Polygonal can manufacturing method, polygonal can manufacturing system, and polygonal can
The method addresses waviness in square cans by incorporating intermediate and residual stress relief steps to control ironing ratios, improving shape stability and ensuring proper battery fit.
Patent Information
- Application Number
- PCT/JP2026/011260
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-03-23
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for manufacturing square cans, particularly those used as battery cases, suffer from waviness in the long side direction due to unbalanced thermal shrinkage and residual stress, which can prevent proper housing of batteries.
A method and system that includes intermediate forming, rectangular forming, and residual stress relief steps to alleviate residual stress, specifically by controlling the ratio of ironing amounts in drawing and residual stress relief processes to reduce compressive residual stress on long sides, thereby preventing waviness.
The method enhances shape stability by reducing compressive residual stress on long sides, preventing waviness and ensuring proper fit of batteries in the can.
Smart Images

Figure JP2026011260_12112026_PF_FP_ABST
Abstract
Description
Square can manufacturing method, square can manufacturing system, and square can
[0001] The present invention relates to a square can manufacturing method and a square can manufacturing system for manufacturing a square can that includes a bottom surface portion, and a square tubular portion having a pair of long side surfaces and a pair of short side surfaces, and particularly relates to a square can manufacturing method and a square can manufacturing system for a square can used as a battery case for a lithium ion battery or the like.
[0002] Conventionally, as a method for manufacturing a metallic square can having a bottom surface portion, a pair of long side surfaces and a pair of short side surfaces, it is known to manufacture the square can by subjecting a metal blank to multiple drawing processes or drawing and ironing processes (see, for example, Patent Document 1).
[0003] In the square can manufacturing method known in Patent Document 1, an elliptical blank 7 is cut out from a coil material by a press machine 6 (the names and reference numerals of components in this paragraph follow the notations in Patent Document 1), the blank 7 is drawn to form an intermediate product 14 having a substantially elliptical cross-sectional shape, then the intermediate product 14 is drawn by a press mechanism 21 to gradually deform the outer diameter shape, and the process is performed by ironing to gradually reduce the plate thickness or stretching the side wall portions upward. The drawing and ironing process by the press machine 21 consists of the first step to the sixth step. When a final product with a rectangular cross-sectional shape is formed from the intermediate product 14 by drawing, and ironing is performed to gradually reduce the plate thickness of the side wall portions in the process where the outer diameter shape changes, if the curvature radius of the corner portion 20 sandwiched between adjacent side wall portions becomes less than a predetermined value, the ironing process is performed such that the difference between the ironing rate of one side wall portion sandwiching the corner portion 20 and the ironing rate of the other side wall portion is equal to or less than a predetermined difference, whereby the side wall portions of the intermediate product 14 or the final product can be ironed without causing wrinkles or fractures on each side wall portion.
[0004] JP 2021-158014 A
[0005] However, in the rectangular can manufacturing method known from Patent Document 1, etc., drawing and ironing is performed on the short and long sides in all of the first to sixth steps. However, when the upper end is trimmed to the desired height after the final product has been formed by drawing and ironing, there was a risk of waviness occurring in the long side direction, as shown in Figure 6B. This waviness in the long side could prevent the battery from being properly housed in the rectangular can. It was found that the waviness in the long side direction is due to the fact that the short side is processed in a manner similar to cylindrical drawing and shrinks in the circumferential direction, while the long side is generally folded and hardly shrinks in the circumferential direction, and that the temperature of the short side tends to be higher than that of the long side due to the heat generated in the workpiece and mold in each step, resulting in unbalanced thermal shrinkage, and that excessive compressive residual stress exists in the long side after the final product has been formed.
[0006] The present invention aims to solve these problems and to provide a method and system for manufacturing rectangular cans that have a simple configuration, alleviate residual stress in the rectangular cylindrical portion, and have excellent shape stability.
[0007] The present invention provides a method for manufacturing a rectangular can, comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, and comprising an intermediate forming step of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a rectangular forming step of forming the intermediate molded body into a rectangular shape by drawing or drawing and ironing, and a residual stress relief step of relieving residual stress in the intermediate molded body after the rectangular forming step, thereby solving the aforementioned problems. Furthermore, the present invention provides a rectangular can manufacturing system, comprising an intermediate forming means for forming an intermediate molded body by drawing or drawing and ironing a metal blank, a rectangular forming means for forming the intermediate molded body into a rectangular shape by drawing or drawing and ironing, and a residual stress relief means for relieving residual stress in the intermediate molded body formed into a rectangular shape by the rectangular forming means, thereby solving the aforementioned problems. Furthermore, the rectangular can of the present invention is a rectangular can comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, wherein the pair of long sides have tensile residual stress at the center in the long side direction and at the top in the height direction, thereby solving the aforementioned problems.
