Porous fragrance carrier, method for producing same, non-combustion-heating-type flavor inhaler, and non-combustion-heating-type flavor inhalation system
A porous fragrance carrier made of cellulose acetate and hydroxypropyl cellulose, with optional additives, addresses fragrance retention and continuous release issues, ensuring long-term storage stability and consistent fragrance delivery in non-combustion heating type flavor inhalers.
Patent Information
- Application Number
- PCT/JP2025/017034
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-12
AI Technical Summary
Existing fragrance carriers for non-combustion heating type flavor inhalers suffer from fragrance volatilization during storage and lack continuous fragrance release during use.
A porous fragrance carrier composed of cellulose acetate, hydroxypropyl cellulose, and a fragrance, optionally with lactic acid ester and emulsifier, is produced through a specific mixing and drying process, allowing fragrance retention during storage and continuous release during heating.
The porous fragrance carrier effectively retains fragrance during storage and continuously releases it during heating, enhancing user experience by providing consistent fragrance delivery.
Smart Images

Figure JP2025017034_12112026_PF_FP_ABST
Abstract
Description
Porous Fragrance Carrier, Method for Producing the Same, Non-Combustion Heating Type Flavor Inhaler, and Non-Combustion Heating Type Flavor Inhalation System
[0001] The present invention relates to a porous fragrance carrier, a method for producing the same, a non-combustion heating type flavor inhaler, and a non-combustion heating type flavor inhalation system.
[0002] A fragrance carrier in which a volatile fragrance such as menthol is supported on a carrier is known. The fragrance carrier can be used, for example, in a non-combustion heating type flavor inhaler that obtains a flavor by heating the fragrance carrier.
[0003] For example, Patent Document 1 discloses a flavor-carrying constituent member for a tobacco product, which includes a constituent member of a tobacco product, and a flavor composition supported on the constituent member and containing an emulsifier having an HLB in the range of 1 to 7 and a flavor. Further, Patent Document 2 describes a method for producing a fragrance-containing sheet for smoking articles, which includes the steps of spreading a raw material slurry in a sol state at 60 to 90°C containing a polysaccharide and a fragrance and having a water content of 70 to 95% by weight on a base material, cooling the spread raw material slurry to a sample temperature of 0 to 40°C to cause gelation, and a heat drying step including heating the gelled raw material and drying it at a sample temperature of 70 to 100°C. On the other hand, Patent Document 3 discloses a method for producing a polysaccharide monolith structure that can be used as a chromatography packing material capable of separating biopolymers.
[0004] International Publication No. 2023 / 281764, International Publication No. 2012 / 118032, International Publication No. 2016 / 063702
[0005] For fragrance carriers, it is desired that volatilization of the fragrance is suppressed even during long-term storage. Further, when the fragrance carrier is used in a non-combustion heating type flavor inhaler, it is desired that the fragrance can be continuously released during use (during heating).
[0006] An object of the present invention is to provide a fragrance carrier that has high fragrance retention during storage and can continuously release fragrance during heating, and a non-combustion heating type flavor inhaler and a non-combustion heating type flavor inhalation system including the fragrance carrier.
[0007] The present invention includes the following embodiments.
[0008] [1] A porous fragrance carrier comprising cellulose acetate, hydroxypropyl cellulose, and a fragrance.
[0009] [2] The porous fragrance carrier according to [1], wherein the fragrance is at least one compound selected from the group consisting of menthol, linalyl acetate, cinnamaldehyde, ionone, undecanolactone, ethyl maltol, raspberry ketone, vanillin, and terpineol.
[0010] [3] The porous fragrance carrier according to [1] or [2], wherein the content of cellulose acetate in the porous fragrance carrier is 25 to 85% by mass.
[0011] [4] The porous fragrance carrier according to any one of [1] to [3], wherein the content of the hydroxypropyl cellulose in the porous fragrance carrier is 2 to 15% by mass.
[0012] [5] The porous fragrance carrier according to any one of [1] to [4], wherein the content of the fragrance in the porous fragrance carrier is 0.1 to 60% by mass.
[0013] [6] A porous fragrance carrier according to any one of [1] to [5], further comprising a lactic acid ester.
[0014] [7] The porous fragrance carrier according to [6], wherein the lactic acid ester is ethyl lactate.
[0015] [8] A porous fragrance carrier according to any one of [1] to [7], further comprising an emulsifier.
[0016] [9] The porous fragrance carrier according to [8], wherein the emulsifier is at least one of enzymatically hydrolyzed lecithin and dextrin.
[0017]
[10] The porous fragrance carrier according to [8] or [9], wherein the content of the emulsifier in the porous fragrance carrier is 1 to 10% by mass.
[0018]
[11] The porous fragrance carrier is the porous fragrance carrier according to any one of [1] to
[10] , having a porous skeleton formed by the cellulose acetate.
[0019]
[12] The porous fragrance carrier according to
[11] , wherein the hydroxypropyl cellulose and the fragrance are present in the pores of the porous fragrance carrier or inside the framework of the porous skeleton.
[0020] A non-combustion heating type flavor inhaler comprising a porous fragrance carrier as described in any of [1] to
[12] .
[0021] A non-combustion heating type flavor suction system comprising: a non-combustion heating type flavor suction device described in
[14] and
[13] ; and a heating device for heating the non-combustion heating type flavor suction device.
[0022]
[15] A method for producing a porous fragrance carrier, comprising: a step of mixing cellulose acetate and a lactic acid ester at a temperature of 80 to 100°C to prepare a first mixture; a step of mixing the first mixture with at least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin at a temperature of 80 to 100°C to prepare a second mixture; a step of mixing the second mixture with an emulsifier at a temperature of 80 to 100°C to prepare a third mixture; a step of mixing the third mixture with a fragrance composition at a temperature of 80 to 100°C to prepare a fourth mixture; a step of mixing the fourth mixture with hydroxypropyl cellulose at a temperature of 80 to 100°C to prepare a fifth mixture; and a step of cooling the fifth mixture to 10 to 25°C and drying it.
[0023] According to the present invention, it is possible to provide a fragrance carrier that has high fragrance retention properties during storage and can continuously release fragrance when heated, a non-combustion heating type fragrance inhaler and a non-combustion heating type fragrance inhalation system including the fragrance carrier.
[0024] This is an enlarged view showing an example of a cross-section of a porous fragrance carrier according to this embodiment. This is a cross-sectional view showing an example of a non-combustion heating type flavor inhaler according to this embodiment. This is a cross-sectional view of an example of a non-combustion heating type flavor inhalation system according to this embodiment, showing (a) the state before inserting the non-combustion heating type flavor inhaler into the heating device, and (b) the state after inserting the non-combustion heating type flavor inhaler into the heating device and heating it. This is a cross-sectional view showing an example of a combustion type flavor inhaler according to this embodiment. This is a graph showing the amount of menthol supplied per puff, measured using a non-combustion heating type flavor inhaler containing the porous fragrance carrier of Example 6. This is a graph showing the amount of menthol supplied per puff, measured using a non-combustion heating type flavor inhaler containing the porous fragrance carrier of Example 7.
