Use of polyester having alicyclic structure

A resin composition combining biodegradable resin with alicyclic polyester improves melt strength and elasticity, addressing the molding challenges of biodegradable plastics by enhancing their melt strength and enabling better molding processes.

WO2026234860A1PCT designated stage Publication Date: 2026-11-12LAWTER INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2025/080063
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Biodegradable plastics like polylactic acid lack sufficient melt strength for molding processes such as blow-molding and inflation-molding, and existing compositions with non-reactive melt strength additives or aliphatic polyester resins have insufficient melt strength for molding applications.

Method used

A resin composition comprising biodegradable resin and polyester with an alicyclic structure, where the polyester has a melt viscosity of 60 to 3,000 mPa·s, enhancing the melt strength and elasticity of the biodegradable resin.

Benefits of technology

The composition enables improved molding processes, particularly for large elongation applications like blow-molding and inflation-molding, with enhanced melt strength and dimensional stability of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IMGF000027_0001_TABLE
    Figure IMGF000027_0001_TABLE
Patent Text Reader

Abstract

The present invention mainly relates to a use of (b) polyester having alicyclic structure(s) in order to enhance the melt strength of (a) biodegradable resin, wherein the melt viscosity of the (b) polyester at 195°C is from 60 to 3,000 mPa·s. The present invention also relates to a resin composition, comprising: (a) biodegradable resin; and (b) polyester having alicyclic structure(s), wherein the melt viscosity of the (b) polyester at 195°C is from 60 to 3,000 mPa·s. The present invention can enhance the melt strength of the (a) biodegradable resin, and can enhance the molding processability of the (a) biodegradable resin.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] DESCRIPTION

[0002] TITLE OF INVENTION USE OF POLYESTER HAVING ALICYCLIC STRUCTURE TECHNICAL FIELD

[0003] The present invention relates to a use of polyester(s) with alicyclic structure(s), exhibiting a specific melt viscosity range.

[0004] BACKGROUND ART

[0005] Plastics made from synthetic resins have been widely used in various fields such as molded products, films, sheets, bags, and fibers, due to excellent mechanical properties and easy processability. However, environmental pollutions by plastics have become recent problems. For example, there are problems related to plastic product waste entering the ocean after use. The plastics coming into ocean may become small particles (microplastics) due to the action of winds, waves and the like. It is believed that usual plastics are not decomposed semi¬ permanently, even after becoming microplastics, and will remain in the ocean. Consequently, sea creatures such as fish may accidentally ingest such microplastics, which can negatively impact the ecosystem.

[0006] As one of the means to solve such problems, biodegradable plastics are drawing attention.

[0007] Biodegradable plastics are decomposed by the action of microorganisms in the natural world, and have little environmental impact. Thus, biodegradable plastics are expected to become an alternative for conventional plastics which have no biodegradability (non-biodegradable plastics). As a representative of such biodegradable plastics, mention may be made of polylactic acid.

[0008] However, polylactic acid has insufficient melt strength at a high temperature, and therefore, it is difficult to perform molding which needs large elongation of materials, such as molding a bottle by blow-molding and the like, and manufacturing a bag by inflation-molding.

[0009] JP-T-2011-516718 discloses, as a plastic composition which includes polylactic acid and may be subjected to blow-molding, a polymer composition including polylactic acid, polyolefin, and a non-reactive melt strength enhancing additive.

[0010] However, the non-reactive melt strength enhancing additive is limited to (meth)acrylic copolymers. In addition, the polymer composition disclosed in JP-T-2011-516718 includes a large amount of polyolefin which is derived from petroleum and is non-biodegradable, and therefore, there is room for improvement in terms of reducing environmental impacts.

[0011] JP-A-2023-140314 discloses, as a biodegradable plastic composition for which hydrolysis by compost treatments may be promoted while unintentional decompositions of molded products may be suppressed, a composition including (A) a rosin-based resin, and (B) an aliphatic polyester resin including (bl) constitutional units derived from aliphatic diols and (b2) constitutional units derived from aliphatic dicarboxylic acids.However, the composition disclosed in JP-A-2023-140314 has insufficient melt strength when being subjected to molding.

[0012] DISCLOSURE OF INVENTION

[0013] In view of the above circumstance, an objective of the present invention is to provide a resin composition comprising biodegradable resin(s), having enhanced melt strength which is preferable for molding.

[0014] As a result of diligent studies, the inventors discovered that a resin composition comprising biodegradable resin(s), having enhanced melt strength which is preferable for molding, can be obtained by mixing at least one biodegradable resin and at least one polyester having at least one alicyclic structure, wherein the polyester has a specific range of melt viscosity, thereby completing the present invention.

[0015] The objective of the present invention can be achieved by a resin composition comprising:

[0016] (a) at least one biodegradable resin; and

[0017] (b) at least one polyester having at least one alicyclic structure,

[0018] wherein

[0019] the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0020] The first aspect [1] of the present invention relates to a resin composition, comprising:

[0021] (a) at least one biodegradable resin; and

[0022] (b) at least one polyester having at least one alicyclic structure,

[0023] wherein

[0024] the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0025] The first aspect [1] of the present invention encompasses the following embodiments.

[0026] [2] The resin composition according to [1], wherein the (a) biodegradable resin is meltable.

[0027] [3] The resin composition according to [1] or [2], wherein the (a) biodegradable resin is derived from biomass.

[0028] [4] The resin composition according to any one of [1] to [3], wherein the (a) biodegradable resin is selected from the group consisting of polylactic acid, polycaprolactone, polyhydroxyalkanoate, polybutylene succinate, modified starch, polybutylene adipate terephthalate, cellulose acetate, polyvinyl alcohol, polyglycolic acid, polybutylene succinate-co-adipate, polyethylene terephthalate succinate, and mixtures thereof.

[0029] [5] The resin composition according to any one of [1] to [4], wherein the amount of the (a) biodegradable resin(s) in the resin composition ranges from 50% to 99% by mass, preferably from 70% to 98.5% by mass, more preferably from 80% to 98% by mass, and even more preferably from 90% to 98% by mass, relative to the total mass of the composition.

[0030] [6] The resin composition according to any one of [1] to [5], wherein the melt viscosity at 195 °C of the (b) polyester is from 200 to 2,000 mPa's, preferably from 350 to 1,500 mPa’s, more preferably from 500 to 1,200 mPa's, and even more preferably from 600 to 1,000 mPa·s.

[0031] [7] The resin composition according to any one of [1] to [6], wherein the methanol tolerance at 25 °C ofthe (b) polyester is 250 g or less, preferably 200 g or less, more preferably 150 g or less, and even more preferably 100 g or less.

[0032] [8] The resin composition according to any one of [1] to [7], wherein the acid value of the (b) polyester is 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and more preferably 15 mgKOH / g or more.

[0033] [9] The resin composition according to any one of [1] to [8], wherein the hydroxyl value of the (b) polyester is less than 32 mgKOH / g, preferably less than 30 mgKOH / g, and more preferably less than 28 mgKOH / g or more than 60 mgKOH / g, preferably more than 65 mgKOH / g, and more preferably more than 70 mgKOH / g.

[0034]

[0010] The resin composition according to any one of [1] to [9], wherein the weight-average molecular weight of the (b) polyester is from 1,000 to 9,000, preferably from 1,500 to 8,000, and more preferably from 2,000 to 7,000.

[0035]

[0011] The resin composition according to any one of [1] to

[0010] , wherein the (b) polyester is selected from rosin-modified polyesters.

[0036]

[0012] The resin composition according to any one of

[0001] to

[0011] , wherein the amount of the (b) polyester(s) in the resin composition ranges from 0.1% to 20% by mass, preferably from 0.5% to 10% by mass, and more preferably from 1% to 5% by mass, relative to the total mass of the composition. The second aspect

[0013] of the present invention relates to a molded product comprising the resin composition according to any one of [1] to

[0012] ,

[0037] The third aspect

[0014] of the present invention relates to a process for producing a resin composition having a melt strength higher than the melt strength of (a) biodegradable resin(s), comprising the step of:

[0038] mixing the (a) biodegradable resin with (b) at least one polyester having at least one alicyclic structure to obtain the resin composition, wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0039] The fourth aspect

[0015] of the present invention relates to a use of (b) at least one polyester having at least one alicyclic structure in order to enhance the melt strength of (a) biodegradable resin(s), wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa’s.

[0040] The fifth aspect

[0016] of the present invention relates to an enhancer for the melt strength of (a) biodegradable resin(s), comprising (b) at least one polyester having at least one alicyclic structure wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0041] According to the present invention, the melt strength as well as melt elasticity of the (a) biodegradable resin can be enhanced, and therefore, the molding processability of the (a) biodegradable resin can be improved. For example, it is possible to perform by the present invention more easily molding which needs large elongation of materials, such as molding a bottle by blow-molding and the like, and manufacturing a bag by inflation-molding, by using (a) biodegradable resin(s). In addition, it is possible to improve dimensional stability of a molded product including the (a) biodegradable resin by the present invention.

[0042] BEST MODE FOR CARRYING OUT THE INVENTIONThe present invention is characterized by the use of (b) at least one polyester having at least one alicyclic structure, wherein the melt viscosity at 195 °C of the (b) polyester is from 60 to 3,000 mPa·s, in order to enhance the melt strength of (a) biodegradable resin(s). In the specification, the phrase “enhance the melt strength of (a) biodegradable resin(s)” means to provide a resin composition having the melt strength which is higher than the melt strength of the (a) biodegradable resin, by combining the (a) biodegradable resin(s) with the (b) polyester and the like.