[0008] According to the invention of claim 1 or claim 3, by having an intermediate forming step of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a square forming step of forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body, and a residual stress relief step of relieving the residual stress of the intermediate molded body after the square forming step, or by having an intermediate forming means of forming an intermediate molded body by drawing or drawing and ironing a metal blank, a square forming means of forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body, and a residual stress relief means of relieving the residual stress of the intermediate molded body formed into a square shape by the square forming means, the residual stress in the compression direction present on the pair of long sides is relieved, that is, the residual stress on the pair of long sides is reduced, thereby suppressing the occurrence of waviness on the pair of long sides when the upper end is trimmed.
[0009] According to the configurations described in claims 2 and 4, the residual stress relief step includes ironing, or the residual stress relief means includes residual stress relief ironing means, so that the height and thickness of the intermediate molded body can be formed to the dimensions of a square can by ironing or residual stress relief ironing means, while relieving the compressive residual stress present on a pair of long sides with a simple configuration. Furthermore, if I1 is the amount of ironing due to the drawing process in the square forming process and I2 is the amount of ironing due to the residual stress relief process, then satisfying the relationship 0 < I2 / (I1 + I2) ≤ 0.6, or if I1 is the amount of ironing due to the drawing process in the square forming means and I2 is the amount of ironing due to the residual stress relief ironing means in the residual stress relief means, then satisfying the relationship 0 < I2 / (I1 + I2) ≤ 0.6, then the effect of residual stress relief by the ironing or residual stress relief ironing means can be further enhanced, and the shape stability of the square can can be improved. If I2 / (I1 + I2) = 0, then ironing is not performed in the residual stress relief process, and therefore the residual stress present on the pair of long sides cannot be relieved. If the relationship 0.6 < I2 / (I1+I2) holds, the shape stability of the square can may be impaired because the amount of ironing by ironing in the residual stress relaxation process is greater than the amount of ironing by drawing ironing in the square forming process, or because the amount of ironing by the residual stress relaxation ironing means in the residual stress relaxation means is greater than the amount of ironing by drawing ironing in the square forming means.
[0010] According to the invention of claim 5, the pair of long sides have tensile residual stress in the center of the long side direction and the upper part in the height direction, thereby preventing waviness in the long side direction from occurring on the pair of long sides and improving the shape stability of the rectangular can. According to the configuration of claim 6, the tensile residual stress in the center of the long side direction and the upper part in the height direction is 20 to 60 MPa, which more effectively prevents waviness in the long side direction from occurring on the pair of long sides and improves the shape stability of the rectangular can. If the tensile residual stress is less than 20 MPa, it may not be able to absorb the effects of residual stress (compressive residual stress) in other parts of the long side, and waviness in the long side direction may occur. If the tensile residual stress is greater than 60 MPa, the upper part of the long side may become weaker against impacts, etc.
[0011] An explanatory diagram showing a square can manufactured by a square can manufacturing method according to one embodiment of the present invention. A bottom view of the square can shown in Figure 1A. An explanatory diagram showing a metal blank in the blank preparation process. An explanatory diagram showing a metal blank after the coining process. An explanatory diagram showing the first intermediate molding unit in the first intermediate molding process. An explanatory diagram showing the first intermediate molded body formed by the first intermediate molding unit. An explanatory diagram showing the second intermediate molding unit in the second intermediate molding process. An explanatory diagram showing the second intermediate molded body formed by the second intermediate molding unit. An explanatory diagram showing the square molding unit in the square molding process. An explanatory diagram showing the third intermediate molded body formed by the square molding unit. An explanatory diagram showing the residual stress relaxation unit in the residual stress relaxation process. An explanatory diagram showing the fourth intermediate molded body formed by the residual stress relaxation unit. An explanatory diagram showing the drawing and ironing process of the square molding process as seen from the direction of the long side of the planned long side. An enlarged view showing the area enclosed by circle A in Figure 4A. An explanatory diagram showing the ironing process of the residual stress relaxation process as seen from the direction of the long side of the planned long side. An enlarged view showing the area enclosed by circle B in Figure 5A. An explanatory diagram from above showing a rectangular can manufactured by the rectangular can manufacturing method according to one embodiment of the present invention. An explanatory diagram from above showing a rectangular can with undulations on its long side.
[0012] Below, an embodiment of the present invention, a method for manufacturing rectangular cans and a rectangular can manufacturing system 100, will be described with reference to the drawings.
[0013] <Rectangular Can 200> First, the rectangular can 200 manufactured by the rectangular can manufacturing method and rectangular can manufacturing system 100 is made of a metal such as aluminum, and in this embodiment is used as a case for a lithium-ion battery, and as shown in Figures 1A and 1B, it has a flat (or substantially flat) bottom portion 210 and a rectangular cylindrical portion 220. The aluminum can be, for example, pure aluminum or aluminum alloys such as the JIS standard A1000 series, A3000 series, and A5000 series, but the A3000 series (for example, A3003) is more preferred.
