Porous water electrolysis separator, alkaline water electrolysis member, alkaline water electrolysis cell, alkaline water electrolysis device, and hydrogen production method

The porous separator for water electrolysis, with a high metal element ratio on its surface, addresses the issue of gas barrier properties in alkaline water electrolysis, enhancing safety and efficiency by preventing hydrogen gas ingress.

WO2026234959A1PCT designated stage Publication Date: 2026-11-12FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015501
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-17
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing alkaline water electrolysis separators exhibit poor gas barrier properties, allowing hydrogen gas to pass through, posing safety risks and reducing efficiency.

Method used

A porous separator for water electrolysis comprising an organic polymer and hydrophilic inorganic particles, with a metal element ratio of 5 at% or more on at least one surface, enhancing gas barrier properties by increasing the surface area ratio of hydrophilic inorganic particles.

Benefits of technology

The separator effectively suppresses hydrogen gas ingress into the anode, improving safety and efficiency of hydrogen production by alkaline water electrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015501_12112026_PF_FP_ABST
    Figure JP2026015501_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a porous water electrolysis separator containing an organic polymer and hydrophilic inorganic particles, wherein, on at least one surface of the porous water electrolysis separator, the ratio of metal elements to all elements measured by means of X-ray photoelectron spectroscopy is 5 at% or more. Further provided are an alkaline water electrolysis member, an alkaline water electrolysis cell, an alkaline water electrolysis device, and a hydrogen production method that use said separator.
Need to check novelty before this filing date? Find Prior Art

Description

Porous separator for water electrolysis, alkaline water electrolysis component, alkaline water electrolysis cell, alkaline water electrolysis apparatus, and method for producing hydrogen.

[0001] The present invention relates to a porous separator for water electrolysis, an alkaline water electrolysis component, an alkaline water electrolysis cell, an alkaline water electrolysis apparatus, and a method for producing hydrogen.

[0002] Hydrogen is a clean energy source that does not emit carbon dioxide and is used as fuel in fuel cell vehicles and household fuel cells, for example. Alkaline water electrolysis, which uses a high-concentration alkaline aqueous solution as an electrolyte, is a known method for producing hydrogen. By performing alkaline water electrolysis using a renewable energy power generation system as the power source, hydrogen can be produced without emitting carbon dioxide, and therefore hydrogen is attracting increasing attention as a fundamental energy source for a sustainable society.

[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H) generated at the cathode is produced. 2 O + 2e - →H 2 +2OH - This prevents the oxygen (4OH) from moving to the anode, and also prevents the bubble-like oxygen (4OH) generated at the anode from moving to the anode. - →O 2 +2H 2 O+4e -To prevent the ions from moving towards the cathode, a gas barrier separator (diaphragm) is placed between the cathode and the anode. For example, Patent Document 1 describes an invention for an alkaline water electrolysis diaphragm containing an organic polymer and inorganic particles, wherein, in a cross section perpendicular to the surface of the membrane, the ratio B / A of the ratio A (Pa / Sa) of the sum of the areas of the organic polymer to the sum of the areas of the inorganic particles and organic polymer (Sa) in the range between the surface of the membrane and a position 1 μm away in the depth direction from the surface of the membrane, and the ratio B (Pb / Sb) of the ratio of the sum of the areas of the organic polymer to the sum of the areas of the inorganic particles and organic polymer (Sb) in the range between a position 2 μm away in the depth direction from the surface of the membrane and a position 15 μm away from the surface of the membrane, is 0.6 or more and 1.0 or less. According to the above-mentioned Patent Document 1, in an alkaline water electrolysis diaphragm containing an organic polymer and inorganic particles, by using a high molecular weight of polyvinylpyrrolidone during film formation, the resin composition ratio on the surface increases, resulting in a dense surface structure, and providing an alkaline water electrolysis diaphragm that achieves both high ion conductivity and high gas barrier properties.

[0004] Patent No. 7284001

[0005] The above-mentioned alkaline water electrolysis separator ensures ion conductivity by having a porous structure, but due to this porous structure, a certain amount of gas also passes through. In the technology described in Patent Document 1, the separator surface is made dense to enhance gas barrier properties, but suppressing the ingress of hydrogen gas into the anode side is increasingly required from a safety standpoint.

