Multilayer ceramic capacitor

The multilayer ceramic capacitor addresses reliability issues by controlling manganese distribution and dielectric grain sizes through specific electrode and layer configurations, ensuring both reliability and capacitance stability.

WO2026234800A1PCT designated stage Publication Date: 2026-11-12MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/017041
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional multilayer ceramic capacitors lack the necessary reliability to meet the increasing demand for highly reliable components.

Method used

The multilayer ceramic capacitor design includes specific configurations of internal electrodes and dielectric layers, with varying coverage and thickness variations to control the distribution of manganese (Mn) and dielectric grain sizes, ensuring uniformity and reliability while minimizing capacitance loss.

Benefits of technology

This design enhances the reliability of the capacitor by suppressing grain growth and maintaining electrostatic capacitance, thereby providing a highly reliable multilayer ceramic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2025017041_12112026_PF_FP_ABST
    Figure JP2025017041_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a highly reliable multilayer ceramic capacitor. A multilayer ceramic capacitor 1 comprises: a laminate 2 comprising a plurality of dielectric layers 4 and a plurality of internal electrodes 5 to be laminated; a first external electrode 30A disposed on a third surface F3; and a second external electrode 30B disposed on a fourth surface F4. Among the plurality of internal electrodes 5, the internal electrode 5 disposed closest to a first surface F1 side is defined as a first first internal electrode 511, the internal electrode 5 adjacent to the first first internal electrode 511 in a lamination direction T is defined as a second first internal electrode 512, and the internal electrode 5 adjacent to the second first internal electrode 512 in the lamination direction T and located closer to a second surface F2 side than is the second first internal electrode 512 is defined as a third first internal electrode 513. A region between the first first internal electrode 511 and the first surface F1 contains Mn. The coverage of the second first internal electrode 512 is lower than the coverage of the third first internal electrode 513.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer ceramic capacitor

[0001] The present invention relates to a multilayer ceramic capacitor.

[0002] Conventionally, there exists a multilayer ceramic capacitor including cover layers covering the top and bottom of a capacitance section in which internal dielectric layers and internal electrodes are stacked, and side margin sections covering both sides in the width direction of inner layer sections covering the left and right sides (for example, Patent Document 1). For example, in the multilayer ceramic capacitor of Patent Document 1, the internal dielectric layers contain Mn as a sub-component.

[0003] JP 2024-100560 A

[0004] In recent years, the demand for highly reliable multilayer ceramic capacitors has been increasingly growing, and conventionally proposed techniques have been insufficient to meet this demand.

[0005] An object of the present invention is to provide a multilayer ceramic capacitor with excellent reliability.

[0006] To solve the above problem, the multilayer ceramic capacitor of the present invention includes a laminate having a plurality of dielectric layers and a plurality of internal electrodes stacked on one another, a first surface and a second surface opposed in the stacking direction, a third surface and a fourth surface opposed in a first direction orthogonal to the stacking direction, and a fifth surface and a sixth surface opposed in a second direction orthogonal to the stacking direction and the first direction; and a first external electrode disposed on the third surface, and a second external electrode disposed on the fourth surface. When, among the plurality of internal electrodes, the internal electrode disposed closest to the first surface side is defined as a 1-1 internal electrode, the internal electrode adjacent to the 1-1 internal electrode in the stacking direction is defined as a 1-2 internal electrode, and the internal electrode adjacent to the 1-2 internal electrode in the stacking direction and located closer to the second surface side than the 1-2 internal electrode is defined as a 1-3 internal electrode, a region between the 1-1 internal electrode and the first surface contains Mn, and the coverage of the 1-2 internal electrode is lower than the coverage of the 1-3 internal electrode.

[0007] To solve the above problems, the multilayer ceramic capacitor of the present invention comprises a plurality of stacked dielectric layers and a plurality of internal electrodes, a laminate comprising a first and second surface facing each other in the stacking direction, a third and fourth surface facing each other in a first direction perpendicular to the stacking direction, and a fifth and sixth surface facing each other in a second direction perpendicular to the stacking direction and the first direction, a first external electrode disposed on the third surface, and a second external electrode disposed on the fourth surface, wherein the internal electrode disposed on the first surface side of the plurality of internal electrodes is designated as the 1-1 internal electrode, and the internal electrodes adjacent to the 1-1 internal electrode in the stacking direction are designated as the 1-2 If an internal electrode is defined as the first-third internal electrode, and the internal electrode adjacent to the first-second internal electrode in the stacking direction and located on the second plane side of the first-second internal electrode, and the internal electrode adjacent to the first-third internal electrode in the stacking direction and located on the second plane side of the first-third internal electrode, then the internal electrode adjacent to the first-third internal electrode in the stacking direction and located on the second plane side of the first-third internal electrode, and the region between the first-first internal electrode and the first plane contains Mn, then the thickness variation of the portion of the dielectric layer sandwiched between the first-third internal electrode and the first-fourth internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-second internal electrode and the first-third internal electrode.

[0008] This allows us to provide highly reliable multilayer ceramic capacitors.

[0009] This is a schematic perspective view of a multilayer ceramic capacitor according to an embodiment. This is a cross-sectional view taken along line II-II in Figure 1. This is a cross-sectional view taken along line III-III in Figure 1. This is a cross-sectional view taken along line IVA-IVA in Figure 2. This is a cross-sectional view taken along line IVB-IVB in Figure 2. This is a conceptual diagram showing the coverage of the internal electrodes. This is a diagram showing a modified first internal electrode, corresponding to Figure 4A. This is a diagram showing a modified second internal electrode, corresponding to Figure 4B.