[0014] As shown in Figure 1B, the bottom portion 210 is formed in a substantially rectangular shape (or rectangular shape) with a pair of long-side corner portions 230 and a pair of short-side corner portions 240 on its outer edge, which are corner portions that connect the bottom portion 210 and the rectangular cylindrical portion 220. The long-side corner portions 230 are portions that extend linearly (or substantially linearly) along the direction of the long side, and are formed to connect the bottom portion 210 and the long side portion 221, which is the long side surface of the bottom portion 210, as will be described later. The short-side corner portions 240 are portions that extend linearly (or substantially linearly) along the direction of the short side, forming a 90° angle with the long-side corner portions 230, and are formed to connect the bottom portion 210 and the short side portion 222, which is the short side surface of the bottom portion 210, as will be described later. Between the long-side corner portion 230 and the short-side corner portion 240, a bottom curved corner portion 250 is formed that is convex on the outer circumference, smoothly connecting the long-side corner portion 230 and the short-side corner portion 240. In this embodiment, the bottom curved corner portion 250 is formed with the same single radius of curvature (R).
[0015] As shown in Figure 1A, the rectangular cylindrical portion 220 has a pair of long sides 221 and a pair of short sides 222 that are arranged opposite each other in the direction of the short side. Each long side 221 is a flat (or substantially flat) portion formed to rise upward from the long side corner portion 230, as shown in Figure 1A, and the pair of long sides 221 are formed parallel to each other. Each short side 222 is a flat (or substantially flat) portion formed to rise upward from the short side corner portion 240, forming a 90° angle with the long side 221, as shown in Figure 1A, and the pair of short sides 222 are formed parallel to each other. Between the long sides 221 and the short sides 222, there is a rounded corner 223 that is formed to rise upward from the bottom curved corner portion 250 and smoothly connects the long sides 221 and the short sides 222, with the outer circumference being convex. In this embodiment, each corner surface 223 is formed by curving with the same single radius of curvature (R).
[0016] <Method for Manufacturing Square Cans> The method for manufacturing square cans is for manufacturing square cans 200, and as shown in Figures 2A to 3F, it includes a blank preparation step of preparing a metal blank 200A, a coining step of performing coining on predetermined locations on the metal blank 200A, a first intermediate forming step of performing a first drawing on the metal blank 200A after the coining step to form a first intermediate molded body 200B, a second intermediate forming step of performing a second drawing on the first intermediate molded body 200B to form a second intermediate molded body 200C, a square forming step of performing drawing and ironing on the second intermediate molded body 200C to form a square shape, a residual stress relief step of relieving residual stress on the third intermediate molded body 200D obtained by the square forming step, and a trimming step of cutting off unnecessary parts near openings such as flanges on the fourth intermediate molded body 200E obtained by the residual stress relief step. The coining step may be omitted as appropriate depending on the size of the square can and product specifications. Furthermore, a reforming process may be provided for the fourth intermediate molded body 200E obtained by the residual stress relaxation process, in which fine adjustments such as the dimensions and flatness of each part may be made. The reforming process may also be provided as a pre-process or post-process of the trimming process.
[0017] The following provides a detailed explanation of each step in the manufacturing process for rectangular cans.
[0018] First, as shown in Figure 2A, the blank preparation process involves forming a metal blank 200A by punching out a metal strip such as aluminum.
[0019] The coining process, as shown in Figure 2B, involves performing a coining process to reduce the thickness of the metal blank 200A by pressing it in the thickness direction at a predetermined location. In this embodiment, the coining process is performed to reduce the thickness of the metal blank 200A by pressing it in the thickness direction at the outer circumference of the long side of the planned bottom portion 210A (the portion that will become the bottom portion 210 in the state of the rectangular can 200).
[0020] The first intermediate forming process, as shown in Figures 2C and 2D, involves performing a first drawing process on the metal blank 200A that has undergone the coining process to form a cup-shaped first intermediate molded body 200B. Specifically, the first intermediate forming process is carried out by the first intermediate forming unit 110, which is the first intermediate forming means. The metal blank 200A is held down from above by a blank holder 113, which functions as a wrinkle suppressor to prevent wrinkles from forming on the first intermediate molded body 200B. The metal blank 200A is then pushed (pulled in) from above by a punch 112 into a die-processing through-hole 111a formed in the die 111, thereby plastically deforming the metal blank 200A and forming a cup-shaped first intermediate molded body 200B.
[0021] As shown in Figures 3A and 3B, the second intermediate molding process involves performing a second drawing process on the first intermediate molded body 200B obtained in the first intermediate molding process to form the second intermediate molded body 200C. In this embodiment, the drawing process in the second intermediate molding process and the configuration of the second intermediate molding unit 120, which is the second intermediate molding means, are the same as those of the first intermediate molding process and the first intermediate molding unit 110 described above. Therefore, the explanation of the first intermediate molding process and the first intermediate molding unit 110 is omitted by replacing the reference numerals in the 110s range in the specification and drawings with reference numerals in the 120s range.