[0006] The present invention aims to provide a porous separator for water electrolysis that exhibits excellent gas barrier properties. Furthermore, the present invention aims to provide an alkaline water electrolysis component, an alkaline water electrolysis cell, an alkaline water electrolysis apparatus, and a hydrogen production method using the porous separator for water electrolysis of the present invention.

[0007] In view of the above problems, the inventors of this invention conducted extensive research and found that by increasing the surface ratio of hydrophilic inorganic particles on at least one surface of a porous separator for water electrolysis containing an organic polymer and hydrophilic inorganic particles to a predetermined level, the gas barrier properties can be effectively enhanced. The present invention was completed based on this finding and further research.

[0008] The above problems of the present invention have been solved by the following means: [1] A porous separator for water electrolysis comprising an organic polymer and hydrophilic inorganic particles, wherein the ratio of metal elements to total elements measured by X-ray photoelectron spectroscopy on at least one surface of the porous separator for water electrolysis is 5 at% or more. [2] The porous separator for water electrolysis according to [1], wherein the ratio of metal elements to total elements measured by X-ray photoelectron spectroscopy on both surfaces of the porous separator for water electrolysis is 5 at% or more. [3] The porous separator for water electrolysis according to [1] or [2], wherein the ratio of metal elements to total elements measured by X-ray photoelectron spectroscopy on at least one surface of the porous separator for water electrolysis is 10 at% or more. [4] The porous separator for water electrolysis according to [3], wherein the ratio of metal elements to total elements measured by X-ray photoelectron spectroscopy on at least one surface of the porous separator for water electrolysis is 15 at% or more. [5] A porous separator for water electrolysis according to any one of [1] to [4], wherein the thickness of the porous separator for water electrolysis is 100 to 400 μm, and the ratio of metal elements to total elements measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis is 20 at% or more and less than 45 at%. [6] A porous separator for water electrolysis according to [5], wherein the ratio of metal elements to total elements measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis is 25 at% or more and less than 45 at%. [7] A porous separator for water electrolysis according to [6], wherein the ratio of metal elements to total elements measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis is 30 at% or more and less than 45 at%. [8] The porous separator for water electrolysis according to [7], wherein the ratio of metal elements to total elements, as measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis, is 34 at% or more and less than 45 at%.[9] A porous separator for water electrolysis according to any one of [1] to [8], wherein the metal element is Ti, Mg, Zr, Al, Zn, Ca, Ba, Sr, Pb, Ta, Bi, and Ce.

[10] A porous separator for water electrolysis according to [9], wherein the metal element is Zr.

[11] An alkaline water electrolysis component comprising the porous separator for water electrolysis according to any one of [1] to

[10] .

[12] An alkaline water electrolysis cell comprising the porous separator for water electrolysis according to any one of [1] to

[10] , or the alkaline water electrolysis component according to

[11] .

[13] An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell according to

[12] .

[14] A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus according to

[13] .

[15] A method for producing hydrogen according to

[14] , comprising using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as the electrolyte solution and electrolyzing water at 70 to 95°C.

[0009] In the present invention, when describing physical properties, etc., by indicating numerical ranges, if the upper and lower limits of the numerical range are described separately, either upper or lower limit can be appropriately combined to form a specific numerical range. On the other hand, when multiple numerical ranges represented using "~" are set and described, the upper and lower limits forming the numerical range are not limited to the specific combination of upper and lower limits described before and after "~" as a specific numerical range, but can be a numerical range formed by appropriately combining the upper and lower limits of each numerical range. In the present invention, a numerical range represented using "~" means a range that includes the numbers described before and after "~" as the lower and upper limits.

[0010] The porous separator for water electrolysis of the present invention exhibits excellent gas barrier properties. Furthermore, the alkaline water electrolysis component and alkaline water electrolysis cell of the present invention also exhibit excellent gas barrier properties, effectively suppressing, for example, the ingress of hydrogen gas into the anode. In addition, the alkaline water electrolysis apparatus of the present invention effectively suppresses gas movement between electrodes. Moreover, the hydrogen production method of the present invention makes it possible to produce hydrogen more efficiently and stably by alkaline water electrolysis.

[0011] Figure 1 is a schematic diagram showing one embodiment of an alkaline water electrolysis apparatus. Figure 2 is a schematic diagram showing another embodiment of an alkaline water electrolysis apparatus. Figure 3 is a schematic diagram showing yet another embodiment of an alkaline water electrolysis apparatus.