[0010] Embodiments of the present invention will be described below. As shown in Figures 1 to 3, the multilayer ceramic capacitor 1 comprises a laminate 2 and a pair of external electrodes 30 provided at both ends of the laminate 2.

[0011] The laminate 2 has an inner layer portion (effective portion) 6 and an ineffective portion 7. The inner layer portion 6 is a region in which internal electrodes 5 (first internal electrode 5A and second internal electrode 5B) and dielectric layers 4 are alternately stacked. The ineffective portion 7 is a region in which internal electrodes 5 are not arranged and has an outer layer portion 7A that sandwiches the inner layer portion 6 from the stacking direction T and a side gap portion 70 that sandwiches the inner layer portion 6 from a second direction W.

[0012] In the following description, the orientation of the multilayer ceramic capacitor 1 is expressed as follows: the direction in which the internal electrodes 5 and the dielectric layer 4 are stacked is referred to as the stacking direction T. The direction intersecting the stacking direction T and on which the pair of external electrodes 30 are provided is referred to as the first direction L. The direction intersecting both the first direction L and the stacking direction T is referred to as the second direction W. In this embodiment, the first direction L, the second direction W, and the stacking direction T are orthogonal to each other.

[0013] The cross-section of the multilayer ceramic capacitor 1 parallel to the stacking direction T and the first direction L is called the "LT cross-section". The cross-section in Figure 2 is the LT cross-section passing through the center of the multilayer ceramic capacitor 1 in the second direction W. The cross-section of the multilayer ceramic capacitor 1 parallel to the stacking direction T and the second direction W is called the "WT cross-section". The cross-section in Figure 3 is the WT cross-section passing through the center of the multilayer ceramic capacitor 1 in the first direction L. The cross-section of the multilayer ceramic capacitor 1 parallel to the first direction L and the second direction W is called the "LW cross-section". The cross-section in Figure 4A is the LW cross-section with the first internal electrode 5A exposed. The cross-section in Figure 4B is the LW cross-section with the second internal electrode 5B exposed.

[0014] The dimension of the multilayer ceramic capacitor 1 in the first direction L is preferably 1.0 mm or more and 1.6 mm or less. The dimension of the multilayer ceramic capacitor 1 in the second direction W is preferably 0.5 mm or more and 0.8 mm or less. The dimension of the multilayer ceramic capacitor 1 in the stacking direction T is preferably 0.5 mm or more and 0.8 mm or less. More preferably, the dimension of the multilayer ceramic capacitor 1 in the first direction L is 1.0 mm, the dimension of the multilayer ceramic capacitor 1 in the second direction W is 0.5 mm or more, and the dimension of the multilayer ceramic capacitor 1 in the stacking direction T is 0.8 mm.

[0015] (Laminate) The laminate 2 has a first surface F1 and a second surface F2 facing the lamination direction T, a third surface F3 and a fourth surface F4 facing the first direction L, and a fifth surface F5 and a sixth surface F6 facing the second direction W.

[0016] In this embodiment, it is preferable that the edges between two adjacent faces of the laminate 2 are rounded. This helps to suppress chipping at the sharp corners of the laminate 2.

[0017] (Dielectric layer) Dielectric layer 4 is made of BaTiO as a ceramic. 3 The main component is barium titanate, and at least one of Dy, Si, Mg, Mn, Sn, Cu, rare earth elements, Ni, and Al is included as a minor component. The particle size of the ceramic in the dielectric layer 4 is preferably 100 nm or more and 200 nm or less.

[0018] (Thickness Variation) The dimension of the dielectric layer 4 in the stacking direction T is defined as the "thickness of the dielectric layer 4". The thickness of the dielectric layer is measured at nine equally spaced locations in the cross-section of a predetermined multilayer ceramic capacitor. The largest of the measured dielectric layer thicknesses is defined as the "maximum thickness", and the smallest as the "minimum thickness". The average of the measured dielectric layer thicknesses is defined as the "average thickness". In this specification, the value defined by the following formula (A) is defined as "thickness variation". Thickness variation = (maximum thickness - minimum thickness) / average thickness (A)

[0019] Furthermore, if the dielectric layer 4 penetrates the internal electrode 5 in the stacking direction T at a point where the thickness of the dielectric layer 4 is to be measured (referred to as the "measurement point") (in other words, if the internal electrode 5 is divided), the thickness of the dielectric layer 4 shall be measured at a point adjacent to the divided portion instead of at the measurement point.

[0020] (Internal Electrode) The internal electrode 5 has a first internal electrode 5A exposed on the third surface F3 and a second internal electrode 5B exposed on the fourth surface F4.

[0021] As shown in Figure 2, the internal electrode 5 comprises an opposing portion 52 that faces each other between the first internal electrode 5A and the second internal electrode 5B, and an extension portion 51 that does not face each other between the first internal electrode 5A and the second internal electrode 5B, and is drawn out from the opposing portion 52 toward either the third surface F3 or the fourth surface F4. The direction in which the extension portion 51 extends differs between the first internal electrode 5A and the second internal electrode 5B, with the extension being toward the third surface F3 side and the extension being toward the fourth surface F4 side.

