Bumpy calcined ceria particles and use therefor

Bumpy calcined ceria particles with a controlled surface texture address the issue of high defect rates in CMP polishing by enhancing mechanical aggressiveness and stability, achieving efficient removal rates with reduced scratches.

WO2026234118A2PCT designated stage Publication Date: 2026-11-12MERCK PATENT GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2026/063144
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing calcined ceria particles used in chemical mechanical planarization (CMP) polishing compositions suffer from high defect rates due to their smooth surfaces and sharp edges, which cause scratches, despite efforts to increase particle size for higher removal rates.

Method used

The development of bumpy calcined ceria particles with a tailored bumpy surface texture, comprising protrusions such as bumps, branches, or tree bark, which are integral parts of the particle structure, achieved through a controlled calcination and sintering process, allowing for smaller particle sizes without increasing defect rates.

Benefits of technology

The bumpy calcined ceria particles provide enhanced mechanical aggressiveness and improved CMP polishing performance with reduced defects, maintaining high removal rates and stability during the polishing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000049_0001_TABLE
    Figure IMGF000049_0001_TABLE
  • Figure 00000041_0000
    Figure 00000041_0000
  • Figure 00000041_0001
    Figure 00000041_0001
Patent Text Reader

Abstract

Present invention provides a new type of colloidally stable, calcined ceria particles with a tailorable bumpy surface having a surface texture including but not limited to bumps, protrusions, branches or tree bark, and combinations thereof, and thus referred as bumpy calcined ceria particles. The new bumpy calcined ceria particles are used as the abrasive particles in Chemical Mechanical Planarization (CMP) polishing compositions to provide better removal rates and low scratches.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No.: P25-207-SEC-W002TITLE OF THE INVENTION:BUMPY CALCINED CERIA PARTICLES AND USE THEREFORCROSS REFERENCE TO RELATED PATENT APPLICATIONS

[0001] The present application claims the benefit of U.S. Application No.63 / 803,256 filed on May 9, 2025, the disclosure of which is hereby incorporated by reference as if fully set forth.BACKGROUND OF THE INVENTION

[0002] This invention relates to bumpy calcined ceria particles and their important use as abrasive particles for chemical mechanical planarization (CMP) polishing in semiconductor manufacture.

[0003] The bumpy calcined ceria particles and the method of making those particles have been disclosed. CMP polishing compositions, formulations, or slurries (they are used interchangeably) using bumpy calcined ceria particles, the method and the system of using the compositions have also been disclosed.

[0004] Chemical mechanical planarization (CMP) is an important step in the manufacturing process of transistors. It is performed after each step where materials are deposited, such as by Chemical Vapor Deposition (CVD) and / or Plasma-Enhanced Chemical Vapor Deposition (PE-CVD). Typical deposition methods cannot achieve the required surface planarity, especially on patterned wafers.

[0005] The CMP polishing process enables the creation of smooth, defects free layers that are later being covered with other layers to produce the stack. To achieve planarity, CMP combines chemical attack and mechanical abrasion to remove excess material. The CMP polishing compositions (formulation or slurries are interchangeable) are aqueous composition that contains several components such as abrasive particles (for mechanical abrasion), chemical additives (for chemically dissolving and solubilizing the material to be planarized) such as oxidant, catalyst, stabilizers, ligands, and other additives as described in International journal of precision engineering and manufacturing, 2016, 17(12), 1751.

[0006] The abrasives used in CMP polishing compositions are nanoparticles of inorganic oxide particles, metal oxide-coated inorganic oxide particles, organic polymer particles, metal oxide-coated organic polymer particles, and combinations thereof. Abrasive particles comprise inorganic oxide particles, such as ceria, silica is commonly used.

[0007] The size, structure, and surface chemistry of the abrasive particles are key factors in determining CMP polishing performance. Performance is measured,Attorney Docket No.: P25-207-SEC-W002besides other factors, mainly by the material removal rate and the number of defects (scratches) caused by the abrasives.

[0008] For Shallow Trench Isolation (STI) applications, the calcined and subsequently milled ceria abrasives are considered state-of-the-art. They offer better performance compared to colloidal ceria abrasives processed at lower temperatures in water. The performance of calcined ceria abrasives is mainly influenced by the particle size due to limitations in shape and surface morphologies resulting from the calcination and milling process.

[0009] Larger particle sizes contribute to higher CMP removal rates, which is beneficial. However, larger particles also increase the occurrence of defects like scratches. Therefore, significant efforts have been made to synthesize the largest possible ceria particles that maintain an acceptable level of defects. Achieving this involves complex and costly purification steps to remove particles above a certain threshold size.

[0010] Thus, there is a significant need of abrasive particles used in CMP polishing compositions that can afford high removal rates with a low defect rate.BRIEF DESCRIPTION OF SEVERAL VIEWS OF THE DRAWINGS

[0011] Fig. 1 shows a comparison of invented bumpy calcined ceria particles with ceria particles known in literature.

[0012] Fig. 2 shows a visualization of the difference between a nanoparticle which was “glued” to an abrasive core and the innovative bumpy calcined ceria particles.

[0013] Fig. 3 is a flowchart showing three processes to make bumpy ceria particles.

[0014] Fig. 4 illustrates the general evolution of bumpy calcined ceria particles.

[0015] Fig. 5 illustrates one of the examples for the formation of bumpy calcined ceria particles starting from the ceria particles having different sizes which can be a direct mixing of ceria particles having different sizes or mixing one size ceria particles with a ceria precursor which can produce different size of ceria particles.

[0016] Fig. 6 illustrates one of the examples for the evolution of hybrid bumpy calcined ceria particles, that is, hybrid particles starting from a mixture of different oxides (oxide particles) and thus having domains of different physical and / or chemical properties.

[0017] Fig. 7 illustrates one of the examples for the formation of hybrid bumpy calcined ceria particles, comprising selectively doped and undoped domains.

[0018] Fig. 8 illustrates one of the examples for the formation of inventive hybrid particles comprising 2 or more cerium oxides having different physico-chemical properties.Attorney Docket No.: P25-207-SEC-W002

[0019] Fig. 9 is the SEM image showing fluffy nano powder or nanoparticles used as the starting material.

[0020] Fig. 10 is the SEM image of ceria particles after granulation with water and sintering the starting ceria nanoparticles as shown in Fig. 9

[0021] Fig. 11 is the SEM image of bumpy calcined ceria particles having mean particle size of 50-70 nm after the wet milling of ceria particles as shown in Fig. 10.

[0022] Fig. 12 is the SEM image of ceria particles after granulation with water and organic binder and sintering the starting ceria nanoparticles as shown in Fig. 9.

[0023] Fig. 13 is the SEM image of bumpy calcined ceria particles having mean particle size of 50-70 nm after the wet milling of ceria particles as shown in Fig. 12.

[0024] Fig.14 is the SEM image of ceria particles after sintering the starting ceria nanoparticles as shown in Fig. 9.

[0025] Fig. 15 is the SEM image of bumpy calcined ceria particles having mean particle size of 40-60 nm after the wet milling of ceria particles as shown in Fig. 14.

[0026] Fig. 16 is the SEM image of ceria particles after granulation with water and sintering the mixture of the starting ceria nanoparticles as shown in Fig. 9 and cerium (III) carbonate as the precursor.

[0027] Fig. 17 is the SEM image of bumpy calcined ceria particles having mean particle size of 80-85 nm after the wet milling of ceria particles as shown in Fig. 16.

[0028] Fig. 18 is the SEM image of non-inventive ceria particles.SUMMARY OF THE INVENTION

[0029] The present invention satisfies the need by providing a new type of colloidally stable, calcined ceria particles with a tailorable bumpy surface having a surface texture including but not limited to bumps, protrusions, branches or tree bark, and combinations thereof, and thus referred as colloidally stable bumpy calcined ceria particles or bumpy calcined ceria particles in present invention .

[0030] The new bumpy calcined ceria particles can be used as abrasive particles in CMP polishing compositions to provide decent removal rates with a mean particle size below the threshold which commonly believed to cause scratches.

[0031] In one aspect (Aspect 1), there is provided colloidally stable bumpy calcined ceria particles; wherein the colloidally stable bumpy calcined ceria particle having a bumpy surface covering a core, wherein the bumpy surface contains a base surface and a plurality of protrusions protruding above the base surface; the plurality of protrusions are selected from the group consisting of bumps, protrusions, branches or tree bark, and combinations thereof; and the base surface also covers the core but does not have protrusions.Attorney Docket No.: P25-207-SEC-W002

[0032] The plurality of protrusions is integral part of the colloidally stable calcined ceria particle, since the plurality of protrusions along with other parts of the colloidally stable bumpy calcined ceria particle as a whole are formed and made in the same one process.

[0033] The mean particle size of the bumpy calcined ceria particle is between 20 and 200nm, 30-150 nm, or 50-120 nm, wherein the mean particle size is measured by disc centrifuge technique.

[0034] The contact angles of the plurality of protrusions to the base surface is preferably > 90°.

[0035] The height of the plurality of protrusions relative to mean particle size of the bumpy calcined ceria particles is between 1 and 75%, 1 and 50%, preferably 5 -25%.

[0036] The contact area between each of the plurality of protrusions and the base surface is equal to or larger than the largest cross section area of the plurality of protrusions, wherein the largest cross section area is parallel to the contact area. The contact areas of all the plurality of protrusions are 10 - 80%, 20 - 60%, or 30 - 40 % of the base area.

[0037] The plurality of protrusions and rest part of the colloidally stable calcined ceria particle can contain the same materials with same physicochemical properties such as density, hardness, crystallinity, level of doping, Celll / lv-ratio or Ce-OH content.

[0038] The colloidally stable calcined ceria particle can be a hybrid particle containing at least two different domains with different physicochemical properties.

