Underfill material, electronic component device, and method for manufacturing electronic component device

The underfill material with a maleimide compound and specific peroxides maintains low viscosity for extended periods and enables low-temperature processing, addressing the challenges of conventional materials by reducing warping and processing time in semiconductor packages.

WO2026234890A1PCT designated stage Publication Date: 2026-11-12RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/007203
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-02-26
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional underfill materials require long processing times and high temperatures, leading to warping of semiconductor packages, especially with increasing substrate sizes, and fail to maintain low viscosity for extended periods.

Method used

An underfill material comprising a radical polymerizable compound, such as a maleimide compound, with a peroxide having a 10-hour half-life temperature of 90°C to 110°C, which maintains low viscosity for a longer period and can be processed at lower temperatures, using specific peroxides as radical polymerization initiators.

Benefits of technology

The material allows for efficient low-temperature processing, reducing warping and extending the time the material remains fluid, making it suitable for large-area substrates without thickening prematurely.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

An underfill material comprising a radically polymerizable compound and a peroxide having a 10-hour half-life temperature of 90-110° C, the radically polymerizable compound comprising a maleimide compound.
Need to check novelty before this filing date? Find Prior Art

Description

Underfill material, electronic component device, and method for manufacturing an electronic component device.

[0001] This disclosure relates to underfill material, electronic component apparatus, and a method for manufacturing electronic component apparatus.

[0002] Underfill materials are widely used in semiconductor devices with bare chip mounting, such as COB (Chip on Board), COG (Chip on Glass), and TCP (Tape Carrier Package). Furthermore, in semiconductor devices (also called flip-chip devices) in which semiconductor elements are directly bump-connected to a wiring board made of ceramic, glass epoxy resin, glass imide resin, polyimide film, etc., underfill materials are used to fill the gap between the bump-connected semiconductor elements and the wiring board.

[0003] In recent years, with the advancement of information technology, electronic devices have become even smaller, more integrated, and more multifunctional, leading to smaller bump diameters, narrower pitches, and narrower gaps due to the increased number of pins. Therefore, the development of underfill materials with excellent gap injection properties is being investigated (see, for example, Patent Document 1).

[0004] Japanese Patent Publication No. 2002-97342

[0005] However, in recent years, the increasing size of substrates has led to a situation where filling with underfill material requires a long time. Furthermore, underfill material is generally filled at a temperature of around 110°C and cured at 150°C to 175°C. In addition, the heating and cooling process in the semiconductor package manufacturing process is a factor in the warping of semiconductor packages, and there are concerns that warping will increase with the increase in substrate size. For this reason, there is a need for underfill material that can be processed at lower temperatures. In view of these circumstances, the object of this disclosure is to provide an underfill material that maintains a lower viscosity for a longer period than conventional materials and can be processed at lower temperatures, an electronic component device obtained therefrom, and a method for manufacturing an electronic component device using the same.

[0006] The means for solving the above problems include the following embodiments: <1> An underfill material comprising a radical polymerizable compound and a peroxide having a 10-hour half-life temperature of 90°C to 110°C, wherein the radical polymerizable compound comprises a maleimide compound. <2> The underfill material according to <1>, wherein the radical polymerizable compound further comprises a (meth)acrylic compound. <3> The underfill material according to <1> or <2>, wherein the amount of heat generated by curing at 120°C for 2 hours is 20% or less of the amount of heat generated before curing. <4> The underfill material according to any one of <1> to <3>, wherein it does not contain any polymerizable compounds other than the radical polymerizable compound, or the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and the radical polymerizable compound is 20% by mass or less. <5> The underfill material according to any one of <1> to <4>, further comprising an inorganic filler. <6> The underfill material according to <5>, comprising 20% ​​by mass or more of the inorganic filler. <7> An underfill material according to any one of <1> to <6>, wherein the amount of linear expansion at 50°C to 220°C when cured is 9000 μm / m or less. <8> An electronic component apparatus comprising: an electronic component; a substrate electrically connected to the electronic component via a connection portion; and a cured underfill material according to any one of <1> to <7> that seals the connection portion. <9> A method for manufacturing an electronic component apparatus, comprising the step of sealing the connection portion between the electronic component and the substrate electrically connected to the electronic component via a connection portion with the underfill material according to any one of <1> to <7>.

[0007] According to this disclosure, an underfill material is provided that maintains a lower viscosity for a longer period than conventional materials and is suitable for low-temperature processes, an electronic component device obtained therefrom, and a method for manufacturing an electronic component device using the same.

[0008] In this disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes, provided that the purpose of the process is achieved. In this disclosure, numerical ranges indicated using "~" include the numbers before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced by the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced by the values ​​shown in the examples. In this disclosure, each component may contain multiple types of the corresponding substance. If multiple types of the substance corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple types of substances present in the composition, unless otherwise specified. In this disclosure, each component may contain multiple types of particles. If multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In this disclosure, "(meth)acrylic" means at least one of acrylic or methacrylic, "(meth)acrylate" means at least one of acrylate or methacrylate, "(meth)acryloyl" means at least one of acryloyl or methacryloyl, and "(meth)acryloxy" means at least one of acryloxy or methacryloxy.

[0009] <Underfill Material> The underfill material of this disclosure comprises a radical polymerizable compound and a peroxide having a 10-hour half-life temperature of 90°C to 110°C, wherein the radical polymerizable compound comprises a maleimide compound. The underfill material may further contain other components as needed. Hereinafter, "10-hour half-life temperature of 90°C to 110°C" will also be referred to as "specific peroxide".

[0010] Furthermore, the underfill material of this disclosure is preferably liquid at room temperature (25°C). Specifically, being liquid at room temperature (25°C) means that the viscosity measured by an E-type viscometer at 25°C is 1000 Pa·s or less.

[0011] The underfill material of this disclosure maintains low viscosity for a longer period than conventional materials and is suitable for low-temperature processes. The reason for this is thought to be as follows: The underfill material of this disclosure uses a radical polymerizable compound. Even when heat is applied, the polymerization reaction of a radical polymerizable compound is suppressed as long as radicals are not present, and thickening due to heating during injection is suppressed. In particular, since the underfill material of this disclosure uses a peroxide with a 10-hour half-life temperature of 90°C or higher, thickening is suppressed over a long period of time, making it suitable even for large-area substrates. Furthermore, the underfill material of this disclosure contains a peroxide with a 10-hour half-life temperature of 90°C to 110°C as a radical polymerization initiator. Therefore, even if the heating temperature when injecting the underfill material is set as low as 80°C, the generation of radicals is suppressed. As a result, it is possible to extend the time during which low viscosity is maintained (hereinafter also referred to as "pot life"). When heated at a temperature exceeding 90°C to 110°C, radicals are generated and the polymerization reaction proceeds. This temperature is lower than the conventional curing temperature of 150°C to 175°C. Therefore, the underfill material of this disclosure can also be cured at a lower temperature. Furthermore, because it does not thicken easily at room temperature, it has excellent storage stability.

[0012] In contrast, conventionally widely used epoxy resins undergo a gradual polymerization reaction due to heating during injection, causing the underfill material containing epoxy resin to thicken. As a result, the pot life is shortened. In particular, as the substrate area increases, the time required for injection of underfill material containing epoxy resin becomes increasingly longer, or it becomes difficult to inject it over the entire surface. If the curing temperature is lowered to shorten the pot life, the curing reaction does not proceed sufficiently.

[0013] The following describes each component contained in the underfill material of this disclosure.

[0014] [Radical Polymerizable Compounds] The underfill material contains radical polymerizable compounds. These radical polymerizable compounds include maleimide compounds.