[0022] The end of the lead portion 51 of the first internal electrode 5A is exposed to the third surface F3 and electrically connected to the first external electrode 30A. The end of the lead portion 51 of the second internal electrode 5B is exposed to the fourth surface F4 and electrically connected to the second external electrode 30B. Charge is accumulated between the opposing portions 52 of the first internal electrode 5A and the second internal electrode 5B, which are adjacent in the stacking direction T, and they function as a capacitor.

[0023] The internal electrode 5 is mainly composed of Ni, for example. However, it is not limited to this, and the internal electrode 5 may be formed from a metallic material such as Cu, Ag, Pd, Ag-Pd alloy, or Au. In addition, the internal electrode 5 may also contain BT particles (particles containing Ba and Ti) as a co-material. The internal electrode 5 may also contain Sn. It is preferable that at least one of the first internal electrode 5A and the second internal electrode 5B has an Sn layer.

[0024] As shown in Figures 4A and 4B, the shape of the first internal electrode 5A is, for example, a roughly rectangular plate shape, and the shape of the second internal electrode 5B is, for example, a roughly rectangular plate shape. However, it is not limited to these.

[0025] (Coverage) As shown in Figure 5, the internal electrode 5 includes a cavity where no metal is present. In this specification, the proportion of the internal electrode 5 occupied by metal is defined as coverage. Specifically, for example, within a predetermined dimension WA (not shown) in the second direction W of the internal electrode 5, the dimension WB (not shown) in the second direction W where metal is substantially observed is determined. Note that WB is the remaining dimension obtained by subtracting the dimension of the area in the internal electrode 5 where no metal is observed from dimension WA. Then, WB / WA is the coverage of the internal electrode 5.

[0026] Coverage can be measured, for example, by the following method. First, the laminate 2 is polished to expose the WT cross section, as shown in Figure 3, which extends from the center of the first direction L in the second direction W and the lamination direction T, passing through the second direction W and the lamination direction T.

[0027] Next, a scanning electron microscope (SEM) is used to observe the exposed WT step surface and determine the dimension WB in the second direction W where metal is substantially observed (the remaining length after subtracting the length of the region where metal of the internal electrode is not observed from the total length) within the range of dimension WA in a predetermined second direction W of the internal electrode 5.

[0028] Then, we calculate the coverage in each domain, i.e., WB / WA.

[0029] (Outer layer) The outer layer 7A is positioned on the first surface F1 side and the second surface F2 side of the inner layer 6, respectively, so as to sandwich the inner layer 6 in the stacking direction T.

[0030] (Side gap portion) As shown in Figure 3, a side gap portion 70 is provided in the region from the ends of the first internal electrode 5A and the second internal electrode 5B in the second direction W to the fifth surface F5 or the sixth surface F6.

[0031] (External Electrodes) The external electrode 30 has a first external electrode 30A and a second external electrode 30B and is connected to the internal electrode 5. The first external electrode 30A is positioned on the third surface F3 and extends further to the first surface F1, the second surface F2, the fifth surface F5 and the sixth surface F6. The second external electrode 30B is positioned on the fourth surface F4 and extends further to the first surface F1, the second surface F2, the fifth surface F5 and the sixth surface F6. The external electrode 30 has, for example, a base electrode 31 and a plating layer 33 from the laminate 2 side.

[0032] (Underlay electrode) The underlay electrode 31 includes, for example, a conductive component (such as Cu) and a glass component, but is not limited to these.

[0033] (Plating layer) The plating layer 33 includes, for example, a Ni plating layer 33a and a Sn plating layer 33b.

[0034] Here, the internal electrode 5 that is positioned closest to the first surface F1 among the multiple internal electrodes 5 is designated as the 1-1 internal electrode 511. The internal electrode 5 adjacent to the 1-1 internal electrode 511 in the stacking direction T is designated as the 1-2 internal electrode 512. The internal electrode 5 adjacent to the 1-2 internal electrode 512 in the stacking direction T and located closer to the second surface F2 than the 1-2 internal electrode 512 is designated as the 1-3 internal electrode 513.

[0035] The region between the first-first internal electrode 511 and the first surface F1 contains Mn. The region between the first-first internal electrode 511 and the first surface F1 is the outer layer 7A located on the first surface F1 side of the inner layer 6.

[0036] Preferably, the coverage of the first-second internal electrode 512 is lower than the coverage of the first-third internal electrode 513.

[0037] Preferably, the coverage of the first-first internal electrode 511 is higher than the coverage of the first-second internal electrode 512.

[0038] Preferably, the coverage of the first-third internal electrode 513 is higher than the coverage of the first-first internal electrode 511.

[0039] Preferably, the coverage of the first-first internal electrode 511 and the coverage of the first-second internal electrode 512 are both lower than the coverage of the first-third internal electrode 513.

[0040] According to such a configuration, Mn in the outer layer portion 7A passes through the 1-1 internal electrode 511 and the 1-2 internal electrode 512, which have relatively low coverage, and moves toward the center of the laminate 2. However, the movement of Mn is suppressed by the 1-3 internal electrode 513, which has relatively high coverage. For this reason, Mn accumulates in a region relatively close to the surface of the laminate 2, and Mn is less likely to excessively reach a region relatively close to the center of the laminate 2. In addition, Mn suppresses grain growth of dielectric grains. As a result, in the region relatively close to the surface of the laminate 2, the grain size of the dielectric grains is reduced to improve reliability, while in the region close to the center of the laminate 2, the grain size of the dielectric grains is increased, so that a decrease in electrostatic capacitance can be suppressed. Accordingly, it is possible to provide the multilayer ceramic capacitor 1 that is excellent in reliability and capable of suppressing a decrease in electrostatic capacitance.