[0043] It is possible to obtain a resin composition having excellent melt strength, comprising (a) biodegradable resin(s) by using the (b) polyester(s) having alicyclic structure(s).

[0044] Although not intended to be bound by theory, the mechanism of the present invention is contemplated as follows.

[0045] Biodegradable resins can be decomposed by the action of microorganisms in the nature world to carbon dioxide and water. The chemical structures vulnerable to the action of microorganisms include ester bonds and ether bonds. In other words, biodegradable resins include many ester and ether bonds in their chemical structures. The ester and ether bonds include oxygen atoms, thereby the intermolecular forces of biodegradable resins when being molded (melted state) become relatively stronger, and resistance power against elongation works; thus, the melt strength of the biodegradable resins become insufficient.

[0046] According to the present invention, at least one polyester having at least one alicyclic structure is incorporated into biodegradable resin(s). The polyester having the alicyclic structure has high affinity with the ester and ether bonds in the biodegradable resin(s) because the polyester has ester bonds. Thus, the polyester can interact with the biodegradable resin(s), suppress the intermolecular forces among the biodegradable resin(s), reduce the resistance power against elongation, and enhance the melt strength of the biodegradable resin(s). In addition, the presence of the alicyclic structure which has low polarity can also contribute to the enhancement of the melt strength of the biodegradable resin(s) by suppressing the intermolecular forces among the biodegradable resin(s).

[0047] Hereinafter, each aspect of the present invention will be explained in a more detailed manner.

[0048] [Resin Composition]

[0049] The resin composition according to the present invention comprises:

[0050] (a) at least one biodegradable resin; and

[0051] (b) at least one polyester having at least one alicyclic structure,

[0052] wherein

[0053] the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0054] The resin composition according to the present invention has high melt strength and is preferable to molding because the resin composition includes, in combination with the (a) biodegradable resin(s), the (b) polyester(s) having alicyclic structure(s), wherein the melt viscosity at 195°C of the polyester(s) is from 60 to 3,000 mPa·s.

[0055] Hereinafter, the resin composition according to the present invention will be explained in a more detailed manner.< Biodegradable Resin>

[0056] The resin composition according to the present invention comprises (a) at least one biodegradable resin. The resin composition according to the present invention may comprise a single biodegradable resin or two or more biodegradable resins.

[0057] According to the present invention, the (a) biodegradable resin is different from the (b) polyester having alicyclic structure(s).

[0058] In the present invention, the “biodegradable resin” means a resin which is decomposable by the action of microorganisms in the natural world, finally to carbon dioxide and water.

[0059] It is preferable that the (a) biodegradable resin is derived from biomass. Here, “biomass” means reproducible resources derived from organism or living thing, and does not include exhaustible resources such as petroleum. As the biomass, plants or microorganisms as well as substances, such as starches, derived from these are preferable.

[0060] It is preferable that the (a) biodegradable resin is biodegradable plastics. Here, “biodegradable plastics” mean biodegradable resins other than elastomers.

[0061] It is preferable that the (a) biodegradable resin is meltable. In other words, it is preferable that the (a) biodegradable resin is thermoplastic.

[0062] As the (a) biodegradable resin, mention may be made of, for example, polylactic acid (PLA), poly caprolactone (PCL), polyhydroxyalkanoate (PHA), polybutylene succinate (PBS), modified starch, polybutylene adipate terephthalate (PBAT), cellulose acetate, polyvinyl alcohol (PVA), polyglycolic acid (PGA), polybutylene succinate-co-adipate (PBSA), polyethylene terephthalate succinate (PETS), and mixtures thereof.

[0063] As the polyhydroxyalkanoate, mention may be made of, for example, polyhydroxybutyrate (PHB), polyhydroxyhexanoate (PHH), polyhydroxyvalerate (PHV), poly(3-hydroxybutyrate-co- 3 -hydroxyhexanoate) (PHBH), poly(3-hydroxybutyrate-co-3 -hydroxyvalerate) (PHBV) and the like.

[0064] It is preferable that the (a) biodegradable resin is selected from the group consisting of polyesters, polyethers, and mixtures thereof.

[0065] It is more preferable that the (a) biodegradable resin is selected from the group consisting of polylactic acid (PLA), polyhydroxyalkanoate (PHA), modified starch, polybutylene adipate terephthalate (PBAT), and mixtures thereof.

[0066] As the (a) biodegradable resin, polylactic acid (PLA) is even more preferable. Polylactic acid can be produced from plants as raw materials, and has biodegradability; and therefore, polylactic acid is excellent in terms of reducing environmental impacts.

[0067] The resin composition according to the present invention may comprise the (a) biodegradable resin(s) in an amount of, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 90% by mass or more, relative to the total mass of the composition. On the other hand, the resin composition according to the present invention may comprise the (a) biodegradable resin(s) in an amount of, for example, 99%by mass or less, preferably 98.5% by mass or less, and more preferably 98% by mass or less, relative to the total mass of the composition. Thus, the resin composition according to the present invention may comprise the (a) biodegradable resin(s) in an amount of, for example, from 50% to 99% by mass, preferably from 70% to 98.5% by mass, more preferably from 80% to 98% by mass, and particularly preferably from 90% to 98% by mass, relative to the total mass of the composition.

[0068] < Polyester Having Alicyclic Structure>

[0069] The resin composition according to the present invention comprises (b) at least one polyester having at least one alicyclic structure. The resin composition according to the present invention may comprise a single polyester or two or more polyesters.

[0070] The (b) polyester having at least one alicyclic structure has at least one alicyclic structure in the chemical structure of the polyester.

[0071] In the present invention, the “alicyclic structure” means a chemical structure comprising one or more non-aromatic rings including carbon atoms. It is preferable that the non-aromatic ring is a saturated or unsaturated, carbocyclic or heterocyclic ring. The number of atoms forming the alicyclic structure is not limited, but 5 or 6 is preferable. Thus, it is preferable that the ring unit forming the alicyclic structure is a 5-membered ring or a 6-membered ring.

[0072] In the present invention, the “polyester” means a condensed polymer of one or more polyvalent carboxylic acids (polycarboxylic acids) and one or more polyvalent alcohols (polyols).

[0073] The resin composition according to the present invention can comprise any (b) polyester having alicyclic structure(s) as long as the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0074] The method to prepare the (b) polyester having alicyclic structure(s) is not limited. For example, the (b) polyester having alicyclic structure(s) can be prepared by polymerizing one or more polyvalent carboxylic acids and one or more polyvalent alcohols via dehydration condensation. In one embodiment, the (b) polyester having alicyclic structure(s) can be prepared by using, as raw materials, one or more polyvalent carboxylic acids having alicyclic structure(s) and / or one or more polyvalent alcohols having alicyclic structure(s).

[0075] In another embodiment, one or more monovalent carboxylic acids (monocarboxylic acids) and / or one or more monovalent alcohols (monoalcohols) may be used together when preparing the (b) polyester. The monovalent carboxylic acid can be introduced into a polyester by, for example, the dehydration condensation with the hydroxy group of the polyvalent alcohol. On the other hand, the monovalent alcohol can be introduced into a polyester by, for example, the dehydration condensation with the carboxy group of the polyvalent carboxylic acid.

[0076] Thus, even if both the polyvalent carboxylic acid(s) and the polyvalent alcohol(s) used to prepare a polyester have no alicyclic structure, the (b) polyester having alicyclic structure(s) can be prepared by using one or more monovalent carboxylic acids having alicyclic structure(s) and / or one or more monovalent alcohol having alicyclic structure(s).

[0077] As the polyvalent carboxylic acid, dicarboxylic acid is preferable. As the polyvalent alcohol,diol is preferable.

[0078] It is preferable to prepare the (b) polyester having alicyclic structure(s) by using at least one raw material selected from the group consisting of dicarboxylic acids having at least one alicyclic structure, diols having at least one alicyclic structure and monocarboxylic acids having at least one alicyclic structure.

[0079] It is more preferable to use rosins to prepare the (b) polyester having alicyclic structure(s).

[0080] (Dicarboxylic Acid Having Alicyclic Structure(s))

[0081] The dicaboxylic acids having alicyclic structure(s) are not limited as long as they include, in one molecule, one or more alicyclic structures and two carboxy groups, and they may be in the form of anhydrides.

[0082] As the dicarboxylic acid having alicyclic structure(s), mention may be made of, for example, chlorendic acid, norbomene dicarboxylic acid, dimer acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,2,3,6-tetrahydrophthalic acid, endomethylene- 1,2,3,6-tetrahydrophthalic acid, methyl-3,6-endomethylene- 1,2,3,6-tetrahydrophthalic acid, 1 -cyclopentene- 1,2-dicarboxy lie acid, methylcyclohexenedicarboxylic acid, methyl-5-norbornene-2,3-dicarboxylic acid, and the like, as well as anhydrides thereof. As the dicarboxylic acid having alicyclic structure(s), 1,2,3,6-tetrahydrophthalic anhydride is preferable.