[0015] (Maleimide Compounds) Maleimide compounds as radical polymerizable compounds can be any compound having a maleimide group in one molecule, and may be used alone or in combination of two or more.

[0016] Maleimide compounds preferably have a melting point of 150°C or lower. Since maleimide compounds are usually solids, it is preferable to have them in a molten state when using them as underfill materials. One method for moltening maleimide compounds is to heat a mixture of (meth)acrylic compounds and maleimide compounds to near the melting point of the maleimide compound to make it compatible with the (meth)acrylic compound. Since (meth)acrylic compounds and maleimide compounds undergo an ene reaction and thicken at 150°C to 250°C, the temperature at which the maleimide compound is heated to dissolve is preferably 150°C or lower, and therefore, maleimide compounds having a melting point of 150°C or lower are preferred.

[0017] The maleimide compound may be a polyfunctional maleimide compound having two or more maleimide groups in one molecule, or a monofunctional maleimide compound having one maleimide group in one molecule. The monofunctional maleimide compound and the polyfunctional maleimide compound may be used independently or in combination.

[0018] Examples of polyfunctional maleimide compounds include bismaleimide compounds represented by the following general formula (I); and polymaleimide resins (hereinafter referred to as polymaleimide resin (A1)) having a substructure represented by the following general formula (1), a substructure represented by general formula (T-1) chemically bonded to the substructure represented by general formula (1), and a substructure represented by general formula (T-2) chemically bonded to the substructure represented by general formula (1).

[0019]

[0020] In general formula (I), R 1 This represents a divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents.

[0021] In general formula (I), R 1The divalent hydrocarbon group having 1 to 18 carbon atoms, which may have substituents represented by , preferably includes a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms, an alicyclic hydrocarbon group having 3 to 18 carbon atoms, and an aromatic hydrocarbon group having 6 to 18 carbon atoms.

[0022] R 1 The divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms represented by is preferably a divalent aliphatic hydrocarbon group having 1 to 14 carbon atoms, and more preferably a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. Specific examples of the divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms include methylene, ethylene, propylene, isopropylene, butylene, pentylene, hexylene, octylene, decylene, dodecylene, vinylene, ethylidene, vinylidene, propenylene, and butadienylene. The divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms is preferably a methylene, ethylene, propylene, isopropylene, butylene, or hexylene group, and more preferably a methylene, ethylene, propylene, isopropylene, or butylene group.

[0023] R 1 The divalent alicyclic hydrocarbon group having 3 to 18 carbon atoms represented by is preferably a divalent alicyclic hydrocarbon group having 3 to 14 carbon atoms, and more preferably a divalent alicyclic hydrocarbon group having 5 to 12 carbon atoms. Specific examples of divalent alicyclic aliphatic hydrocarbon groups having 3 to 18 carbon atoms include cyclopentylene, cyclohexylene, cycloheptylene, cyclopentenylene, cyclohexenylene, and cyclohexylidene.

[0024] R 1 The divalent aromatic hydrocarbon group having 6 to 18 carbon atoms represented by is preferably a divalent aromatic hydrocarbon group having 6 to 14 carbon atoms, and more preferably a divalent aromatic hydrocarbon group having 6 to 12 carbon atoms. Specific examples of the divalent aromatic hydrocarbon group having 6 to 18 carbon atoms include phenylene groups, biphenylene groups, terphenylene groups, and the like.

[0025] In particular, R in general formula (I) 1is more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and even more preferably a divalent aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent.

[0026] R in general formula (I) 1 Examples of the substituent that may be possessed include an alkyl group, an alkoxy group, an aryl group, an aryloxy group, a hydroxyl group, an amino group, a halogen atom, a methacryloxy group, a mercapto group, an imino group, a ureido group, and an isocyanate group. R 1 preferably has no substituent.

[0027] Examples of the bismaleimide compound represented by general formula (I) include 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane.

[0028]

[0029] In general formula (1), R 13 each independently represents an alkyl group having 1 to 18 carbon atoms, m 2 represents an integer of 0 to 4, n 1 represents the average number of repeating units, two * each represent a bond, one bond is chemically bonded at the position of L in the following general formula (T-1) 13 or L 14 , and the other bond is chemically bonded at the position of L in the following general formula (T-2) 11 or L 12 .

[0030] In general formula (T-1) or (T-2), R 11 and R 15 each independently represent a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, R 12 and R 14Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, L 11 ~L 14 Each of these independently represents a bonding bond or a hydrogen atom, however, L 11 or L 12 At the position, it is chemically bonded to the substructure represented by general formula (1), and L 13 or L 14 At this position, L is chemically bonded to the substructure represented by general formula (1), and L is not chemically bonded to the substructure represented by general formula (1). 11 ~L 14 is a hydrogen atom, m 1 and m 3 Each of these represents 2.

[0031] The molecular structure of polymaleimide resin (A1) has only one bonding site each at the ortho and para positions of the benzene ring to which the maleimide group is attached. As a result, after the reaction, a polymaleimide resin with a linearly elongated chain is obtained, making molecular weight control easy, and tending to improve heat resistance, dielectric properties, and solvent solubility.

[0032] In general formula (1), the two *s each represent a bond. And one of the two bonds is L in general formula (T-1). 13 or L 14 A chemical bond is formed at the position. The other bond is L in general formula (T-2). 11 or L 12 Chemical bonding occurs at the position. Therefore, the polymaleimide resin of this embodiment has a structural unit in which a substructure represented by general formula (T-1) and a substructure represented by general formula (T-2) are linked by a substructure represented by general formula (1), and the substructure represented by general formula (1) is chemically bonded to the maleimide group on the benzene ring in general formula (T-1) and general formula (T-2) at the para position or one ortho position. Note that in general formula (1), n 1 If the number is 2 or more, there are multiple R 13 They may be the same or they may be different. 2 If the number is 2 or more, there are multiple R 13 They may be the same or they may be different.

[0033] In general formula (1), R 13 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrocarbon group having 1 to 6 carbon atoms, even more preferably a hydrocarbon group having 1 to 3 carbon atoms, and even more preferably a hydrocarbon group having 1 or 2 carbon atoms. 2 If R is an integer greater than or equal to 2, there are multiple R's. 13 These may be the same or different. Preferred R in general formula (1) 13 Preferably, the group is a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, n-pentyl group, isopentyl group, tert-pentyl group, or neopentyl group, and a linear alkyl group is more preferred.

[0034] In general formula (1), m 2 R represents an integer between 0 and 4, preferably an integer less than or equal to 2, and more preferably 2. Note that R in general formula (1) 13 In a benzene ring to which R is bonded, if the 1st and 3rd positions are bonded by a methylene group, then the 4th and 6th positions are R 13 It is preferable that each of them is combined. In general formula (1), n 1 n represents the average number of repeating units. 1 From the viewpoint of the viscosity of the resulting polymaleimide resin, the ratio is preferably 0 to 50, preferably 0 to 30, and preferably 0 to 15. The average number of repeating units can be calculated from the charge ratio or NMR analysis results, etc.

[0035] The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (1) in 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass.

[0036] In general formula (T-1), R 15Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Particularly preferred R 15 These are hydrogen atoms or linear alkyl groups having 1 to 6 carbon atoms. 3 Since is 2, two R 15 They may be the same or different. In general formula (T-1), R 14 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, and more preferably a hydrocarbon group having 1 to 6 carbon atoms. Particularly preferred R 14 As such, it is a linear alkyl group having 1 to 6 carbon atoms. By allowing a bonding site with the substructure represented by general formula (1) at the ortho position (position 6) of the benzene ring of general formula (T-1) or general formula (T-2), it has high solubility in solvents and exhibits superior low dielectric loss tangent and high heat resistance during curing. In general formula (T-1), L 13 or L 14 Each of these independently represents a bond or a hydrogen atom. However, L 13 or L 14 At least one of the positions of the substructure is chemically bonded to the substructure represented by general formula (1) and the substructure represented by general formula (T-1). In addition, L does not chemically bond to the substructure represented by general formula (1). 13 or L 14 L is a hydrogen atom. 13 and L 14 A substructure represented by general formula (1) may be chemically bonded to each of the two locations.