[0025] [Porous Fragrance Carrier] The porous fragrance carrier according to this embodiment comprises cellulose acetate, hydroxypropyl cellulose (hereinafter also referred to as HPC), and a fragrance. In the porous fragrance carrier according to this embodiment, since the fragrance is located inside the carrier having a porous structure, the volatilization of the fragrance is suppressed when stored at room temperature, and it can be retained for a long period of time. Furthermore, the fragrance held in the pores and skeleton of the porous structure is gradually released to the outside when heated. Therefore, for example, when the fragrance carrier according to this embodiment is used in a non-combustion heating type fragrance inhaler, the fragrance is not released all at once during use (heating), but is released continuously. Therefore, even when puffing is repeated, the fragrance is continuously supplied to the user. In addition to cellulose acetate, HPC, and fragrance, the porous fragrance carrier according to this embodiment may also contain, for example, lactic acid esters, emulsifiers, solvents, etc. Furthermore, the porous fragrance carrier according to this embodiment may not contain tobacco components. Furthermore, the porous fragrance carrier according to this embodiment is not limited to non-combustion heating type flavor inhalers, but can also be used in combustion type flavor inhalers.
[0026] (Cellulose Acetate) The porous fragrance carrier according to this embodiment contains cellulose acetate. In this embodiment, cellulose acetate can form the porous skeleton (pore walls) of the fragrance carrier. The cellulose acetate according to this embodiment is not particularly limited. For example, the degree of acetic acid of cellulose acetate can be 30 to 60%, and may be 53 to 56%. The degree of substitution of acetyl groups in cellulose acetate can be 30 to 60%, and may be 38 to 40%. The average degree of polymerization of cellulose acetate can be 50 to 800%, and may be 100 to 200. The weight-average molecular weight of cellulose acetate can be 20,000 to 100,000%, and may be 35,000 to 45,000.
[0027] The content of cellulose acetate in the porous fragrance carrier according to this embodiment is preferably 25 to 85% by mass. By having a content of 25 to 85% by mass, a fragrance carrier having a porous structure can be manufactured more favorably. The range of the content may be 30 to 80% by mass, 35 to 75% by mass, 40 to 70% by mass, or 45 to 65% by mass. The lower limit of the content range may be 30% by mass or more, 40% by mass or more, 50% by mass or more, or 60% by mass or more. The upper limit of the content range may be 80% by mass or less, 70% by mass or less, 60% by mass or less, 50% by mass or less, or 40% by mass or less. The content is a value measured by a method described later.
[0028] (Hydroxypropylcellulose (HPC)) The porous fragrance carrier according to this embodiment contains HPC. In this embodiment, HPC can function as a thickening agent during the production of the porous fragrance carrier described later. The HPC according to this embodiment is not particularly limited. For example, the viscosity of HPC (2%, 20°C) can be 2 to 6000 cP, and may be 1000 to 5000 cP. The weight-average molecular weight of HPC can be 80000 to 350000, and may be 95000 to 105000.
[0029] The HPC content in the porous fragrance carrier according to this embodiment is preferably 2 to 15% by mass. By having a content of 2 to 15% by mass, a fragrance carrier having a porous structure can be manufactured more favorably. The range of the content may be 3 to 13% by mass, 5 to 12% by mass, 7 to 11% by mass, or 8 to 10% by mass. The lower limit of the content range may be 3% by mass or more, 5% by mass or more, 7% by mass or more, 9% by mass or more, or 11% by mass or more. The upper limit of the content range may be 13% by mass or less, 11% by mass or less, 9% by mass or less, 7% by mass or less, or 5% by mass or less. The content is a value measured by a method described later.
[0030] (Fragrance) The porous fragrance carrier according to this embodiment contains a fragrance. The fragrance according to this embodiment is not particularly limited, but in the porous fragrance carrier according to this embodiment, from the viewpoint of higher fragrance retention during storage, it is preferable that the fragrance is at least one compound selected from the group consisting of menthol, linalyl acetate, cinnamaldehyde, ionone, undecanolactone, ethyl maltol, raspberry ketone, vanillin, and terpineol. It is more preferable that the fragrance is at least one compound selected from the group consisting of menthol, vanillin, and terpineol. One of these fragrances may be used, or two or more may be used in combination. The fragrance may or may not contain tobacco components.
[0031] The fragrance content in the porous fragrance carrier according to this embodiment is preferably 0.1 to 60% by mass. By having a content of 0.1 to 60% by mass, a fragrance carrier having a porous structure can be manufactured more favorably. Furthermore, when the porous fragrance carrier is heated, the fragrance can be continuously released over a long period of time. The range of the content may be 5 to 55% by mass, 10 to 50% by mass, 15 to 45% by mass, or 20 to 40% by mass. The lower limit of the content range may be 10% by mass or more, 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more. The upper limit of the content range may be 50% by mass or less, 40% by mass or less, 30% by mass or less, 20% by mass or less, or 10% by mass or less. The content is a value measured by a method described later.
[0032] (Lactic Acid Ester) The porous fragrance carrier according to this embodiment may optionally contain a lactic acid ester. By adding a lactic acid ester during the production of the porous fragrance carrier described later, a fragrance carrier having a porous structure can be more preferably produced. Note that most of the lactic acid ester volatilizes during the drying process in the production of the porous fragrance carrier, so it does not need to be included in the porous fragrance carrier according to this embodiment, but a portion of it may remain in the porous fragrance carrier. The lactic acid ester according to this embodiment is not particularly limited, but from the viewpoint of more preferably producing a fragrance carrier having a porous structure, ethyl lactate, butyl acetate, etc. are preferred, and ethyl lactate is more preferred. One of these lactic acid esters may be used, or two or more may be used in combination.
[0033] When the porous fragrance carrier according to this embodiment contains lactic acid ester, the content of lactic acid ester in the porous fragrance carrier may be 10% by mass or less, 5% by mass or less, 1% by mass or less, or 0.1% by mass or less. The lower limit of the range of this content is not particularly limited, but for example it can be 0.01% by mass or more. The content may also be 0% by mass. This content is a value measured by the method described later.
[0034] (Emulsifier) The porous fragrance carrier according to this embodiment may optionally contain an emulsifier. By adding an emulsifier during the production of the porous fragrance carrier described later, raw materials such as cellulose acetate, HPC, and fragrance can be mixed uniformly, and a porous fragrance carrier in which each component is uniformly contained can be easily produced. The emulsifier according to this embodiment is not particularly limited, but from the viewpoint of enabling more uniform mixing of raw materials, enzyme-hydrolyzed lecithin, dextrin, sorbitan monostearate, etc. are preferred, and at least one of enzyme-hydrolyzed lecithin and dextrin (enzyme-hydrolyzed lecithin, dextrin, or enzyme-hydrolyzed lecithin and dextrin) is more preferred. One of these emulsifiers may be used, or two or more may be used in combination.