[0083] It is possible to use a polymerized rosin, which is dimer of rosin, as the dicarboxylic acid having alicyclic structure(s). It is also possible to use, as dicarboxylic acids having alicyclic structure(s), a.p-unsaturated carboxylic acid-modified rosins, e.g., acrylated rosins, which are Diels- Alder reaction products of rosins having alicyclic structure(s) and a conjugated double bond with a, P- unsaturated carboxylic acid, such as acrylic acid, described below.

[0084] The content of the dicarboxylic acid(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic stmcture(s) may be, for example, 10 parts by mass or more, preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, and 80 parts by mass or less, preferably 70 parts by mass or less, and more preferably 60 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the dicarboxylic acid(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 10 to 80 parts by mass, preferably from 20 to 70 parts by mass, and more preferably from 30 to 60 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). (Diol Having Alicyclic Structure(s))

[0085] The diols having alicyclic structure(s) are not limited as long as they include, in one molecule, one or more alicyclic structures and two hydroxy groups.

[0086] As the diols having alicyclic structure(s), mention may be made of, for example, 1,2- cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediethanol, cyclopentadienedimethanol, hydrogenated bisphenol A (2,2’-bis(4-hydroxycyclohexyl)propane) and the like. As the diol having alicyclic structure(s), hydrogenated bisphenol A is preferable.The content of the diol(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 10 parts by mass or more, preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, and 80 parts by mass or less, preferably 70 parts by mass or less, and more preferably 60 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the diol(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 10 to 80 parts by mass, preferably from 20 to 70 parts by mass, and more preferably from 30 to 60 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0087] (Monocarboxylic Acid Having Alicyclic Structure(s))

[0088] The monocaboxylic acids having alicyclic structure(s) are not limited as long as they include, in one molecule, one or more alicyclic structures and one carboxy group.

[0089] As the monocarboxylic acid having alicyclic structure(s), mention may be made of, for example, rosins, monocarboxylic acids having cycloalkyl group(s).

[0090] As the rosins, mention may be made of, for example, non-modified rosins (unmodified rosins), modified rosins (rosin derivatives) and the like.

[0091] The non-modified rosins are natural resins including, as main ingredients, resin acids. Resin acids are compounds which are derived from trees and have carboxy group(s). Specifically, mention may be made of, for example, resin acids having a conjugated double bond, such as abietic acid, palustric acid, neoabietic acid, and levopimaric acid, as well as resin acids having no conjugated double bond, such as dehydroabietic acid, dihydroabietic acid, tetrahydroabietic acid, pimaric acid, and isopimaric acid.

[0092] As the non-modified rosins, more specifically, mention may be made of, for example, tall rosins, gum rosins, wood rosins and the like. Gum rosin is preferable as the non-modified rosin.

[0093] As the non-modified rosins, one non-modified rosin may be used. On the other hand, two or more non-modified rosins may be used in combination.

[0094] Modified rosins are denaturated products of the non-modified rosins. As examples, mention may be made of stabilization-treated rosins and the like.

[0095] Stabilization-treatments are treatments to reduce or eliminate the conjugated double bond(s) in the resin acids having the conjugated double bond(s). As the stabilization-treatments, specifically, mention may be made of, hydrogenation treatments, disproportionation treatments, and the like. As the stabilization-treated rosins, mention may be made of hydrogenated rosins obtained by hydrogenation treatments of non-modified rosins, disproportionated rosins obtained by disproportionation treatments of non-modified rosins, and the like.

[0096] As the modified rosins, one modified rosin may be used. On the other hand, two or more modified rosins may be used in combination.

[0097] It is preferable to use non-modified rosins, and more preferably gum rosins, as the rosins.As the rosins, one rosin may be used. On the other hand, two or more rosins may be used in combination.

[0098] As the monocarboxylic acids having cycloalkyl group(s), mention may be made of, for example, cyclopentanecarboxylic acid, cyclopentenecarboxylic acid, cyclohexanecarboxylic acid, cyclohexenecarboxylic acid, and the like.

[0099] As the monocarboxylic acids having alicyclic structure(s), rosins are preferable.

[0100] In addition, if the monocarboxylic acids having alicyclic structure(s) are rosins having a conjugated double bond, they may be converted into a.p-unsaturated carboxylic acid-modified rosins which are polycarboxylic acids and Diels-Alder reaction products of the rosins and a,|3- unsaturated carboxylic acids and anhydrides thereof, such as maleic acid, maleic anhydride, fumaric acid, and acrylic acid, described below. It is possible to introduce the alicyclic structure(s) into polyesters by the polycondensation of the a,p-unsaturated carboxylic acid-modified rosins and, for example, polyvalent alcohols.

[0101] The content of the monocarboxylic acid(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and more preferably 15 parts by mass or more, and 90 parts by mass or less, preferably 85 parts by mass or less, and more preferably 80 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the monocarboxylic acid(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 5 to 90 parts by mass, preferably from 10 to 85 parts by mass, and more preferably from 15 to 80 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0102] If the raw materials for the (b) polyester having alicyclic structure(s) include rosins in an amount range shown above, a resin composition with excellent melt strength can be obtained.

[0103] (Monoalcohol Having Alicyclic Structure(s))

[0104] The monoalcohol having alicyclic structure(s) is not limited as long as they include, in one molecule, one or more alicyclic structures and one hydroxy group.

[0105] As the monoalcohol having alicyclic structure(s), mention may be made of, for example, alicyclic monoalcohols such as cyclohexanol and cyclododecanol.

[0106] The content of the monoalcohol(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 5 parts by mass or more, preferably 7 parts by mass or more, and more preferably 9 parts by mass or more, and 80 parts by mass or less, preferably 70 parts by mass or less, and more preferably 60 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the monoalcohol(s) having alicyclic structure(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 5 to 80 parts by mass, preferably from 7 to 70 parts by mass, and more preferably from 9 to 60 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0107] (Other Ingredients)Any other carboxylic acid and / or any other alcohol may be used together in the preparation of the polyester. Another carboxylic acid may be introduced into the polyester by, for example, the Diels-Alder reaction and the dehydration condensation with the hydroxy group of the polyvalent alcohol. On the other hand, another alcohol can be introduced into the polyester by, for example, the dehydration condensation with the carboxy group of the polyvalent carboxylic acid.

[0108] Other Carboxylic Acids:

[0109] As the other carboxylic acids, except for the di- and mono-carboxylic acids having alicyclic structure(s), mention may be made of carboxylic acids having no alicyclic structure. A single type of the other carboxylic acid may be used alone, or two or more different types of the other carboxylic acids may be used in combination.

[0110] As the carboxylic acids having no alicyclic structure, mention may be made of mono- or polycarboxylic acids having no alicyclic structure.

[0111] As the monocarboxylic acid having no alicyclic structure, mention may be made of, for example, a, P-unsaturated mono-carboxylic acids such as acrylic acid,

[0112] aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, myristic acid, palmitic acid, and stearic acid, as well as aliphatic monocarboxylic acids derived from natural resources such as tall oil fatty acid, soy oil fatty acid, coconut oil fatty acid, and rice bran oil fatty acid, and

[0113] aromatic monocarboxylic acids such as benzoic acid, methylbenzoic acid, t-butylbenzoic acid, benzoylbenzoic acid, and naphtoic acid. As the monocarboxylic acid having no alicyclic structure, a,p-unsaturated mono-carboxylic acids and aliphatic monocarboxylic acids derived from natural resources are preferable, acrylic acid and tall oil fatty acid are more preferable, and tall oil fatty acid is even more preferable. One monocarboxylic acid having no alicyclic structure may be used. On the other hand, two or more monocarboxylic acids having no alicyclic structure may be used in combination.

[0114] As the polycarboxylic acid having no alicyclic structure, mention may be made of, for example, a,p-unsaturated di-carboxylic acids or anhydrides thereof, such as maleic acid, maleic anhydride, fumaric acid and the like,

[0115] aliphatic dicarboxylic acid such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, oxaloacetic acid, methylmalonic acid, dimethylmalonic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, methylglutaric acid, dimethyl glutaric acid, 1,3- acetonedicarboxylic acid, a-keto-glutaric acid, 2-oxo-adipic acid, 4-oxo-heptanedioic acid, 5- oxoazelaic acid and anhydrides thereof,

[0116] aromatic dicarboxylic acid such as phthalic acid, isophthalic acid, terephthalic acid, toluenedicarboxylic acid, 2,5-dimethylterephthalic acid, 2,2 ’-biphenyldicarboxylic acid, 4,4- biphenyldicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8 -naphthalenedicarboxy lie acid, diphenylmethane-4,4’-dicarboxylic acid, phenylindandicarboxylic acid, 1,2-azulenedicarboxylic acid, 1,3 -azulenedicarboxylic acid, 4,5- azulenedicarboxylic acid, 1,4-anthracenedicarboxylic acid, 1,5-anthracenedicarboxylic acid, 1,8- anthracenedicarboxylic acid, 2,3 -anthracenedicarboxylic acid, 1,2-phenanthrenedicarboxylic acid, 4,5-phenanthrenedicarboxylic acid, 3,9-perylenedicarboxylic acid, 4-methylphthalic acid, phenylmaleic acid, 2, 3 -diphenylmaleic acid, and anhydrides thereof, and

[0117] aromatic polycarboxylic acid such as trimellitic acid, pyromellitic acid, and anhydrides thereof.As the polycarboxylic acid having no alicyclic structure, maleic acid, maleic anhydride, and fumaric acid are preferable, maleic anhydride and fumaric acid are more preferable, and maleic anhydride is even more preferable. One polycarboxylic acid having no alicyclic structure may be used. On the other hand, two or more polycarboxylic acids having no alicyclic structure may be used in combination.