[0037] In general formula (T-2), R 11 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, more preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. Preferred R 11 These are hydrogen atoms or linear alkyl groups having 1 to 6 carbon atoms. 1 Since is 2, two R 11They may be the same or different. In the general formula (T-2), R 12 Each of these independently represents a hydrocarbon group having 1 to 18 carbon atoms, preferably a hydrocarbon group having 1 to 12 carbon atoms, and more preferably a hydrocarbon group having 1 to 6 carbon atoms. Preferred R 12 As such, it represents a linear alkyl group having 1 to 6 carbon atoms. In the general formula (T-2), L 11 or L 12 Each of these independently represents a bond or a hydrogen atom. However, L 11 or L 12 At least one of the positions of the substructure is chemically bonded to the substructure represented by general formula (1) and the substructure represented by general formula (T-2). In addition, L does not chemically bond to the substructure represented by general formula (1). 11 or L 12 L is a hydrogen atom. 11 and L 12 A substructure represented by general formula (1) may be chemically bonded to each of the two locations.

[0038] The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (T-1) per 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass. The polymaleimide resin (A1) preferably contains 1 to 99% by mass of the substructure represented by general formula (T-2) per 100% by mass of the polymaleimide resin (A1), more preferably 1 to 97% by mass, even more preferably 3 to 97% by mass, and particularly preferably 5 to 95% by mass.

[0039] There are no particular restrictions on the method for producing the polymaleimide resin (A1), and the method for producing the polymaleimide resin and the examples in Japanese Patent Application Publication No. 2024-4392 can be referred to.

[0040] The polymaleimide resin (A1) may be a maleimide compound represented by the following general formula (II).

[0041]

[0042] In general formula (II), n is 0 or an integer greater than or equal to 1.

[0043] Examples of bismaleimide compounds represented by general formula (II) include phenylmethanemaleimide.

[0044] (Meth)acrylic compound) The radical polymerizable compound may contain a (meth)acrylic compound in addition to the maleimide compound. The (meth)acrylic compound may be used alone or in combination of two or more. From the viewpoint of adhesive strength with the package substrate, the combined use of the (meth)acrylic compound and the maleimide compound is one of the preferred embodiments.

[0045] The radical polymerizable compound may include other radical polymerizable compounds besides (meth)acrylic compounds and maleimide compounds. Examples of other radical polymerizable compounds include vinyl compounds.

[0046] The total content of (meth)acrylic compounds and maleimide compounds in the underfill material is preferably 40% by mass or more, more preferably 60% by mass or more, even more preferably 80% by mass or more, and may be 100% by mass.

[0047] The (meth)acrylate compound used as the radical polymerizable compound is not particularly limited, and conventionally known (meth)acrylate compounds can be used. The (meth)acrylate compound may be used alone or in combination of two or more. When two or more (meth)acrylate compounds are used in combination, the combination of (meth)acrylate compounds is not particularly limited. From the viewpoint of dispensability, it is preferable to use in combination at least one polyfunctional (meth)acrylate compound containing at least two (meth)acryloyl groups in one molecule and at least one monofunctional (meth)acrylate compound containing one (meth)acryloyl group in one molecule. This often results in a low viscosity underfill material, which tends to improve injectability.

[0048] Examples of polyfunctional (meth)acrylate compounds include diethylene glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, polyethylene glycol diacrylate, polypropylene glycol diacrylate, tricyclodecane dimethylol diacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol hexaacrylate, tris(β-hydroxyethyl) isocyanurate triacrylate, polycarbonate acrylate, urethane acrylate, and diethylene Examples include methyl glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, tricyclodecane dimethylol dimethacrylate, ditrimethylolpropane tetramethacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol hexamethacrylate, tris(β-hydroxyethyl) isocyanurate trimethacrylate, polycarbonate methacrylate, urethane methacrylate, and difunctional (meth)acrylate compounds represented by the following formula (II).

[0049] Among these, examples include compounds having an aliphatic cyclic skeleton and at least two (meth)acryloyloxy groups (hereinafter sometimes referred to as alicyclic monomers), and compounds having two (meth)acryloyloxy groups in the molecule, with the two (meth)acryloyloxy groups linked by a linear divalent organic group (hereinafter sometimes referred to as linear monomers). These are polyfunctional (meth)acrylate compounds because they contain two (meth)acryloyl groups in one molecule.

[0050] Alicyclic monomers and linear monomers may be used individually or in combination. From the viewpoint of reducing the linear thermal expansion coefficient of the cured product, it is preferable to include at least alicyclic monomers. The ratio of alicyclic monomers to the total amount of alicyclic monomers and linear monomers is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and may be 100% by mass.

[0051] The aliphatic cyclic skeleton contained in the alicyclic monomer is not particularly limited, and examples include the tricyclodecane skeleton, cyclohexane skeleton, cyclopentane skeleton, 1,3-adamantane skeleton, hydrogenated bisphenol A skeleton, hydrogenated bisphenol F skeleton, hydrogenated bisphenol S skeleton, isobornyl skeleton, etc. Among these, the tricyclodecane skeleton is preferred.

[0052] As the alicyclic monomer, compounds represented by the following general formula (1) are preferred.

[0053]

[0054] In general formula (1), R 1 and R 2 Each of these is independently an aliphatic hydrocarbon group having 1 to 4 carbon atoms or a group represented by the following general formula (2). n1 represents 0 or 1, n2 represents an integer from 0 to 2, and n1 + n2 is 2 or 3. n1 R 1 and n2 R 2 At least two of these are groups represented by the following general formula (2).

[0055]

[0056] In general formula (2), R 1A represents a hydrogen atom or a methyl group, and m represents an integer from 1 to 10.

[0057] R 1 and R 2 Specific examples of aliphatic hydrocarbon groups having 1 to 4 carbon atoms, represented by , include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, and the like.

[0058] The compound represented by general formula (1) may also be a compound represented by the following formula (3A) or formula (3B).

[0059]

[0060] Examples of compounds represented by formula (3A) include tricyclodecanedimethanol diacrylate, and examples of compounds represented by formula (3B) include tricyclodecanedimethanol dimethacrylate.

[0061] The linear monomer is preferably a compound represented by the following general formula (4) or the following general formula (5).

[0062]

[0063] In general formula (4) or general formula (5), R 3 Each of these independently represents either a hydrogen atom or a methyl group, R 4 R represents an alkylene group with 1 to 8 carbon atoms. 5 R represents an alkylene group with 1 to 8 carbon atoms, and p represents an integer from 2 to 5. 3 and R 5 They may be the same or they may be different.

[0064] R in general formula (4) or general formula (5) 3 A methyl group is preferred as the component. R in general formula (4) 4 Specific examples of alkylene groups having 1 to 8 carbon atoms represented by include methylene group, ethylene group, trimethylene group, tetramethylene group, hexamethylene group, octamethylene group, etc. R in general formula (5) 5Specific examples of alkylene groups having 1 to 8 carbon atoms represented by the formula include methylene, ethylene, trimethylene, methylethylene, dimethylmethylene, tetramethylene, hexamethylene, and octamethylene groups, with methylethylene and ethylene groups being preferred, and ethylene groups being more preferred. In general formula (5), p is preferably an integer between 3 and 4.