[0035] When the porous fragrance carrier according to this embodiment contains an emulsifier, the content of the emulsifier in the porous fragrance carrier is preferably 1 to 10% by mass. By having a content of 1 to 10% by mass, the uniformity of each raw material such as fragrance constituting the porous fragrance carrier is improved, and the fragrance retention during storage and the continuous release of fragrance during heating can be further improved. The range of the content may be 2 to 9% by mass, 3 to 8% by mass, 4 to 7% by mass, or 4.5 to 6.5% by mass. The lower limit of the content range may be 2% by mass or more, 3% by mass or more, 4% by mass or more, 5% by mass or more, or 6% by mass or more. The upper limit of the content range may be 9% by mass or less, 8% by mass or less, 7% by mass or less, 6% by mass or less, or 5% by mass or less. The content is a value measured by the method described later.
[0036] (Solvent) The porous fragrance carrier according to this embodiment may optionally contain a solvent. In order to uniformly add the fragrance during the production of the porous fragrance carrier described later, the fragrance can be dissolved in the solvent and added as a fragrance composition. Examples of solvents include propylene glycol (PG) and glycerin (G). One of these solvents may be used, or two or more may be used in combination. When the porous fragrance carrier according to this embodiment contains a solvent, the content of the solvent in the porous fragrance carrier is not particularly limited, but may be, for example, 0.1 to 20% by mass, 1 to 15% by mass, or 2 to 10% by mass. The lower limit of the content range may be 0.1% by mass or more, 1% by mass or more, 2% by mass or more, 3% by mass or more, or 5% by mass or more. The upper limit of the content range may be 20% by mass or less, 15% by mass or less, 10% by mass or less, 5% by mass or less, or 3% by mass or less. The content may also be 0% by mass. The content is a value measured by the method described later.
[0037] (Structure and Shape of Porous Fragrance Carrier) The porous fragrance carrier according to this embodiment has a porous structure. The porous structure has a plurality of pores formed by a porous skeleton (pore walls). Figure 1 shows an enlarged photograph of a cross-section of an example of the porous fragrance carrier according to this embodiment. As shown in Figure 1, the porous fragrance carrier according to this embodiment has a large number of pores of different sizes. The porous fragrance carrier according to this embodiment may have a porous skeleton formed of cellulose acetate. That is, the porous skeleton may be composed mainly of cellulose acetate, or may consist of cellulose acetate. In addition, HPC and fragrance can be present in the pores of the porous fragrance carrier or inside the skeleton of the porous skeleton. In this embodiment, by having the fragrance present in the pores of the porous fragrance carrier or inside the skeleton of the porous skeleton, the fragrance retention during storage and the continuous release of fragrance during heating can be further improved. When a porous fragrance carrier contains lactic acid esters or emulsifiers, these components, like HPC and fragrances, can be present within the pores of the porous fragrance carrier or within the framework of the porous skeleton.
[0038] The shape of the porous fragrance carrier is not particularly limited and can be in the form of powder, sheet, strip, pellet, or cylindrical.
[0039] [Method for Manufacturing a Porous Fragrance Carrier] The method for manufacturing a porous fragrance carrier according to this embodiment preferably includes the following steps. By including the following steps in the method according to this embodiment, the porous fragrance carrier according to this embodiment can be manufactured more simply and efficiently. A step to prepare a first mixture by mixing cellulose acetate and lactic acid ester at a temperature of 80 to 100°C (hereinafter also referred to as the first mixture preparation step); a step to prepare a second mixture by mixing the first mixture with at least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin at a temperature of 80 to 100°C (hereinafter also referred to as the second mixture preparation step); a step to prepare a third mixture by mixing the second mixture with an emulsifier at a temperature of 80 to 100°C (hereinafter also referred to as the third mixture preparation step); a step to prepare a fourth mixture by mixing the third mixture with a fragrance composition at a temperature of 80 to 100°C (hereinafter also referred to as the fourth mixture preparation step); a step to prepare a fifth mixture by mixing the fourth mixture with HPC at a temperature of 80 to 100°C (hereinafter also referred to as the fifth mixture preparation step); The fifth step involves cooling the mixture to 10-25°C and drying it (hereinafter also referred to as the cooling and drying step). The details of each step will be described below, but the method according to this embodiment may further include other steps not mentioned above.
[0040] (First Mixture Preparation Step) In this step, cellulose acetate and lactate ester are mixed at a temperature of 80 to 100°C to prepare the first mixture. When cellulose acetate, which is the main component of the porous skeleton (pore wall), and lactate ester, which is the solvent, are mixed at a temperature of 80 to 100°C, the resulting first mixture becomes gel-like. The cellulose acetate and lactate ester described above can be used as the cellulose acetate and lactate ester, respectively. From the viewpoint of good porous skeleton formation, the amount of lactate ester added per 100 parts by mass of cellulose acetate is preferably 100 to 500 parts by mass, more preferably 150 to 450 parts by mass, even more preferably 200 to 400 parts by mass, and particularly preferably 250 to 350 parts by mass. The mixing temperature of cellulose acetate and lactate ester is preferably 85 to 100°C, more preferably 90 to 100°C, even more preferably 95 to 100°C, and particularly preferably 100°C. The mixing time for cellulose acetate and lactic acid ester is not particularly limited as long as it allows for uniform mixing, but it can be, for example, 5 to 20 minutes.
[0041] (Second Mixture Preparation Step) In this step, the first mixture prepared in the first mixture preparation step is mixed with at least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin at a temperature of 80 to 100°C to prepare the second mixture. When the solvent is added to the gel-like first mixture and mixed, the gel becomes slightly softer and easier to mix. At least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin can be used as the solvent, and ethanol is preferred. From the viewpoint of appropriate gel flexibility, the amount of solvent added to 100 parts by mass of the first mixture is preferably 20 to 300 parts by mass, more preferably 50 to 200 parts by mass, and even more preferably 80 to 150 parts by mass. The mixing temperature of the first mixture and the solvent is preferably 85 to 100°C, more preferably 90 to 100°C, even more preferably 95 to 100°C, and particularly preferably 100°C. The mixing time between the first mixture and the solvent is not particularly limited as long as it allows for uniform mixing, but can be, for example, 5 to 10 minutes. Note that if the solvent is ethanol, it will not be present in the resulting porous fragrance carrier because it will completely evaporate during the drying process described later.
[0042] (Third mixed liquid preparation step) In this step, the second mixed liquid prepared in the aforementioned second mixed liquid preparation step and an emulsifier are mixed at a temperature of 80 to 100°C to prepare a third mixed liquid. By adding and mixing the emulsifier into the second mixed liquid, the uniformity of each component contained in the mixed liquid is improved. As the emulsifier, the aforementioned emulsifier can be used. The added amount of the emulsifier relative to 100 parts by mass of the second mixed liquid is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 5 parts by mass, from the viewpoint of improving the uniformity of each component. The mixing temperature of the second mixed liquid and the emulsifier is preferably 85 to 100°C, more preferably 90 to 100°C, even more preferably 95 to 100°C, and particularly preferably 100°C. The mixing time of the second mixed liquid and the emulsifier is not particularly limited as long as it allows uniform mixing, and can be, for example, 5 to 10 minutes.