[0118] If the monocarboxylic acid having alicyclic structure(s) is a non-modified rosin, it is known that the above a,|3-unsaturated carboxylic acids or anhydrides thereof cause the Diels Alder reaction preferentially with resin acids having a conjugated double bold in the non-modified rosin to form u.p-unsaturated carboxylic acids-modified rosin. Thus, if the monocarboxylic acid having alicyclic structure(s) is a non-modified rosin, it is preferable to use a, P-unsaturated carboxylic acids or anhydrides thereof, as the other carboxylic acids.

[0119] In addition, among the other carboxylic acids, aromatic monocarboxylic acid having no alicyclic structure and aromatic polycarboxylic acids having no alicyclic structure are also preferable.

[0120] The content of the other carboxylic acid(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 1 parts by mass or more, preferably 2 parts by mass or more, and more preferably 5 parts by mass or more, and 50 parts by mass or less, preferably 30 parts by mass or less, and more preferably 15 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the other carboxylic acid(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 1 to 50 parts by mass, preferably from 2 to 30 parts by mass, and more preferably from 5 to 15 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0121] Other Alcohols:

[0122] As the other alcohols, except for the di- and mono-alcohols having alicyclic structure(s), mention may be made of alcohols having no alicyclic structure. A single type of the other alcohol may be used alone, or two or more different types of the other alcohols may be used in combination.

[0123] As the other alcohol, mention may be made of, for example,

[0124] monovalent alcohol such as methanol, ethanol, n-propanol, isopropanol, n-butanol, n-octylalcohol, 2-ethylhexylalcohol, decylalcohol, and lauryl alcohol,

[0125] divalent alcohol such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, propylene glycol, neopentyl glycol, and trimethylene glycol,

[0126] trivalent alcohol such as glycerin, trimethylolethane, and trimethylolpropane,

[0127] tetravalent alcohol such as pentaerythritol, diglycerin, and di(trimethyrolpropane), pentavalent alcohol such as triglycerol, and

[0128] hexavalent alcohol such as dipentaerythritol. As the other alcohol, divalent alcohol, trivalent alcohol, tetravalent alcohol are preferable; tetravalent alcohol is more preferable; and glycerin is even more preferable.

[0129] If the other alcohol is a polyvalent alcohol, polyvalent alcohols may be condensed each other. The content of the other alcohol(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 1 parts by mass or more, preferably 3 parts by mass or more, and more preferably 5 parts by mass or more, and 85 parts by mass or less, preferably 80 parts by mass or less, and more preferably 75 parts by mass or less, relative to 100 pars by mass of the totalraw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the other alcohol(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 1 to 85 parts by mass, preferably from 3 to 80 parts by mass, and more preferably from 5 to 75 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0130] (Epoxy Compounds)

[0131] The raw material for the (b) polyester having alicyclic structure(s) may comprise at least one epoxy compound.

[0132] As the epoxy compound, mention may be made of, for example, allyl glycidyl ether, phenol (EO) 5 glycidyl ether (CAS No. 54140-67-9), lauryl alcohol (EO) 15 glycidyl ether (CAS No. 86630-59-3), glycerol poly glycidyl ether, diglycerol polyglycidyl ether, poly glycerol poly glycidyl ether, sorbitol polyglycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, epoxy cresol novolak, and the like. One epoxy compound may be used. On the other hand, two or more epoxy compounds may be used in combination.

[0133] The content of the epoxy compound(s) in the raw materials for the (b) polyester having alicyclic structure(s) can be adjusted depending on the type, use purpose, and the like of the epoxy compound(s). In general, if an epoxy compound or epoxy compounds exist(s), 1 mole of epoxy groups can react with 1 mole of carboxy groups. If 1 mole of epoxy groups react with 1 mole of carboxy groups, 1 mole of ester bonds and 1 mole of hydroxy groups are formed in polyester(s). The formed 1 mole of hydroxy groups can further react with 1 mole of carboxy groups.

[0134] The content of the epoxy compound(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, 1 parts by mass or more, preferably 3 parts by mass or more, and more preferably 5 parts by mass or more, and 50 parts by mass or less, preferably 40 parts by mass or less, and more preferably 30 parts by mass or less, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s). Thus, the content of the epoxy compound(s) in the raw materials for the (b) polyester having alicyclic structure(s) may be, for example, from 1 to 50 parts by mass, preferably from 3 to 40 parts by mass, and more preferably from 5 to 30 parts by mass, relative to 100 pars by mass of the total raw materials for the (b) polyester having alicyclic structure(s).

[0135] It is preferable that the ratio of the total mole number of the hydroxy groups in all the alcohols (Y) including diol(s) having alicyclic stmcture(s) and the like, to the total mole number of the carboxy groups in all the carboxylic acids (X) including dicarboxylic acids having aliphatic structure(s) and the like, in the raw materials for the (b) polyester having alicyclic structure(s) [total mole number of hydroxy groups in the alcohols (Y) / total mole number of carboxy groups in the carboxylic acids (X)] (i.e., [OH group] / [COOH group]) is 0.70 or more, more preferably 0.80 or more, even more preferably 0.90 or more, and particularly preferably 0.99 or more. On the other hand, it is preferable that the ratio of the total mole number of the hydroxy groups in all the alcohols (Y) to the total mole number of the carboxy groups in all the carboxylic acids (X) [total mole number of hydroxy groups in the alcohols (Y) / total mole number of carboxy groups in the carboxylic acids (X)] is 1.40 or less, more preferably 1.30 or less, even more preferably 1.20 or less, and particularly preferably 1.10 or less. By controlling the above ratio within the above range, the hydroxy groups of the alcohols (Y) can be sufficiently esterified by the carboxy groups of the carboxylic acids (X), and the carboxy groups of the carboxylic acid (X) can be sufficientlyesterified by the hydroxy groups of the alcohols (Y), thereby increasing the esterification degree. By this, it is possible to introduce sufficient ester bonds into the (b) polyester having alicyclic structure(s), which can result in even better compatibility between the (b) polyester having alicyclic structure(s) and the (a) biodegradable resin, and to enhance further the melt strength of the resin composition according to the present invention.

[0136] (Preparation Method for Polyester Having Alicyclic Structure)

[0137] The (b) polyester having alicyclic structure(s) can be obtained by reacting the above raw materials with known methods (esterification reaction), as a reaction product.

[0138] The mode of the above reaction is not limited. For example, the reaction can be performed by mixing the above raw materials and heating them.

[0139] It is preferable to make the above raw materials react by esterification with no solvent. In this case, it is preferable to distill out the water, produced by the esterification reaction, in a known manner.

[0140] On the other hand, if necessary, the above raw materials may be reacted to esterify under the presence of solvent(s).

[0141] As the solvent, known organic solvents may be used without limitation. For example, mention may be made of, petroleum-based hydrocarbon solvents, aromatic hydrocarbon-based solvents, ketone-based solvents, ester-based solvents, aprotic polar solvents, and the like.

[0142] As the petroleum-based hydrocarbon solvents, mention may be made of, for example, hexane, mineral spirit, and the like.

[0143] As the aromatic hydrocarbon-based solvent, mention may be made of, for example, benzene, toluene, xylene and the like.

[0144] As the ketone-based solvent, mention may be made of, for example, acetone, methylethylketone, methylisobutylketone, diisobutylketone, cyclohexanone, and the like.

[0145] As the ester-based solvent, mention may be made of, for example, methyl acetate, ethyl acetate, butyl acetate, y-butyrolactone, propyleneglycol monomethylether acetate, and the like.

[0146] As the aprotic polar solvent, mention may be made of, for example, N, N-dimethylformamide, N, N-dimethylacetoamide, dimethylsulfoxide, N-methylpyrrolidone, pyridine, and the like.

[0147] One solvent may be used alone. On the other hand, two or more solvents may be used in combination.

[0148] As the solvent, a solvent which can be used for azeotropic distillation with water is preferable. Specifically, mention may be made of xylene, toluene, and the like. If a solvent which can be used for azeotropic distillation with water is used, the water produced by the esterification reaction of the raw materials can be distilled out.

[0149] The amount of solvent(s) is not limited, and may be adjusted appropriately depending on the purpose of use, and the like.After the reaction, the solvent can be removed by using a known method.

[0150] In the esterification reaction, if necessary, esterification catalyst(s) may be added.

[0151] The esterification catalyst is not limited, but mention may be made of organic acid, mineral acid, metal catalyst and the like.

[0152] As the organic acid, mention may be made of, for example, benzenesulfonic acid, p-toluenesulfonic acid, p-dodecylbenzenesulfonic acid, methanesulfonic acid, ethanesulfonic acid, trifluoromethylsulfuric acid, trifluoromethylacetic acid and the like.

[0153] As the mineral acid, mention may be made of, for example, sulfuric acid, hydrochloric acid, and the like.

[0154] As the metal catalyst, mention may be made of, for example tetrabutylzirconate, tetraisopropyltitanate, tetraisobutyltitanate, aluminum oxide, titanium oxide, magnesium oxide, magnesium hydroxide, magnesium acetate, calcium oxide, calcium hydroxide, calcium acetate, zinc oxide, zinc acetate, and the like.