[0022] As shown in Figures 3C, 3D, and 4A, the rectangular molding process involves drawing and ironing mainly on the cylindrical planned portion 220C of the second intermediate molded body 200C (the portion that will become the rectangular cylindrical portion 220 in the state of the rectangular can 200) in the gap between the punch 132 inserted into the die processing through hole 131a formed in the die 131, thereby forming the third intermediate molded body 200D. In addition, in the rectangular molding process, drawing and ironing is also performed on a part of the bottom planned portion 210C of the second intermediate molded body 200C (the portion that will become the bottom portion 210 in the state of the rectangular can 200).
[0023] In this embodiment, the configuration of the rectangular molding unit 130, which is the drawing and ironing process and rectangular molding means in the rectangular molding process, is the same as that of the first intermediate molding process and the first intermediate molding unit 110 described above, except for some configurations. Therefore, by replacing the reference numerals in the 110s shown in the specification and drawings relating to the first intermediate molding process and the first intermediate molding unit 110 with reference numerals in the 130s, the explanation of configurations other than the differences will be omitted. In this embodiment, the second intermediate molded body 200C is drawn by the rectangular molding unit 130 such that, when the length in the short side direction of the planned short side portion 222D of the third intermediate molded body 200D described later is set to 1, the length in the long side direction of the planned long side portion 221D of the third intermediate molded body 200D described later becomes 11.
[0024] As shown in Figures 3C and 4A, the die-machined inner circumferential surface 131b of die 131 has a pair of die long-side machining sections 131c that machine the planned long side portion 221C of the second intermediate molded body 200C (the portion that will become the long side portion 221 in the state of the rectangular can 200), and a pair of die short-side machining sections 131d that machine the planned short side portion 222C of the second intermediate molded body 200C (the portion that will become the short side portion 222 in the state of the rectangular can 200). Furthermore, as shown in Figures 3C and 4A, the punch-machined outer circumferential surface 132a of punch 132 has a pair of punch long-side machining sections 132b that work in cooperation with the die long-side machining sections 131c to machine the planned long side portion 221C of the second intermediate molded body 200C, and a pair of punch short-side machining sections 132c that work in cooperation with the die short-side machining section 131d to machine the planned short side portion 222C of the second intermediate molded body 200C. As a result, during the drawing and ironing process, the second intermediate molded body 200C is pushed (pulled in) into the gap between the die long side processing section 131c and the punch long side processing section 132b, thereby performing an ironing process that thins the plate thickness mainly on the long side planned section 221C of the second intermediate molded body 200C. At the same time, the second intermediate molded body 200C is pushed (pulled in) into the gap between the die short side processing section 131d and the punch short side processing section 132c, thereby performing a drawing and ironing process mainly on the short side planned section 222C and the corner side planned section 223C (the part that becomes the corner side 223 in the state of the square can 200) of the second intermediate molded body 200C. At this time, as shown in Figure 4B, the plate thickness 221Ct of the planned long side portion 221C of the second intermediate molded body 200C is reduced by ironing to the plate thickness 221Dt of the planned long side portion 221D of the third intermediate molded body 200D, which will be described later, and the plate thickness 222Ct of the planned short side portion 222C of the second intermediate molded body 200C is reduced by ironing to the plate thickness 222Dt of the planned short side portion 222D of the third intermediate molded body 200D, which will be described later.
[0025] As shown in Figures 3E, 3F, and 5A, the residual stress relief process involves ironing the cylindrical planned portion 220D of the third intermediate molded body 200D (the portion that will become the rectangular cylindrical portion 220 in the state of the rectangular can 200) in the gap between the die 141 and the punch 142 inserted into the die processing through hole 141a formed in the die 141, thereby forming the fourth intermediate molded body 200E. Specifically, the residual stress relief process is carried out by a residual stress relief unit 140, which is a residual stress relief ironing process included in the residual stress relief means. As shown in Figures 3E and 5A, with the punch 142 inserted from above the third intermediate molded body 200D, the punch 142 is moved relative to the die 141 (in this embodiment, the punch 142 is moved relative to the die 141, which is fixed in place). This pushes (pushes in) the third intermediate molded body 200D into the die-processed through-hole 141a with the punch 142, and the third intermediate molded body 200D is plastically deformed in the gap between the die-processed inner circumferential surface 141b of the die-processed through-hole 141a and the punched outer circumferential surface 142a of the punch 142 to form the fourth intermediate molded body 200E.
