the current via the impedance (Z) by the equation U = Z x I. This software is also capable of calculating the impedance (Z) based on the modeling assumptions described below.

[0141] For each of these three examples, we consider in a non-limiting way that the zone Z has a general configuration of the type described above with reference to Figure 1. In other words, we now assume that the zone Z has a rectangular tank 10 and that this tank 10 is intended to have one or more fusion modules M[i], each of said modules M[i] being square and having electrodes placed in pairs along the diagonals of said square.

[0142] For each of these three examples, we also consider: - the same specific current for each of the electrode groups G[i, A], G[i, B], G[i, C], G[i, D] of the modules M[i], said specific current being equal to 1.5 A.cm -2 , - a minimum distance between the tank and the electrodes of lm - maximum and minimum current intensities for the electrical supply to the electrodes are respectively equal to 10000 A and 6000 A, - an electrical melting for the production of a transparent soda-lime glass with 40% calcine (i.e. calcine rate = 0.4).

[0143] For example no. 1, we consider a fixed fusion flux q> equal to 80 kW.m -2 , i.e. a specific draw of 2.83 t / d / m 2 .

[0144] For example #2, we consider a fixed fusion flux q> equal to 40 kW.m -2 , i.e. a specific draw of 1.53 t / d / m 2 .

[0145] For example #3, we consider a fixed fusion flux q> equal to 54 kW.m -2 , i.e. a specific draw of 2.0 t / d / m 2 .

[0146] Figure 8 is a table summarizing the simulation results for example no. 1.

[0147] In the table in Figure 8, the input parameters are: - the output of the furnace (in tonnes per day: t.j') 1 ). This parameter is scaled in steps of 100 in the interval [200; 1400]; - the surface area S of the tank 10 (m 2 ). This parameter is scaled in steps of 100 / 2.83 in the interval [71; 495]; - the number N of fusion modules M[i]. The possible values ​​of this parameter are 1, 2, 3 or 4.

[0148] As can be noted, the simulated electrical current values ​​range from 4520 A to 18756 A. The boxes in the table that are greyed are those that respect the minimum and maximum electrical current values ​​mentioned previously, namely 6000 A and 10000 A.

[0149] Figure 9 is a table summarizing the simulation results for example no. 2.

[0150] In the table in Figure 9, the input parameters are: - the output of the furnace (in tonnes per day: t.j') 1 ). This parameter is scaled in steps of 100 in the interval [200; 1400]; - the surface area S of the tank 10 (m 2). This parameter is scaled in steps of 100 / 1.53 in the interval [131; 915]; - the number N of fusion modules M[i]. The possible values ​​of this parameter are 1, 2, 3 or 4.

[0151] As can be noted, the simulated electrical current values ​​range from 3193 A to 14544 A. The boxes in the table that are greyed are those that respect the minimum and maximum electrical current values ​​mentioned previously, namely 6000 A and 10000 A.

[0152] Figure 10 is a table summarizing the simulation results for example no. 3.

[0153] In the table in Figure 10, the input parameters are: - the output of the furnace (in tonnes per day: t.j') 1 ). This parameter is scaled in steps of 100 in the interval [200; 1400]; - the surface area S of the tank 10 (m 2 ). This parameter is scaled in steps of 50 in the interval [100; 700]; - the number N of fusion modules M[i]. The possible values ​​of this parameter are 1, 2, 3 or 4.

[0154] As can be noted, the simulated electrical current values ​​range from 3622 A to 15964 A. The boxes in the table that are greyed are those that respect the minimum and maximum electrical current values ​​mentioned previously, namely 6000 A and 10000 A.

[0155] It is possible to combine the results of example no. 1, example no. 2 and example no. 3 to determine the possible configurations of zone Z in terms of measurement of the surface area S of tank 10 and number N of fusion modules.

[0156] Figure 11 is a graph combining the results of the previous examples #1, #2 and #3.

[0157] For this purpose, the x-axis of the graph in Figure 11 represents the fusion flux q, while the y-axis represents the characteristic distance between electrodes L(i). It should be noted that in the specific case of examples 1, 2, and 3, the fusion moduli are all of the same square shape.

[0158] In this configuration the surface area of ​​the module is equal to 2).