[0155] One esterification catalyst may be used alone. On the other hand, two or more esterification catalysts may be used in combination.

[0156] The amount of esterification catalyst(s) is not limited, and may be adjusted appropriately depending on the purpose of use, and the like.

[0157] In the above esterification reaction, the method of mixing the raw materials is not limited, and therefore, the raw materials may be mixed at once, or may be mixed sequentially. In terms of productivity, it is preferable to mix the raw materials at once. If the raw materials include non¬ modified rosin and a,p-unsaturated carboxylic acid, it is preferable to separately perform the Diels- Alder reaction and the dehydration condensation reaction. In this case, the melt-strength of the resin composition can be further enhanced by performing each reaction separately.

[0158] Regarding the reaction conditions of the above esterification reaction, for example, in inert gas atmosphere and under atmospheric pressure, the reaction temperature may be, for example, 150°C or more, and preferably 200°C or more, while 280°C or less, and preferably 260°C or less, and the reaction time may be, for example, 4 hours or more, and preferably 6 hours or more, while 20 hours or less, and preferably 15 hours or less.

[0159] Thus, by the above esterification reaction, the (b) polyester having alicyclic structure(s) can be obtained as the reaction product.

[0160] Preferably, the reaction product of the raw materials is a rosin-modified polyester. In other words, it is preferable that the (b) polyester having alicyclic structure(s) is a rosin-modified polyester.

[0161] The rosin esters which are the reaction products of non-modified rosins, hydrogenated rosin or disproportionated rosins with polyvalent alcohols are not rosin-modified polyesters because the non-modified rosins, hydrogenated rosins and disproportionated rosins are not polyvalent carboxylic acids, and the rosin esters are not the reaction products of polyvalent carboxylic acidsand polyvalent alcohols. On the other hand, the reaction product of the above rosin ester and polyvalent carboxylic acid may be a rosin-modified polyester.

[0162] On the other hand, polymerized rosins and a, P-unsaturated carboxylic acid-modified rosins are polyvalent carboxylic acids, and therefore, the rosin esters which the reaction products of polymerized rosins or a, P-unsaturated carboxylic acid-modified rosins with polyvalent alcohols are rosin-modified polyesters.

[0163] Hereafter, the properties of the (b) polyester having alicyclic structure(s) are explained.

[0164] (Melt Viscosity)

[0165] The (b) polyester having alicyclic structure(s) used in the present invention has, under the atmospheric pressure, the melt viscosity at 195°C of from 60 to 3,000 mPa·s, preferably from 200 to 2,000 mPa’s, more preferably from 350 to 1,500 mPa's, even more preferably from 500 to 1,200mPa-s, and in particularly preferably from 600 to 1,000 mPa's. The lower limit of the melt viscosity at 195°C of the (b) polyester having alicyclic structure(s) may be, for example, 200 mPa's, 350 mPa-s, 500 mPa's, or 600 mPa·s. The upper limit of the melt viscosity at 195°C of the (b) polyester having alicyclic structure(s) may be, for example, 2,000 mPa’s, 1,500 mPa·s, 1,200 mPa-s, or 1,000 mPa-s.

[0166] If the melt viscosity at 195°C of the (b) polyester having alicyclic structure(s) is within from 60 to 3,000 mPa·s, it is possible to obtain a resin composition with high melt strength by mixing the (b) polyester having alicyclic structure(s) with the (a) biodegradable resin.

[0167] The melt viscosity at 195°C of the (b) polyester having alicyclic structure(s) can be measured by the following method.

[0168] Measurement Apparatus: Rheometer (MCR102 from Anton Paar)

[0169] Sample Amount: about 2 g

[0170] Measurement Method: A sample (polyester) is placed on a hotplate of the measurement apparatus to melt the sample completely by maintaining the sample for 3 minutes at 200°C under nitrogen atmosphere. A parallel plate PP25 (from Anton Paar) is attached to the measurement apparatus such that the gap (interval) between the parallel plate and the hot plate is set to be 0.5 mm.

[0171] Under nitrogen atmosphere, the parallel plate is rotated at shear rate of 50 / s for 1 minute at 200°C and bubbles in the sample are removed. Cooling is performed from 200°C to 150°C at the temperature of the hot plate for 930 seconds. The viscosity at 195°C is measured.

[0172] (Methanol Tolerance)

[0173] The methanol tolerance at 25°C of the (b) polyester having alicyclic structure(s) (5 g) used in the present invention may be, for example, 5 g or more, preferably 15 g or more, more preferably 25 g or more, and even more preferably 35 g or more. The methanol tolerance at 25°C of the (b) polyester having alicyclic stmcture(s) (5 g) may be, for example, 250 g or less, preferably 200 g or less, more preferably 150 g or less, and even more preferably 100 g or less. The methanol tolerance at 25°C of the (b) polyester having alicyclic structure(s) (5 g) at 25°C may be, for example, from 5 g to 250 g, preferably from 15 g to 200 g, more preferably from 25 g to 150 g, and more preferably from 35 g to 100 g.

[0174] If the methanol tolerance at 25°C of the (b) polyester having alicyclic structure(s) (5 g) is withinany of the above ranges, the (b) polyester having alicyclic structure(s) may provide a resin composition with excellent melt strength by being combined with the (a) biodegradable resin. The methanol tolerance at 25°C of the (b) polyester having alicyclic structure(s) (5 g) can be measured by the following method.

[0175] A standard solution is prepared by dissolving 5 g of the (b) polyester having alicyclic structure(s) in 50 mL of toluene in a transparent conical glass flask (volume 100 mL). Methanol is added dropwise to the standard solution at 25°C with stirring. The mass (g) of methanol added until the standard solution becomes clouded is determined. The mass (g) of methanol is defined as the methanol tolerance at 25°C of the (b) polyester having alicyclic structure(s). The timing of “the standard solution becomes clouded” is determined by the timing when the characters (10-point font size) printed on a newspaper cannot be recognized visually via the standard solution from a viewpoint above the newspaper, due to the clouding of the standard solution, under the conditions that the conical flask is put on the newspaper while the conical flask contacts with the newspaper. (Acid Value)

[0176] The acid value of the (b) polyester having alicyclic structure(s) used in the present invention may be, for example, 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and more preferably 15 mgKOH / g or more. The acid value of the (b) polyester having alicyclic structure(s) may be, for example, 60 mgKOH / g or less, preferably 50 mgKOH / g or less, more preferably 40 mgKOH / g or less, and even more preferably 35 mgKOH / g or less. The acid value of the (b) polyester having alicyclic structure(s) may be, for example, from 5 to 60 mgKOH / g, preferably from 10 to 50 mgKOH / g, more preferably from 15 to 40 mgKOH / g, and even more preferably from 15 to 35 mgKOH / g.

[0177] If the acid value of the (b) polyester having alicyclic structure(s) is within any of the above ranges, the (b) polyester having alicyclic structure(s) may provide a resin composition with excellent melt strength by being combined with the (a) biodegradable resin.

[0178] The acid value of the (b) polyester having alicyclic structure(s) can be measured by the following method, in accordance with JIS K0070 (1992).

[0179] 1 g of the (b) polyester having alicyclic structure(s) is dissolved in a 20 mL mixed solution of xylene and ethanol (xylene:ethanol = 2:1 (mass ratio)). Then, 3 mL of a phenolphthalein solution with a concentration of 3% by mass is added, as an indicator. Then, neutralization titration is performed by using a potassium hydroxide ethanol solution with a concentration of 0.1 mol / L to determine the acid value (mgKOH / g).

[0180] (Hydroxyl Value)

[0181] The hydroxyl value of the (b) polyester having alicyclic structure(s) used in the present invention may be, for example, less than 32 mgKOH / g, preferably less than 30 mgKOH / g, and more preferably less than 28 mgKOH / g, or more than 60 mgKOH / g, preferably more than 65 mgKOH / g, and more preferably more than 70 mgKOH / g.

[0182] If the hydroxyl value of the (b) polyester having alicyclic structure(s) is within any of the above ranges, the (b) polyester having alicyclic structure(s) may provide a resin composition with excellent melt strength by being combined with the (a) biodegradable resin.The hydroxyl value of the (b) polyester having alicyclic structure(s) can be measured in accordance with JIS K0070 (1992).

[0183] (Weight- Average Molecular Weight)

[0184] The weight-average molecular weight (standard polystyrene equivalent) of the (b) polyester having alicyclic structure(s) used in the present invention is not limited, but may be, for example, 1,000 or more, preferably 1,500 or more, more preferably 2,000 or more, and particularly preferably 2,300 or more. The weight-average molecular weight (standard polystyrene equivalent) of the (b) polyester having alicyclic structure(s) may be, for example, 9,000 or less, preferably 8,000 or less, more preferably 7,000 or less, and particularly preferably 6,000 or less. The weight-average molecular weight (standard polystyrene equivalent) of the (b) polyester having alicyclic structure(s) may be, for example, from 1,000 to 9,000, preferably from 1,500 to 8,000, more preferably from 2,000 to 7,000, and particularly preferably from 2,300 to 6,000.