[0026] As shown in Figures 3E and 5A, the die-machined inner circumferential surface 141b of die 141 has a pair of die long-side machining sections 141c that machine the planned long side portion 221D of the third intermediate molded body 200D (the portion that will become the long side portion 221 in the state of the rectangular can 200), and a pair of die short-side machining sections 141d that machine the planned short side portion 222D of the third intermediate molded body 200D (the portion that will become the short side portion 222 in the state of the rectangular can 200). Furthermore, as shown in Figures 3E and 5A, the punch-machined outer circumferential surface 142a of punch 142 has a pair of punch long-side machining sections 142b that work in cooperation with the die long-side machining sections 141c to machine the planned long side portion 221D of the third intermediate molded body 200D, and a pair of punch short-side machining sections 142c that work in cooperation with the die short-side machining section 141d to machine the planned short side portion 222D of the third intermediate molded body 200D. As a result, during the ironing process, the third intermediate molded body 200D is pushed (pulled in) into the gap between the die's long side processing section 141c and the punch's long side processing section 142b, thereby performing ironing to reduce the thickness of the long side portion 221D of the third intermediate molded body 200D, while the third intermediate molded body 200D is pushed (pulled in) into the gap between the die's short side processing section 141d and the punch's short side processing section 142c, thereby performing ironing to reduce the thickness of the short side portion 222D of the third intermediate molded body 200D. At this time, as shown in Figure 5B, the plate thickness 221Dt of the planned long side portion 221D of the third intermediate molded body 200D is reduced by ironing to the plate thickness 221Et of the planned long side portion 221E of the fourth intermediate molded body 200E, which will be described later, and the plate thickness 222Dt of the planned short side portion 222D of the third intermediate molded body 200D is reduced by ironing to the plate thickness 222Et of the planned short side portion 222E of the fourth intermediate molded body 200E, which will be described later.
[0027] Furthermore, in this embodiment, if the amount of ironing due to the drawing process in the square molding process is I1 and the amount of ironing due to the residual stress relaxation process is I2, the configuration satisfies the relationship 0 < I2 / (I1 + I2) ≤ 0.6. In other words, with respect to the long side surface 221, if I1 is the amount of ironing due to the ironing process performed on the long side surface planned portion 221C of the second intermediate molded body 200C in the square molding process (the difference between the plate thickness 221Ct of the long side surface planned portion 221C of the second intermediate molded body 200C and the plate thickness 221Dt of the long side surface planned portion 221D of the third intermediate molded body 200D), and I2 is the amount of ironing due to the ironing process performed on the long side surface planned portion 221D of the third intermediate molded body 200D in the residual stress relaxation process (the difference between the plate thickness 221Dt of the long side surface planned portion 221D of the third intermediate molded body 200D and the plate thickness 221Et of the long side surface planned portion 221E of the fourth intermediate molded body 200E), then the structure is configured to satisfy the relationship 0 < I2 / (I1 + I2) ≤ 0.6. Furthermore, with respect to the short side 222, even if we define I1' as the amount of ironing due to the ironing process performed on the short side portion 222C of the second intermediate molded body 200C during the square molding process (the difference between the plate thickness 222Ct of the short side portion 222C of the second intermediate molded body 200C and the plate thickness 222Dt of the short side portion 222D of the third intermediate molded body 200D), and I2' as the amount of ironing due to the ironing process performed on the short side portion 222D of the third intermediate molded body 200D during the residual stress relaxation process (the difference between the plate thickness 222Dt of the short side portion 222D of the third intermediate molded body 200D and the plate thickness 222Et of the short side portion 222E of the fourth intermediate molded body 200E), the relationship 0 < I2' / (I1' + I2') ≤ 0.6 is still satisfied. Furthermore, as long as the above relationship of cutting amounts is satisfied, cutting amounts I1 and I1' may be equal or different, and cutting amounts I2 and I2' may also be equal or different. In addition, the measurement points for the plate thicknesses 221Ct, 221Dt, 221Et of each long side and 222Ct, 222Dt, 222Et of each short side, used to calculate the above cutting amounts, are the parts near the center of each long side and each short side. However, the measurement points are not particularly limited as long as they are at or near the center in the width direction of the side and at a height position on the vertical wall portion that is at or above the center and appropriately away from the upper edge in the height direction of the side.Furthermore, the measurement height position of the fourth intermediate molded body 200E may be the same as the measurement height position of the third intermediate molded body 200D, or it may be different, such as being set slightly higher to account for movement due to ironing.
[0028] The trimming process involves trimming and cutting off the flange portion 260E formed near the opening of the fourth intermediate molded body 200E obtained by the residual stress relaxation process, thereby forming the rectangular can 200. As a result, the planned cylindrical portion 220E of the fourth intermediate molded body 200E becomes the rectangular cylindrical portion 220 of the rectangular can 200, the planned long side portion 221E of the fourth intermediate molded body 200E becomes the long side portion 221 of the rectangular can 200, and the planned short side portion 222E of the fourth intermediate molded body 200E becomes the short side portion 222 of the rectangular can 200. Furthermore, the thickness of the long side 221 of the rectangular can 200 is the same as the thickness 221Et of the planned long side portion 221E of the fourth intermediate molded body 200E, and the thickness of the short side 222 of the rectangular can 200 is the same as the thickness 222Et of the planned short side portion 222E of the fourth intermediate molded body 200E.