[0041] The internal electrode 5 adjacent to the 1-3 internal electrode 513 in the lamination direction T and located on the second surface F2 side relative to the 1-3 internal electrode 513 is defined as a 1-4 internal electrode 514. The internal electrode 5 adjacent to the 1-4 internal electrode 514 in the lamination direction T and located on the second surface F2 side relative to the 1-4 internal electrode 514 is defined as a 1-5 internal electrode 515.

[0042] The coverage of the 1-4 internal electrode 514 is preferably higher than the coverage of the 1-2 internal electrode 512, and the coverage of the 1-5 internal electrode 515 is preferably higher than the coverage of the 1-2 internal electrode 512.

[0043] The thickness variation of the portion of the dielectric layer 4 sandwiched between the 1-3 internal electrode 513 and the 1-4 internal electrode 514 (referred to as "1-3-4 dielectric region R134") is preferably smaller than the thickness variation of the portion of the dielectric layer 4 sandwiched between the 1-2 internal electrode 512 and the 1-3 internal electrode 513 (referred to as "1-2-3 dielectric region R123").

[0044] It is preferable that the thickness variation of the portion of the dielectric layer 4 sandwiched between the 1-1 internal electrode 511 and the 1-2 internal electrode 512 (referred to as "1-1-2 dielectric region R112") is smaller than the thickness variation of the 1-2-3 dielectric region R123.

[0045] It is preferable that the thickness variation of the 1-1-2 dielectric region R112 is smaller than the thickness variation of the 1-3-4 dielectric region R134.

[0046] It is preferable that the thickness variation of the portion of the dielectric layer 4 sandwiched between the 1-4 internal electrode 514 and the 1-5 internal electrode 515 (referred to as "1-4-5 dielectric region R145") is smaller than the thickness variation of the 1-2-3 dielectric region R123.

[0047] The D50 diameter (in terms of volume) of dielectric grains in the 1-3-4 dielectric region R134 is preferably larger than the D50 diameter of dielectric grains in the 1-2-3 dielectric region R123, and more preferably 150% or more and 200% or less of the D50 diameter of dielectric grains in the 1-2-3 dielectric region R123. The D50 diameter of dielectric grains in the 1-3-5 dielectric region R134 is preferably larger than the D50 diameter of dielectric grains in the 1-2-3 dielectric region R123, and more preferably 150% or more and 200% or less of the D50 diameter of dielectric grains in the 1-2-3 dielectric region R123. For example, when the dielectric grain diameter D50 in the 1-3-4 region R134 is 289.2 nm, the dielectric grain diameter D50 in the 1-2-3 region R123 is 151.3 nm.

[0048] According to such a configuration, in the region closer to the center of the laminate 2, the average grain size of the dielectric grains is increased, so that a decrease in capacitance can be suppressed. In the region near the surface of the laminate 2, the average grain size of the dielectric grains is decreased, so that reliability can be improved. Accordingly, it is possible to provide the multilayer ceramic capacitor 1 that is excellent in reliability and capable of suppressing a decrease in capacitance.

[0049] The particle size of the dielectric grain is measured, for example, by observing the WT cross-section of the multilayer ceramic capacitor 1, which has been exposed by polishing, using a SEM.

[0050] It is preferable that the amount of Mn contained in the first-3-4 dielectric region R134 is smaller than the amount of Mn contained in the first-2-3 dielectric region R123. It is also preferable that the amount of Mn contained in the first-3-5 dielectric region R134 is smaller than the amount of Mn contained in the first-2-3 dielectric region R123.

[0051] This makes it possible to increase the D50 diameter of the dielectric grain in the first-third-fourth dielectric region R134, increase the D50 diameter of the dielectric grain in the first-third-fifth dielectric region R134, and decrease the D50 diameter of the dielectric grain in the first-second-third dielectric region R123.

[0052] The amount of Mn contained in the dielectric layer 4 is measured, for example, by analyzing the WT cross-section of the multilayer ceramic capacitor 1 exposed by polishing using energy-dispersive X-ray analysis (EDX).

[0053] (Method for manufacturing the multilayer ceramic capacitor 1) Next, a method for manufacturing the multilayer ceramic capacitor 1 according to the embodiment will be described.

[0054] (Dielectric layer fabrication process) First, a ceramic green sheet for the dielectric layer is created by forming a ceramic slurry into a sheet. The ceramic slurry is, for example, BaTiO 3 It contains barium titanate. Mn is added to the ceramic green sheet for the outer layer, which will become the outer layer 7A. The amount of Mn added to the ceramic green sheet for the outer layer is adjusted so that the molar ratio of Mn to Ti in the outer layer 7A is 0.005 or more and 0.010 or less. For example, it can contain 0.5 mol% to 1.0 mol% of Mn per 100 mol of Ti.