[0185] If the weight-average molecular weight of the (b) polyester having alicyclic structure(s) is within any of the above ranges, the (b) polyester having alicyclic structure(s) may provide a resin composition with excellent melt strength by being combined with the (a) biodegradable resin. The weight-average molecular weight (mass-average molecular weight) of the (b) polyester having alicyclic structure(s) can be measured by the following method, in accordance with JIS K7252 (2016).

[0186] The (b) polyester having alicyclic structure(s) is dissolved in tetrahydrofuran to obtain a sample with a concentration of 1.0 g / L. Next, the chromatogram (chart) of the molecular weight distribution of the sample is obtained by gel permeation chromatography (GPC) using a refractive index detector (RID). Then, the weight-average molecular weight is determined from the obtained chromatogram (chart) using a calibration curve of standard polystyrene.

[0187] Measurement apparatuses and conditions are as follows.

[0188] Data-Processing Device: Agilent 1260 Infinity II (from Agilent)

[0189] Refractive Index Detector: RID (G7162A) in Agilent 1260 Infinity II

[0190] Column: PL gelmixed-B7.5×300mm (from Agilent) three columns

[0191] Mobile Phase: Tetrahydrofaran

[0192] Column Flow Rate: 1.0 ml / min

[0193] Sample Concentration: 1.0 g / L

[0194] Injection Amount: 10 pL

[0195] Measurement Temperature: 30°C

[0196] Molecular Weight Marker: Standard Polystyrene (EasiCal Polystyrene Standards PS-1) (from Agilent)

[0197] (Softening Point)

[0198] The softening point of the (b) polyester having alicyclic structure(s) used in the present invention may be, for example, 65°C or more, preferably 85°C or more, and more preferably 105°C or more. The softening point of the (b) polyester having alicyclic structure(s) may be, for example, less than 130°C, preferably 125°C or less, and more preferably 120°C or less. The softening point of the (b) polyester having alicyclic structure(s) may be, for example, 65°C or more and less than130°C, preferably from 85 to 125°C, and more preferably from 105 to 120°C.

[0199] The softening point can be measured in accordance with ASTM D3104.

[0200] The resin composition according to the present invention may comprise the (b) polyester having alicyclic structure(s) in an amount of, for example, 0.1% by mass or more, preferably 0.5% by mass or more, and more preferably 1% by mass or more, relative to the total mass of the composition. On the other hand, the resin composition according to the present invention may comprise the (b) polyester having alicyclic structure(s) in an amount of, for example, 20% by mass or less, preferably 10% by mass or less, and more preferably 5% by mass or less, relative to the total weight of the composition. Thus, the resin composition according to the present invention may comprise the (b) polyester having alicyclic structure(s) in an amount of, for example, from 0.1% to 20% by mass, preferably from 0.5% to 10% by mass, and more preferably from 1% to 5% by mass, relative to the total mass of the composition.

[0201] Preparation Method for Resin Composition>

[0202] The resin composition according to the present invention can be prepared by mixing the (a) biodegradable resin(s) and the (b) polyester(s) having alicyclic structure(s), wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa’s.

[0203] The method of mixing the (a) biodegradable resin(s) and the (b) polyester(s) having alicyclic structure(s) is not limited, and any conventional method may be used. Kneading using a kneader, an extruder and the like is preferable as the method of mixing.

[0204] The temperature when mixing the (a) biodegradable resin(s) and the (b) polyester(s) having alicyclic structure(s) is preferably 150°C or more and 250°C or less, and more preferably 170°C or more and 200°C or less. Homogeneous mixing of the ingredients may be difficult at a temperature of less than 150°C, and the ingredients may be decomposed at a temperature of more than 250°C.

[0205] If the (a) biodegradable resin(s) and the (b) polyester(s) having alicyclic structure(s) are kneaded by using an extruder, it is preferable for the rotating speed of the screw therein to be 20 rpm or more and 200 rpm or less, and more preferably 40 rpm or more and 100 rpm or less.

[0206] If the (a) biodegradable resin(s) and the (b) polyester(s) having alicyclic stmcture(s) are kneaded by using an extruder, it is preferable for the extruding speed therefrom to be 200 g / h or more and 1000 g / h or less, and more preferably 300 g / h or more and 600 g / h or less.

[0207] The mixing time may be appropriately adjusted depending on the amount of each ingredient, and may be, in general, 1 minute or more and less than 60 minutes.

[0208] The resin composition obtained after the mixing, may become in the form of a solid at room temperature by cooling. The method of cooling may be appropriately adjusted. For example, by immersing into water at from 1°C to 50°C, a solid resin composition may be obtained in a relatively short period of time.

[0209] The resin composition thus obtained may be dried, if necessary. The method of drying is not limited, and includes placing a drier at from 50°C to 100°C, reducing pressure, and the like. The drying time may be appropriately adjusted depending on the state of the resin composition, andmay be, in general, 10 minutes or more and less than 10 hours.

[0210] The resin composition according to the present invention may, if necessary, include a variety of additives, unless the effects of the present invention are inhibited. As the additives, mention may be made of, for example, antioxidants, photo-stabilizers, coloring inhibitors, mold releasing agents, antibacterial agents, flame retardants, conductivity imparting agents, damping agents, and the like.

[0211] The content of the above additive(s) in the resin composition according to the present invention is not limited, and may be, for example, 0.005 parts by mass or more, and preferably 0.01 parts by mass or more, or 5 parts by mass or less, and preferably 1 part by mass or less, relative to 100 parts by mass of the resin composition according to the present invention.

[0212] [Molded Product]

[0213] The present invention also relates to a molded product comprising the resin composition according to the present invention.

[0214] It is preferable that the molded product according to the present invention comprises the resin composition according to the present invention as a main ingredient. The ratio of the resin composition according to the present invention in the molded product according to the present invention is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, relative to the total mass of the molded product. It is, in particular, preferable that the molded product according to the present invention consists of the resin composition according to the present invention.

[0215] The molded product according to the present invention can be obtained by molding the resin composition according to the present invention by using known molding methods. The shape of the molded product according to the present invention is not limited, and mention may be made of, for example, a film, a sheet, a bag, a tube, a cylinder, a box and the like.

[0216] The molding method to obtain the molded product according to the present invention is not limited, and mention may be made of, for example, extrusion molding including extrusion coating, blow molding, extrusion blow molding, injection molding, film molding with stretching, inflation molding, press molding, insert molding, foam molding, transfer molding and the like. In particular, molding which needs large elongation of material(s), such as molding a bottle by blow molding and the like, and molding a bag by inflation molding and the like, can be easily performed.

[0217] The molded product obtained by molding the resin composition according to the present invention can have excellent dimension stability.

[0218] The molded product according to the present invention can be used for various applications such as containers of various articles such as foods, drinks and medicines; various bags such as garbage bags and compost bags; films and sheets for packaging; and various materials such as agricultural materials and building materials.

[0219] [Process for Producing Resin Composition Having Melt Strength Higher Than Melt Strength of Biodegradable Resin]The present invention also relates to a process for producing a resin composition having a melt strength higher than the melt strength of the (a) biodegradable resin, characterized by using the (b) polyester(s) having alicyclic structure(s).

[0220] The process according to the present invention for producing a resin composition having a melt strength higher than the melt strength of (a) biodegradable resin comprises the step of: mixing the (a) biodegradable resin with (b) at least one polyester having at least one alicyclic structure to obtain the resin composition, wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa’s.

[0221] To the (a) biodegradable resin and the (b) polyester having alicyclic structure(s) wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s in the above producing process according to the present invention, the above explanations for the (a) biodegradable resin and the (b) polyester having alicyclic structure(s) included in the resin composition according to the present invention can apply.

[0222] The method of mixing the (a) biodegradable resin and the (b) polyester(s) having alicyclic structure(s) is not limited, and any conventional method may be used. Kneading using a kneader, an extruder and the like is preferable as the method of mixing.

[0223] The temperature when mixing the (a) biodegradable resin and the (b) polyester(s) having alicyclic structure(s) is preferably 150°C or more and 250°C or less, and more preferably 170°C or more and 200°C or less. Homogeneous mixing of the ingredients may be difficult at a temperature of less than 150°C, and the ingredients may be decomposed at a temperature of more than 250°C. A resin composition with a melt strength higher than that of the (a) biodegradable resin can be obtained by the step of mixing the (a) biodegradable resin and the (b) polyester(s) having alicyclic structure(s).

[0224] It is preferable to obtain a molded product, by molding the resin composition obtained by the above producing process according to the present invention.

[0225] The type of the molding is not limited, and mention may be made of, for example, extrusion molding including extrusion coating, blow molding, extrusion and blow molding, injection molding, film molding with stretching, inflation molding, press molding, insert molding, foam molding, transfer molding and the like.

[0226] The above molding may be molding which needs large elongation of material(s) such as molding a bottle by blow molding and the like, and molding a bag by inflation molding and the like. The molded product obtained by the above molding can have excellent dimensional stability. [Use for Enhancing Melt Strength of Biodegradable Resin]

[0227] The present invention also relates to a use of (b) at least one polyester having at least one alicyclic structure in order to enhance the melt strength of (a) biodegradable resin, wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0228] To the (a) biodegradable resin and the (b) polyester having alicyclic structure(s) wherein the meltviscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s in the use according to the present invention, the above explanations for the (a) biodegradable resin, and the (b) polyester having alicyclic structure(s) included in the resin composition according to the present invention can apply.