[0065] Examples of linear monomers include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, tripropylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate.

[0066] Examples of monofunctional (meth)acrylate compounds include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, and decyl 2-(tricyclo)[5.2.1.02,6]decyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]decyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]decal(meth)acrylate, 2-(tricyclo)[5.2.1.02,6]deca-3-en-8-yloxyethyl(meth)acrylate, 2-(tricyclo)[5.2.1.02,6] Deca-3-en-9-yloxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, dimergol mono (meth)acrylate, diethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxy Polyethylene glycol (meth)acrylate, 2-benzoyloxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, benzyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, γ-(meth)acryloyloxypropyltrimethoxysilane, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, tetrahydropyranyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 1,2,2,6,6-pentamethylpiperidyl (meth)acrylate, 2,2,6,Examples include 6-tetramethylpiperidinyl (meth)acrylate, (meth)acryloxyethyl phosphate, (meth)acryloxyethyl phenyl acid phosphate, β-(meth)acryloyloxyethyl hydrogen phthalate, β-(meth)acryloyloxyethyl hydrogen succinate, and ethylene oxide-modified neopentyl glycol (meth)acrylate, 2-(meth)acryloyloxyethyl succinate, 2-methacryloyloxyethyl hexahydrophthalate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and neopentyl glycol (meth)acrylic acid benzoate. ,

[0067] (Meth)acrylic compounds may contain other polymerizable functional groups besides the (meth)acrylic group. Examples of other polymerizable functional groups include glycidyl groups, amino groups, and hydroxyl groups. These functional groups interact with the packaging substrate to increase the adhesive strength to the substrate. Examples of such compounds include 4-hydroxybutyl acrylate glycidyl ether (4HBAGE), 4-hydroxybutyl acrylate (4HBA), and 1,4-cyclohexanedimethanol monoacrylate (CHDMMA). However, from the viewpoint of suppressing viscosity increase during filling, it is desirable not to use other polymerizable functional groups in combination. Examples of combinations that polymerize include epoxy groups and amino groups, and epoxy groups and hydroxyl groups.

[0068] When at least one polyfunctional (meth)acrylate compound and at least one monofunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, from the viewpoint of achieving a low modulus of elasticity. Furthermore, the content of the monofunctional (meth)acrylate compound relative to the total amount of polyfunctional (meth)acrylate compounds is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of lowering the linear thermal expansion coefficient of the cured product.

[0069] When a maleimide compound and a (meth)acrylate compound are used in combination as a radical polymerizable compound, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, from the viewpoint of reducing viscosity, the content of the maleimide compound relative to the total amount of the maleimide compound and the (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.

[0070] Examples of radical polymerizable compounds include those using a polyfunctional maleimide compound alone, those using a polyfunctional maleimide compound in combination with a polyfunctional (meth)acrylate compound, and those using a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound. Among these, the form using a polyfunctional maleimide compound, a polyfunctional (meth)acrylate compound, and a monofunctional (meth)acrylate compound is preferred from the viewpoint of achieving both low viscosity and adhesion.

[0071] When a polyfunctional maleimide compound and a polyfunctional (meth)acrylate compound are used in combination as radical polymerizable compounds, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of adhesion to the semiconductor package substrate. Furthermore, the content of the polyfunctional maleimide compound relative to the total amount of the polyfunctional maleimide compound and the polyfunctional (meth)acrylate compound is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of reducing viscosity.

[0072] [Other Polymerizable Compounds] The underfill material may contain other polymerizable compounds besides radical polymerizable compounds. Examples of polymerizable functional groups in other polymerizable compounds include glycidyl groups, amino groups, and hydroxyl groups. Other polymerizable compounds may be monofunctional or polyfunctional. From the viewpoint of suppressing viscosity increase during filling, it is desirable not to use other polymerizable compounds in combination that polymerize. Examples of polymerizable combinations include epoxy groups and amino groups, and epoxy groups and hydroxyl groups. Since other polymerizable compounds do not have radical polymerizable functional groups, they may seep into the interface with the substrate during the curing process. From the viewpoint of preventing seepage, it is preferable that other polymerizable compounds are not included, or if other polymerizable compounds are included, the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and radical polymerizable compounds is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0073] [Specific Peroxides] The underfill material contains peroxides (specific peroxides) with a 10-hour half-life temperature of 90°C to 110°C. These specific peroxides function as radical polymerization initiators.

[0074] The 10-hour half-life temperature of the specific peroxide is 90°C to 110°C, with 95°C to 105°C being more preferable. By setting the 10-hour half-life temperature of the specific peroxide within the above range, it becomes possible to lower the curing temperature of the underfill material compared to the conventional curing temperature (150°C to 175°C). As a result, package warping can be suppressed.

[0075] The half-life temperature of a specific peroxide is calculated using the following formula (in °C). The half-life temperature is listed in the catalog of commercially available products, so you may refer to that.

[0076]

[0077] τ: Half-life, C: Constant, Ea: Activation energy, R: Gas constant, T: Absolute temperature

[0078] The specific peroxide preferably contains a peroxy group and a hydrocarbon group, and from the viewpoint of application to low-temperature processes, the hydrocarbon group preferably does not contain an aromatic ring. The hydrocarbon group is preferably linear or branched. The specific peroxide may further contain a ketone group.

[0079] The content of specific peroxides in the underfill material is not particularly limited. For example, the content of specific peroxides is preferably 0.1 to 10 parts by mass per 100 parts by mass of the total radical polymerizable compound, and more preferably 0.5 to 5 parts by mass from the viewpoint of curability. When the content of specific peroxides is 10 parts by mass or less per 100 parts by mass of the total radical polymerizable compound, volatile matter is less likely to be generated, and the generation of voids in the cured product tends to be suppressed. In addition, since a rapid increase in radical concentration is suppressed, termination reactions of radical polymerization are less likely to occur, and a long-chain crosslinked structure tends to be obtained. As a result, cracks are less likely to occur in the cured product. Furthermore, when the content of specific peroxides is 0.3 parts by mass or more per 100 parts by mass of the total radical polymerizable compound, the curability tends to improve.

[0080] [Other Radical Polymerization Initiators] The underfill material may contain other radical polymerization initiators other than the specified peroxides. The other radical polymerization initiators are not particularly limited, and conventionally known radical polymerization initiators can be used. Examples of radical polymerization initiators include organic peroxides described later; azo compounds such as azobisisobutyronitrile, azobis-4-methoxy-2,4-dimethylvaleronitrile, azobiscyclohexanone-1-carbonitride, and azodibenzoyl; potassium persulfate; and redox catalysts consisting of a combination of a water-soluble catalyst such as ammonium persulfate and a peroxide, or a combination of a persulfate and a reducing agent. The radical polymerization initiator may be used alone or in combination of two or more.

[0081] In the total radical polymerization initiator, including the specified peroxide, the content of the specified peroxide is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass, from the viewpoint of application to low-temperature processes.

[0082] The content of total radical polymerization initiator in the underfill material is not particularly limited. For example, the content of total radical polymerization initiator is preferably 0.1 to 20 parts by mass per 100 parts by mass of the total radical polymerizable compound, and more preferably 0.5 to 10 parts by mass from the viewpoint of curability. When the content of total radical polymerization initiator is 20 parts by mass or less per 100 parts by mass of the total radical polymerizable compound, volatile matter is less likely to be generated and the generation of voids in the cured product tends to be suppressed. In addition, since a rapid increase in radical concentration is suppressed, termination reactions of radical polymerization are less likely to occur, and a long-chain crosslinked structure tends to be obtained. As a result, cracks are less likely to occur in the cured product. Furthermore, when the content of total radical polymerization initiator is 0.3 parts by mass or more per 100 parts by mass of the total radical polymerizable compound, the curability tends to improve.