[0039] The colloidally stable calcined ceria particle can be a hybrid particle containing cerium dioxide and other oxide selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

[0040] The colloidally stable calcined ceria particle can be a hybrid particle; wherein the plurality of protrusions comprise oxide selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof; and rest of the colloidally stable calcined ceria particle is cerium dioxide.

[0041] The colloidally stable calcined ceria particles can be doped with rare earth elements including but are not limited to lanthanum (La), gadolinium (Gd); Zirconium (Zr); or combinations thereof.

[0042] The bumpy surface of the colloidally stable calcined ceria particle can be surface modified with including but are not limited to with (1) mechanically implanted or adsorbed inorganic ions, (2) a modifier selected from the group consisting ofAttorney Docket No.: P25-207-SEC-W002oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof.

[0043] The surface modified colloidally stable bumpy calcined ceria particles can have a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

[0044] In another aspect (Aspect 2), there is provided a process of making colloidally stable bumpy calcined ceria particles, comprising, consisting essentially of, or consisting of:step 1 comprises providing starting nanoparticles comprising ceria nanoparticles, step 2 comprises sintering the starting nanoparticles to obtain sintered nanoparticles; andstep 3 comprises disaggregating or deagglomerating the sintered nanoparticles to obtain colloidally stable bumpy calcined ceria particles;whereinthe starting nanoparticles are in fluffy nano powder or granulated powder form; the starting nanoparticles have a low-medium packing density for the formation of a colloidally stable bumpy calcined ceria particle; andthe sintering is at a temperature < 1200°C, or between 600 to 1100°C, 700 to 1000°C, 800 to 1000°, and 800 to 900°C for 5 minutes to 24 hours, 1 hour to 16 hours, or 2 to 6 hours.

[0045] The starting nanoparticles have a mean primary particle size of <50% or preferably <30% of the mean particle size of the colloidally stable bumpy calcined ceria particles.

[0046] The low-medium packing density (bulk density) of the starting nanoparticles can be of 10 - 500 g / l, preferably 50 - 200 g / l.

[0047] The packing density can be adjusted by suitable techniques: dry or wet granulation techniques like for example a granulating, such as suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation spray drying; compacting, or combinations thereof, so that the desired structure forms. The packing (or bulk) density after the granulating or compacting step is 200 -2500 g / l, preferably 500 - 1000 g / l.

[0048] The starting nanoparticles are made by any known thermal process / thermal treatment (used interchangeably), or wet chemical process.

[0049] The starting nanoparticles can be homogenous ceria nanoparticles have one size or different sizes and made with same thermal process.

[0050] The starting nanoparticles can be heterogenous ceria nanoparticles have one size or different sizes and are made with different thermal processes.Attorney Docket No.: P25-207-SEC-W002

[0051] The starting nanoparticles can be made by a thermal process comprising thermal treatment of a precursor selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, cerium(lll) triformate, and combinations thereof, at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours.

[0052] The starting nanoparticles can be made by a thermal process comprising thermal treatment of a mixture of (1)a precursor selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, cerium formate or cerium(lll) triformate, and combinations thereof; and (2)oxide nanoparticles selected from the group consisting of cerium dioxide, silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof; at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours.

[0053] The starting nanoparticles may further comprise other oxide particles selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

[0054] The starting nanoparticles may comprise doped and undoped ceria nanoparticles have the same size or different sizes.

[0055] The starting nanoparticles may comprise doped and undoped ceria nanoparticles have the same size or different sizes; and the doped ceria nanoparticles doped with lanthanum (La), gadolinium (Gd), Zirconium (Zr), or combinations thereof.

[0056] The starting nanoparticles may further comprise nanoparticles having surface-modified by organic polymers selected from the group consisting of cellulose and derivatives, homo- and copolymers of acrylic acids, polyacrylic amines, polyamidoamines, polyamines, and combinations thereof.

[0057] The process may further comprises at least one step after step 1 and before step 2 to treat the starting nanoparticles, to achieve homogenization of particle size and distribution and is selected from the group consisting of (a) a granulating such as, dry or wet granulation techniques, for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation, compacting, or combinations thereof; to achieve a reproducible, targeted packing density and to avoid nanoparticle dust of the starting nanoparticles; (b) wet or dry milling to achieve homogenization of particle size and distribution; (c)a drying step to removeAttorney Docket No.: P25-207-SEC-W002physisorbed or crystal water from the starting nanoparticles; and combinations of steps (a) to (c); wherein step (a) is done using (i)water, (ii)an additive selected from the group consisting of a surfactants, an organic binder of polyvinylalcohol or hydroxypropylcellulose, or the combinations of (i) and (ii); wherein the additive is decomposed in step 2 and free from contaminants of metal or halogen impurities.

[0058] Step 2 is done in an atmosphere selected from the group consisting of vacuum, air, synthetic air, inert gases, reactive gases, the preferred atmosphere is air.

[0059] Step 2 can be done with adapted heating and cooling rates ranging from 300 K / min to 1 K / min, 100 K / min to 5 K / min, or 50 K / min to 10 K / min to foster the formation of target surface morphology for the bumpy calcined ceria particles.

[0060] Step 2 is done in a device made with high purity ceramic material or silica to avoid contamination with metal ions.

[0061] Step 3 is a process selected from the group consisting of ball or jet milling, ultrasound treatment, jet homogenization, and combinations thereof.

[0062] Step 3 can be a wet process by ball milling dispersion of the sintered nanoparticles from step 2 in a solvent comprising water, wherein the ball mill parts are preferably made of zirconia.

[0063] The process may further comprise a surface modification step before, during or after step 3 using a modifier selected from the group consisting of oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof; wherein the surface modified colloidally stable bumpy calcined ceria particles having a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

[0064] The process may comprise a step after step 3 selected from the group consisting of (a)centrifugation, vortex, filtration, adsorption, or combinations therefore to remove too large or too small particles; (b) ion exchange to remove unwanted ions, and combinations thereof.

[0065] In yet another aspect (Aspect 3), there is provided a Chemical Mechanical Planarization (CMP) polishing composition comprising, or consisting essentially of: bumpy calcined ceria particles in Aspect 1 or the bumpy calcined ceria particles made in Aspect 2 as abrasive particles.

[0066] In yet another aspect (Aspect 4), there is provided a Chemical Mechanical Planarization (CMP) polishing method for chemical mechanical planarization of a semiconductor substrate comprising at least one surface containing silicon oxide comprising, consisting essentially of, or consisting of the steps of:providing the Chemical Mechanical Planarization (CMP) polishing compositions in Aspect 3,Attorney Docket No.: P25-207-SEC-W002providing a polishing pad;contacting the at least one surface containing silicon oxide with the polishing pad and the chemical mechanical planarization polishing composition;polishing the at least one surface containing silicon oxide.

[0067] In yet another aspect (Aspect 5), there is provided a system of Chemical Mechanical Planarization (CMP) polishing a semiconductor substrate having at least one surface comprising silicon oxide, the system comprising:a. a semiconductor substrate;b. the Chemical Mechanical Planarization (CMP) polishing composition in Aspect 3;c. a polishing pad,wherein the at least one surface comprising silicon oxide film is in contact with the polishing pad and the Chemical Mechanical Planarization (CMP) polishing composition.

[0068] Other aspects, features and embodiments of the invention will be more fully apparent from the ensuing disclosure and appended claims. The embodiments of the invention can be used alone or in combinations with each other.DETAILED DESCRIPTION OF THE INVENTION

[0069] In the field of CMP, smooth polishing of different layers is required to produce the semiconductor stack. Thus, there is a significant need of abrasive particles used in CMP polishing compositions that can afford high removal rates with a low defect rate.

[0070] The currently known processes for producing calcined ceria or calcined ceria particles have limitations in terms of shape and surface morphologies due to the high temperature calcination and milling process. As a result, calcined ceria particles typically have a flat and relatively smooth surface due to the high-temperature treatment and the breaking or milling of larger particles into smaller fragments. However, these smaller fragments often have sharp edges, which can result in the generation of scratches during use. In this aspect, known calcined ceria resembles broken glass.

[0071] For example, calcined ceria has been produced through a high-temperature process using ceria precursors such as cerium carbonate or precipitated cerium hydroxide / oxide. The ceria precursors are heated to temperatures typically ranging from 800 to 1200°C until the ceria forms large crystals, then followed by high-energy milling in zirconia ball mills. This milling process breaks the ceria crystals into smaller fragments with a mean particle diameter around 100 nm.Attorney Docket No.: P25-207-SEC-W002

[0072] The surface of the ceria particles has been then modified with a colloidal stabilizer, such as polyacrylic acid (PAA) during the milling step. The resulting particles have flat, smooth surfaces comparable to broken glass, as well as irregular shapes and sizes with sharp and pointy edges.

[0073] Colloidal ceria, on the other hand, has been produced through a wet chemistry precipitation process using cerium salts such as cerium (III) nitrate. The dissolved salt is precipitated by adding a base such as ammonia, and the resulting particles may undergo further treatment, such as autoclaving at elevated temperatures and pressure. Examples of commercial colloidal ceria abrasive include but are not limited to Zenus® made by Solvay which are large, often monocrystalline ceria crystals with an even, smooth surface.

[0074] Apart from these two common types of ceria, various attempts to produce ceria with different particle structures have been described in the literature. Some of these approaches involve attaching ceria nanoparticles to a core made of the same or a different material.

[0075] For example, JGC Catalysts and Chemicals, Ltd (JGC&C) discloses ceria coated silica hybrid particles consisting of a silica core with a layer of multiple ceria nanoparticles "glued" to the surfaces using a TEOS silica binder (JP 2013-119131). The multiple ceria nanoparticles form a dense, closed layer on the surfaces of silica without decided protrusions.