[0055] (Internal Electrode Printing Process) Next, a conductive paste for internal electrodes is printed onto the prepared ceramic green sheet for the dielectric layer. At this time, for example, the amount of organic components in the internal electrode paste is controlled, and the internal electrode paste printed on the ceramic sheet is changed layer by layer. This makes it possible to change the coverage of each internal electrode. Also, if the coverage of the internal electrode 5 is low, the thickness of the internal electrode 5 tends to become uneven. The shape of the dielectric layer 4 changes according to the shape of the dielectric layer 4 and the adjacent internal electrode 5. For this reason, if the coverage of the internal electrode 5 is low, the thickness variation of the internal electrode 5 and the adjacent dielectric layer 4 tends to increase.

[0056] (Outer layer lamination process) Next, outer layer ceramic green sheets, which will become the outer layer 7A, are stacked on both sides of the lamination direction T of the multiple laminated dielectric layer ceramic green sheets to form a mother block.

[0057] (Pressing process) Then, the created mother block is subjected to rigid pressing.

[0058] (Cutting process) The rigidly pressed mother block is cut to manufacture a rectangular stacked chip.

[0059] (Side gap formation process) Next, a ceramic slurry similar to that used for the dielectric layer is applied to a resin film and dried to produce a ceramic green sheet for the side gap. The ceramic green sheet for the side gap is attached to the side of the laminated chip where the internal electrodes 5 are exposed to form a layer that will become the side gap 70.

[0060] (Firing Process) The laminated chip, on which the side gap portion 70 is formed, is fired at a predetermined temperature to form the laminate 2. At this time, dielectric grains grow in each dielectric layer 4. In addition, Mn contained in the outer layer portion 7A diffuses into the dielectric layer through each internal electrode 5. Mn suppresses the grain growth of dielectric grains. Therefore, in dielectric layers 4 containing more Mn, the dielectric grain diameter becomes smaller, and the variation in dielectric grain diameter becomes smaller.

[0061] (External electrode layer formation process) (Underlayment electrode formation process) Next, using a dip method or the like, a paste for underlayment electrodes containing conductive metal and glass components, which will become the external electrodes 30, is applied to the end face C of the laminate 2. The paste for underlayment electrodes is also applied to the first surface F1, second surface F2, fifth surface F5, and sixth surface F6 of the laminate 2. After that, the laminate 2 to which the underlayment electrode paste has been applied is fired again at a predetermined temperature. Alternatively, the firing process S7 described above may be omitted, and the laminate chip and the underlayment electrodes 31 may be fired simultaneously in the firing process after this external electrode layer formation process S8.

[0062] A Ni plating layer 33a is formed on the surface of the base electrode 31. Furthermore, a Sn plating layer 33b is formed on the surface of the Ni plating layer 33a. Through these steps, the multilayer ceramic capacitor 1 of the embodiment is manufactured.

[0063] As a result of the above steps, the multilayer ceramic capacitor 1 shown in Figure 1 is obtained.

[0064] <Effects according to the embodiment> The multilayer ceramic capacitor 1 of the above embodiment can be obtained as follows.

[0065] According to the above embodiment, the region between the first-first internal electrode 511 and the first surface F1 contains Mn. The coverage of the first-second internal electrode 512 is lower than the coverage of the first-third internal electrode 513.

[0066] In the dielectric layer 4, if the particle size of the dielectric grain increases, the insulation resistance of the dielectric layer 4 decreases, which may reduce reliability. However, with this configuration, by lowering the coverage of the first-second internal electrodes 512, Mn can be more easily transmitted through the first-second internal electrodes 512. Therefore, the amount of Mn present in the region between the first-second internal electrodes 512 and the first-third internal electrodes 513 can be increased. Mn suppresses the grain growth of dielectric grain. Therefore, grain growth of dielectric grain can be suppressed in the region between the first-second internal electrodes 512 and the first-third internal electrodes 513. Furthermore, the region between the first-second internal electrodes 512 and the first-third internal electrodes 513 is located relatively close to the surface of the laminate 2. Therefore, by improving the reliability of the region between the first-second internal electrodes 512 and the first-first internal electrode 511, the reliability of the multilayer ceramic capacitor 1 can be suitably improved. Thus, a multilayer ceramic capacitor 1 with excellent reliability can be provided.

[0067] On the other hand, in the dielectric layer 4, if the particle size of the dielectric grain becomes small, there is a risk that the capacitance will decrease. However, with this configuration, by increasing the coverage of the first to third internal electrodes 513, it is possible to suppress Mn from penetrating too far into the interior of the laminate 2. As a result, it is possible to suppress the particle size of the dielectric grain from becoming too small, and thus suppress the decrease in capacitance.

[0068] Preferably, the coverage of the first-first internal electrode 511 is higher than the coverage of the first-second internal electrode 512.

[0069] By reducing the coverage of the first and second internal electrodes 512, Mn can be more easily transmitted through the first and second internal electrodes 512, thereby ensuring a sufficient supply of Mn to the region between the first and second internal electrodes 512 and the first and third internal electrodes 513.

[0070] The region between the first-first internal electrode 511 and the first-second internal electrode 512 is close to the region between the first-first internal electrode 511 and the first surface F1, so it is considered that Mn can be supplied sufficiently even when the coverage of the first-first internal electrode 511 is relatively high. For this reason, by making the coverage of the first-first internal electrode 511 relatively high, it is possible to suppress the decrease in capacitance caused by the low coverage of the internal electrode 5 while ensuring reliability.

[0071] Preferably, the coverage of the first-third internal electrode 513 is higher than the coverage of the first-first internal electrode 511.