[0083] [Inorganic Filler] The underfill material may contain an inorganic filler. Examples of inorganic fillers include silica such as spherical silica, crystalline silica, and fused silica; powders of calcium carbonate, clay, alumina, silicon nitride, silicon carbide, boron nitride, calcium silicate, potassium titanate, aluminum nitride, beryllia, zirconia, zircon, fossterite, steatite, spinel, mullite, titania, etc., or beads or glass fibers made by shaping these into spheres. Furthermore, as an inorganic filler with flame retardant properties, aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, etc. may be used. The inorganic filler may be used alone or in combination of two or more types. Among these, silica is preferred from the viewpoint of ease of availability, chemical stability, and material cost, and spherical silica is more preferred from the viewpoint of fluidity and permeability into the fine gaps of the underfill material. Examples of spherical silica include silica obtained by deflagration and fused silica. The inorganic filler may be surface-treated beforehand using various surface treatment agents such as silane coupling agents, as described later.

[0084] The volume-average particle size of the inorganic filler is not particularly limited. For example, in the case of spherical silica, the volume-average particle size is preferably 0.1 μm to 10 μm, more preferably 0.2 μm to 7 μm, even more preferably 0.3 μm to 5 μm, and may also be 0.3 μm to 2.0 μm. When the volume-average particle size is 0.1 μm or more, it tends to have excellent dispersibility in the underfill material, is less likely to impart thixotropy to the underfill material, and has excellent flow characteristics. When the volume-average particle size is 10 μm or less, it tends to reduce the sedimentation of the inorganic filler in the underfill material, improve the permeability and fluidity into fine gaps of the underfill material, and prevent voids and unfilled areas. The volume-average particle size of the inorganic filler can be measured as the particle size (D50) when the cumulative amount from the small diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction scattering particle size distribution analyzer.

[0085] The content ratio of the inorganic filler is not particularly limited, and is preferably 20 mass% or more, more preferably 25 mass% or more, and even more preferably 30 mass% or more, based on the entire underfill material. Further, the content ratio of the inorganic filler is preferably 80 mass% or less, more preferably 75 mass% or less, and even more preferably 70 mass% or less, based on the entire underfill material. When the content ratio of the inorganic filler is 20 mass% or more, the linear thermal expansion coefficient can be easily reduced, and when it is 80 mass% or less, an increase in the viscosity of the underfill material can be easily suppressed, and the fluidity, permeability and injectivity tend to be favorable.

[0086] [Surfactant] The underfill material may contain a surfactant as necessary. Examples of the surfactant include silicone oil, higher fatty acid esters, phosphate esters, polyacrylates and the like, and silicone oil is preferred from the viewpoint of lowering the viscosity. The silicone oil is preferably a polyether-modified silicone oil, and more preferably a silicone oil having a polyether moiety in a side chain. The polyether moiety preferably contains at least one selected from the group consisting of an ethyleneoxy moiety and a propyleneoxy moiety. The ethyleneoxy moiety and the propyleneoxy moiety may be connected to a silicon atom via a linking group.

[0087] The silicone oil may further have an amine moiety in a side chain.

[0088] The main chain of the silicone oil may be any of dimethylsilicone, diphenylsilicone, and methylphenylsilicone, and is preferably dimethylsilicone.

[0089] The viscosity of the surfactant at 25°C is preferably 500 mm 2 / s to 5000 mm 2 / s, more preferably 1000 mm 2 / s to 4500 mm 2 / s, and even more preferably 1500 mm 2 / s to 4200 mm 2It is even more preferable that the viscosity of the surfactant at 25°C is within the above range. When the cured underfill material is heated during rework, the amount of surfactant seeping into the interface with the substrate is appropriate, and the cured underfill material tends to peel off easily from the substrate.

[0090] If a surfactant is included, the surfactant content is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and more preferably 5 parts by mass or more, per 100 parts by mass of the radical polymerizable compound. Furthermore, from the viewpoint of preventing the surfactant from seeping into the interface with the substrate, the surfactant content is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and more preferably 20 parts by mass or less, per 100 parts by mass of the radical polymerizable compound.

[0091] [Coupling Agent] The underfill material may contain a coupling agent as needed. When the underfill material contains a coupling agent, it tends to strengthen the interfacial adhesion between the radical polymerizable compound and the inorganic filler, or between the radical polymerizable compound and the components of the electronic component. There are no particular restrictions on the type of coupling agent, and conventionally known ones can be used. Examples include silane compounds having primary and / or secondary and / or tertiary amino groups, epoxysilanes, mercaptosilanes, alkylsilanes, ureidosilanes, vinylsilanes, (meth)acrylsilanes, and various other silane compounds, titanium compounds, aluminum chelates, and aluminum / zirconium compounds. The coupling agent may be used alone or in combination of two or more types.

[0092] As coupling agents, for example, monomers or oligomers may be used. Examples of monomer coupling agents include vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, glycidoxyoctyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropyltriethoxysilane, γ-(N γ-(N,N-dimethyl)aminopropyltrimethoxysilane, γ-(N,N-diethyl)aminopropyltrimethoxysilane, γ-(N,N-dibutyl)aminopropyltrimethoxysilane, γ-(N-methyl)anilinopropyltrimethoxysilane, γ-(N,N-ethyl)anilinopropyltrimethoxysilane, γ-(N,N-dimethyl)aminopropyltriethoxysilane, γ-(N,N-diethyl)aminopropyltriethoxysilane, γ-(N,N-dibutyl)aminopropyltriethoxysilane, γ-(N-methyl)anilinopropyltriethoxysilane, γ-(N-ethyl)anilinopropyltriethoxysilane, γ-(N,N-dimethyl)aminopropylmethyldimethoxysilane, γ-(N,Silane coupling agents such as N-dibutyl)aminopropylmethyldimethoxysilane, γ-(N-methyl)anilinopropylmethyldimethoxysilane, γ-(N-ethyl)anilinopropylmethyldimethoxysilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilazane, vinyltrimethoxysilane, hexenyltrimethoxysilane, octenyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, methacryloxyoctyltrimethoxysilane, etc.; isopropyltriisostearoyl titanate, isopropyltris(dioctylpyrophosphate) titanate, etc. Examples of titanate coupling agents include sopropyltri(N-aminoethyl-aminoethyl)titanate, tetraoctylbis(ditridecylphosphite)titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecylphosphite)titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyltrioctanoyltitanate, isopropyldimethacrylateisostearoyltitanate, isopropyltridodecylbenzenesulfonyltitanate, isopropylisostearoyldiacrylictitanate, isopropyltri(dioctylphosphate)titanate, isopropyltricumylphenyl titanate, and tetraisopropylbis(dioctylphosphite)titanate.

[0093] Furthermore, examples of oligomer coupling agents include methyl-based, methyl / phenyl-based, propyl / phenyl-based, epoxy-modified, mercapto-modified, amine-modified, (meth)acrylic-modified, or polyester resin-modified alkoxy oligomers.

[0094] The content of the coupling agent in the underfill material is not particularly limited. From the viewpoint of adhesion, fluidity, etc., the content of the coupling agent is preferably 0.01% to 20% by mass, and more preferably 0.01% to 10% by mass, relative to the total amount of radical polymerizable compounds.

[0095] [Other Components] In addition to the components mentioned above, the underfill material may contain various additives such as polymerization inhibitors, flexible agents, curing accelerators, and ion exchangers. The underfill material may also contain various additives known in the art, as needed, in addition to the additives exemplified below.