[0076] Rhodia (WO 2021 / 105169) also describes a ceria abrasive with a core of ceria and multiple attached ceria nanoparticles that may be doped with other elements on their surface. Again, the multiple ceria nanoparticles form a dense, closed layer on the surfaces of the core ceria without decided protrusions or branching.

[0077] Degussa / Evonik described a ceria CMP product (DE 10251 029, EP0803471) which is produced by flame pyrolysis. This well-known process typically yields fine, highly branched aggregates of small primary nanoparticles. These products are typically challenging to disperse, lead to structural viscosity and did not prove to be commercially viable for the CMP polishing process. This type of ceria could however serve as a raw or starting material for the inventive bumpy calcined ceria particles.

[0078] IBU-tec advanced materials describes a ceria product “IBUpart® CeO2“, which is produced by spraying a solution of ceria precursors into the hot exhaust gas stream of a specially designed natural gas burner. The product consists of a collection of hollow spheres or nanoparticle agglomerates with a very low mechanical strength. When this product is subjected to mechanical stress, it disintegrates intoAttorney Docket No.: P25-207-SEC-W002very small primary particles which makes it not useful for CMP applications. It can serve however as raw or starting material for the inventive bumpy calcined ceria particles.

[0079] Some of the existing ceria particles also have the drawback that some of the attached ceria nanoparticles may detach from the surface and cause undesired side effects, as these small nanoparticles can strongly adhere to the wafer surface after the CMP polishing process.

[0080] These limitations of the traditional calcination and milling process pose challenges for product optimizations. Simply aiming for smaller particle sizes within the current process does not effectively address the issue, as reducing the size without changing the flat surface morphology would only lead to a decrease in removal rate.

[0081] Fig. 1 is a comparison of invented bumpy calcined ceria particles with ceria particles known in literature.

[0082] The surface morphology of the bumpy calcined ceria particles disclosed in the present invention has not been described before. It can be used for CMP with a significantly increased aggressiveness of the surface.

[0083] Disclosed in the present invention is a new type of bumpy calcined ceria particles. The bumpy calcined ceria particles are colloidally stable bumpy calcined ceria particles.

[0084] The term “calcined” is used here in relation to a ceria particle which has been treated in a dry state at temperatures which exceed the temperatures where water is in a liquid state.

[0085] The inventive bumpy calcined ceria particles differ from any ceria particles made from the state-of-the-art methods in that they exhibit bumpy surfaces covering cores of the colloidally stable bumpy calcined ceria particles. Each bumpy surface comprises a base surface that covers the core or the bulk of the particle and discrete plurality of protrusions selected from the group consisting of bumps, protrusions, branches or tree bark, and combinations thereof. The plurality of protrusions protrudes or rises above the base surface. Unlike surface-attached nanoparticles where the nanoparticles attached on the surfaces and core particles are made in separated different processes, the plurality of protrusions are integral parts of the bumpy calcined ceria particles since the plurality of protrusions along with other parts of the colloidally stable bumpy calcined ceria particle as a whole are made in the same process.

[0086] The bumpy calcined ceria particles can comprise a branched structure with no distinct center or core of the particles.Attorney Docket No.: P25-207-SEC-W002

[0087] The bumpy calcined ceria particles can be used as the abrasive particles in a polishing composition to provide decent removal rates with a mean particle size (measured by disc centrifuge (DCS)) below the threshold to cause scratches, for example <120 nm.

[0088] Typically, nanoparticles consist of particles having a plurality of sizes, ranging from small to large size. The mean particle size is characterized by methods such as the differential disc centrifuge (DCS) in which the abrasive particles are separated in a density gradient and subsequently detected. From this, a mean particle size is calculated.

[0089] Most of the protrusions have a contact angle to the base surface of the bumpy calcined ceria particles > 90°, such that the contact area between the protrusion and the base surface is equal or larger than the largest cross section of the protrusion. The cross section of the protrusion is parallel to the contact area.

[0090] Please note that a nanoparticle that is surface-attached with other nanoparticles in art has a contact area smaller than the largest cross section of the surface-attached other nanoparticles.

[0091] The height of the protrusions relative to the mean particle size of the bumpy calcined ceria particles is between 1 and 75%, 1 and 50%, preferably 5 - 25%.

[0092] As a result, a much greater force is required to break or detach protrusions from the inventive bumpy calcined ceria particles compared to detaching surface-attached nanoparticles in the art.

[0093] This unique characteristics of the surface textures enhance the stability and durability of the ceria particles during the use in CMP polishing compositions.

[0094] Without being bound by any theory, Fig. 2 is a visualization of the difference between a nanoparticle which was “glued” to an abrasive core wherein “glue” refers to the case that the nanoparticle and the abrasive core are not made in the same process; and the innovative bumpy calcined ceria particles having a bumpy surface structure, in which the protrusions is an inseparable or integrated part of the particles.

[0095] The protrusions can have the same or different chemical composition or physical parameters or physicochemical properties, such as density, porosity, and hardness than the core or bulk of the bumpy calcined ceria particles.

[0096] The new type of colloidally stable bumpy calcined ceria particles can be hybrid abrasive particles comprising cerium oxide, in which separate domains of different physical and chemical properties are sintered together to provide a bumpy surface having a surface texture including but not limited to bumps, protrusions, branches or tree bark, and combinations thereof.Attorney Docket No.: P25-207-SEC-W002

[0097] With a tailorable bumpy surface, that is, a rough surface with protrusions, the colloidally stable bumpy calcined ceria particles can enhance the mechanical aggressiveness as abrasive particles, enabling even particles smaller than conventionally produced calcined / milled ceria to exhibit comparable or improved CMP polishing performance, such as, removal rates.

[0098] By targeting a smaller mean particle size alongside a more aggressive surface morphology, the new bumpy calcined ceria particles offer excellent CMP polishing performance and a potentially low defect rate.

[0099] The present invention also discloses a novel process to produce the bumpy calcined ceria particles with a new bumpy surface morphology.

[0100] In the traditional process for calcined ceria, a ceria precursor is heated to high temperatures until the ceria forms large crystals, followed by milling of the resulting large crystals into smaller fragments.

[0101] The process to produce new bumpy calcined ceria particles is through a calcination process that differs significantly from the state-of-the-art methods.

[0102] The new calcination process involves several distinct steps.

[0103] Firstly, the starting nanoparticles or nano powder with a mean particle size less than or equal to 50% or preferably <30% of the target mean particle size range for the new bumpy calcined ceria particles are synthesized. The starting nanoparticles preferably have a controlled, low-medium packing density, such as 10 - 500 g / l, preferably 50 - 200 g / l.

[0104] Next, the starting nanoparticles are subjected to a temperature treatment (interchangeable with thermal process, or sintering process) equal to or above 600°C but less than 1100°C for a sufficient time to form the sintered nanoparticles or the sintered nano powder. This temperature threshold of above 600°C initiates the sintering of ceria, causing starting nanoparticles to come together and form larger sintered nanoparticles and desired surface structures.

[0105] During the temperature treatment, the loosely packed ceria nanoparticles begin to sinter and form larger structures. Primary particles form dimers, trimers, and irregular branched structures. As the temperature and process time increase, the branched structures start to collapse and form bigger particles, while the original branched structure gives rise to the protrusions that extend from the particles. With further temperature treatment, the protrusions become more leveled, and the particle surface becomes smoother. Thus, the temperature and time of the process need to be controlled to influence particle growth and achieve the desired bumpy surface morphology.Attorney Docket No.: P25-207-SEC-W002

[0106] It is crucial in the process that the starting / raw materials, nanoparticles made as starting materials, are not too densely packed before undergoing temperature treatment. If they are too densely packed, the irregular branched structures necessary for the formation of protrusions cannot arise, and subsequently particles with protrusions will not be produced. Instead, a solid piece of porous ceria would form which would have to be broken into pieces like a traditional calcined ceria.

[0107] Granulation such as dry or wet granulation techniques, for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation; and compacting steps to achieve a reproducible and manageable packing density before the temperature treatment may be necessary to ensure a reproducible product quality and can be used to tailor the size of the resulting particles. The packing density after granulation and / or compacting steps is 200 -2500 g / l, preferably 500 - 1000 g / l.

[0108] During the temperature treatment, the formed bumpy calcined ceria particles may undergo agglomeration and / or aggregation. Therefore, a deagglomeration or disaggregation step is necessary to produce a stable water-borne ceria particle suspension. This is typically achieved using a ball mill. This step is however unlike the milling of a conventional calcined ceria, in which densely sintered crystals are glass-like broken into pieces.

[0109] The exemplary flowchart shown in Fig. 3 shows the process steps, and the ceria particles made by the process through different paths. The numbers used in the flowchart such as mean particle sizes, sintering temperatures et al are for exemplary purposes only.

[0110] As shown in Fig. 3, there are three processes to make the bumpy ceria particles.

[0111] Starting from the same fluffy starting material containing ceria nanoparticle or powder (starting nanoparticles in the flowchart), the ending ceria particles can have different structures depending on if there is a pretreatment, such as granulation, before the sintering step (such as 900 °C). The granulation changes the packing (or bulk) density of the ceria nanoparticles before sintering and thereby changes the calcination behavior and the shape of the final bumpy particles after disaggregation and deagglomeration.

[0112] In the first process, the ceria nanoparticles are first stirred in water and then dried, a granulation compaction takes place which leads to a packing (or bulk) density of about 200 -2500 g / l, preferably 500 - 1000 g / l that is higher than the packing density of the starting fluffy nanoparticles. When the treated ceriaAttorney Docket No.: P25-207-SEC-W002nanoparticles are sintered, bumpy calcined ceria particles are formed after disaggregation.

[0113] In the second process, the granulation is done with water and organic additives, such as surfactants and / or organic polymers as organic binders, the packing density of the treated ceria nanoparticles is crucial in addition of sintering temperature and time in the formation of final ceria particle structures.