[0029] In this embodiment, when the dimensional ratio of the long side portion 221D to the short side portion 222D of the third intermediate molded body 200D is large, the long side portion 221C of the second intermediate molded body 200C is subjected to drawing and ironing during the square molding process, and is stretched in the height direction (up and down direction in Figure 4A) while being bent. On the other hand, the short side portion 222C and the corner side portion 223C of the second intermediate molded body 200C are subjected to drawing and ironing, and are compressed in the circumferential direction. As a result, in the state of the third intermediate molded body 200D, there is an excessive residual stress (compressive residual stress) in the compression direction (direction toward the center of the long side of the long side portion 221D) of the long side portion 221D. Therefore, if the flange portion 260D formed near the opening of the third intermediate molded body 200D is cut off by trimming, the tension rigidity near the opening due to the flange portion 260D is lost, releasing the residual stress present in the planned long side portion 221D, causing waviness in the long side direction of the planned long side portion 221D and impairing its shape stability.
[0030] In contrast, in this embodiment, after the cylindrical planned portion 220C of the second intermediate molded body 200C is subjected to drawing in the square molding process, the cylindrical planned portion 220D of the third intermediate molded body 200D is subjected to drawing in the residual stress relaxation process under conditions that satisfy the above-mentioned relationship of drawing amount. As a result, the long side planned portion 221D of the third intermediate molded body 200D is compressed and deformed in the thickness direction, becoming thinner, while being stretched in the height direction, and the residual stress on the long side planned portion 221D of the third intermediate molded body 200D is reduced. Consequently, when the flange portion 260E of the fourth intermediate molded body 200E is cut off in the trimming process to form the square can 200, even if the tension rigidity near the opening due to the flange portion 260E is lost, the residual stress on the long side 221 is reduced, so that waviness in the long side direction does not occur on the long side 221, and the shape stability of the square can 200 can be improved. Furthermore, by satisfying the relationship 0 < I2 / (I1+I2) ≤ 0.6 between the amount of ironing I1 by the drawing process in the square molding process and the amount of ironing I2 by the ironing process in the residual stress relief process, the ironing process can be performed on the cylindrical planned portion 220D to the extent that the residual stress present in the long side planned portion 221D of the third intermediate molded body 200D can be relieved, and the residual stress can be relieved without causing processing defects such as tearing in the cylindrical planned portion 220D. Moreover, by satisfying the above relationship, the residual stress present in the long side planned portion 221D can be relieved by performing the ironing process once in the residual stress relief process, making it possible to relieve residual stress while minimizing the increase in the number of processes.
[0031] <Square Can Manufacturing System 100> Next, the square can manufacturing system 100 will be described.
[0032] As shown in Figures 2C, 3A, 3C, and 3E, the rectangular can manufacturing system 100 includes a first intermediate molding unit 110, which is a first intermediate molding means for carrying out a first intermediate molding process; a second intermediate molding unit 120, which is a second intermediate molding means for carrying out a second intermediate molding process; a rectangular molding unit 130, which is a rectangular molding means for carrying out a rectangular molding process; a residual stress relaxation unit 140, which is a residual stress relaxation ironing process included in a residual stress relaxation means for carrying out a residual stress relaxation process; and a trimming processing unit (not shown), which is a trimming processing means for carrying out a trimming process. As shown in Figure 2C, the first intermediate molding unit 110 comprises a die 111, a punch 112, and a blank holder 113. As shown in Figure 3A, the second intermediate molding unit 120 comprises a die 121, a punch 122, and a blank holder 123. As shown in Figure 3C, the square molding unit 130 comprises a die 131, a punch 132, and a blank holder 133. As shown in Figure 3E, the residual stress relief unit 140 comprises a die 141 and a punch 142. A trimming unit (not shown) comprises a blade for trimming the flange portion 260E of the fourth intermediate molded body 200E. Each unit further comprises various peripheral equipment such as drive means consisting of actuators and motors for driving each part such as the punch, and support members. The specific configuration and function of each of these parts are as described above.
[0033] The present invention will be further described below with reference to examples, but these examples are not intended to limit the present invention.