[0096] (Polymerization inhibitors) Examples of polymerization inhibitors include phenolic compounds such as hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and pyrogallol; and hindered amine compounds.

[0097] (Flexible Agent) The underfill material may contain a flexible agent from the viewpoint of improving thermal shock resistance and reducing stress on semiconductor elements. The type of flexible agent is not particularly limited, and those commonly used in this field, such as silicone rubber, acrylic elastomer, and phenoxy resin, may be used. Among these, rubber particles are preferred as the flexible agent. Examples of rubber particles include styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), butadiene rubber (BR), urethane rubber (UR), and acrylic rubber (AR). One type of flexible agent may be used alone, or two or more types may be used in combination.

[0098] (Catalyst) For promoting the condensation reaction of the coupling agent, and the reaction between the silanol groups in the coupling agent and the silanol groups of an inorganic filler such as silica, to improve the dispersibility of the inorganic filler, reduce the viscosity of the underfill material, etc., a catalyst such as an acid that supplies protons or a Lewis acid may be added. Among these, as the Lewis acid, a chelating agent containing a metal species is preferred from the viewpoint of storage stability. Examples of the chelating agent containing a metal species include chelating agents of aluminum, boron, cobalt, titanium and the like. The content of the Lewis acid is preferably 0.001 parts by mass to 1.0 parts by mass, more preferably 0.002 parts by mass to 0.8 parts by mass, and even more preferably 0.005 parts by mass to 0.6 parts by mass, relative to 100 parts by mass of the inorganic filler.

[0099] (Ion Exchanger) The underfill material may contain an ion exchanger as necessary. When the underfill material contains an ion exchanger, the migration resistance, moisture resistance, high-temperature standing properties and the like of a semiconductor element such as an IC tend to be improved. Examples of the ion exchanger include compounds represented by the following compositional formula (A) or (B). Mg 1-X Al X (OH) 2 (CO 3 ) X / 2 ·mH 2 O ··· (A) (0<X≤0.5, m is a positive number) BiO x (OH) y (NO 3 ) z  ··· (B) (0.9≤x≤1.1, 0.6≤y≤0.8, 0.2≤z≤0.4)

[0100] The added amount of the ion exchanger is preferably 0.1 mass% to 3.0 mass%, and more preferably 0.3 mass% or more and 1.5 mass% or less. The volume average particle diameter of the ion exchanger is preferably 0.1 μm to 3.0 μm. The volume average particle diameter of the ion exchanger can be measured as the particle diameter (D50) at which the cumulative total from the small diameter side reaches 50% in the volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution analyzer. The maximum particle diameter of the ion exchanger is preferably 10 μm.

[0101] An example of the compound represented by formula (A) above is the commercially available DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd., trade name). An example of the compound represented by formula (B) above is the commercially available IXE500 (manufactured by Toagosei Co., Ltd., trade name). In addition, other anion exchangers may be added as needed. The type of anion exchanger is not particularly limited, and conventionally known ones can be used. For example, hydrated oxides of elements selected from magnesium, aluminum, titanium, zirconium, antimony, etc. Anion exchangers may be used individually or in combination of two or more types.

[0102] (Other additives) The underfill material may contain other additives as needed, such as dyes, colorants such as carbon black, diluents, leveling agents, and defoamers.

[0103] [Method for preparing underfill material] The resin liquid composition may be prepared by any method as long as the various components can be uniformly dispersed and mixed. For example, it can be obtained by weighing the components, mixing and kneading them using a mixer, mixing roll, planetary mixer, etc., and degassing as necessary.

[0104] [Physical Properties of Underfill Material] (Viscosity) From the viewpoint of fluidity, the viscosity of the underfill material is preferably 100 Pa·s or less, more preferably 50 Pa·s or less, and even more preferably 30 Pa·s or less at 25°C. The viscosity of the underfill material at 25°C is measured using an EHD type rotational viscometer. Specifically, it can be measured by the method described in the examples.

[0105] Furthermore, from the viewpoint of filling properties when filling narrow gaps with underfill material at temperatures around 60°C to 100°C for applications such as underfill material, the viscosity of the underfill material at 80°C is preferably, for example, 1 Pa·s or less, and more preferably 0.5 Pa·s or less. The viscosity of the underfill material at 80°C is measured using a rheometer. Specifically, it can be measured by the method described in the examples.

[0106] (Heat generation) The heat generation of the underfill material is not particularly limited. However, from the viewpoint of increasing the crosslinking density and preventing cracks, the heat generation of the underfill material is preferably 60 J / g or more, more preferably 70 J / g or more, and even more preferably 80 J / g or more. The heat generation of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0107] (Temperature at the peak of the exothermic reaction) The temperature at the peak of the exothermic reaction of the underfill material (hereinafter also referred to as the "exothermic reaction peak temperature") is not particularly limited. From the viewpoint of enabling processing at low temperatures, the exothermic reaction peak temperature of the underfill material is preferably 160°C or lower, more preferably 150°C or lower, and even more preferably 140°C or lower. Furthermore, from the viewpoint of suppressing viscosity increase during filling, the exothermic reaction peak temperature of the underfill material is preferably 90°C or higher, more preferably 95°C or higher, and even more preferably 100°C or higher. The exothermic reaction peak temperature of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0108] (Onset Temperature of Heat Generation Peak) The onset temperature of the heat generation peak of the underfill material (hereinafter also referred to as the "heat generation onset temperature") is not particularly limited. From the viewpoint of enabling processing at low temperatures, the heat generation onset temperature of the underfill material is preferably 150°C or lower, more preferably 140°C or lower, and even more preferably 130°C or lower. Furthermore, from the viewpoint of suppressing viscosity increase during filling, the heat generation onset temperature of the underfill material is preferably 80°C or higher, more preferably 85°C or higher, and even more preferably 90°C or higher. The heat generation onset temperature of the underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0109] [Physical Properties of Cured Underfill Material] In the measurement of the heat generation, linear thermal expansion coefficient, elastic modulus, fracture energy, and glass transition temperature of the cured underfill material described below, the cured material shall be assumed to be obtained by heating the underfill material at 120°C for 2 hours.

[0110] (Heat Generation) The progress of curing of the underfill material can be determined from the amount of heat generated by the underfill material after curing. From the viewpoint of suppressing tack and changes in physical properties after curing of the cured material, the amount of heat generated by the cured material is preferably 20% or less, more preferably 10% or less, even more preferably 8% or less, and particularly preferably 5% or less compared to the amount of heat generated before curing. The amount of heat generated by the cured underfill material is measured using a differential scanning calorimeter. Specifically, it can be measured by the method described in the examples.

[0111] (Linear Thermal Expansion Coefficient) The linear thermal expansion coefficient of the underfill material when it is cured is not particularly limited. For example, the linear thermal expansion coefficient (CTE1) obtained by measuring the temperature increase from 0°C to 300°C at 5°C / min using the compression method, and measuring it as the slope of the tangent between 10°C and 30°C, is preferably 35 ppm / K or less, more preferably 32 ppm / °C or less, even more preferably 30 ppm / K or less, and particularly preferably 28 ppm / K or less. When the CTE1, which is the linear thermal expansion coefficient below the glass transition temperature, is 35 ppm / K or less, the occurrence of bump cracks during reflow tends to be suppressed and the temperature cycle resistance characteristics tend to improve. The linear thermal expansion coefficient of CTE1 may be 15 ppm / K or more.