[0114] When the treated nanoparticles having a packing density of at about 200 -2500 g / l, preferably 500 - 1000 g / l, bumpy calcined ceria particles are formed after disaggregation. However, when the treated ceria particles have higher packing density, that is, the treated nanoparticles are packed too closely then the calcination process would yield the formation of ceria particles in dense, smooth crystals form (known in art) without the bumps in the middle path in the flowchart.

[0115] In the third process, without pretreatment, the ceria nanoparticles sinter to form bumpy ceria particles after the disaggregation step.

[0116] The sintering step for all different paths is at the same temperature range.

[0117] The above-described process also offers an opportunity to design new hybrid bumpy ceria particles.

[0118] Homogenous ceria nanoparticles having one size and with the same thermal history are sintered together.

[0119] Different raw materials can be combined to create hybrid bumpy ceria particles. Examples of different raw materials include but are not limited to the following.

[0120] Heterogenous ceria nanoparticles, for example, ceria nanoparticles have 25-30 nm size made with different thermal treatment / process / histories, such as one raw material are produced at 1000°C and one other raw material are produced at 700°, can be sintered together. The sintering can be done such as at 800°C, so that the resulting ceria particle contains domains which have experienced different temperatures and thereby have different chemical / physical properties.

[0121] As the starting material, for instance, cerium carbonate is intimately mixed with a nanoparticle raw material which contains 30% of lanthanum oxide. Sintering the mixture for example at 900°C yields cerium oxide particles with lanthanum-rich protrusions, but there is no lanthanum in the rest of the particles.

[0122] Smaller ceria particles can decorate bigger ceria particles, for instance, cerium oxide nanoparticles of 25 nm size are intimately mixed with cerium oxide nanoparticles of 80 nm size. The mixture is sintered for example at 900°C which leads to big cerium oxide particles with sintered ceria protrusions.Attorney Docket No.: P25-207-SEC-W002

[0123] The starting ceria nanoparticles material can be one type of ceria nanoparticle or more than one type of ceria nanoparticle, such as a mixture of two or more nanoparticles with different chemical and physical properties, resulting in hybrid sintered particles.

[0124] The starting ceria nanoparticles can also be mixed with other precursors including but not limited to cerium oxide, cerium hydroxide or carbonate. In the following thermal process, nanoparticles can be decomposed and influence the growth of the resulting particles, so that the inventive bumpy ceria particles with bumps, protrusions and / or roughness form.

[0125] By this, the process costs for the synthesis of ceria can be lowered without affecting the result in a negative way. The starting fluffy ceria nanoparticles drive the evolution of the mix of raw materials in a desired direction, they act like a structuredirecting component, like a template.

[0126] It is also possible to include oxides or precursors of oxides of other elements, such as aluminum oxide, silicon dioxide, or zirconium oxide in the process so that ceria hybrids with domains of different chemical compositions having different physical and / or chemical properties are formed.

[0127] In one special case, cerium oxide nanoparticles of 25 nm size are mixed with silicon dioxide nanoparticles of 45 nm size, and the mixture is sintered for example at 900 °C to yield a bumpy silica-ceria hybrid particle.

[0128] As another example, silicon oxide (fumed silica-electronic grade) is mixed with cerium oxalate, and the mixture is sintered for example at 800°C to yield a bumpy cerium oxide-silicon oxide hybrid with a silica core and cerium oxide shell. Here, the fumed silica acts as a structure-template for the forming of the silica-ceria hybrid.

[0129] The bumpy calcined ceria particles comprise cerium. The bumpy calcined ceria particles can be doped with doping elements. Doping elements can comprise rare earth elements, such as Lanthanum (La) or Gadolinium (Gd), or other elements such as Zirconium (Zr).

[0130] The bumpy calcined ceria particles can comprise a mixture of two or more cerium oxides with different thermal history or preparation method, crystal size, crystal structure or doping. The resulting particles can comprise domains having 2 or more cerium oxides with different physicochemical properties.

[0131] Those are new cost-effective ways to produce hybrid- or doped particles.

[0132] Surface modifications can also be done for the inventive ceria bumping particles with a colloidal stabilizer.Attorney Docket No.: P25-207-SEC-W002

[0133] The colloidal stabilizer can be but is not limited to a selection from the group consisting of, such as, organic or inorganic, monomer, oligomer, or polymer and combinations thereof. Organic monomers, oligomers or polymers can be homo- or copolymers (statistical or block). The organic monomers, oligomers or polymers can comprise charged moieties and / or uncharged moieties at a given pH. They can be net cationic, anionic or non-ionic at any given pH. They can comprise a mixture of anionic, non-ionic and cationic moieties at a given pH.

[0134] The organic monomers, oligomers or polymers which can be bonded to the surface by any type of bond like covalent, ionic, chelating, van der Waals, dipoledipole interactions.

[0135] Preferably, the colloidal stabilizer has carboxy groups for chelating function.

[0136] The inventive ceria bumping particles can also comprise a surface modification with mechanically implanted or adsorbed inorganic ions, especially zirconium species like ions or oxide clusters. This is typically the outcome of a deagglomeration / disaggregation in a ball mill with zirconium oxide milling beads where miniscule parts of the milling beads are transferred to the particles.

[0137] The inventive ceria bumping particles can be used as abrasive particles for CMP polishing. The particles are in a stable suspension comprising water as solvent or / and carrier. Solid content is between 20-50wt. %, preferably 35-45 wt.%.

[0138] The mean particle size of the inventive colloidally stable bumpy ceria particles is determined by the requirements of the CMP polishing process. Typically, the mean particle size as determined by a disc centrifuge is between 20 and 200 nm, preferably 30 and 150 nm and more preferably between 50 and 120 nm.

[0139] Colloidally stable means that a waterborne suspension does not substantially change, for example < 10%, preferably < 5% and most preferably < 2% of its mean particle size (MPS) and particle size distribution characteristics over a period of 6 months storage. Additionally, after formulation of a CMP polishing slurry with other CMP additives with an adjusted pH, if there were a slight change of the MPS and the particle size distribution, the change would not affect the desired CMP polishing performance.

[0140] The inventive bumpy calcined ceria particles are also mechanically stable under the pressure and forces of the CMP polishing process, such that the abrasive particle does not disintegrate or form a substantial amount of a smaller particle fraction during the CMP polishing process.

[0141] The following sketches shall help to illustrate the invention but shall not limit the scope of the invention.Attorney Docket No.: P25-207-SEC-W002

[0142] The flow diagram as shown in Fig. 4 illustrates the general evolution of bumpy calcined ceria particles.

[0143] The flow diagram as shown in Fig. 5 illustrates one of the examples for the formation of bumpy calcined ceria particles, starting from the ceria particles having different sizes.

[0144] The flow diagram as shown in Fig. 6 illustrates one of the examples for the evolution of bumpy calcined ceria particles, that is, hybrid particles starting from a mixture of different oxides (oxide particles) and thus having domains of different physical and / or chemical properties.

[0145] The flow diagram as shown in Fig. 7 illustrates one of the examples for the formation of bumpy calcined ceria particles, comprising selectively doped and undoped domains.

[0146] The flow diagram as shown in Fig. 8 illustrates one of the examples for the formation of inventive hybrid particles, starting from a mixture of two or more cerium oxides made with different thermal histories, preparation methods, crystal sizes, crystal structures or dopings. The resulting bumpy calcined ceria particles can comprise 2 or more cerium oxides having different physico-chemical properties.

[0147] In one aspect (Aspect 1), there is provided colloidally stable bumpy calcined ceria particles; wherein the colloidally stable bumpy calcined ceria particle having a bumpy surface covering a core, wherein the bumpy surface contains a base surface and a plurality of protrusions protruding above the base surface; the plurality of protrusions are selected from the group consisting of bumps, protrusions, branches or tree bark, and combinations thereof; and the base surface also covers the core but does not have protrusions.

[0148] The plurality of protrusions is integral part of the colloidally stable calcined ceria particles, since the plurality of protrusions along with other parts of the colloidally stable bumpy calcined ceria particle as a whole are made in the same process.

[0149] The mean particle size of the bumpy calcined ceria particle is between 20 and 200nm, 30-150 nm, or 50-120 nm, wherein the mean particle size is measured by differential disc centrifuge technique.

[0150] The contact angles of the plurality of protrusions to the base surface is preferably > 90°.

[0151] The height of the plurality of protrusions relative to mean particle size of the bumpy calcined ceria particles is between 1 and 75%, 1 and 50%, preferably 5 -25%.Attorney Docket No.: P25-207-SEC-W002

[0152] The contact area between each of the plurality of protrusions and the base surface is equal to or larger than the largest cross section area of the plurality of protrusions, wherein the largest cross section area is parallel to the contact area.

[0153] The total contact areas of the plurality of protrusions are 10 - 80%, 20-60%, or 30-40 % of the base surface area.

[0154] The plurality of protrusions and rest part of the colloidally stable calcined ceria particles can have the same materials with same physicochemical properties.

[0155] The colloidally stable calcined ceria particle can be a hybrid particle containing at least two different domains with different physicochemical properties.

[0156] The colloidally stable calcined ceria particle can be a hybrid particle containing cerium dioxide and other oxide selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

[0157] The colloidally stable calcined ceria particle can be a hybrid particle; wherein the plurality of protrusions comprise oxide selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof; and rest of the colloidally stable calcined ceria particle is cerium dioxide.

[0158] The colloidally stable calcined ceria particles can be doped with rare earth elements including but are not limited to lanthanum (La), gadolinium (Gd); Zirconium (Zr); or combinations thereof.

[0159] The bumpy surface of the colloidally stable calcined ceria particle can be surface modified with including but are not limited to with (1) mechanically implanted or adsorbed inorganic ions, (2) a modifier selected from the group consisting of oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof.