[0072] With this configuration, by increasing the coverage of the first to third internal electrodes 513, Mn can be more easily transmitted through the first to third internal electrodes 513, thereby ensuring a sufficient amount of Mn in the region between the first to second internal electrodes 512 and the first to third internal electrodes 513.

[0073] Furthermore, by preventing the coverage of the first internal electrode 511 from becoming too high, it is possible to ensure that Mn is sufficiently supplied to the interior of the inner layer 6.

[0074] Preferably, the coverage of the first-fourth internal electrode 514 is higher than the coverage of the first-second internal electrode 512, and preferably, the coverage of the first-fifth internal electrode 515 is higher than the coverage of the first-second internal electrode 512.

[0075] With this configuration, by lowering the coverage of the first and second internal electrodes 512, it becomes easier to sufficiently supply Mn into the interior of the inner layer 6.

[0076] Furthermore, by increasing the coverage of the first to fourth internal electrodes 514 and the first to fifth internal electrodes 515, it is possible to suppress the decrease in capacitance caused by too much Mn entering the center of the inner layer 6.

[0077] It is preferable that the thickness variation of the first-3-4 dielectric region R134 is smaller than the thickness variation of the first-2-3 dielectric region R123.

[0078] Since the first-third-fourth dielectric region R134 is located relatively close to the center of the inner layer 6, it is thought that Mn has difficulty reaching it, and the particle size of the dielectric grain tends to increase. However, by making the thickness of the dielectric layer 4 more uniform, the areas in which the dielectric layer 4 becomes too thin in certain parts are reduced, and thus the decrease in insulation resistance can be suppressed. Therefore, with this configuration, the reliability of the first-third-fourth dielectric region R134 can be improved by reducing the thickness variation of the first-third-fourth dielectric region R134.

[0079] On the other hand, in this embodiment, Mn tends to accumulate relatively easily in the first-2-3 dielectric region R123, so the grain size tends to be small. Therefore, even if there is a relatively large variation in the thickness of the dielectric layer 4 in the first-2-3 dielectric region R123, the small grain size ensures sufficient reliability.

[0080] It is preferable that the thickness variation of the first-1-2 dielectric region R112 is smaller than the thickness variation of the first-2-3 dielectric region R123.

[0081] With this configuration, by reducing the thickness variation of the first-1-2 dielectric region R112, reliability can be suitably improved in the first-1-2 dielectric region R112, which is located at a smaller distance from the surface of the laminate 2.

[0082] It is preferable that the thickness variation of the first-1-2 dielectric region R112 is smaller than the thickness variation of the first-3-4 dielectric region R134.

[0083] With this configuration, by reducing the thickness variation of the first-1-2 dielectric region R112, reliability can be suitably improved in the first-1-2 dielectric region R112, which is located at a smaller distance from the surface of the laminate 2.

[0084] It is preferable that the thickness variation of the first-fourth-fifth dielectric region R145 is smaller than the thickness variation of the first-twoth-third dielectric region R123.

[0085] With this configuration, by reducing the thickness variation of the first-4-5 dielectric region R145, reliability can be suitably improved in the first-4-5 dielectric region R145, where the distance from the surface of the laminate 2 is greater and the particle size of the dielectric grain tends to be larger.

[0086] The present invention is not limited to the configuration of the above embodiments, and can be modified and applied as appropriate without altering the essence of the invention. Furthermore, a combination of two or more of the desirable configurations described in the above embodiments also constitutes the present invention.

[0087] For example, the shape of the internal electrode 5 is not limited to the shape described above. For example, as shown in Figures 6A and 6B, the shape of the lead portion 51 of the first internal electrode 5A31 may be a tapered shape such that the length in the second direction W narrows toward the third surface F3, and the shape of the lead portion 51 of the second internal electrode 5B may be a tapered shape such that the length in the second direction W narrows toward the fourth surface F4.

[0088] The configuration of the external electrode 30 is not limited to the configuration described above. For example, the conductive metal included in the base electrode 31 is not limited to Cu, but may be Ni, Ag, Pd, Au, Ag-Pd alloy, etc. The base electrode 31 may also contain ceramic powder as a co-material. The external electrode 30 may have a base electrode 31 containing Ni and a co-material. The base electrode 31 containing Ni and a co-material may be provided in place of the base electrode 31 containing Cu and a glass component in an external electrode 30 having a base electrode 31 containing Cu and a glass component, a Ni plating layer 33a, and a Sn plating layer 33b, or it may be provided in addition to the base electrode 31 containing Cu and a glass component.

[0089] The external electrode 30 may have a resin layer containing conductive particles and a thermosetting resin. The resin layer is formed by applying a conductive paste containing conductive particles and a thermosetting resin to the base electrode 31 or laminate 2 and then heat-treating it.

[0090] The external electrode 30 may include, for example, a base electrode 31 containing Cu and a glass component, a resin layer formed on the base electrode 31, a Ni plating layer 33a formed on the resin layer, and a Sn plating layer 33b formed on the Ni plating layer 33a. The resin layer may be formed directly on the laminate 2, or it may be provided in place of the base electrode 31. There may be multiple resin layers.

[0091] The base electrode 31 may be a thin film layer of 1 μm or less in thickness, formed by a thin film formation method such as sputtering or vapor deposition, and in which metal particles are deposited.

[0092] The external electrode 30 may be a plated electrode formed only of a plating layer without providing an underlayer electrode 31. In that case, the plating layer is formed directly on the surface of the laminate 2 and is directly electrically connected to the internal electrode 5. When the external electrode 30 has such a structure, a catalyst may be placed on the surface of the laminate 2 as a pretreatment before the plating layer is formed.