[0112] Furthermore, the linear thermal expansion coefficient (CTE2), determined by measuring the temperature increase from 0°C to 300°C at a rate of 5°C / min using the compression method, is preferably 130 ppm / °C or less, more preferably 115 ppm / °C or less, and even more preferably 100 ppm / °C or less. When the CTE2, which is the linear thermal expansion coefficient above the glass transition temperature, is 115 ppm / °C or less, the sealing portion tends to become even less likely to peel off from the substrate.

[0113] The amount of linear thermal expansion of the underfill material when it has been cured is not particularly limited between 50°C and 220°C. For example, when the temperature is increased from 0°C to 300°C at a rate of 5°C / min using the compression method, the amount of linear expansion between 50°C and 220°C is preferably 9000 μm / m or less, more preferably 8500 μm / m or less, and particularly preferably 7000 μm / m or less. When the amount of linear thermal expansion in this temperature range is 9000 μm / m or less, the amount of warping tends to be suppressed.

[0114] The linear thermal expansion coefficient can be measured by TMA (thermomechanical analysis). Specifically, it can be measured by the method described in the examples.

[0115] (Modulus of Elasticity) The modulus of elasticity of the underfill material when it is cured is not particularly limited. For example, from the viewpoint of reducing warping, the modulus of elasticity of the underfill material when it is cured is preferably 5.0 GPa or higher at room temperature (25°C), more preferably 5.5 GPa or higher, and even more preferably 6.0 GPa or higher. Also, from the same viewpoint, the modulus of elasticity of the underfill material when it is cured is preferably 0.5 GPa or higher at 240°C, more preferably 0.75 GPa or higher, and even more preferably 1.0 GPa or higher.

[0116] Furthermore, from the viewpoint of improving conformability to substrates, etc., by lowering the elastic modulus, for example, the elastic modulus at room temperature (25°C) when the underfill material is cured is preferably 8.0 GPa or less, more preferably 7.5 GPa or less, and even more preferably 7.0 GPa or less. From a similar viewpoint, the elastic modulus at 240°C when the underfill material is cured is preferably 1.25 GPa or less, more preferably 1.00 GPa or less, and even more preferably 0.75 GPa or less.

[0117] The elastic modulus of the underfill material after curing can be measured by DMA (dynamic viscoelasticity measurement). Specifically, it can be measured by the method described in the examples.

[0118] (Glass Transition Temperature) The glass transition temperature (Tg) of the underfill material when it is cured is not particularly limited, but is preferably 60°C or higher, more preferably 70°C or higher, and even more preferably 80°C or higher. When the glass transition temperature is 60°C or higher, the protection of bumps at high temperatures is high and wire breakage tends to occur less easily. The glass transition temperature of the cured underfill material can be measured by DMA (dynamic viscoelasticity measurement). Specifically, it can be measured by the method described in the examples.

[0119] [Applications of Underfill Material] In one embodiment, the underfill material of this disclosure is used to seal a connection portion of an electronic component device comprising an electronic component and a substrate electrically connected to the electronic component via a connection portion. Details of the configuration of the electronic component device and the sealing method are described below. The underfill material of this disclosure may also be used in compression molding.

[0120] <Electronic component apparatus> The electronic component apparatus of the present disclosure comprises an electronic component, a substrate electrically connected to the electronic component via a connection portion, and a cured underfill material of the present disclosure that seals the connection portion.

[0121] Examples of electronic components include active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, resistor arrays, coils, and switches.

[0122] Examples of substrates include lead frames, pre-wired tape carriers, printed circuit boards (rigid or flexible), glass, and silicon wafers.

[0123] In the electronic component device of this disclosure, the electronic component and the substrate are electrically connected via a connection part. Examples of connection parts include bumps. For example, the bump may be a bump made of copper pillars.

[0124] Examples of electronic component devices include flip-chip semiconductor devices obtained by flip-chip bonding electronic components onto a substrate using bump connections. Examples of flip-chip semiconductor devices include BGA (Ball Grid Array), LGA (Land Grid Array), and COF (Chip On Film).

[0125] Electronic components may be high-density or large in size. Generally, the area of ​​a large substrate is 50 x 50 mm. 2 The size may be greater than or equal to 60 x 60 mm. 2 The size may be greater than or equal to 70 x 70 mm. 2 The above is also acceptable. Even with electronic components having such enlarged substrates, the underfill material of this disclosure is suitably applicable because it has excellent injection properties. Furthermore, because the underfill material of this disclosure has excellent injection properties, the electronic components may be of conventional size. An example of an electronic component of conventional size is a semiconductor chip with a length of 10 mm and a width of 10 mm.

[0126] In the electronic component device of this disclosure, the connection portion is sealed with a cured underfill material of this disclosure. The sealing method is not particularly limited and includes dispensing, casting, printing, and the like.

[0127] <Method for Manufacturing an Electronic Component Device> The method for manufacturing an electronic component device according to the present disclosure includes a step of sealing the connection portion between an electronic component and a substrate electrically connected to the electronic component via a connection portion with the underfill material according to the present disclosure. The electronic component, substrate, underfill, etc. are as described above.

[0128] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0129] <Preparation of Underfill Material> The components used in the underfill material of the examples and comparative examples are shown below.

[0130] Radical polymerizable compound M1: 4,4'-diphenylmethanedimaleimide; Radical polymerizable compound M2: 1,6'-bismaleimide-(2,2,4-trimethyl)hexane; Radical polymerizable compound M3: The polymaleimide resin (A1) mentioned above; a polymaleimide resin in which an aromatic ring substituted with one hydrocarbon group having 1 to 18 carbon atoms is bonded to the nitrogen atom of a maleimide group. Radical polymerizable compound M3 was prepared according to Example 1 of Japanese Patent Application Publication No. 2024-4392, and the solvent was removed in a vacuum dryer heated to 70°C for 6 hours until the solid content concentration reached 95% or more. The solid content concentration was calculated from the weight change rate before and after heating by heating the material after the solvent was removed in an oven at 175°C for 1 hour. Radical polymerizable compound A1: Tripropylene glycol diacrylate Radical polymerizable compound A2: Tricyclodecanedimethanol dimethacrylate Radical polymerizable compound A3: Tricyclodecanedimethanol diacrylate Radical polymerizable compound A4: 4-Hydroxybutyl acrylate

[0131] • Epoxy resin 1: Bisphenol F type epoxy resin (epoxy equivalent 160 g / eq) • Epoxy resin 2: Aminophenol type epoxy resin (epoxy equivalent 98 g / eq) • Hardener 1: Amine hardener (amine value 630 KOH mg / g) • Hardener 2: Diethyldiaminodiphenylmethane (amine equivalent: 63 g / eq)

[0132] • Surfactant 1: Dimethyl silicone oil having polyether and amine moieties in its side chain (viscosity 3300 mm at 25°C) 2 / s) • Surfactant 2: Phosphate ester-based wetting and dispersing agent

[0133] • Peroxide 1: t-butyl peroxyl laurate (10-hour half-life temperature 98.3°C) • Peroxide 2: di-t-butyl peroxide (10-hour half-life temperature 123.7°C)

[0134] • Inorganic filler 1: Silica particles (average particle size: 0.5 μm) The volume-average particle size of the above inorganic filler is the median diameter (D50). This volume-average particle size was measured using a laser diffraction scattering particle size analyzer.

[0135] Coupling agent 1: 3-glycidoxypropyltrimethoxysilane; Coupling agent 2: γ-methacryloxypropyltrimethoxysilane

[0136] Each component was blended in the composition (parts by mass) shown in Table 1 or Table 2, and after kneading and dispersing using a three-roll mill and a vacuum grinder, the underfill materials for the examples and comparative examples were prepared.

[0137]

[0138]

[0139] The inorganic filler content in Tables 1 and 2 represents the inorganic filler content (mass%) relative to the total amount of the composition. In Comparative Example 1, the curing agents 1 and 2 were blended in amounts of 0.5 eq each per 1 eq of the total epoxy groups of the epoxy resin.