[0043] (Fourth Mixture Preparation Step) In this step, the third mixture prepared in the third mixture preparation step and the fragrance composition are mixed at a temperature of 80 to 100°C to prepare the fourth mixture. The fragrance composition may include, for example, a fragrance and a solvent. The fragrances mentioned above can be used as the fragrance. Examples of solvents include propylene glycol (PG) and glycerin (G). One of these solvents may be used, or two or more may be used in combination. The fragrance content in the fragrance composition may be, for example, 1 to 80% by mass. The fragrance composition may consist only of fragrances. The amount of fragrance added to 100 parts by mass of the third mixture is preferably 5 to 600 parts by mass, more preferably 10 to 400 parts by mass, and even more preferably 20 to 200 parts by mass, from the viewpoint of being able to more favorably produce a fragrance carrier having a porous structure and to continuously release the fragrance over a long period of time when the porous fragrance carrier is heated. The mixing temperature between the third mixture and the fragrance composition is preferably 85 to 100°C, more preferably 90 to 100°C, even more preferably 95 to 100°C, and particularly preferably 100°C. The mixing time between the third mixture and the fragrance composition is not particularly limited as long as it is sufficient for uniform mixing, but can be, for example, 1 to 10 minutes.
[0044] (Fifth Mixture Preparation Step) In this step, the fourth mixture prepared in the fourth mixture preparation step is mixed with HPC at a temperature of 80 to 100°C to prepare the fifth mixture. When HPC is added to the fourth mixture and mixed, the viscosity of the mixture increases. The HPC described above can be used as the HPC. The amount of HPC added per 100 parts by mass of the fourth mixture is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 20 parts by mass, and even more preferably 1 to 10 parts by mass, from the viewpoint of being able to more favorably produce a fragrance carrier having a porous structure and to hold the fragrance more firmly. The mixing temperature of the fourth mixture and HPC is preferably 85 to 100°C, more preferably 90 to 100°C, even more preferably 95 to 100°C, and particularly preferably 100°C. The mixing time between the fourth mixture and the HPC is not particularly limited as long as it allows for uniform mixing, but it can be, for example, 1 to 10 minutes.
[0045] (Cooling and Drying Process) In this process, the fifth mixture prepared in the fifth mixture preparation process is cooled to 10 to 25°C and dried. When the fifth mixture is cooled to 10 to 25°C, a porous fragrance carrier having a porous skeleton formed of cellulose acetate precipitates. Here, from the viewpoint of sufficiently precipitating the porous fragrance carrier, it is preferable to cool the fifth mixture at a temperature of 80 to 100°C in a relatively short time. Specifically, it is preferable to cool the fifth mixture at a temperature of 80 to 100°C to a temperature of 10 to 25°C in 1 to 10 minutes, and more preferably in 3 to 5 minutes. The cooling temperature is preferably 15 to 25°C, and more preferably 20 to 25°C. After cooling, the precipitated porous fragrance carrier is removed and dried. The drying temperature is not particularly limited, but can be, for example, 30 to 70°C, or 40 to 60°C. The drying time depends on the drying temperature, but can be, for example, 0.5 to 2 hours. Drying can be carried out using a drying machine.
[0046] [Non-combustion-heating type flavor inhaler] The non-combustion-heating type flavor inhaler according to the present embodiment includes the porous flavor carrier according to the present embodiment. Since the non-combustion-heating type flavor inhaler includes the porous flavor carrier according to the present embodiment, it exhibits high flavor retention even when stored for a long period of time. In addition, when the non-combustion-heating type flavor inhaler is in use, the flavor is not released all at once from the porous flavor carrier, but is released continuously. The porous flavor carrier according to the present embodiment can be contained in, for example, a tobacco-containing segment or a filter segment described later.
[0047] An example of the non-combustion-heating type flavor inhaler according to the present embodiment is shown in Figure 2. The non-combustion-heating type flavor inhaler 1 shown in Figure 2 is provided with a tobacco-containing segment 2 filled with the porous flavor carrier according to the present embodiment, a cylindrical cooling segment 3 having perforations 8 on the circumference, a center hole segment 4, and a filter segment 5. The non-combustion-heating type flavor inhaler according to the present embodiment may have other segments in addition to the tobacco-containing segment, the cooling segment, the center hole segment, and the filter segment.
[0048] The axial length of the non-combustion-heating type flavor inhaler according to the present embodiment is not particularly limited, but is preferably 40 mm or more and 90 mm or less, more preferably 50 mm or more and 75 mm or less, and even more preferably 50 mm or more and 60 mm or less. In addition, the circumferential length of the non-combustion-heating type flavor inhaler is preferably 16 mm or more and 25 mm or less, more preferably 20 mm or more and 24 mm or less, and even more preferably 21 mm or more and 23 mm or less. For example, an embodiment in which the length of the tobacco-containing segment is 20 mm, the length of the cooling segment is 20 mm, the length of the center hole segment is 8 mm, and the length of the filter segment is 7 mm can be mentioned. The length of the filter segment can be selected within the range of 4 mm or more and 10 mm or less. In that case, the ventilation resistance of the filter segment is 15 mmH per segment 2 O / seg or more and 60 mmH 2The ratio can be selected to be 0 / seg or less. The length of each of these segments can be changed as appropriate according to manufacturability, required quality, etc. Furthermore, even if only the filter segment is placed downstream of the cooling segment without using the center hole segment, it can function as a non-combustion heating type flavor aspirator.
[0049] (Tobacco-containing segment) The tobacco-containing segment 2 has tobacco raw material filled inside a rolling paper (hereinafter also referred to as a wrapper). The method of filling the tobacco raw material inside the rolling paper is not particularly limited, but for example, the tobacco raw material may be wrapped in a wrapper, or the tobacco raw material may be filled inside a cylindrical wrapper. If the shape of the tobacco raw material has a longitudinal direction, such as a rectangular shape, the tobacco raw material may be filled so that the longitudinal direction is in an unspecified direction within the wrapper, or it may be filled in an aligned direction in the axial direction of the tobacco-containing segment 2 or in a direction perpendicular to the axial direction.
[0050] The tobacco-containing segment 2 comprises a tobacco filler filled with tobacco raw materials including tobacco, an aerosol-generating substrate, and a porous flavor carrier according to this embodiment, and a tubular wrapper covering the tobacco filler. The aerosol-generating substrate is a component capable of generating an aerosol by heating, such as glycerin or propylene glycol. There are no particular restrictions on the size of the tobacco used as the filler or its preparation method. For example, dried tobacco leaves that have been shredded may be used. Alternatively, dried tobacco leaves may be crushed and homogenized, processed into a sheet, and then shredded. Furthermore, the above-mentioned sheet-processed material may be gathered without being shredded and used as the filler. Whether dried tobacco leaves are shredded or crushed and homogenized into a sheet, various types of tobacco can be used in the tobacco filler. Yellow varieties, Burley varieties, Oriental varieties, native varieties, and other Nicotiana tabacum and Nicotiana rustica varieties can be blended as appropriate to achieve the desired flavor. Details of the aforementioned tobacco varieties are disclosed in "Encyclopedia of Tobacco," Tobacco Research Center, March 31, 2009. The porous flavor carrier according to this embodiment can be cut into a shape similar to that of tobacco and then filled, for example.