[0160] The surface modified colloidally stable bumpy calcined ceria particles can have a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

[0161] In another aspect (Aspect 2), there is provided a process of making colloidally stable bumpy calcined ceria particles, comprising, consisting essentially of, or consisting of:step 1 comprises providing starting nanoparticles comprising ceria nanoparticles, step 2 comprises sintering the starting nanoparticles to obtain sintered nanoparticles; andstep 3 comprises disaggregating or deagglomerating the sintered nanoparticles to obtain colloidally stable bumpy calcined ceria particles;whereinthe starting nanoparticles are in fluffy nano powder or granulated powder form;Attorney Docket No.: P25-207-SEC-W002the starting nanoparticles have a low-medium packing density for the formation of a colloidally stable bumpy calcined ceria particle; andthe sintering is at a temperature < 1200°C, or between 600 to 1100°C, 700 to 1000°C, 800 to 1000°, and 800 to 900°C for 5 minutes to 24 hours, 1 hour to 16 hours, or 2 to 6 hours.

[0162] The starting nanoparticles have a mean primary particle size of <50% or preferably <30% of the mean particle size of the colloidally stable bumpy calcined ceria particles.

[0163] The low-medium packing density (bulk density) of the starting nanoparticles can be of 10 - 500 g / l, preferably 50 - 200 g / l. The packing density can be adjusted by suitable dry or wet granulation techniques for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation; compacting; or combinations thereof; so that the desired structure forms.

[0164] The starting nanoparticles are made by any known thermal process / thermal treatment (used interchangeably), or wet chemical process.

[0165] The starting nanoparticles can be homogenous ceria nanoparticles have one size or different sizes and made with same thermal process.

[0166] The starting nanoparticles can be heterogenous ceria nanoparticles have one size or different sizes and can be made with different thermal processes.

[0167] The starting nanoparticles can be made by a thermal process comprising thermal treatment of a precursor selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, or cerium(lll) triformate, and combinations thereof at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours.

[0168] The starting nanoparticles can be made by a thermal process comprising thermal treatment of a mixture of (1)a precursor selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, or cerium(lll) triformate, and combinations thereof; and (2)oxide nanoparticles selected from the group consisting of cerium dioxide, silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof; at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours.Attorney Docket No.: P25-207-SEC-W002

[0169] The starting nanoparticles may further comprise other oxide particles selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

[0170] The starting nanoparticles may comprise doped and undoped ceria nanoparticles have the same size or different sizes.

[0171] The starting nanoparticles may comprise doped and undoped ceria nanoparticles have the same size or different sizes; and the doped ceria nanoparticles are doped with lanthanum (La), gadolinium (Gd), Zirconium (Zr), or combinations thereof.

[0172] The starting nanoparticles may further comprise nanoparticles having surface-modified by organic polymers selected from the group consisting of cellulose and derivatives, homo- and copolymers of acrylic acids, polyacrylic amines, polyamidoamines, polyamines, and combinations thereof

[0173] The process may further comprises at least one step after step 1 and before step 2 to treat the starting nanoparticles, to achieve homogenization of particle size and distribution and is selected from the group consisting of (a) dry or wet granulation, for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation; compacting; or combinations thereof; to achieve a reproducible, targeted packing density and to avoid nanoparticle dust of the starting nanoparticles; (b) wet or dry milling to achieve homogenization of particle size and distribution; (c)a drying step to remove physisorbed or crystal water from the starting nanoparticles; and combinations of steps (a) to (c); wherein step (a) is done using (i)water, (ii)an additive selected from the group consisting of a surfactants, an organic binder of polyvinylalcohol or hydroxypropylcellulose, or the combinations of (i) and (ii); wherein the additive is decomposed in step 2 and free from contaminants of metal or halogen impurities.

[0174] Step 2 is done in an atmosphere selected from the group consisting of vacuum, air, synthetic air, inert gases, reactive gases, the preferred atmosphere is air.

[0175] Step 2 can be done with adapted heating and cooling rates ranging from 300 K / min to 1 K / min, 100 K / min to 5 K / min, or 50 K / min to 10 K / min to foster the formation of target surface morphology for the bumpy calcined ceria particles.

[0176] Step 2 is done in a device made with high purity ceramic material or silica to avoid contamination with metal ions.

[0177] Step 3 is a process selected from the group consisting of ball milling, ultrasound treatment, jet homogenization, and combinations thereof.Attorney Docket No.: P25-207-SEC-W002

[0178] Step 3 can be a wet process by ball milling dispersion of the sintered nanoparticles from step 2 in a solvent comprising water, wherein the ball mill parts are made of zirconia.

[0179] The process may further comprise a surface modification step before or after step 3 using a modifier selected from the group consisting of oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof; wherein the surface modified colloidally stable bumpy calcined ceria particles having a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

[0180] The process may further comprise a step after step 3 selected from the group consisting of (a)centrifugation, vortex, filtration, adsorption, or combinations thereof to remove too large or too small particles; (b) ion exchange to remove unwanted ions, and c) combinations thereof.

[0181] In yet another aspect (Aspect 3), there is provided a CMP polishing composition comprising, or consisting essentially of:bumpy calcined ceria particles in Aspect 1 as abrasive particles or the bumpy calcined ceria particles made in Aspect 2.

[0182] In yet another aspect (Aspect 4), there is provided a Chemical Mechanical Planarization (CMP) polishing method for Chemical Mechanical Planarization of a semiconductor substrate comprising at least one surface containing silicon oxide comprising, consisting essentially of, or consisting of the steps of:providing the Chemical Mechanical Planarization (CMP) polishing compositions in Aspect 3,providing a polishing pad;contacting the at least one surface containing silicon oxide with the polishing pad and the Chemical Mechanical Planarization (CMP) polishing composition;polishing the at least one surface containing silicon oxide.

[0183] In yet another aspect (Aspect 5), there is provided a system of Chemical Mechanical Planarization (CMP) polishing a semiconductor substrate having at least one surface comprising silicon oxide, the system comprising:a. a semiconductor substrate;b. the Chemical Mechanical Planarization(CMP) polishing composition in Aspect 3;c. a polishing pad,wherein the at least one surface comprising silicon oxide film is in contact with the polishing pad and the chemical mechanical planarization polishing composition.Attorney Docket No.: P25-207-SEC-W002

[0184] Process of making the inventive ceria bumping particles are described below.Process Step 1 - Synthesis of suitable nanoparticles as raw materials

[0185] Suitable nanoparticles as the starting materials comprise ceria nanoparticles. Suitable nanoparticles can have ceria nanoparticles in combination with nanoparticles of other oxides and / or mixed oxides. Suitable nanoparticles can also be doped or undoped.

[0186] Suitable nanoparticles have a mean particle size which is equal or smaller than the targeted mean particle size of the inventive bumpy calcined ceria particles. Preferably, suitable nanoparticles have a mean primary particle size of <50% or preferably <30% of the mean particle size of the to-be synthesized inventive target bumpy calcined ceria particles.

[0187] Suitable nanoparticles may also comprise mixtures of nanoparticles of different sizes, different shapes, different thermal history, different compositions or in general, nanoparticles with different physical and / or chemical properties.

[0188] Preferably, at least one component of a mixture of starting materials comprises nanoparticles which have a mean primary particle size <50% the mean targeted size of bumpy calcined ceria particles.

[0189] It is preferred that the starting material comprises cerium oxide nanoparticles with a mean particle size of <30% of the target bumpy calcined ceria particles size or the starting material comprises cerium oxide nanoparticles with a mean particle size of <30% of the target bumpy calcined ceria particles size alone or in a mixture with cerium carbonate or -oxycarbonate or -hydroxide as precursor for cerium oxide.

[0190] For example, if the mean target size of the inventive bumpy calcined ceria particles is 70 nm, the starting nanoparticle component added in the mixture with a mean primary particle size of 35 nm or less, preferably 21 nm or less.

[0191] A suitable starting material (including mixtures) must comprise at least one suitable type of nanoparticles as described above.

[0192] Suitable starting nanoparticles may further comprise components like oxide precursors, dopants, sintering agents (agents which might promote the coalescence of the nanoparticles into a bigger structure), or agents which are used to temporarily bind nanoparticles together for better handling (e.g. granulating agents like cellulose derivatives or other polymers which decompose during the thermal sintering treatment). Suitable dopants and sintering agents comprise oxides or oxide precursors (salts, alkoxides) of lanthanum, silicium, aluminium, zirconium, or other rare earth elements.Attorney Docket No.: P25-207-SEC-W002

[0193] The raw materials preferably are in the form of a powder or granulated powder. The packing density of the raw materials or the mixture of raw materials must be chosen in a way that the inventive structure forms.

[0194] The packing density can be adjusted by any available techniques, such as by suitable dry or wet granulation techniques, for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation; compacting; or combinations thereof, so that the desired structure forms.

[0195] Preparation of suitable nanoparticles as raw materials is described below.

[0196] In general, any method known to a person skilled in the art, which is capable to provide suitable nanoparticles as described above, such as thermal process and wet chemical process, could be used.

[0197] It is preferred to use thermal methods to produce suitable nanoparticles as starting materials. Any method which involves the treatment of a cerium oxide nanoparticle or a precursor thereof at elevated temperatures > 200°C, preferred > 300°C. An example can be the thermal treatment of cerium carbonate at 500°C which converts essentially all the carbonate to oxide without leading to particle aggregation or coalescence.

[0198] It is preferred to use thermal methods which involve a short temperature pulse to convert a ceria precursor to ceria and / or crystallize or densify a ceria nanoparticle.

[0199] Examples of preferred methods are spray drying, plasma torches, electrical arc discharge, flame pyrolysis (burning a precursor in a flame) or the introduction of a precursor in a stream of hot gas like the pulsation reactor technology of company IBU-tec.