[0159] The graph in Figure 11 contains two curves: - curve Cl la: this is a power-law approximation between the 3 points corresponding to the minimum values ​​of electrical intensity which are, on the one hand, contained in the tables of figures 9, 10 and 11 (i.e. fusion flux q > between 40 kW.m -2 and 80 kW.m -2 ) and, on the other hand, included in the interval [6000 A; 10000 A]; - Cllb curve: this is a power-law approximation between the 3 points corresponding to the maximum values ​​of electrical intensity which are, on the one hand, contained in the tables of figures 8, 9 and 10 (i.e. fusion flux q > between 40 kW.m -2 and 80 kW.m -2 ) and, on the other hand, included in the interval [6000 A; 10000 A],

[0160] In this example from Figure 11, we have more precisely the equation of the curve Cllb which is written: L(i) = 1114.25 × φ -1.0149

[0161] The equation of the curve Cl is written as follows: L(i) = 1533.54 × φ -1.2703

[0162] It follows that, in the graph in Figure 11, the interior of the quadrilateral whose four corners are the endpoints of the curves Cl la and Cllb (the interior of the quadrilateral is hatched in Figure 11) is defined by the following inequalities: L(j) < 1114.25 x ç 10149 L(i) > 1533.54 × φ -1.2703

[0163] These two inequalities can be combined into a single inequality denoted "(IN)", namely:

[0164] In summary, the preceding inequality (IN) allows us to determine the parameters L(i), S and N, and therefore ultimately the parameters S and N, allowing us to configure zone Z of tank 10 so as to comply with the constraints mentioned above in sections A) to E), namely: - a temperature Tf below 1500 °C, or even below 1450 °C to limit foaming and corrosion, - a fusion flux q > between 40 kW.m -2 and 80 kW.m -2 , - a specific draw of less than 2.83 tj -1 .m -2 , or even less than 2.2 tj^.m' 2 - a specific draw greater than 1.5 tj -1 .m -2 to limit specific electricity consumption, - a number N of fusion modules between 1 and 7, preferably between 1 and 4, to limit power consumption, - a specific intensity of each electrode group of less than 2 A.cm -2 , preferably less than 1.6 A.cm -2 , for example equal to 1.5 A.cm -2 to limit electrode wear, and preferably greater than 1 A.cm -2 . - a maximum current supply to the electrodes of 10000 A to limit the risks of exposure of personnel to the electromagnetic field, - a minimum current supply to the electrodes of 6000 A.

[0165] It is therefore possible to note the correspondence with the formula (F) mentioned previously, considering that the coefficients al[i] and bl[i] are respectively equal to 1114.25 and -1.0149, and that the coefficients a2[i] and b2[i] are respectively equal to 1533.54 and -1.2703 (inequality (IN) having been established by considering, in no way restrictively, that the fusion moduli are all of the same square shape, the said coefficients al[i], bl[i], a2[i] and b2[i] are here all equal).

[0166] As previously indicated, the examples just described relate in a non-limiting way to the case of soda-lime glass and the determination process according to the invention also applies to the manufacture of a melting zone for other types of glass such as boron glass, depending on the applications.

[0167] Thus, for a boron glass intended for the manufacture of glass wool or textile yarns, we obtain in the same way a correspondence with formula (F), considering that the coefficients a 1 [i] and bl[i] are respectively equal to 1033.98 and -1.0318, and that the coefficients a2[i] and b2[i] are respectively equal to 1701.18 and -1.3434 (inequality (IN) having been established by considering, in no way limitingly, that the melting moduli are all of the same square shape, the said coefficients al[i], bl[i], a2[i] and b2[i] are here all equal).

[0168] Figure 12 is a table corresponding to an example of a numerical simulation carried out under conditions similar to those of Figures 8 and 9, but now considering a fusion flux q > 65 kW / m² -2 and by evaluating the fraction of the inequality (IN).

[0169] The boxes in the table in Figure 12 which are shaded therefore determine values ​​of the parameters S and N (and therefore in the end of the parameter L[i]) for which the inequality (IN) is verified.

[0170] It should be noted that the physical phenomena considered in the implementation of the determination method were described above in sections A) to E), including application / simulation examples for a transparent soda-lime glass with 40% cullet. Nevertheless, the results obtained remain applicable regardless of the cullet content. More generally, and as previously mentioned, the preceding results apply to glass in the broadest sense.

[0171] Returning to Figure 2, we understand that at the end of step S10, it is possible to obtain one or more combinations of respective values ​​of the parameters S, N, L[i] allowing us to satisfy formula (F).