[0034] <Comparison with and without residual stress relief process> Referring to each step of the square can manufacturing method shown in Figures 2A to 3F, six metal blanks 200A made of aluminum alloy A3003 with a plate thickness of 1.2 mm were prepared, and coining, a first intermediate forming process, a second intermediate forming process, and a square forming process were performed to produce six third intermediate molded bodies 200D shown in Figure 3D. Subsequently, ironing in the residual stress relief process was performed on five of the above six third intermediate molded bodies 200D, and those with ironing amounts I2 and I2' of 0.02 mm, 0.05 mm, 0.08 mm, 0.10 mm, and 0.12 mm were designated as Examples 1 to 5, respectively. In addition, one of the above six third intermediate molded bodies 200D other than Examples 1 to 5 was designated as Comparative Example 1, in which the residual stress relief process was not performed. Table 1 shows the plate thicknesses 221Ct, 221Dt, and 221E of the long side planned portions 221C, 221D, and 221E, the plate thicknesses 222Ct, 222Dt, and 222E of the short side planned portions 222C, 222D, and 222E, the ironing amounts I1 to I2' in the above processes, and the values of I2 / (I1+I2) and I2' / (I1'+I2') at the end of the second intermediate molding process, the square molding process, and the residual stress relaxation process for Examples 1 to 5.
[0035]
[0036] As shown in the results in Table 1, the ironing amounts I1 to I2' of Examples 1 to 5 satisfy the relationships 0 < I2 / (I1 + I2) ≤ 0.6 and 0 < I2' / (I1' + I2') ≤ 0.6, respectively. When the trimming process was performed on Examples 1 to 5 and the flange portion 260E was cut off to form a rectangular can 200, no waviness was observed in the long-side direction of the pair of long sides 221. On the other hand, when the trimming process was performed on Comparative Example 1 and the flange portion 260D was cut off to form a rectangular can 200, the waviness was observed in the long-side direction of the pair of long sides 221.
[0037] <Comparison based on residual stress> Table 3 shows the results of measuring the residual stress at predetermined positions in the height direction for Example 3, specifically for the planned long side portion 221E before the trimming process and the long side portion 221 after the trimming process, and for Comparative Example 1, for measuring the residual stress at predetermined positions in the height direction for the planned long side portion 221D before the trimming process and the long side portion 221 after the trimming process. A μ-X360s manufactured by PulseTech Industries Co., Ltd. was used to measure the residual stress. The measurements were performed under the conditions shown in Table 2.
[0038]
[0039] Furthermore, Figure 6A shows the square can 200 of Example 3 after the trimming process, and Figure 6B shows the square can of Comparative Example 1 after the trimming process. In Table 3, a positive residual stress value represents tensile residual stress, and a negative residual stress value represents compressive residual stress. Also, in Table 3, measurement position A is the position on the short side of one of the planned long sides, measurement position B is the position in the long side direction of one of the planned long sides, measurement position C is the position on the short side of the other planned long side, measurement position D is the position opposite measurement position A on the other planned long side, measurement position E is the position opposite measurement position B on the other planned long side, and measurement position F is the position opposite measurement position C on the other planned long side.
[0040]
[0041] As shown in the results in Table 3, in Example 3, even before the trimming process, the residual stress (compressive residual stress) at heights of 30 mm to 90 mm is sufficiently reduced compared to Comparative Example 1, and at heights of 30 mm to 70 mm, it is tensile residual stress. Furthermore, it was confirmed that the residual stress at measurement positions B and E in the range of heights of 90 mm to 110 mm, that is, at the center of the long side direction and the upper part in the height direction of the pair of long sides 221, was compressive residual stress before the trimming process, while after the trimming process, the compressive residual stress was reduced and changed to tensile residual stress. In addition, it was confirmed that the measurement results of residual stress at measurement positions B and E at a height of 110 mm, and the measurement results of residual stress at measurement position E at a height of 100 mm, were within the range of 20 to 60 MPa. The vertical height of the square can 200 in the Example and Comparative Example is 111 mm. On the other hand, in Comparative Example 1, it was confirmed that the residual stress at measurement position B remained in the compressive direction before and after the trimming process. Furthermore, it was confirmed that the residual stress measurement results were outside the range of 20 to 60 MPa at all measurement positions within the height range of 90 mm to 110 mm. In Example 3, by performing ironing in the residual stress relaxation process, the planned long side portion 221D of the third intermediate molded body 200D is compressed and deformed in the thickness direction, reducing the thickness, while being stretched in the height direction, which relaxes the residual stress. As a result, there is a state where there is a compressive residual stress in the height range of 100 mm to 110 mm near the rigid flange portion 260E, and a state where there is a tensile residual stress in the height range of 10 mm to 70 mm. When the flange portion 260E of the fourth intermediate molded body 200E, which is in this residual stress state, is cut off by a trimming process, the tensile rigidity of the flange portion 260E is lost and the stress is released. As a result, residual stress in the tensile direction exists in the height range of 100 mm to 110 mm at measurement positions B and E, and it is presumed that this is why no waviness occurred in the long side direction of the pair of long sides 221.