[0200] More preferred are the flame pyrolysis and the pulsation reactor technology; to use cerium propionate dissolved in a suitable solvent like isopropanol / water as a precursor and convert it to cerium oxide by a pulsation reactor; and to use cerium carbonate or / and cerium oxycarbonate as precursor, dispersed in a suitable medium such as water or / and alcohols and to convert it to cerium oxide by a pulsation reactor.

[0201] The pulsation reactor technology is using a gas burner to produce a hot exhaust gas stream in which the precursor is introduced. The hot gases with the precursor travel through a tube of certain length which determines the contact time of the precursor with the hot gas. Typical process times range from 0.5 to 2 seconds before the formed nanoparticles are collected in filters. Temperatures can typically range between 300 and 1100°C.Attorney Docket No.: P25-207-SEC-W002

[0202] Another preferred method to produce suitable nanoparticles is to use a rotary kiln. The dry precursor like cerium carbonate and / or cerium oxycarbonate is continuously added to the rotating tube and travels through a heated zone of 500 -1000°C which results in a short thermal pulse in the range of 5 - 45 minutes before the intermitting product is collected.

[0203] Nanoparticles, produced by wet chemistry precipitation can also be used. The nanoparticles preferably are dried to a free-flowing powder or granules before the sintering process step which produces the inventive bumpy structure.

[0204] It is preferred to use a method which provides the starting material as a dry powder with a low-medium packing density, such as 10 - 500 g / l, preferably 50 - 200 g / i.

[0205] Examples of precursors for the preparation of suitable nanoparticles as raw materials include but are not limited to:a. precursors yield cerium oxide nanoparticles when heated include but are not limited to cerium salts, alkoxides, other organic compounds or hydroxides.Examples are cerium (III) carbonate, cerium oxide / hydroxide, cerium (lll)nitrate, cerium (IV) ammonium nitrate, cerium acetate, cerium (III) propionate, cerium oxalate, cerium (III) formate; preferred are cerium (III) carbonate and cerium (III) propionate;b. excipients known in the art which help to produce suitable nanoparticles.Examples for suitable excipients include but are not limited to organic binders like cellulose derivatives, sugars, silane, inorganic sinter additives which lower the sintering temperature of the main components, and colloidal stabilizers like homo- and copolymers of acrylic acids or polyethers.

[0206] The nanoparticles as raw materials can be surface-modified prior to the sintering step. Any surface modifiers which decompose in the sintering step is preferred. Potentially suitable surface modifiers comprise organic polymers like cellulose derivatives or homo- and copolymers of acrylic acids as well as polyacrylic amines, polyamidoamines or polyamines and copolymers thereof.Optional intermediate process step

[0207] Prior to process step 2, the nanoparticles, and optional precursors and / or excipients can be further processed separately or together with other nanoparticles and / or precursors and / or other excipients by an intermediate step of mixing, wet or dry milling, dry or wet granulation, for example suspension in water followed by spray drying, fluidized bed granulation or dry roller granulation; compacting; or combinations thereof; and any other physical treatment which supports and achievesAttorney Docket No.: P25-207-SEC-W002a reproducible, a homogenization of particle size and distribution, and / or targeted packing density of the raw materials, a proper handling, to avoid nanoparticle dust or a too low packing density and the formation of the inventive morphologies in the subsequent process step 2.

[0208] The preferred intermediate step is a granulating or compacting step to achieve a reproducible, targeted packing density of the raw materials and a proper handling, to avoid nanoparticle dust or a too low packing density. The packing density after the granulating or compacting step is 200 -2500 g / l, preferably 500 -1000 g / l.

[0209] This intermediate step can involve the use of water and / or other solvents for wet-granulating or compacting by drying suspended nanoparticles in water and / or other solvents.

[0210] The granulating or compacting step can be done with the help of water, additives like surfactants and / or organic binders such as polyvinylalcohol or hydroxypropylcellulose, and combinations of water and additives. All methods and substances or organic binders known in the art could be used, preferably substances which easily decompose in the following thermal treatment and are essentially free from contaminants like metal or halogen impurities.

[0211] Another preferred type of the optional intermediate step after the granulating or compacting step is ball milling, either dry or wet to break down and disperse any present agglomerates and aggregates to a mean particle size < 5 pm, preferably <2pm, and most preferably < 1.5 pm.

[0212] An optional drying step to remove physisorbed or crystal water can be beneficial prior to the inventive process step 2.Process Step 2 - Thermal treatment of the starting materials to generate the inventive surface morphology for the bumpy calcined ceria particles

[0213] The starting material for process step 2 comprises at least one type of suitable nanoparticle as described in step 1, and can comprise additional nanoparticles, oxides, oxide precursors and excipients.

[0214] The starting material for process step 2 is in the physical form of a powder or granules.

[0215] The starting material for process step 2 is subjected to a thermal treatment which is sufficient to initiate a deliberate, partly (incomplete) coagulation of the nanoparticles to or onto bigger structures when bigger oxides are used in a mix with nanoparticles.Attorney Docket No.: P25-207-SEC-W002

[0216] The thermal treatment of the oxide precursors and the nanoparticles or the mixture to sinter them.

[0217] At the beginning stage of the treatment, the temperature is high enough to decompose mostly any organic excipients, and surface modifiers. As the temperature rises, thermal treatment of the oxide precursors and the nanoparticles or the mixture starts.

[0218] The thermal treatment is performed long enough and at sufficiently high temperatures, so that the inventive bumpy calcined ceria particles with bumpy surface morphology forms. The thermal treatment can be performed at higher temperatures for a shorter time and at lower temperatures for a longer time.

[0219] The thermal treatment preferably is done at temperatures exceeding 600°, most preferably exceeding 700°C and even more preferably exceeding 800°C.

[0220] The thermal treatment is done preferably at temperatures lower than 1200°C and more preferably lower than 1100°Cto avoid the complete crystallization and / or sintering to big crystals which must be broken in a subsequent milling step.

[0221] During the thermal treatment, there are many crystals developed within a particle. Mean crystal size refers to the average size of individual crystal within a particle. The mean crystal size may grow during the treatment. It is preferred to tailor the thermal treatment in a way so that a mean crystal size results in favorable for the CMP polishing performance of the inventive abrasive particles, especially the removal rate, selectivity, and defect rate like scratches, dishing, and erosion.

[0222] Any suitable device for the thermal treatment can be used. It is preferred to choose devices which minimize the hazard of contamination, allow a controlled atmosphere, and operate economically in a continuous or batch operation mode. Examples of suitable devices are furnaces like rotary kilns, horde ovens or electrical furnaces.

[0223] To avoid contamination of the product with metal ions, it is preferred to use furnaces and carriers which are made of high purity ceramic material or silica.

[0224] The thermal treatment is done in a controlled atmosphere which can be either vacuum, air, synthetic air, inert gases, or reactive gases such as gases which can act as reducing or oxidizing agents, examples are carbon monoxide, hydrogen, dinitrogen monoxide or oxygen. The preferred atmosphere for the thermal treatment in process step 2 is air.

[0225] The thermal treatment may be done with adapted heating and cooling rates to foster the formation of the target surface morphology, to tailor the crystal structure of the crystals within the particle.Attorney Docket No.: P25-207-SEC-W002

[0226] The result of step 2, that is, after the thermal treatment, a product of sintered particles having the desired mean particle size and bumpy surface morphology. The particles typically are agglomerated and partly aggregated to larger structures which can be disaggregated and deagglomerated in a subsequent milling step.Process Step 3 - Disaggregation / deagglomeration and surface modification

[0227] The third step of the process for producing the inventive bumpy calcined ceria particles is to perform a disaggregation / deagglomeration process with the product from step 2.

[0228] This comprises typically a wet process where the product from step 2 is dispersed in a suitable solvent, preferably comprising water at a suitable pH.

[0229] The pH of the solvent is adjusted with any suitable inorganic or organic substance to a value which is appropriate to achieve sufficient colloidal stability in the process. A preferred acid is nitric acid, and a preferred base is ammonia.

[0230] The result of process step 3 is a colloidally stable suspension of the inventive bumpy calcined ceria particles which is suitable to be used as CMP abrasive. Colloidally stable means that a waterborne suspension does not substantially change, for example <10%, <5%, or < 2% of its MPS mean particle size and particle size distribution characteristics over a period of 6 months storage.Additionally, after formulation of a CMP polishing slurry with other CMP additives with an adjusted pH, if there were a slight change of the MPS and the particle size distribution, the change would not affect the desired CMP polishing performance.

[0231] The disaggregation / deagglomeration process can be done with any technology known in the art. Examples of suitable processes are ball milling, ultrasound treatment or jet homogenization. It is preferred to use ball milling.

[0232] To avoid metal contamination of the product, it is preferred to use devices which are made of high purity ceramic material or silica. An example is a ball mill in which all relevant milling parts are made of zirconia.

[0233] During milling, traces of material of the mill like zirconium oxide can be mechanically implanted in the surface of the product and lead to a surface modification.

[0234] During the disaggregation / deagglomeration process step, agglomerated and / or aggregated material from process step 2 can be broken, cleaved, separated so that a suitable particle size distribution for the application such as CMP abrasive results. It is preferred that particle-particle bonds are broken and separated, but the particles themselves are not broken to avoid sharp, pointy edges like in state-of-the-art calcined ceria processes.Attorney Docket No.: P25-207-SEC-W002

[0235] During, before or after the disaggregation / deagglomeration process step, a surface modification of the particles can be done. Suitable surface modifiers are organic molecules, oligomers or polymers, silanes, siloxanes, phosphorous derivatives, or any other material which is beneficial for the colloidal stability and / or the CMP polishing performance of the particles. It is preferred to add surface modifiers during the disaggregation / deagglomeration process step.