[0051] (Cooling Segment) As shown in Figure 2, the cooling segment 3 can be configured as a cylindrical member 7. The cylindrical member 7 may be, for example, a paper tube made by processing cardboard into a cylindrical shape.
[0052] The cylindrical member 7 and the mouthpiece lining paper 12 (described later) are provided with perforations 8 that penetrate both. Due to the presence of the perforations 8, outside air is introduced into the cooling segment 3 when inhaled. As a result, the aerosol vaporized components generated by the heating of the tobacco-containing segment 2 come into contact with the outside air, their temperature decreases, causing them to liquefy and form an aerosol. The diameter (length across) of the perforations 8 is not particularly limited, but may be, for example, 0.5 mm or more and 1.5 mm or less. The number of perforations 8 is not particularly limited and may be one or two or more. For example, multiple perforations 8 may be provided around the circumference of the cooling segment 3.
[0053] The amount of outside air introduced through the perforation 8 is preferably 85% by volume or less, and more preferably 80% by volume or less, relative to the total volume of gas drawn in by the user. By keeping the proportion of outside air at 85% by volume or less, the reduction in flavor due to dilution by outside air can be sufficiently suppressed. This can also be referred to as the ventilation ratio. From the viewpoint of cooling performance, the lower limit of the ventilation ratio is preferably 55% by volume or more, and more preferably 60% by volume or more.
[0054] The cooling segment may also include a segment comprising a wrinkled, pleated, gathered, or folded sheet of suitable constituent material. The cross-sectional profile of such an element may show randomly oriented channels. The cooling segment may also include a bundle of longitudinally extending tubes. Such a cooling segment can be formed, for example, by winding a pleated, gathered, or folded sheet material with a roll of paper.
[0055] The axial length of the cooling segment can be, for example, 7 mm or more and 28 mm or less, and can be, for example, 18 mm. The cooling segment can also have a substantially circular axial cross-sectional shape, and its diameter can be, for example, 5 mm or more and 10 mm or less, and can be, for example, about 7 mm.
[0056] (Center Hole Segment) As shown in Figure 2, the center hole segment 4 can be composed of a first filling layer 9 having a hollow section and a first inner plug wrapper 10 covering the first filling layer 9. The center hole segment 4 has the function of increasing the strength of the mouthpiece segment 6. The first filling layer 9 can be, for example, a rod with an inner diameter of φ1.0 mm or more and φ5.0 mm or less, which is filled with cellulose acetate fibers at high density and has a plasticizer containing triacetin added at a rate of 6% to 20% by mass relative to the mass of cellulose acetate, and then hardened. Because the first filling layer 9 has a high fiber filling density, when inhaled, air and aerosols flow only through the hollow section, and hardly any flow occurs inside the first filling layer 9. Since the first filling layer 9 inside the center hole segment 4 is a fiber filling layer, the feel from the outside during use is less likely to cause discomfort to the user. The center hole segment 4 may not have a first inner plug wrapper 10, and its shape may be maintained by thermoforming.
[0057] (Filter Segment) The structure of the filter segment 5 is not particularly limited, but it may consist of one or more packed layers. The outside of the packed layers may be wrapped with one or more sheets of wrapping paper. The air permeability resistance per segment of the filter segment 5 can be appropriately changed depending on the amount and material of the filler packed into the filter segment 5. For example, if the filler is cellulose acetate fiber, the air permeability resistance can be increased by increasing the amount of cellulose acetate fiber packed into the filter segment 5. When the filler is cellulose acetate fiber, the packing density of the cellulose acetate fiber is 0.13 to 0.18 g / cm³. 3 It can be. Note that the airflow resistance is a value measured using an airflow resistance meter (product name: SODIMAX, manufactured by SODIM).
[0058] The circumference of the filter segment 5 is not particularly limited, but is preferably 16 to 25 mm, more preferably 20 to 24 mm, and even more preferably 21 to 23 mm. The axial length of the filter segment 5 can be selected from 4 to 10 mm, and its airflow resistance is, for example, 15 to 60 mmH.2 It can be selected so that the ratio is 0 / segment. The axial length of the filter segment 5 is preferably 5 to 9 mm, and more preferably 6 to 8 mm. The cross-sectional shape of the filter segment 5 is not particularly limited, but can be circular, elliptical, polygonal, etc. The porous fragrance carrier according to this embodiment may be included in the filter segment 5.
[0059] As shown in Figure 2, the center hole segment 4 and the filter segment 5 can be connected by an outer plug wrapper (outer wrapping paper) 11. The outer plug wrapper 11 can be, for example, a cylindrical piece of paper. In addition, the tobacco-containing segment 2, the cooling segment 3, and the connected center hole segment 4 and filter segment 5 can be connected by a mouthpiece lining paper 12. These connections can be made, for example, by applying an adhesive such as vinyl acetate adhesive to the inner surface of the mouthpiece lining paper 12, inserting the three segments, and rolling it up. Note that these segments may be connected in multiple steps using multiple lining papers.
[0060] [Non-combustion heating type flavor suction system] The non-combustion heating type flavor suction system according to this embodiment comprises a non-combustion heating type flavor suction device according to this embodiment and a heating device for heating the non-combustion heating type flavor suction device. Because the non-combustion heating type flavor suction system according to this embodiment is equipped with a non-combustion heating type flavor suction device according to this embodiment, it has high flavor retention even when stored for a long period of time. In addition, when the non-combustion heating type flavor suction device is used, the flavor is not released all at once from the porous flavor carrier, but is released continuously. The non-combustion heating type flavor suction system according to this embodiment may have other configurations besides the non-combustion heating type flavor suction device and the heating device according to this embodiment.
[0061] An example of a non-combustion heating type flavor inhalation system according to this embodiment is shown in Figure 3. The non-combustion heating type flavor inhalation system shown in Figure 3 comprises a non-combustion heating type flavor inhaler 1 according to this embodiment and a heating device 13 that heats the tobacco-containing segment of the non-combustion heating type flavor inhaler 1 from the outside.
[0062] Figure 3(a) shows the state before inserting the non-combustion heating type flavor inhaler 1 into the heating device 13, and Figure 3(b) shows the state after inserting the non-combustion heating type flavor inhaler 1 into the heating device 13 and heating it. The heating device 13 shown in Figure 3 comprises a body 14, a heater 15, a metal tube 16, a battery unit 17, and a control unit 18. The body 14 has a cylindrical recess 19, and the heater 15 and the metal tube 16 are positioned on the inner side surface of the recess 19, corresponding to the tobacco-containing segment of the non-combustion heating type flavor inhaler 1 that is inserted into the recess 19. The heater 15 can be an electrical resistance heater, and power is supplied from the battery unit 17 by instructions from the temperature control unit 18, which controls the temperature, and the heater 15 is heated. The heat emitted from the heater 15 is transmitted to the tobacco-containing segment of the non-combustion heating type flavor inhaler 1 through the metal tube 16, which has high thermal conductivity.