[0229] The use according to the present invention can be performed by adding the (b) polyester(s) having alicyclic structure(s), wherein the melt viscosity at 195 °C of the (b) polyester is from 60 to 3,000 mPa's, to the (a) biodegradable resin.

[0230] The melt strength of the (a) biodegradable resin can be enhanced by the use according to the present invention. Thus, the molding processability of the resin composition including the (a) biodegradable resin can be enhanced by the use according to the present invention. For example, as a result of the use according to the present invention, molding which needs large elongation of material(s) such as molding a bottle by blow molding and the like and molding a bag by inflation molding and the like can be easily performed by using the (a) biodegradable resin. In addition, the dimensional stability of a molded product comprising the (a) biodegradable resin can be enhanced.

[0231] [Melt Strength Enhancer for Biodegradable Resin]

[0232] The present invention also relates to an enhancer for the melt strength of (a) biodegradable resin, comprising (b) at least one polyester having at least one alicyclic structure wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s. The enhancer for the melt strength of (a) biodegradable resin means a substance that exists independently and can provide a resin composition having a melt strength which is higher than the melt strength of the (a) biodegradable resin by being combined with the (a) biodegradable resin.

[0233] To the (b) polyester having alicyclic structure(s) wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa's which is the melt strength enhancer according to the present invention, as well as the (a) biodegradable resin which is the subject to which the melt strength enhancer is used, the above explanations for the (b) polyester having alicyclic structure(s) and the (a) biodegradable resin included in the resin composition according to the present invention can apply.

[0234] The term “comprising” here means “including” unless otherwise defined. Thus, the melt strength enhancer according to the present invention for the (a) biodegradable resin may include any additional ingredient, in addition to the (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0235] As the additional ingredients, mention may be made of, for example, antioxidants, photostabilizers, coloring inhibitors, mold releasing agents, antibacterial agents, flame retardants, conductivity imparting agents, damping agents, and the like.

[0236] In one embodiment, the melt strength enhancer according to the present invention for (a) biodegradable resin may consist of the (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

[0237] The melt strength of the (a) biodegradable resin can be enhanced by the use of the melt strength enhancer according to the present invention. Thus, the molding processability of a resin composition including the (a) biodegradable resin can be enhanced by the use of the melt strengthenhancer according to the present invention. For example, as a result of the use of the melt strength enhancer according to the present invention, molding which needs large elongation of material(s) such as molding a bottle by blow molding and the like and molding a bag by inflation molding and the like can be easily performed by using the (a) biodegradable resin. In addition, the dimensional stability of a molded product comprising the (a) biodegradable resin can be enhanced.

[0238] INDUSTRIAL APPLICABILITY

[0239] The resin composition according to the present invention can be used for the manufacture of a variety of molded products.

[0240] The above molded products can be used for various applications such as containers of various articles such as foods, drinks and medicines; various bags such as garbage bags and compost bags; films and sheets for packaging; and various materials such as agricultural materials and building materials.

[0241] The molded product according to the present invention is biodegradable and has little environmental impact. Thus, the molded product according to the present invention can be preferably used as substitutes of, for example, molded products which are made from raw materials such as polyolefins derived from petroleum and are difficult to be decomposed in the natural world.

[0242] Any of the process for enhancing the melt strength of (a) biodegradable resin, the use in order to enhance the melt strength of (a) biodegradable resin, and the enhancer for the melt strength of (a) biodegradable resin, according to the present invention, can enhance the melt strength of the (a) biodegradable resin by using the (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195°C of the 0?) polyester is from 60 to 3,000 mPa·s. Thus, they can enhance the molding processability of the resin composition including the (a) biodegradable resin. For example, molding which needs large elongation of material(s) such as molding a bottle by blow molding and the like and molding a bag by inflation molding and the like can be easily performed by using the (a) biodegradable resin. In addition, the dimensional stability of a molded product comprising the (a) biodegradable resin can be enhanced.

[0243] EXAMPLES

[0244] The present invention will be described in more detail by way of examples, which however should not be construed as limiting the scope of the present invention.

[0245] < Resins l-7>

[0246] Resin 1:

[0247] 25 parts by mass of gum rosin produced in China and 3 parts by mass of glycerin were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, and heated to 270°C to react while nitrogen gas was introduced, and continued the reaction until the acid value became 14 mgKOH / g or less. Then, the reactor was cooled to 180°C, and 3 parts by mass of maleic anhydride was charged into the reactor, followed by stirring for 1 hour. Then, 69 parts by mass of polyethylene glycol (PEG4000) was charged into the reactor, heated to 260°C to react, and continued the reaction until the acid value became 16mgKOH / g. Thus, resin 1, which was an acid-modified rosin polyester, was obtained.

[0248] Resin 2:

[0249] 79 parts by mass of gum rosin produced in China, 3 parts by mass of tall oil fatty acid, and 6 parts by mass of maleic anhydride were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, and heated to 200°C to react while nitrogen gas was introduced, followed by stirring for 1 hour. Then, 6 parts by mass of glycerin and 6 parts by mass of pentaerythritol were charged into the reactor, heated to 270°C to react, and the reaction continued until the acid value became 15 mgKOH / g. Thus, resin 2, which was an acid-modified rosin polyester, was obtained.

[0250] Resin 3:

[0251] 43 parts by mass of 1,2,3,6-tetrahydrophthalic anhydride, 22 parts by mass of neopentyl glycol, and 35 parts by mass of hydrogenated bisphenol A were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, heated to 240°C to react while nitrogen gas was introduced, and the reaction continued until the acid value became 17 mgKOH / g. Thus, resin 3, which was a polyester, was obtained.

[0252] Resin 4:

[0253] 40 parts by mass of 1,2,3, 6-tetrahydrophthalic anhydride, 2 parts by mass of glycerin, and 58 parts by mass of hydrogenated bisphenol A were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, heated to 240°C to react while nitrogen gas was introduced, and the reaction continued until the acid value became 30 mgKOH / g. Thus, resin 4, which was a polyester, was obtained.

[0254] Resin 5:

[0255] 88 parts by mass of gum rosin produced in China, and 12 parts by mass of glycerin were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, heated to 270°C to react while nitrogen gas was introduced, and the reaction continued until the acid value became 13 mgKOH / g. Thus, resin 5, which was a rosin ester, was obtained.

[0256] Resin 6:

[0257] 80 parts by mass of gum rosin produced in China, and 5 parts by mass of maleic anhydride were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, heated to 200°C to react while nitrogen gas was introduced, followed by stirring for 1 hour. Then, 15 parts by mas of pentaerythritol was charged into the reactor, heated to 270°C to react, and the reaction continued until the acid value became 14 mgKOH / g. Thus, resin 6, which was an acid-modified rosin polyester, was obtained.

[0258] Resin 7:

[0259] 56 parts by mass of adipic acid, 41 parts by mass of neopentyl glycol, and 3 parts by mass of trimethylolpropane were charged into a reactor equipped with a stirrer, a reflux condensing tube, nitrogen gas introduction tube, and a thermometer, heated to 230°C to react while nitrogen gas wasintroduced, and the reaction continued until the acid value became 13 mgKOH / g. Thus, resin 7, which was a polyester, was obtained,

[0260] (Melt Viscosity)

[0261] The melt viscosity at 195°C of the resins 1-7 was measured by the following method.

[0262] Measurement Apparatus: Rheometer (MCR102 from Anton Paar)

[0263] Sample Amount: about 2 g

[0264] Measurement Method: each sample of the resins 1-7 was placed on a hotplate of the measurement apparatus to melt the sample completely by maintaining the sample for 3 minutes at 200°C under nitrogen atmosphere. A parallel plate PP25 (from Anton Paar) was attached to the measurement apparatus such that the distance (gap) between the parallel plate PP25 and the hot plate was 0.5 mm. Under nitrogen atmosphere, the parallel plate was rotated at shear rate of 50 / s for 1 minute at 200°C and bubbles in the sample were removed. Cooling was performed from 200°C to 150°C at the temperature of the hot plate for 930 seconds. The viscosity at 195°C was measured. The results are shown in the line of “Melt Viscosity (mPa's)” in Table 1 below.

[0265] (Methanol Tolerance)

[0266] The methanol tolerance at 25 °C of the resins 1-7 was measured by the following method.

[0267] A standard solution was prepared by dissolving 5 g each sample of the resins 1-7 in 50 mL of toluene in a transparent conical glass flask (volume 100 mL). Methanol was added dropwise to the standard solution at 25°C with stirring. The mass (g) of methanol added until the standard solution became clouded was determined. The mass (g) of methanol was defined as the methanol tolerance at 25°C of each of the resins 1-7. The timing of “the standard solution became clouded” was determined by the timing when the characters (10-point font size) printed on a newspaper could not be recognized visually via the standard solution from a viewpoint above the newspaper, due to the clouding of the standard solution, under the conditions that the conical flask was put on the newspaper while the conical flask contacted with the newspaper.

[0268] The results are shown in the line of “Methanol Tolerance (g)” in Table 1 below.

[0269] (Acid Value)

[0270] The acid values of the resins 1-7 were measured by the following method, in accordance with JIS K0070 (1992).

[0271] 1 g sample of each of the resins 1-7 was dissolved in a 20 mL mixed solution of xylene and ethanol (xylene: ethanol = 2:1 (mass ratio)). Then, 3 mL of a phenolphthalein solution with a concentration of 3% by mass was added, as an indicator. Then, neutralization titration was performed by using a potassium hydroxide ethanol solution with a concentration of 0.1 mol / L to determine the acid value (mgKOH / g).