[0042] Although embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and various design modifications can be made without departing from the present invention as described in the claims. In the embodiments described above, two drawing processes were performed in the first intermediate forming process and the second intermediate forming process, which are intermediate forming processes, but the number of drawing processes may be one or three or more, and the process may also include a drawing ironing process or an ironing process. Furthermore, the coining process may be omitted. In addition, the first intermediate forming unit 110 and the second intermediate forming unit 120, which are intermediate forming means, may separately have intermediate forming means for performing the above-mentioned drawing ironing process or ironing process. Furthermore, the ratio of the length of the short side 222 of the rectangular can 200 in the short side direction to the length of the long side 221 of the rectangular can 200 is not particularly limited as long as it is between 1:1 and 1:40. Furthermore, the vertical height of the rectangular can 200 is not limited to 111 mm, and any rectangular can shape is not particularly limited.
[0043] 100 ... Rectangular can manufacturing system 110 ... First intermediate molding unit (first intermediate molding means) 111 ... Die 111a ... Die processing through hole 112 ... Punch 113 ... Blank holder 120 ... Second intermediate molding unit (second intermediate molding means) 121 ... Die 121a ... Die processing through hole 122 ... Punch 123 ... Blank holder 130 ... Rectangular molding unit (rectangular molding means) 131 ... Die 131a ... Die processing through hole 131b ... Die processing inner circumferential surface 131c ... Die long side processing section 131d ... Die short side processing section 132 ... Punch 132a ... Punch processing outer circumferential surface 132b ... Punch long side processing section 132c ... Punch short side processing section 133 ... Blank holder 140 ...Residual stress relief unit (residual stress relief means) 141 ...Die 141a ...Die processed through hole 141b ...Die processed inner circumferential surface 141c ...Die long side processed part 141d ...Die short side processed part 142 ...Punch 142a ...Punch processed outer circumferential surface 142b ...Punch long side processed part 142c ...Punch short side processed part 200 ...Square can 200A ...Metal blank 200B ...First intermediate molded body 200C ...Second intermediate molded body 200D ...Third intermediate molded body 200E ...Fourth intermediate molded body 210 ...Bottom part 210A ...Planned bottom part 210C ...Planned bottom part 220 ...Square cylindrical part 220C ...Planned cylindrical part 220D ...Planned cylindrical part 220E ...Cylindrical section 221 ...Long side 221C ...Long side section 221Ct ...Thickness of long side section 221D ...Long side section 221Dt ...Thickness of long side section 221E ...Long side section 221Et ...Thickness of long side section 222 ...Short side 222C ...Short side section 222Ct ...Thickness of short side section222D...Planned short side section 222Dt...Plate thickness of planned short side section 222E...Planned short side section 222Et...Plate thickness of planned short side section 223...Corner side section 223C...Planned corner side section 230...Long side corner section 240...Short side corner section 250...Bottom curved corner section 260D...Flange section 260E...Flange section I1...Amount of ironing I2...Amount of ironing I1'...Amount of ironing I2'...Amount of ironing
Claims
1. A method for manufacturing a rectangular can, comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, the method comprising: an intermediate forming step of forming an intermediate molded body by drawing or drawing and ironing a metal blank; a rectangular forming step of forming the intermediate molded body into a rectangular shape by drawing or drawing and ironing the intermediate molded body; and a residual stress relief step of relieving residual stress in the intermediate molded body after the rectangular forming step.
2. The method for manufacturing a rectangular can according to claim 1, wherein the residual stress relief step includes ironing, and when the amount of ironing by the drawing ironing in the rectangular forming step is I1 and the amount of ironing by the ironing in the residual stress relief step is I2, the relationship 0 < I2 / (I1 + I2) ≤ 0.6 is satisfied.
3. A square can manufacturing system for manufacturing a square can having a bottom portion and a square cylindrical portion having a pair of long sides and a pair of short sides, comprising: an intermediate forming means for forming an intermediate molded body by drawing or drawing and ironing a metal blank; a square forming means for forming the intermediate molded body into a square shape by drawing or drawing and ironing the intermediate molded body; and a residual stress relief means for relieving residual stress of the intermediate molded body formed into a square shape by the square forming means.
4. The rectangular can manufacturing system according to claim 3, wherein the residual stress relief means includes a residual stress relief ironing process, and when the amount of ironing by the drawing ironing process in the rectangular forming means is I1 and the amount of ironing by the residual stress relief ironing process in the residual stress relief means is I2, the relationship 0 < I2 / (I1 + I2) ≤ 0.6 is satisfied.
5. A rectangular can comprising a bottom portion and a rectangular cylindrical portion having a pair of long sides and a pair of short sides, wherein the pair of long sides have tensile residual stress at the center in the long side direction and at the top in the height direction.
6. The rectangular can according to claim 5, characterized in that the tensile residual stress is 20 to 60 MPa.