[0063] In Figure 3(b), although a gap is shown between the outer circumference of the non-combustion heating type flavor inhaler 1 and the inner circumference of the metal tube 16 for illustrative purposes, in reality, it is preferable that there be no gap between the outer circumference of the non-combustion heating type flavor inhaler 1 and the inner circumference of the metal tube 16 in order to efficiently transfer heat. The heating device 13 heats the tobacco-containing segment of the non-combustion heating type flavor inhaler 1 from the outside, but it may also heat from the inside.
[0064] The heating temperature of the heating device is not particularly limited, but is preferably 400°C or lower, more preferably 150°C to 400°C, and even more preferably 200°C to 350°C. Note that the heating temperature refers to the temperature of the heater in the heating device.
[0065] [Combustion-type Flavor Inhaler] The combustion-type flavor inhaler according to this embodiment includes a porous flavor carrier according to this embodiment. Because the combustion-type flavor inhaler includes a porous flavor carrier according to this embodiment, it has high flavor retention even when stored for a long period of time. In addition, when the combustion-type flavor inhaler is used, the flavor is not released all at once from the porous flavor carrier, but is released continuously. The porous flavor carrier according to this embodiment can be included in, for example, a tobacco-containing segment or a filter segment, as described later.
[0066] An example of a combustion-type flavor inhaler according to this embodiment is shown in Figure 4. As shown in Figure 4, the combustion-type flavor inhaler 20 includes a tobacco-containing segment 21 and a filter segment 22 provided adjacent to the tobacco-containing segment 21. The tobacco-containing segment 21 includes a tobacco filling 23 containing a porous flavor carrier according to this embodiment and a wrapper 24 wrapped around the tobacco filling 23. The tobacco-containing segment 21 and the filter segment 22 are connected by a chip paper member 25 wound over the tobacco-containing segment 21 and the filter segment 22. The chip paper member 25 may have ventilation holes in a part of its outer circumference. The number of ventilation holes may be one or more, for example, 10 to 40 may be formed. If there are multiple ventilation holes, the ventilation holes may be arranged in a ring in a row on the outer circumference of the chip paper member 25. Multiple ventilation holes may be arranged at approximately constant intervals. By providing ventilation holes, air is drawn into the filter segment 22 from the ventilation holes when inhaled. By diluting the mainstream smoke with outside air from the vents, it is possible to design a product with a desired tar value. Examples of such combustion-type flavor inhalers include cigarettes. The user can inhale the flavor by igniting the tip of the tobacco-containing segment 21 and inhaling by placing the mouthpiece end of the filter segment 22 in their mouth.
[0067] The embodiment will be described in detail below with reference to examples, but this embodiment is not limited to these examples.
[0068] [Example 1] (Production of porous fragrance carrier) 1.5 g of cellulose acetate (trade name: Cellulose Acetate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 4.6 g of ethyl lactate were mixed in a glass sample bottle at 100°C for 10 minutes to prepare the first mixture. 7.1 g of ethanol was added to the first mixture and mixed at 100°C for 10 minutes to prepare the second mixture. 0.2 g of emulsifier (trade name: Sunlecithin A-1, manufactured by Taiyo Kagaku Co., Ltd., a mixture of 33% enzyme-degraded lecithin and 67% dextrin) was added to the second mixture and mixed at 100°C for 5 minutes to prepare the third mixture. 3.0 g of menthol was added to the third mixture and mixed at 100°C for 5 minutes to prepare the fourth mixture. 0.2 g of HPC (product name: Hydroxypropyl Cellulose 1,000-5,000 cP, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the fourth mixture and mixed at 100°C for 5 minutes to prepare the fifth mixture. The fifth mixture at 100°C was cooled to 25°C in 10 minutes to precipitate a porous fragrance carrier. The precipitated porous fragrance carrier was separated and dried in a dryer at 50°C for 60 minutes to obtain a porous fragrance carrier. The porous fragrance carrier was confirmed to be a porous body having numerous fine pores by electron microscopy.
[0069] Table 1 shows the content of each component in the obtained porous fragrance carrier. The content of each component was measured by the following method: The porous fragrance carrier was immersed in methanol, and each component was extracted with the methanol. The obtained extract was analyzed by GC-FID. From the analysis results, ethyl lactate, menthol, and ethanol were quantified (PG was also quantified in Examples 2 to 5 described later). The total mass of cellulose acetate, emulsifier, and HPC was calculated by subtracting the masses of ethyl lactate, menthol, and ethanol (and PG in Examples 2 to 5 described later) from the mass of the porous fragrance carrier. The content of cellulose acetate, emulsifier, and HPC was calculated by distributing the above total mass according to the mass ratio of cellulose acetate, emulsifier, and HPC at the time of raw material input.
[0070] (Evaluation of fragrance retention during storage) The obtained porous fragrance carrier was stored at room temperature, and the remaining menthol percentage was measured on the 7th, 14th, and 28th day of storage. The remaining menthol percentage was calculated as the ratio of the remaining menthol amount to the amount of menthol on the first day of storage, with the remaining menthol percentage on the first day of storage set as 100%. The results are shown in Table 2. Note that the remaining percentage in Table 2 may exceed 100% due to measurement errors.
[0071] [Example 2] A porous fragrance carrier was prepared in the same manner as in Example 1, except that when preparing the fourth mixture, a fragrance composition consisting of 3.0 g of menthol and 3.0 g of PG was added to the third mixture and mixed at 100°C for 10 minutes, and the porous fragrance carrier was evaluated for its fragrance retention during storage. The results are shown in Tables 1 and 2. It was confirmed by electron microscopy that the porous fragrance carrier is a porous material having a large number of fine pores.
[0072] [Example 3] A porous fragrance carrier was prepared in the same manner as in Example 1, except that when preparing the fourth mixture, a fragrance composition consisting of 0.5 g of α-terpineol and 1.0 g of PG was added to the third mixture and mixed at 100°C for 10 minutes, and the porous fragrance carrier was evaluated for its fragrance retention during storage. The results are shown in Tables 1 and 2. It was confirmed by electron microscopy that the porous fragrance carrier is a porous body having a large number of fine pores.
[0073] [Example 4] A porous fragrance carrier was prepared in the same manner as in Example 1, except that when preparing the fourth mixture, a fragrance composition consisting of 3.0 g of menthol, 2.0 g of vanillin, and 1.0 g of PG was added to the third mixture and mixed at 100°C for 10 minutes, and the porous fragrance carrier was evaluated for its fragrance retention during storage. The results are shown in Tables 1 and 2. It was confirmed by electron microscopy that the porous fragrance carrier is a porous body having a large number of fine pores.
[0074] [Example 5] A porous fragrance carrier was prepared in the same manner as in Example 1, except that when preparing the fourth mixture, a fragrance composition consisting of 0.5 g of vanillin and 1.0 g of PG was added to the third mixture and mixed at 100°C for 10 minutes, and the porous fragrance carrier was evaluated for its fragrance retention during storage. The results are shown in Tables 1 and 2. It was confirmed by electron microscopy that the porous fragrance carrier is a porous body having a large number of fine pores.