[0272] The results are shown in the line of “Acid Value (mgKOH / g)” in Table 1 below.

[0273] (Hydroxyl Value)The hydroxyl values of the resins 1-7 were measured in accordance with JIS K0070 (1992). The results are shown in the line of “Hydroxyl Value (mgKOH / g)” in Table 1 below.

[0274] (Weight- Average Molecular Weight)

[0275] The weight-average molecular weights of the resins 1-7 were measured by the following method. Each of the resins 1-7 was dissolved in tetrahydrofuran to obtain a sample with a concentration of 1.0 g / L. Next, the chromatogram (chart) of the molecular weight distribution of the sample was obtained by gel permeation chromatography (GPC) using a refractive index detector (RID).

[0276] Then, the weight-average molecular weight was determined from the obtained chromatogram (chart) using a calibration curve of standard polystyrene.

[0277] Measurement apparatuses and conditions were as follows.

[0278] Data-Processing Device: Agilent 1260 Infinity II (from Agilent)

[0279] Refractive Index Detector: RID (G7162A) in Agilent 1260 Infinity II

[0280] Column: PL gelmixed-B7.5×300mm (from Agilent) three columns

[0281] Mobile Phase: Tetrahydrofuran

[0282] Column Flow Rate: 1.0 ml / min

[0283] Sample Concentration: 1.0 g / L

[0284] Injection Amount: 10 pL

[0285] Measurement Temperature: 30°C

[0286] Molecular Weight Marker: Standard Polystyrene (EasiCal Polystyrene Standards PS-1) (from Agilent)

[0287] The results are shown in the line of “Weight- Average Molecular Weight” in Table 1 below.

[0288] < Biodegradable Resin>

[0289] Polylactic acid (RENEW601 from Futtero S.A.) was used as a biodegradable resin.

[0290] Preparation of Resin Composition>

[0291] Each of the polylactic acid and the resins 1-7 was pulverized such that the maximum particle size was 3 mm³ or less. Then, both of the polylactic acid and of each of the resins 1-7 were mixed to obtain a mixture with a mixing mass ratio of 97.5:2.5.

[0292] A resin composition was prepared by kneading the mixture thus obtained by using a twin-screw extruder (Process 11 from Thermo Fisher Scientific) under the conditions of a kneading temperature of about 195°C, a screw rotating speed of about 65 rpm, extruding speed of about 400 g / h, and a cooling water temperature of about 25°C.

[0293] < Melt Strength Evaluation>

[0294] About 1 g of the resin composition thus obtained was placed on a hotplate of a Rheometer (MCR102 from Anton Paar). The temperature of the hot plate was set to be 190°C. A parallel plate PP25 (from Anton Paar) was attached to the Rheometer such that the distance (gap) between the parallel plate PP25 and the hot plate was 0.5 mm, and maintained for 3 minutes. Then, thehot plate was cooled to 165°C and maintained 25 seconds at a shear rate of 10 / s. Then, at the same temperature, frequency sweep measurement (shearing strain 5% and frequency 3-300 rad / s) was performed to determine the angular frequency ωcopat the point (loss factor or loss tangent (tanδ) = 1) where the storage modulus G’ is equal to the loss modulus G”. Specifically, the angular frequency ωcop was calculated by complementing the two points which are the closest to the point where the land = 1. If the ωcopwas not present in the measurement range, it was calculated by extrapolation.

[0295] A resin composition having a lower angular frequency ωcopwhere the loss tangent (tanδ) = 1 has a higher elasticity at a high temperature when being molded (at melting temperature).

[0296] Accordingly, a resin composition having a lower ωcophas a higher melting strength.

[0297] The ωcopdetermined for each resin composition was evaluated in accordance with the following criteria.

[0298] Score 5: coCoP<210 rad / s

[0299] Score 4: 210 rad / s < cowp <225 rad / s

[0300] Score 3: 225 rad / s < roCoP<305 rad / s

[0301] Score 2: 305 rad / s < coCoP<350 rad / s

[0302] Score 1: 350 rad / s ≤ ωcop

[0303] Regarding Comparative Example 4, the melt strength of the polylactic acid was measured in the same manner as done for the resin composition.

[0304] The results are shown in the line of “Melt Strength” in Table 1 below. Score 3 or more is practical.Table 1

[0305]

[0306] PLA: Polylactic Acid

[0307] < Summary>

[0308] In Examples 1-4, the melt strength of the resin composition including the (a) biodegradable resin was enhanced as compared to the melt strength of the (a) biodegradable resin by using the (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195°C of the (b) polyester was from 60 to 3,000 mPa·s. In Examples 2 and 4, the melt strength of the resin composition including the (a) biodegradable resin was particularly enhanced by using the (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195 °C of the (b) polyester was relatively higher.

[0309] In Comparative Example 1, the melt strength of the resin composition including the (a) biodegradable resin was not enhanced as compared to the melt strength of the (a) biodegradable resin, because the ester having alicyclic structure(s) with a melt viscosity at 195°C of less than 60 mPa·s (i.e., 55 mPa's) was used.

[0310] In Comparative Example 2, the melt strength of the resin composition including the (a) biodegradable resin was inferior to the melt strength of the (a) biodegradable resin itself, because the polyester having alicyclic structure(s) with a melt viscosity at 195°C of more than 3,000 mPa's (i.e., 3,867 mPa's) was used.

[0311] In Comparative Example 3, the melt strength of the resin composition including the (a) biodegradable resin was inferior to the melt strength of the (a) biodegradable resin itself, because the polyester having no alicyclic structure was used although the melt viscosity at 195°C of the polyester was within from 60 to 3,000 mPa-s (i.e., 900 mPa's).

[0312] In Comparative Example 4, only the (a) biodegradable resin was used, while (b) polyester having alicyclic structure(s), wherein the melt viscosity at 195°C of the (b) polyester was from 60 to 3,000 mPa's was not used. Thus, the melt strength was insufficient.

Claims

CLAIMS1. A resin composition, comprising:(a) at least one biodegradable resin; and(b) at least one polyester having at least one alicyclic structure,whereinthe melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

2. The resin composition according to Claim 1, wherein the (a) biodegradable resin is meltable.

3. The resin composition according to Claim 1, wherein the (a) biodegradable resin is derived from biomass.

4. The resin composition according to Claim 1, wherein the (a) biodegradable resin is selected from the group consisting of polylactic acid, polycaprolactone, polyhydroxyalkanoate, polybutylene succinate, modified starch, polybutylene adipate terephthalate, cellulose acetate, polyvinyl alcohol, polyglycolic acid, polybutylene succinate-co-adipate, polyethylene terephthalate succinate, and mixtures thereof.

5. The resin composition according to Claim 1, wherein the amount of the (a) biodegradable resin(s) in the resin composition ranges from 50% to 99% by mass, preferably from 70% to 98.5% by mass, more preferably from 80% to 98% by mass, and even more preferably from 90% to 98% by mass, relative to the total mass of the composition.

6. The resin composition according to Claim 1, wherein the melt viscosity at 195 °C of the (b) polyester is from 200 to 2,000 mPa's, preferably from 350 to 1,500 mPa’s, more preferably from 500 to 1,200 mPa’s, and even more preferably from 600 to 1,000 mPa-s.

7. The resin composition according to Claim 1, wherein the methanol tolerance at 25°C of the (b) polyester is 250 g or less, preferably 200 g or less, more preferably 150 g or less, and even more preferably 100 g or less.

8. The resin composition according to Claim 1, wherein the acid value of the (b) polyester is 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and more preferably 15 mgKOH / g or more.

9. The resin composition according to Claim 1, wherein the hydroxyl value of the (b) polyester is less than 32 mgKOH / g, preferably less than 30 mgKOH / g, and more preferably less than 28 mgKOH / g or more than 60 mgKOH / g, preferably more than 65 mgKOH / g, and more preferably more than 70 mgKOH / g.

10. The resin composition according to Claim 1, wherein the weight-average molecular weight of the (b) polyester is from 1,000 to 9,000, preferably from 1,500 to 8,000, and more preferably from 2,000 to 7,000.

11. The resin composition according to Claim 1, wherein the (b) polyester is selected from rosin- modified polyesters.

12. The resin composition according to Claim 1, wherein the amount of the (b) polyester(s) in the resin composition ranges from 0.1% to 20% by mass, preferably from 0.5% to 10% bymass, and more preferably from 1% to 5% by mass, relative to the total mass of the composition.

13. A molded product comprising the resin composition according to any one of Claims 1 to 12.

14. A process for producing a resin composition having a melt strength higher than the melt strength of (a) biodegradable resin, comprising the step of:mixing the (a) biodegradable resin with (b) at least one polyester having at least one alicyclic structure to obtain the resin composition, wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa·s.

15. A use of (b) at least one polyester having at least one alicyclic structure in order to enhance the melt strength of (a) biodegradable resin, wherein the melt viscosity at 195°C of the (b) polyester is from 60 to 3,000 mPa’s.

16. An enhancer for the melt strength of (a) biodegradable resin, comprising (b) at least one polyester having at least one alicyclic structure, wherein the melt viscosity at 195 °C of the (b) polyester is from 60 to 3,000 mPa·s.