[0093] The plating electrode, which is a plating electrode, preferably includes a lower plating layer formed on the surface of the laminate 2 and an upper plating layer formed on the surface of the lower plating layer. The lower plating layer is preferably formed using Ni, which has solder barrier properties. However, if the internal electrode 5 is formed using Ni, the lower plating layer is preferably formed using Cu, which has good bonding properties with Ni. The upper plating layer is preferably formed using Sn or Au, which has good solder wettability. The upper plating layer may be formed as needed.

[0094] The configuration of the external electrode 30 is not limited to the configuration described above and can be changed as appropriate. The external electrode 30 may be a combination of two or more of the above-described configurations.

[0095] (Experimental Example) 1. Manufacturing of Multilayer Ceramic Capacitors [Example] A multilayer ceramic capacitor having the same structure as the multilayer ceramic capacitor 1 described above (structure shown in Figures 1 to 3) was manufactured by the manufacturing method according to the embodiment described above. The dimensions of the multilayer ceramic capacitor were set to L × W × T = 1.0 mm × 0.5 mm × 0.8 mm. The main component of the internal electrodes was Ni, and the main component of the dielectric layer was BaTiO 3 The number of multilayer ceramic capacitors in the example was set to 10. The thickness of the dielectric region was set to 0.40 μm or more and 0.5 μm or less. The capacitance was adjusted to 47 μF.

[0096] [Comparative Example] A comparative multilayer ceramic capacitor was fabricated by changing the coverage of the internal electrodes and the thickness variation of the dielectric region from those in the example. The number of comparative multilayer ceramic capacitors was set to 10.

[0097] 2. Evaluation [Coverage] The coverage of the first-1st internal electrode, the first-2nd internal electrode, the first-3rd internal electrode, the first-4th internal electrode, and the first-5th internal electrode were measured using the measurement method according to the embodiment described above. At this time, the observation field was set so that the dimension in the direction perpendicular to the stacking direction T was 15 μm.

[0098] [Thickness Variation] The thickness variation of the 1-1-2 dielectric region, the 1-2-3 dielectric region, the 1-3-4 dielectric region, the 1-4-5 dielectric region, and the 1-5-6 dielectric region (described later) were measured using the measurement method according to the embodiment described above. At this time, the observation field was set so that the dimension in the direction perpendicular to the stacking direction T was 15 μm.

[0099] Furthermore, the term "1st-5th-6th dielectric region" refers to the portion of the dielectric layer sandwiched between the 1st-5th internal electrode and the 1st-6th internal electrode, where the 1st-6th internal electrode is defined as the internal electrode that is adjacent to the 1st-5th internal electrode in the stacking direction and is located on the 2nd surface F2 side of the 1st-5th internal electrode.

[0100] [Insulation Resistance Value] The insulation resistance of multilayer ceramic capacitors was measured. A DC 2.5V ripple current was applied between the external electrodes, and the leakage current after 60 seconds was measured using R8340A (manufactured by ADC Corporation). The insulation resistance value was calculated by taking the ratio of the measured leakage current to the applied voltage. The average value of 10 samples was used as the insulation resistance value for each example and comparative example.

[0101] If the insulation resistance value was less than 10 MΩ, it was evaluated as "poor," and if the insulation resistance value was 10 MΩ or more, it was evaluated as "good."

[0102] Table 1 shows the measurement results for coverage, insulation resistance, and evaluation. Table 2 shows the measurement results for thickness variation, insulation resistance, and evaluation.

[0103]

[0104]

[0105] 3. Results Table 1 shows that good results can be obtained when the coverage of the 1st-2nd internal electrode is lower than the coverage of the 1st-3rd internal electrode, the coverage of the 1st-1st internal electrode is higher than the coverage of the 1st-2nd internal electrode, the coverage of the 1st-3rd internal electrode is higher than the coverage of the 1st-1st internal electrode, the coverage of the 1st-4th internal electrode is higher than the coverage of the 1st-2nd internal electrode, and the coverage of the 1st-5th internal electrode is higher than the coverage of the 1st-2nd internal electrode.

[0106] From the results shown in Table 2, it can be seen that good results are obtained when the thickness variation of dielectric region 1-3-4 is smaller than that of dielectric region 1-2-3, the thickness variation of dielectric region 1-1-2 is smaller than that of dielectric region 1-2-3, the thickness variation of dielectric region 1-1-2 is smaller than that of dielectric region 1-3-4, and the thickness variation of dielectric region 1-4-5 is smaller than that of dielectric region 1-2-3.