[0172] Also, in the particular mode of Figure 2, the determination process also includes a step S20 for selecting, from among the plurality of values ​​of the parameters S, N, L[i] resulting from the execution of step S10, a value for each of said parameters. This selection is carried out in accordance with a determined selection criterion.

[0173] For example, the selection criterion may consist of selecting values ​​of the parameters S, N and L[i] that minimize the manufacturing cost of the electrical fusion Z zone.

[0174] In addition or as an alternative, the selection criterion takes into account the availability of space for the implementation of the electrical fusion zone Z.

[0175] More generally, there are no limitations attached to the nature of the selection criterion. It can also be a random selection from among the combinations of respective values ​​of the parameters S, N, L[i] that satisfy formula (F).

[0176] It is also understood that if the result of the execution of step S10 is that there is only one possible combination of respective values ​​of the parameters S, N, L[i] allowing to satisfy the formula (F), said step S20 is not executed.

[0177] The values ​​of parameters S, N, and L[i], determined by the determination method according to the invention, thus define the configuration and dimensions of the electrical melting zone Z. Furthermore, and according to another aspect, the invention relates to a method for manufacturing said zone Z from said values ​​of parameters S, N, and L[i].

[0178] Figure 13 represents, in the form of a flowchart, a particular method of implementing the manufacturing process of zone Z according to the invention.

[0179] As illustrated by Figure 13, the manufacturing process first includes a step T10 of obtaining the values ​​of the parameters S, N and L[i] intended to be used.

[0180] This T10 obtaining step can, for example, correspond to an implementation of the determination process described above.

[0181] Alternatively, the determination process may have been carried out prior to the implementation of the manufacturing process for zone Z. In this case, step T10 may, for example, correspond to a transmission of the values ​​of the parameters S, N, and L[i] determined during that prior execution. This transmission may be carried out using any known communication protocol / interface.

[0182] Subsequently, and as illustrated by Figure 13, the manufacturing process includes a step T20 of effective manufacturing of the Z zone from the values ​​of the parameters S, N and L[i] obtained during the execution of step T10.

[0183] In yet another aspect, the invention relates to a method for manufacturing a glass furnace. This method for manufacturing the glass furnace includes a step for manufacturing the Z-zone for electric melting in accordance with the manufacturing process described above with reference to Figure 13.

[0184] Figure 14 represents, in the form of a flowchart, a particular method of implementing a process for manufacturing glass wool, textile yarns and / or flat or hollow glass according to the invention.

[0185] As illustrated in Figure 14, the manufacturing process comprises a first step U10 of melting vitrifiable materials. This step U10 is carried out by electrically heating the melting bath using a suitable alternating current supplying the electrodes. It should be noted that this step U10 constitutes, as such, a process for melting vitrifiable materials within the meaning of the present invention.

[0186] The manufacturing process also includes a U20 step of the actual production of glass wool, textile glass yarns and / or flat or hollow glass using the vitrifiable materials thus fused via the implementation of the U10 step.

[0187] As will be understood, the invention relates to a method for determining parameter values ​​intended to be used for the manufacture of an electric melting zone of a glass furnace, said zone comprising a tank of surface area S and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups supplied by a two-phase alternating current, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said method comprising a determination of parameter values ​​L[i], S and N, so as to optimize the operation of the furnace.

[0188] Advantageously, the said method of determining parameter values ​​intended for use in the manufacture of an electric melting zone of a glass furnace is a computer-implemented method.

[0189] The present invention is capable of industrial application, the parameter values ​​determined by the said determination process being used for the manufacture of an electric melting zone of a glass furnace in particular intended for the manufacture of glass wool, textile glass yarns and / or flat or hollow glass.

Claims

DEMANDS

1. A computer-implemented method for determining parameter values ​​for use in manufacturing an electric melting zone of a glass furnace, said zone comprising a tank of surface area S in a theoretical horizontal plane, adapted to contain a melt pool and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said method being implemented considering a set of given parameters, including: - an electrical flux φ of fusion between the molten pool and a crust covering the molten pool, - a specific intensity for each electrode group, the specific intensity of an electrode group corresponding to the ratio between the electrical intensity supplying said group and the sum of the surfaces immersed in the melting bath of the electrodes of said group, - the maximum and minimum electrical supply intensities of the electrodes, and said process comprising a determination of the values ​​of the parameters L[i], S and N, such that, for each fusion modulus M[i], the following formula is satisfied: ■ ai[i], bi[i] are coefficients taking into account the influence on L[i] of said maximum and specific intensities, and such that ai[i] x φ b1[i] is an upper bound of L[i], ■ a2[i], b2[i] are coefficients taking into account the influence on L[i] of said minimum and specific intensities, and such that a2[i] x φ b2[i] is a lower bound of L[i].