[0075]
[0076]
[0077] As shown in Table 2, it was found that the porous fragrance carriers of Examples 1 to 5 suppressed the volatilization of the fragrance even during long-term storage, and were able to adequately retain the fragrance.
[0078] [Example 6] (Production of porous fragrance carrier) 1.5 g of cellulose acetate (trade name: Cellulose Acetate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 4.6 g of ethyl lactate were mixed in a glass sample bottle at 100°C for 10 minutes to prepare the first mixture. 7.1 g of ethanol was added to the first mixture and mixed at 100°C for 5 minutes to prepare the second mixture. 0.15 g of emulsifier (trade name: Sunlecithin A-1, manufactured by Taiyo Kagaku Co., Ltd., a mixture of 33% enzyme-degraded lecithin and 67% dextrin) was added to the second mixture and mixed at 100°C for 5 minutes to prepare the third mixture. 1.5 g of menthol was added to the third mixture and mixed at 100°C for 5 minutes to prepare the fourth mixture. 0.3 g of HPC (product name: Hydroxypropyl Cellulose 1,000-5,000 cP, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the fourth mixture and mixed at 100°C for 5 minutes to prepare the fifth mixture. The fifth mixture at 100°C was cooled to 25°C in 10 minutes to precipitate a porous fragrance carrier. The precipitated porous fragrance carrier was separated and dried in a dryer at 50°C for 60 minutes to obtain a porous fragrance carrier. The porous fragrance carrier was confirmed to be a porous material having numerous fine pores by electron microscopy.
[0079] (Evaluation using a non-combustion heating type flavor inhaler) 10% by mass of the tobacco chips contained in MEVIUS for Ploom X (product name, manufactured by Japan Tobacco Inc.), a non-combustion heated tobacco product, was replaced with the porous flavor carrier of Example 6. The non-combustion heated tobacco product was subjected to a smoking test, and the amount of menthol delivered by heating was evaluated. The smoking test was conducted under the following conditions, referencing the Canadian Intense Regime (CIR). An electric heating device, Ploom X Advance (product name, manufactured by Japan Tobacco Inc.), which performs outer-circumferential heating, was used, and the non-combustion heated tobacco product was inserted and heating was started. The smoking test was performed using a single-stick automatic smoking machine manufactured by Borgwaldt, with an automatic smoking procedure under the conditions of a flow rate of 55 cc / 2 seconds and a smoking interval of 30 seconds. At this time, the openings in the cooling segment were positioned so as not to be blocked by the electric heating device. The mainstream smoke generated during the smoking test was collected on a Cambridge pad. After each puff, the Cambridge pad was removed and extracted with 10 mL of methanol. The amount of components in the mainstream smoke collected during each puff was measured using GC. The results are shown in Figure 5.
[0080] [Example 7] A porous fragrance carrier was prepared in the same manner as in Example 6, except that 3.0 g of menthol was added to the third mixture when preparing the fourth mixture and mixed at 100°C for 5 minutes. The product was then evaluated using a non-combustion heating type flavor inhaler. Table 3 shows the content of each component in the obtained porous fragrance carrier. Figure 6 shows the evaluation results using the non-combustion heating type flavor inhaler. It was confirmed by electron microscopy that the porous fragrance carrier is a porous material having numerous fine pores.
[0081]
[0082] As shown in Figures 5 and 6, in the non-combustion heating type flavor inhalers of Examples 6 and 7, it was found that the amount of menthol supplied remained constant even when the number of puffs increased during use, and that menthol was continuously released.
[0083] [Example 8] (Production of porous fragrance carrier) 1.5 g of cellulose acetate (trade name: Cellulose Acetate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 4.6 g of ethyl lactate were mixed in a glass sample bottle at 100°C for 10 minutes to prepare the first mixture. 7.1 g of ethanol was added to the first mixture and mixed at 100°C for 5 minutes to prepare the second mixture. 0.15 g of emulsifier (trade name: Sunlecithin A-1, manufactured by Taiyo Kagaku Co., Ltd., a mixture of 33% enzyme-hydrolyzed lecithin and 67% dextrin) was added to the second mixture and mixed at 100°C for 5 minutes to prepare the third mixture. To the third mixture, a fragrance composition consisting of 3.0 g of menthol and 3.0 g of a fragrance mixture containing linalyl acetate, ethyl maltol, raspberry ketone, vanillin, and PG was added and mixed at 100°C for 5 minutes to prepare the fourth mixture. To the fourth mixture, 0.3 g of HPC (trade name: Hydroxypropyl Cellulose 1,000-5,000 cP, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and mixed at 100°C for 5 minutes to prepare the fifth mixture. The fifth mixture at 100°C was cooled to 25°C in 10 minutes to precipitate a porous fragrance carrier. The precipitated porous fragrance carrier was separated and dried in a dryer at 50°C for 60 minutes to obtain a porous fragrance carrier. The porous fragrance carrier was confirmed to be a porous body having numerous fine pores by electron microscopy.
[0084] (Evaluation of fragrance retention during storage) The obtained porous fragrance carriers were stored at room temperature, and the remaining percentage of each fragrance was measured on the 7th, 14th, and 28th day of storage. The results are shown in Table 4. Note that, regarding the remaining percentages in Table 4, the remaining percentage may exceed 100% due to measurement errors.
[0085]
[0086] As shown in Table 4, it was found that the porous fragrance carrier of Example 8 suppressed the volatilization of various fragrances even during long-term storage, and was able to adequately retain each fragrance.
[0087] [Example 9] (Production of porous fragrance carrier) 1.5 g of cellulose acetate (trade name: Cellulose Acetate, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 4.5 g of ethyl lactate were mixed in a glass sample bottle at 100°C for 10 minutes to prepare the first mixture. 7.1 g of ethanol was added to the first mixture and mixed at 100°C for 5 minutes to prepare the second mixture. 0.15 g of emulsifier (trade name: Sunlecithin A-1, manufactured by Taiyo Kagaku Co., Ltd., a mixture of 33% enzyme-degraded lecithin and 67% dextrin) was added to the second mixture and mixed at 100°C for 5 minutes to prepare the third mixture. 3.0 g of menthol was added to the third mixture and mixed at 100°C for 5 minutes to prepare the fourth mixture. 0.3 g of HPC (product name: Hydroxypropyl Cellulose 1,000-5,000 cP, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the fourth mixture and mixed at 100°C for 5 minutes to prepare the fifth mixture. The fifth mixture at 100°C was cooled to 25°C in 10 minutes to precipitate a porous fragrance carrier. The precipitated porous fragrance carrier was separated and dried in a dryer at 50°C for 60 minutes to obtain a porous fragrance carrier. The content of each component in the obtained porous fragrance carrier is shown in Table 5. It was confirmed by electron microscopy that the porous fragrance carrier is a porous body having a large number of fine pores.
[0088] (Evaluation of fragrance retention during storage) The obtained porous fragrance carrier was stored at room temperature, and the remaining menthol percentage was measured on the 7th, 14th, and 28th day of storage. The results are shown in Table 6.