[0107] 1 Multilayer ceramic capacitor 2 Laminate 4 Dielectric layer 5 Internal electrode 7A Outer layer (region between the 1st-1st internal electrode and the 1st surface) 511 1st-1st internal electrode 512 1st-2nd internal electrode 513 1st-3rd internal electrode 514 1st-4th internal electrode 515 1st-5th internal electrode F1 1st surface F2 2nd surface F3 3rd surface F4 4th surface F5 5th surface F6 6th surface R112 1st-1-2nd dielectric region (part of the dielectric layer sandwiched between the 1st-1st internal electrode and the 1st-2nd internal electrode) R123 1st-2-3rd dielectric region (part of the dielectric layer sandwiched between the 1st-2nd internal electrode and the 1st-3rd internal electrode) R134 1st-3-4th dielectric region (part of the dielectric layer sandwiched between the 1st-3rd internal electrode and the 1st-4th internal electrode) R145 Dielectric regions 1-4-5 (the portion of the dielectric layer sandwiched between internal electrodes 1-4 and 1-5)

Claims

1. A multilayer ceramic capacitor comprising: a laminate comprising a plurality of stacked dielectric layers and a plurality of internal electrodes; a first and second surface facing each other in the stacking direction; a third and fourth surface facing each other in a first direction perpendicular to the stacking direction; and a fifth and sixth surface facing each other in a second direction perpendicular to the stacking direction and the first direction; a first external electrode disposed on the third surface; and a second external electrode disposed on the fourth surface, wherein the internal electrode disposed on the first surface side of the plurality of internal electrodes is designated as the 1-1 internal electrode; the internal electrode adjacent to the 1-1 internal electrode in the stacking direction is designated as the 1-2 internal electrode; and the internal electrode adjacent to the 1-2 internal electrode in the stacking direction and located on the second surface side of the 1-2 internal electrode is designated as the 1-3 internal electrode; the region between the 1-1 internal electrode and the first surface contains Mn; and the coverage of the 1-2 internal electrode is lower than the coverage of the 1-3 internal electrode.

2. The multilayer ceramic capacitor according to claim 1, wherein the coverage of the first-1 internal electrode is higher than the coverage of the first-2 internal electrode.

3. The multilayer ceramic capacitor according to claim 1 or 2, wherein the coverage of the first to third internal electrodes is higher than the coverage of the first to first internal electrode.

4. The multilayer ceramic capacitor according to any one of claims 1 to 3, wherein the internal electrode adjacent to the first-third internal electrode in the stacking direction and located on the second plane side of the first-third internal electrode is designated as the first-fourth internal electrode, and the internal electrode adjacent to the first-fourth internal electrode in the stacking direction and located on the second plane side of the first-fourth internal electrode is designated as the first-fifth internal electrode, wherein the coverage of the first-fourth internal electrode is higher than the coverage of the first-second internal electrode, and the coverage of the first-fifth internal electrode is higher than the coverage of the first-second internal electrode.

5. The multilayer ceramic capacitor according to claims 1 to 4, wherein the thickness variation of the portion of the dielectric layer sandwiched between the first-third internal electrodes and the first-fourth internal electrodes is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-second internal electrodes and the first-third internal electrodes.

6. The multilayer ceramic capacitor according to claims 1 to 5, wherein the thickness variation of the portion of the dielectric layer sandwiched between the 1-1 internal electrode and the 1-2 internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the 1-2 internal electrode and the 1-3 internal electrode.

7. The multilayer ceramic capacitor according to claims 1 to 6, wherein the internal electrode adjacent to the first to third internal electrodes in the stacking direction and located on the second surface side of the first to third internal electrode is designated as the first to fourth internal electrode, and the thickness variation of the portion of the dielectric layer sandwiched between the first to first internal electrode and the first to second internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first to third internal electrode and the first to fourth internal electrode.

8. The multilayer ceramic capacitor according to claims 1 to 7, wherein the thickness variation of the portion of the dielectric layer sandwiched between the first-fourth internal electrode and the first-fifth internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-two internal electrode and the first-third internal electrode.

9. A laminate comprising a plurality of stacked dielectric layers and a plurality of internal electrodes, a first and second surface facing each other in the stacking direction, a third and fourth surface facing each other in a first direction perpendicular to the stacking direction, and a fifth and sixth surface facing each other in a second direction perpendicular to the stacking direction and the first direction, a first external electrode disposed on the third surface, and a second external electrode disposed on the fourth surface, wherein the internal electrode disposed on the first surface side of the plurality of internal electrodes is designated as the 1-1 internal electrode, the internal electrode adjacent to the 1-1 internal electrode in the stacking direction is designated as the 1-2 internal electrode, the internal electrode adjacent to the 1-2 internal electrode in the stacking direction and located on the second surface side of the 1-2 internal electrode is designated as the 1-3 internal electrode, and the internal electrode adjacent to the 1-3 internal electrode in the stacking direction and located on the second surface side of the 1-3 internal electrode is designated as the 1-4 internal electrode, A multilayer ceramic capacitor wherein the region between the first-1 internal electrode and the first surface contains Mn, and the thickness variation of the portion of the dielectric layer sandwiched between the first-3 internal electrode and the first-4 internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-2 internal electrode and the first-3 internal electrode.

10. The multilayer ceramic capacitor according to claim 9, wherein the thickness variation of the dielectric layer sandwiched between the first-1 internal electrode and the first-2 internal electrode is smaller than the thickness variation of the dielectric layer sandwiched between the first-2 internal electrode and the first-3 internal electrode.

11. The multilayer ceramic capacitor according to claim 9 or 10, wherein the thickness variation of the portion of the dielectric layer sandwiched between the first-1 internal electrode and the first-2 internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-3 internal electrode and the first-4 internal electrode.

12. The multilayer ceramic capacitor according to claim 9 or 11, wherein the thickness variation of the portion of the dielectric layer sandwiched between the first-fourth internal electrode and the first-fifth internal electrode is smaller than the thickness variation of the portion of the dielectric layer sandwiched between the first-two internal electrode and the first-third internal electrode.