2. A method according to claim 1, wherein a plurality of values ​​is determined for each of the parameters L[i], S, and N, said method further comprising selecting, from said plurality of values ​​and in accordance with a determined selection criterion, a value for each of said parameters.

3. A method according to any one of claims 1 to 2, wherein the flow <p de fusion électrique est compris entre 40 kW.m -2 and 80 kW.m -2 .

4. A method according to any one of claims 1 to 3, wherein the maximum current supplied to the electrodes is 10000 A.

5. A method according to any one of claims 1 to 4, wherein the minimum current supplying the electrodes is 6000 A.

6. A method according to any one of claims 1 to 5, wherein the specific current of each electrode group is less than 2 A.cm -2 , preferably less than 1.6 A.cm -2 and greater than 1 A.cm -2 , for example equal to 1.5 A.cm -2 .

7. A method according to any one of claims 1 to 6, wherein, for each fusion module M[i], the electrodes are arranged in a quadrilateral along said theoretical horizontal plane, for example a rectangle, preferably a square.

8. A method according to claims 3 to 7, wherein: - the glass intended to be produced by the furnace is a transparent soda-lime glass, - the melting modules are of the same square shape in the said theoretical horizontal plane, - the parameter L[i] corresponds to the diagonal length of said square shape, - for each melting module M[i], four groups of electrodes are respectively positioned at the ends of the two diagonals of said square shape, - the coefficients ai[i] and bi[i] are respectively equal to 1114.25 and -1.0149, - the coefficients a2[i] and b2[i] are respectively equal to 1533.54 and -1.2703.

9. A method according to claims 3 to 7, wherein: - the glass intended to be produced by the furnace is boron glass, - the fusion modules are of the same square shape in said theoretical horizontal plane, - the parameter L[i] corresponds to the diagonal length of said square shape, - for each fusion module M[i], four groups of electrodes are respectively positioned at the ends of the two diagonals of said square shape, - the coefficients al[i] and bl[i] are respectively equal to 1033.98 and -1.0318,- the coefficients a2[i] and b2[i] are respectively equal to 1701.18 and -1.3434.

10. A method according to any one of claims 1 to 9, wherein the surface area S of the tank is between 80 m 2 and 1000 m 2 , preferably between 80 m 2 and 500 m 2 .

11. A method according to any one of claims 1 to 10, wherein the number N of fusion modules is between 1 and 7, preferably between 1 and 4.

12. A method for manufacturing an electric melting zone of a glass furnace, said zone comprising a tank of surface area S in a theoretical horizontal plane, adapted to contain a melting bath and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said manufacturing method being implemented from parameter values ​​L[i], S and N determined in accordance with a method according to any one of claims 1 to 11.

13. A method for manufacturing a glass furnace comprising a step of manufacturing an electric melting zone according to a method according to claim 12.

14. A method according to claim 13, wherein the electrical melting zone is cold-roofed, and the glass furnace includes a corset connecting the electrical melting zone to a glass refining and homogenization zone.

15. A method according to claim 13, wherein the electrical melting zone is cold-roofed, and the glass furnace comprises a groove connecting the electrical melting zone to a fiber-laying installation.

16. A method for melting vitrifiable materials implemented using a glass furnace obtained by a method according to any one of claims 13 to 15.

17. A method for manufacturing glass wool, textile yarns and / or flat or hollow glass, said method employing a melting process according to claim 16.

18. A determination device comprising means configured to implement a method for determining parameter values ​​according to any one of claims 1 to 11, for example said determination device comprising a computer program comprising instructions for implementing said method for determining parameter values ​​when said computer program is executed by a computer.

19. Glass furnace comprising an electric melting zone having a tank of surface area S in a theoretical horizontal plane, adapted to contain a melting bath and divided into N melting modules, each melting module M[i] comprising a plurality of electrode groups, the phase of the alternating current supplying two electrode groups being in quadrature with that of the alternating current supplying two other electrode groups, at least two single-phase groups being separated by a length L[i] characteristic of the extent of the melting module M[i] in the tank, said furnace being manufactured by implementing a method for determining parameter values ​​according to any one of claims 1 to 11 or by a method for manufacturing an electric melting zone of a glass furnace according to any one of claims 12 to 15.