[0089] [Comparative Example 1] A porous fragrance carrier was prepared in the same manner as in Example 9, except that HPC was not added to the fourth mixture, and the fragrance retention during storage was evaluated. The content of each component in the obtained porous fragrance carrier is shown in Table 5. The evaluation results of the fragrance retention during storage are shown in Table 6. It was confirmed by electron microscopy that the porous fragrance carrier is a porous body having a large number of fine pores.
[0090]
[0091]
[0092] As shown in Table 6, the porous fragrance carrier of Example 9 was found to suppress menthol volatilization even during long-term storage, and to be able to retain menthol sufficiently. On the other hand, the porous fragrance carrier of Comparative Example 1, which did not contain HPC, had lower fragrance retention during storage compared to the porous fragrance carrier of Example 9.
[0093] This embodiment preferably includes the following aspects.
[0094] [1] A porous fragrance carrier comprising cellulose acetate, hydroxypropyl cellulose, and a fragrance.
[0095] [2] The porous fragrance carrier according to [1], wherein the fragrance is at least one compound selected from the group consisting of menthol, linalyl acetate, cinnamaldehyde, ionone, undecanolactone, ethyl maltol, raspberry ketone, vanillin, and terpineol.
[0096] [3] The porous fragrance carrier according to [1] or [2], wherein the content of cellulose acetate in the porous fragrance carrier is 25 to 85% by mass.
[0097] [4] The porous fragrance carrier according to any one of [1] to [3], wherein the content of the hydroxypropyl cellulose in the porous fragrance carrier is 2 to 15% by mass.
[0098] [5] The porous fragrance carrier according to any one of [1] to [4], wherein the content of the fragrance in the porous fragrance carrier is 0.1 to 60% by mass.
[0099] [6] A porous fragrance carrier according to any one of [1] to [5], further comprising a lactic acid ester.
[0100] [7] The porous fragrance carrier according to [6], wherein the lactic acid ester is ethyl lactate.
[0101] [8] A porous fragrance carrier according to any one of [1] to [7], further comprising an emulsifier.
[0102] [9] The porous fragrance carrier according to [8], wherein the emulsifier is at least one of enzymatically hydrolyzed lecithin and dextrin.
[0103]
[10] The porous fragrance carrier according to [8] or [9], wherein the content of the emulsifier in the porous fragrance carrier is 1 to 10% by mass.
[0104]
[11] The porous fragrance carrier is the porous fragrance carrier according to any one of [1] to
[10] , having a porous skeleton formed by the cellulose acetate.
[0105]
[12] The porous fragrance carrier according to
[11] , wherein the hydroxypropyl cellulose and the fragrance are present in the pores of the porous fragrance carrier or inside the framework of the porous skeleton.
[0106] A non-combustion heating type flavor inhaler comprising a porous fragrance carrier as described in any of [1] to
[12] .
[0107] A non-combustion heating type flavor suction system comprising: a non-combustion heating type flavor suction device described in
[14] and
[13] ; and a heating device for heating the non-combustion heating type flavor suction device.
[0108]
[15] A method for producing a porous fragrance carrier, comprising: a step of mixing cellulose acetate and a lactic acid ester at a temperature of 80 to 100°C to prepare a first mixture; a step of mixing the first mixture with at least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin at a temperature of 80 to 100°C to prepare a second mixture; a step of mixing the second mixture with an emulsifier at a temperature of 80 to 100°C to prepare a third mixture; a step of mixing the third mixture with a fragrance composition at a temperature of 80 to 100°C to prepare a fourth mixture; a step of mixing the fourth mixture with hydroxypropyl cellulose at a temperature of 80 to 100°C to prepare a fifth mixture; and a step of cooling the fifth mixture to 10 to 25°C and drying it.
[0109] 1 Non-combustion heating type flavor inhaler 2 Tobacco-containing segment 3 Cooling segment 4 Center hole segment 5 Filter segment 6 Mouthpiece segment 7 Cylindrical member 8 Perforation 9 First filling layer 10 First inner plug wrapper 11 Outer plug wrapper 12 Mouthpiece lining paper 13 Heating device 14 Body 15 Heater 16 Metal tube 17 Battery unit 18 Control unit 19 Recess 20 Combustion type flavor inhaler 21 Tobacco-containing segment 22 Filter segment 23 Tobacco filler 24 Wrapper 25 Tip paper member
Claims
1. A porous fragrance carrier containing cellulose acetate, hydroxypropyl cellulose, and a fragrance.
2. The porous fragrance carrier according to claim 1, wherein the fragrance is at least one compound selected from the group consisting of menthol, linalyl acetate, cinnamaldehyde, ionone, undecanolactone, ethyl maltol, raspberry ketone, vanillin, and terpineol.
3. The porous fragrance carrier according to claim 1 or 2, wherein the content of cellulose acetate in the porous fragrance carrier is 25 to 85% by mass.
4. The porous fragrance carrier according to any one of claims 1 to 3, wherein the content of hydroxypropyl cellulose in the porous fragrance carrier is 2 to 15% by mass.
5. The porous fragrance carrier according to any one of claims 1 to 4, wherein the content of the fragrance in the porous fragrance carrier is 0.1 to 60% by mass.
6. A porous fragrance carrier according to any one of claims 1 to 5, further comprising a lactic acid ester.
7. The porous fragrance carrier according to claim 6, wherein the lactic acid ester is ethyl lactate.
8. A porous fragrance carrier according to any one of claims 1 to 7, further comprising an emulsifier.
9. The porous fragrance carrier according to claim 8, wherein the emulsifier is at least one of enzymatically hydrolyzed lecithin and dextrin.
10. The porous fragrance carrier according to claim 8 or 9, wherein the content of the emulsifier in the porous fragrance carrier is 1 to 10% by mass.
11. The porous fragrance carrier according to any one of claims 1 to 10, wherein the porous fragrance carrier has a porous skeleton formed by the cellulose acetate.
12. The porous fragrance carrier according to claim 11, wherein the hydroxypropyl cellulose and the fragrance are present within the pores of the porous fragrance carrier or within the framework of the porous skeleton.
13. A non-combustion heating type flavor inhaler comprising a porous flavor carrier according to any one of claims 1 to 12.
14. A non-combustion heating type flavor suction system comprising: a non-combustion heating type flavor suction device according to claim 13; and a heating device for heating the non-combustion heating type flavor suction device.
15. A method for producing a porous fragrance carrier, comprising: a step of mixing cellulose acetate and a lactic acid ester at a temperature of 80 to 100°C to prepare a first mixture; a step of mixing the first mixture with at least one solvent selected from the group consisting of ethanol, propylene glycol, and glycerin at a temperature of 80 to 100°C to prepare a second mixture; a step of mixing the second mixture with an emulsifier at a temperature of 80 to 100°C to prepare a third mixture; a step of mixing the third mixture with a fragrance composition at a temperature of 80 to 100°C to prepare a fourth mixture; a step of mixing the fourth mixture with hydroxypropyl cellulose at a temperature of 80 to 100°C to prepare a fifth mixture; and a step of cooling the fifth mixture to 10 to 25°C and drying it.