[0236] It is preferred to use surface modifiers which shift the zetapotential of the particles to a value of >25 mV or <-25 mV at a pH of 2 to 10 or 3 to 8.

[0237] The bumpy calcined ceria particles dispersion in a liquid medium can be cationic, anionic, or non-ionic in nature at a given pH.

[0238] It can be beneficial to do process step 3 with two or more different devices or in two or more sub-steps.

[0239] An example of such a process step 3 is the ball milling of the product with at least 2 different milling ball sizes and at least two different milling energy inputs with two different devices.

[0240] Another example is that at first a dry milling of the product from step 2 is done and subsequently the product is deagglomerated in a ball mill with water as a suspension medium.

[0241] Process step 3 also includes any necessary technical steps to remove undesired components from the particle suspension. This especially includes too large or too small particle fractions. This can be done by any method known in the art like centrifugation, vortex, filtration, adsorption and the like. It also includes ion exchange to remove unwanted ions from the suspension at any given time in the process step 3.Working Examples

[0242] Following the process described above, including the flowchart, starting with the starting nano particles, i.e., fluffy nano powder, particles were made after each step described above and shown in Scanning Electron Microscopy (SEM) images.

[0243] All Scanning Electron Microscopy (SEM) images were taken from untreated dry particles to highlight the differences.Example 1 Bumpy ceria particles made by the first process

[0244] Fluffy nano powder or nanoparticles were used as the starting material, as shown in Fig. 9 (the SEM image). The starting material was made by decomposition of cerium-lll-propionate in a pulsation reactor at 700°C for 1 s; mean particle size was 10-30 nm (agglomerated).Attorney Docket No.: P25-207-SEC-W002

[0245] The starting fluffy nanoparticles were first dispersed in deionized water to yield a free-flowing paste and subsequently dried in a vacuum furnace at 50°C for 24 hours. The dry nanoparticle agglomerates were milled with pestil & mortar to a fine powder which was then sintered at 900 °C for about 4 hours in a lab furnace to obtain the sintered nanoparticles, that is, the bumpy calcined ceria particles in an agglomerated and aggregated state as shown in Fig. 10 (the SEM image).

[0246] Next step was wet milling in a ball mill of the sintered nanoparticles (as shown in Fig. 10) dispersed in deionized water with 1 wt.% polyacrylic acid and having 2500 kDa as a colloidal stabilizer, NH3 was used to adjust the pH at pH 9.8. After subsequent wet milling in a ball mill, bumpy calcined ceria particles having mean particle size of 50-70 nm were obtained which are shown in Fig. 11 (the SEM image).Example 2 Bumpy ceria particles made by the second process

[0247] The fluffy nano nanoparticles shown in Fig. 9 were first dispersed in deionized water and polyvinylalcohol as the organic binder (1 weight% related to the dry amount of starting material) to yield a free-flowing paste and subsequently dried in a vacuum furnace at 50°C for 24 hours. The dry nanoparticle agglomerates were milled with pestil & mortar to a fine powder which was then sintered at 900 °C for about 4 hours in a lab furnace to obtain the bumpy calcined ceria particles in an agglomerated and aggregated state as shown in Fig. 12(the SEM image).

[0248] Next step was wet milling in a ball mill of the sintered nanoparticles as shown in Fig. 10 dispersed in deionized water with 1 wt.% polyacrylic acid having 2500 kDa as a colloidal stabilizer, NH3 was used to adjust the pH at pH 9.8. After subsequent wet milling in a ball mill, bumpy calcined ceria particles having mean particle size of 50-70 nm were obtained which are shown in Fig. 13(the SEM image).Example 3 Bumpy ceria particles made by the third process

[0249] The fluffy nano powder shown in Fig. 9 was sintered directly (without the granulation) at 900 °C for about 4 hours in a lab furnace to obtain the sintered particles (agglomerated aggregated as the SEM image shown in Fig. 14) before milling and redispersion to obtain the bumpy calcined ceria particles.

[0250] Next step was wet milling in a ball mill of the sintered nanoparticles as shown in Fig. 10 dispersed in deionized water with 1 wt.% polyacrylic acid having 2500 kDa as a colloidal stabilizer, NH3 was used to adjust the pH at pH 9.8. After subsequent wet milling in a ball mill, bumpy calcined ceria particles having mean particle size of 40-60nm as shown in Fig. 15 (the SEM image).Attorney Docket No.: P25-207-SEC-W002Example 4 Hybrid Bumpy ceria particles made by the third process

[0251] The fluffy nano nanoparticles (starting material) shown in Fig. 9 were first dispersed together with cerium (III) carbonate as the precursor in deionized water to yield a free-flowing paste and subsequently dried in a vacuum furnace at 50°C for 24 hours. The mixture contained 15.6 weight% of the starting fluffy nanoparticles, the rest being cerium (III) carbonate. The dried mixture of ceria nanoparticles and cerium (III) carbonate was milled with pestil & mortar to a fine powder which was then sintered at 800 °C for about 4 hours in a lab furnace to obtain the bumpy calcined ceria particles in an agglomerated and aggregated state as shown in Fig. 16.

[0252] Next step was wet milling in a ball mill of the sintered nanoparticles as shown in Fig. 16 dispersed in deionized water with 1 wt.% polyacrylic acid having 2500 kDa as a colloidal stabilizer, NH3 was used to adjust the pH at pH 9.8. After subsequent wet milling in a ball mill, bumpy calcined ceria particles having mean particle size of 80-85 nm were obtained which are shown in Fig. 17(the SEM image).Comparative Example 1 (non-inventive)

[0253] In this example, cerium (III) carbonate was calcined at 1130°C for 4h in a lab furnace. The resulting cerium oxide particles were pre-milled with a mortar mill and subsequently milled in a ball mill wherein the particles were dispersed in deionized water with 1% PAA (polyacrylic acid, 2500 kDa) was used as a colloidal stabilizer. NH3 was used to adjust the pH at pH 9.8.

[0254] A suspension of cerium oxide with a mean particle size of 94 nm was obtained as shown in Fig. 10 (the SEM image) which showed no protrusions or “bumps”.Polishing ExperimentsCMP MethodologyPARAMETERSGeneral

[0255] A or A: angstrom(s) - a unit of length

[0256] BP: back pressure, in psi units

[0257] CMP: chemical mechanical planarization

[0258] CS: carrier speed

[0259] DF: Down force: pressure applied during CMP, unit: psi

[0260] min: minute(s)

[0261] ml: milliliter(s)Attorney Docket No.: P25-207-SEC-W002

[0262] mV: millivolt(s)

[0263] mM: millimolar

[0264] psi: pounds per square inch

[0265] PS: platen rotational speed of polishing tool, in rpm (revolution(s) per minute)

[0266] SF: composition flow, ml / min

[0267] wt. %: weight percentage of a listed component relative to the composition. The total weight of a CMP polishing composition is100 wt.%.

[0268] Removal Rates: Measured removal rate at a given down pressure. The down pressure of the CMP tool was 3.0 psi in the examples.

[0269] Polishing tools: The Bruker TriboLab CMP

[0270] Polishing pad: IC1010 pads

[0271] CMP polishing compositions using the bumpy calcined ceria particles and other additives can be made to polish a semiconductor substrate comprising at least one surface containing silicon oxide.

[0272] The polishing rate or removal rate, dishing, defects, erosion et all can be measured.Polishing Example

[0273] The CMP slurries #1 to #4 comprised 0.15 wt.% different inventive nanoparticles made in working Examples 1 to 4 as disclosed above respectively. Comparative slurry #1 comprised 0.15 wt.% of the ceria particles made in Comparative Example 1 (non-inventive) as disclosed. All slurries contained deionized water and had a pH of 5.35.

[0274] The slurries were used to polish TECS, and the results were shown in Table 1.Table 1 Removal Rate of TECSExample TECS removal rate in A / min # 1 2813 # 2 2902 # 3 2565 # 4 2730 Comparative Slurry #1 2068Attorney Docket No.: P25-207-SEC-W002

[0275] The slurries using the bumpy ceria particles made according to the present invention have shown a consistent improved removal rate of TEOS when compared to calcined ceria without a bumpy structure.

[0276] The embodiments of this invention listed above, including the working example, are exemplary of numerous embodiments that may be made of this invention. It is contemplated that numerous other configurations of the process may be used, and the materials used in the process may be elected from numerous materials other than those specifically disclosed.

Claims

Attorney Docket No.: P25-207-SEC-W002Claims1. Colloidally stable bumpy calcined ceria particle having a core and a bumpy surface covering the core, wherein the bumpy surface contains a base surface and a plurality of protrusions protruding above the base surface; the base surface itself does not have protrusions, and the plurality of protrusions are selected from the group consisting of bumps, protrusions, branches or tree bark, and combinations thereof.

2. The colloidally stable bumpy calcined ceria particle of claim 1 , wherein the plurality of protrusions, the core and the base surface of the colloidally stable bumpy calcined ceria particle as a whole are made in same process; and the plurality of protrusions are integral parts of the colloidally stable calcined ceria particle.

3. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-2, wherein mean particle size of the bumpy calcined ceria particle is between 20 and 200nm, 30-150 nm, or 50-120 nm, wherein the mean particle size is measured by differential disc centrifuge technique.

4. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-3, wherein contact angles of the plurality of protrusions to the base surface is > 90°.

5. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-4, wherein height of the plurality of protrusions relative to mean particle size of the bumpy calcined ceria particles are between 1 and 75%, 1 and 50%, or 5 - 25%.

6. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-5, wherein contact area between each of the plurality of protrusions and the base surface is equal to or larger than the largest cross section area of the plurality of protrusions, wherein the largest cross section area is parallel to the contact area, and total contact area of the plurality of protrusions are 10 - 80%, 20 - 60%, or 30 - 40 % of the base surface area.33Attorney Docket No.: P25-207-SEC-W0027. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-6, wherein the plurality of protrusions and rest of the colloidally stable calcined ceria particle are same materials having same physicochemical properties.

8. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-7, wherein the colloidally stable calcined ceria particle is a hybrid particle containing at least two different domains with different physicochemical properties.

9. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-8, wherein the colloidally stable calcined ceria particle is a hybrid particle containing at least two different cerium dioxide domains with different physicochemical properties.

10. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-8, wherein the colloidally stable calcined ceria particle is a hybrid particle containing cerium dioxide and other oxide selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

11. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-10, wherein the colloidally stable calcined ceria particle is a hybrid particle; wherein the plurality of protrusions comprise oxide selected from the group consisting of cerium dioxide, silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof; and rest of the colloidally stable calcined ceria particle is cerium dioxide.

12. The colloidally stable calcined ceria particle according to any one of claims 1-11, wherein the colloidally stable calcined ceria particle is doped with rare earth elements.

13. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-12, wherein the colloidally stable calcined ceria particle is doped with lanthanum (La), gadolinium (Gd), Zirconium (Zr), or combinations thereof.Attorney Docket No.: P25-207-SEC-W00214. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-13, wherein the bumpy surface of the colloidally stable calcined ceria particle can be modified.

15. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-14, wherein the bumpy surface of the colloidally stable calcined ceria particle can be modified with (l)mechanically implanted or adsorbed inorganic ions; (2) a modifier selected from the group consisting of oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof; and combinations thereof.

16. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-15, wherein the bumpy surface of the colloidally stable calcined ceria particle is modified and the surface modified colloidally stable bumpy calcined ceria particles have a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

17. The colloidally stable bumpy calcined ceria particle according to any one of claims 1-16, wherein the colloidally stable bumpy calcined ceria particle has its mean particle size and particle size distribution characteristics change < 10 %, 5 % or 2% over a period of 6 months storage.

18. A process of making colloidally stable bumpy calcined ceria particles, comprising:step 1 comprises providing starting nanoparticles comprising ceria nanoparticles, andstep 2 comprises sintering the starting nanoparticles to obtain sintered nanoparticles; andstep 3 comprises disaggregating or deagglomerating the sintered nanoparticles to obtain colloidally stable bumpy calcined ceria particles;whereinthe starting nanoparticles are in fluffy nano powder or granulated powder form; the starting nanoparticles have a low-medium packing density for the formation of a colloidally stable bumpy calcined ceria particle; andthe sintering is at a temperature between 600 to 1100°C, 700 to 1000°C, 750 to 1000°, or 800 to 950°C at a time from 5 minutes to 24 hours, 1 hour to 16 hours, 2 to 6 hours.Attorney Docket No.: P25-207-SEC-W00219. The process of making colloidally stable bumpy calcined ceria particles of claim 18, wherein the starting nanoparticles have a mean primary particle size of <50% or preferably <30% of the mean particle size of the colloidally stable bumpy calcined ceria particles.

20. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-19, wherein the starting nanoparticles have the low packing density of 10 - 500 g / l, preferably 50 - 200 g / l.

21. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-20, wherein the starting nanoparticles are made by a thermal process, or a wet chemical process.

22. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-21, wherein the starting nanoparticles are made by a thermal process comprising thermal treatment of a precursor at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours; wherein the precursor is selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, cerium formate or cerium(lll) triformate, and combinations thereof.

23. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-22, wherein the starting nanoparticles are made by a thermal process comprising thermal treatment of a mixture of (1) and (2) at a temperature of > 200°C and < 1200°C, or > 300°C and < 500°C and a process time ranging from >0.1 s to < 24 hours, or >1 s to < 4 hours; wherein (1) is a precursor selected from the group consisting of cerium(lll) carbonate, cerium dioxide, cerium (IV) hydroxide, cerium(lll) nitrate, cerium(IV) ammonium nitrate, cerium(lll) acetate, cerium(lll) propionate, cerium(lll) oxalate, cerium formate or cerium(lll) triformate, and combinations thereof; and (2)are oxide nanoparticles selected from the group consisting of cerium dioxide, silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

24. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-23, wherein the starting nanoparticles are homogenousAttorney Docket No.: P25-207-SEC-W002ceria nanoparticles have same size or different sizes and made with same thermal process.

25. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-23, wherein the starting nanoparticles are heterogenous ceria nanoparticles have same size or different sizes and made with different thermal processes.

26. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-25, wherein the starting nanoparticles further comprise other oxide particles selected from the group consisting of silicon dioxide, aluminum oxide, zirconium oxide, and combinations thereof.

27. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-26, wherein the starting nanoparticles comprise doped and undoped ceria nanoparticles have same size or different sizes.

28. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-27, wherein the starting nanoparticles comprise doped and undoped ceria nanoparticles have same size or different sizes; and the doped ceria nanoparticles are doped with Lanthanum (La), Gadolinium (Gd), Zirconium(Zr), or combinations thereof.

29. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-28, wherein the starting nanoparticles further comprise surface-modified nanoparticles.

30. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-29, wherein the starting nanoparticles further comprise nanoparticles having surface-modified by organic polymers selected from the group consisting of cellulose and derivatives, homo- and copolymers of acrylic acids, polyacrylic amines, polyamines, and combinations thereof.

31. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-30, wherein the process further comprises at least one step after step 1 and before step 2; wherein the at least one step is selected from the group consisting of (a) dry or wet granulation, compacting, or combinations37Attorney Docket No.: P25-207-SEC-W002thereof to achieve a packing density of 200 -2500 g / l, or 500 - 1000 g / l; (b) wet or dry milling to achieve homogenization of particle size and distribution; (c)a drying step to remove physisorbed or crystal water from the starting nanoparticles; and combinations of steps (a) to (c); wherein step (a) is done using (i)water, (ii)an additive selected from the group consisting of a surfactants, an organic binder of polyvinylalcohol, hydroxypropylcellulose, and combinations thereof ; or the combinations of (i) and (ii); wherein the additive is decomposed in step 2 and free from contaminants of metal or halogen impurities.

32. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-31, wherein the step 2 is done in an atmosphere selected from the group consisting of vacuum, air, synthetic air, inert gases, reactive gases, the preferred atmosphere is air.

33. The process of making colloidally stable bumpy calcined ceria particles according to any one of claims 18-32, wherein the step 2 is done with adapted heating and cooling rates from 300 K / min to 1 K / min, 100 K / min to 5 K / min, or 50 K / min to 10 K / min.

34. The process of making a colloidally stable bumpy calcined ceria particle according to any one of claims 18-33, wherein the step 2 is done in a device made with high purity ceramic material or silica to avoid contamination with metal ions.

35. The process of making a colloidally stable bumpy calcined ceria particle according to any one of claims 18-34, wherein the step 3 is a process selected from the group consisting of ball milling, ultrasound treatment, jet homogenization, and combinations thereof.

36. The process of making a colloidally stable bumpy calcined ceria particle according to any one of claims 18-35, wherein the step 3 is a wet process ball milling to mill dispersion of the sintered nanoparticles from step 2 in a solvent comprising water, wherein the ball mill devices have parts made of zirconia.

37. The process of making a colloidally stable bumpy calcined ceria particle according to any one of claims 18-36, wherein the process further comprises a surface modification step before or after step 3 using a modifier selected from theAttorney Docket No.: P25-207-SEC-W002group consisting of oligomers or polymers, silanes, siloxanes, phosphorous derivatives, and combinations thereof; wherein the surface modified colloidally stable bumpy calcined ceria particles have a zetapotential of >25 mV or <-25 mV at pH 2 to 10, or 3 to 8.

38. The process of making a colloidally stable bumpy calcined ceria particle according to any one of claims 18-37, wherein the process further comprises a step after step 3 selected from the group consisting of (a)centrifugation, vortex, filtration, adsorption, or combinations therefor to remove too large or too small particles; (b) ion exchange to remove unwanted ions, and combinations of (a) and (b).

39. A Chemical Mechanical Planarization (CMP) polishing composition comprising:the colloidally stable bumpy calcined ceria particles according to any one of claims 1 to 17;and optionallyat least one selected from the group consisting of colloidal stabilizer, soluble or solid catalyst, chelating agent, corrosion inhibitor, surfactant, biocide, organic or inorganic salts, non-ionic organic molecule having more than one hydroxyl functional group, and pH adjuster.

40. The Chemical Mechanical Planarization (CMP) polishing composition of claim 39, wherein the stable bumpy calcined ceria particles have a concentration of 0.001 wt.% to 50.0 wt.%, 0.005 wt.% to 45.0 wt.%, 0.01 wt.% to 40.0 wt.%, 0.05 wt.% to 30.0 wt.%, or 0.1 wt.% to 10 wt.%.

41. A Chemical Mechanical Planarization polishing method for chemical mechanical planarization of a semiconductor substrate comprising at least one surface containing least one material selected from the group consisting of silicon oxide, silicon nitride and metal; comprising, consisting essentially of, or consisting of the steps of:providing the chemical mechanical planarization polishing composition according to any one of claims 39 and 40;providing a polishing pad;contacting the at least one surface with the polishing pad and the chemical mechanical planarization polishing composition;polishing the at least one surface.Attorney Docket No.: P25-207-SEC-W00242. A system of chemical mechanical planarization (CMP) polishing a semiconductor substrate having at least one surface comprising at least one surface containing least one material selected from the group consisting of silicon oxide, silicon nitride, and metal; the system comprising, consisting essentially of, or consisting of:a. the semiconductor substrate;b. the chemical mechanical planarization (CMP) polishing composition according to any one of claims 39 and 40;c. a polishing pad,wherein the at least one surface is in contact with the polishing pad and the chemical mechanical planarization polishing composition.