[0140] <Evaluation> (Differential Scanning Calorimetry of Underfill Material) The underfill material was placed in a differential scanning calorimeter (DSC) (TA Instruments "DSC Q200") and heated from 25°C to 500°C at a heating rate of 10°C / min to obtain a DSC curve. The temperature at the rise point of the exothermic peak from the baseline (onset) and the temperature at the top of the exothermic peak (top) were determined. Furthermore, the peak area of ​​the exothermic peak was determined from the DSC curve using a method compliant with JIS K7122:2012, and the amount of heat generated was calculated as the transition heat.

[0141] <Pot life at 25°C> The viscosity at 25°C after mixing was measured and defined as the initial viscosity. Then, the mixture was stored at 25°C for a predetermined time, and the viscosity at 25°C after storage was measured. The viscosity increase rate was then calculated according to the following formula: Viscosity increase rate = (Viscosity after predetermined storage time - Initial viscosity) / Initial viscosity × 100 If the viscosity increase rate after one week of storage is 50% or less, the pot life is judged to be one week or more and evaluated as A. If the viscosity increase rate after one week of storage is more than 50%, the pot life is judged to be less than one week and evaluated as B.

[0142] <Long-term filling capability> The rheometer measuring jig was heated to the same temperature as the filling temperature shown in Table 2 or Table 3, and the underfill material was dropped onto it. The viscosity was continuously measured while maintaining the filling temperature, and the change in viscosity over time at the filling temperature was measured. The viscosity increase rate was then calculated according to the following formula: Viscosity increase rate = (Viscosity after holding at filling temperature for 30 minutes - Initial viscosity at filling temperature) / (Initial viscosity at filling temperature) × 100 If the viscosity increase rate after holding for 30 minutes is 100% or less, it is judged that filling is possible for 30 minutes and is evaluated as A. If the viscosity increase rate after holding for 30 minutes is more than 100%, it is judged that filling is not possible for 30 minutes and is evaluated as B.

[0143] <Differential Scanning Calorimetry of Cured Materials> Test specimens were prepared by curing underfill material at 120°C for 2 hours. These specimens were placed in a differential scanning calorimeter (DSC) (TA Instruments "DSC Q200") and heated from 25°C to 500°C at a heating rate of 10°C / min to obtain a DSC curve. The peak area of ​​the exothermic peak was determined from the DSC curve according to the method in accordance with JIS K7122:2012, and the amount of heat generated was calculated as the transition heat.

[0144] <Evaluation of Linear Thermal Expansion Coefficient and Amount of Linear Expansion> Test specimens were prepared by curing the underfill material at 120°C for 2 hours. The cured underfill material was cut to a size of φ8 mm × 20 mm, and the temperature was measured by increasing the temperature from 0°C to 300°C at a rate of 5°C / min using a thermomechanical analyzer (TA Instruments "TMA450") by compression. The tangent slope between 10°C and 30°C was defined as CTE1, the tangent slope between 180°C and 200°C was defined as CTE2, and the amount of linear expansion between 50°C and 220°C was determined.

[0145] <Evaluation of Elastic Modulus> Test specimens were prepared by curing the underfill material at 120°C for 2 hours. The cured underfill material was cut to a size of 30 mm × 2 mm × 1 mm, and the storage modulus was determined at 30°C and 240°C by raising the temperature from 20°C to 300°C at a rate of 5°C / min using a dynamic viscoelasticity measuring device (DMA, UBM Corporation "Rheogel E-4000") under the conditions of a span distance of 20 mm and a frequency of 1 Hz.

[0146] <Glass Transition Temperature> Test specimens were prepared by curing the underfill material at 120°C for 2 hours. Measurements were performed using the same apparatus and conditions as for the evaluation of the elastic modulus above, and the glass transition temperature (DMA) (°C) was determined from the value of tanδ.

[0147] <Evaluation of Adhesion> Underfill material was formed on a copper plate or silicon wafer to a diameter of 3 mm and a height of 1 mm, and these were used as test specimens. The curing conditions were 120°C for 2 hours. For the obtained test specimens, the shear adhesive strength (MPa) was determined at room temperature (25°C) or while maintaining the stage temperature at 260°C, at a shear rate of 50 μm / s using a bond tester (Nordson Advanced Technologies, Inc., Series 4000).

[0148]

[0149]

[0150]

[0151] The onset temperature of the underfill materials in Examples 1 to 6 was 109 to 116°C, and even if the substrate temperature during injection of the underfill material was set to, for example, 80°C, viscosity increase during injection was suppressed. In fact, Examples 1 to 6 had a longer pot life at 80°C compared to the underfill material of Comparative Example 1, which contained a conventional epoxy resin.

[0152] Furthermore, since the onset temperature of the underfill materials in Examples 1 to 6 is 120°C or lower, the curing reaction can proceed by heating at 120°C. In contrast, the onset temperature of the underfill material in Comparative Example 1 was 164°C, and a cured product could not be obtained at a curing temperature of 120°C.

[0153] Furthermore, while the underfill material of Comparative Example 1 showed significant thickening at 25°C, reaching a thickening rate of 3430.1% after one week of storage, Examples 1 to 4 showed suppressed thickening at 25°C, demonstrating superior storage stability.

[0154] The underfill material of Comparative Example 2, which did not contain a maleimide compound as a radical polymerizable compound, exhibited lower adhesive strength to Cu compared to the underfill materials of Examples 1 to 6. Furthermore, although the underfill material of Comparative Example 2 had an onset temperature of 120°C or lower, and a cured product could be obtained by heating at 120°C, cracks occurred in the cured product.

[0155] Comparative Example 3, which uses a peroxide with a 10-hour half-life temperature exceeding 110°C, has an onset temperature exceeding 120°C, indicating that it is unsuitable for a curing heating process at 120°C. In fact, a cured product could not be obtained at a curing temperature of 120°C.

[0156] The disclosure of Japanese Patent Application No. 2025-077584 is incorporated in its entirety by reference. All documents, patent applications, and technical standards in this disclosure are incorporated by reference to the same extent as if each individual document, patent application, and technical standard had been specifically and individually noted as being incorporated by reference.

Claims

1. An underfill material comprising a radical polymerizable compound and a peroxide having a 10-hour half-life temperature of 90°C to 110°C, wherein the radical polymerizable compound comprises a maleimide compound.

2. The underfill material according to claim 1, wherein the radical polymerizable compound further comprises a (meth)acrylic compound.

3. The underfill material according to claim 1 or claim 2, wherein the amount of heat generated by curing at 120°C for 2 hours is 20% or less of the amount of heat generated before curing.

4. The underfill material according to claim 1 or claim 2, which does not contain any polymerizable compounds other than radical polymerizable compounds, or the content of other polymerizable compounds relative to the total amount of other polymerizable compounds and radical polymerizable compounds is 20% by mass or less.

5. The underfill material according to claim 1 or claim 2, further comprising an inorganic filler.

6. The underfill material according to claim 5, comprising 20% ​​by mass or more of an inorganic filler.

7. The underfill material according to claim 1 or claim 2, wherein the amount of linear expansion at 50°C to 220°C when cured is 9000 μm / m or less.

8. An electronic component apparatus comprising: an electronic component; a substrate electrically connected to the electronic component via a connection portion; and a cured underfill material according to claim 1 or claim 2 that seals the connection portion.

9. A method for manufacturing an electronic component device, comprising the step of sealing the connection portion between an electronic component and a substrate electrically connected to the electronic component via a connection portion with the underfill material described in claim 1 or claim 2.