[0012] [Porous Separator for Water Electrolysis] The porous separator for water electrolysis of the present invention (hereinafter also referred to as "the separator of the present invention") is a porous separator for water electrolysis comprising an organic polymer and hydrophilic inorganic particles, wherein the ratio of metal elements to all elements measured by X-ray photoelectron spectroscopy (XPS) on at least one surface of the porous separator for water electrolysis (hereinafter referred to as "surface metal element ratio") is 5 at% or more. As a result, the separator of the present invention can exhibit excellent gas barrier properties. This is presumed to be because, by increasing the surface metal element ratio on at least one surface of the separator of the present invention to 5 at% or more, the area ratio of hydrophilic inorganic particles (particles of inorganic compounds containing metal elements as constituent elements that exhibit hydrophilicity) present on the separator surface is increased, and as a result of the separator surface being hydrophilized by the hydrophilic inorganic particles, the permeation of hydrophobic gases can be effectively blocked, and excellent gas barrier properties can be exhibited.

[0013] The ratio of metallic elements on the separator surface is measured and determined as follows: <Ratio of metallic elements on the surface> A sample for measurement is cut from the separator, and X-ray photoelectron spectroscopy (XPS) is performed on the surface of the sample by combining Wide Scan (Survey) and Narrow Scan measurements. Specifically, Wide Scan (Survey) measurements are performed for all elements (hydrogen and helium are not measured by XPS), and then Narrow Scan measurements are performed on the electron orbitals of the elements for which peaks are observed, and the X-ray photoelectron spectrum is measured. Peak separation is performed on each obtained X-ray photoelectron spectrum, the abundance ratio of each element is calculated, and the ratio of metallic elements is determined. In other words, the ratio of metallic elements on the surface means the ratio (at%) of the abundance ratio of metallic elements obtained by Narrow Scan measurements to the sum of the abundance ratios of each element obtained by Narrow Scan measurements. Details of the XPS measurement conditions (including Wide Scan and Narrow Scan measurement conditions) are as described in the examples below.

[0014] On at least one surface of the separator of the present invention, the surface metal element ratio is 5 at% or more, preferably 10 at% or more, more preferably 13 at% or more, and even more preferably 15 at% or more, from the viewpoint of superior gas barrier properties. Furthermore, from the viewpoint of being able to retain hydrophilic inorganic particles on the surface of the separator of the present invention, the surface metal element ratio is usually preferably less than 25 at% and more preferably less than 20 at%. Therefore, the preferred range for the surface metal element ratio is preferably 5 at% or more and less than 25 at%, more preferably 10 at% or more and less than 20 at%, even more preferably 13 at% or more and less than 20 at%, and most preferably 15 at% or more and less than 20 at%. The numerical range for the surface metal element ratio (at least one of the upper and lower limits) can be appropriately set to the preferred, more preferred, and even preferred values ​​of the lower limit and / or the preferred and more preferred values ​​of the upper limit, respectively. The metal element ratio on the surface can be adjusted to the above range by adjusting the proportion of hydrophilic inorganic particles to the total of organic polymer and hydrophilic inorganic particles in the film-forming solution to be within a predetermined range, or by speeding up the phase separation rate of the wet phase separation by adjusting the solvent type in the film-forming solution, the solidification bath temperature, etc., and suppressing the formation of a dense film of organic polymer on the separator surface. It is preferable that the metal element ratio on the surface of both surfaces of the separator of the present invention satisfies the numerical range mentioned above (5 at% or more, above the preferred lower limit mentioned above, above the more preferred lower limit, above the still preferred lower limit, above the preferred range mentioned above, above the more preferred range, still preferred range, most preferred range, and / or a range in which the preferred value, more preferred value, and / or the preferred value, and more preferred value of the upper limit mentioned above are appropriately adopted in at least one of these numerical ranges (upper and lower limits)).

[0015] From the viewpoint of suppressing ionic resistance to a low level, the thickness of the separator of the present invention is 100 to 400 μm, and the ratio of metal elements to all elements measured by depth direction analysis through X-ray photoelectron spectroscopy from at least one surface of the separator of the present invention (hereinafter referred to as "metal element ratio by depth direction analysis") is preferably 20 at% or more and less than 45 at%, more preferably 25 at% or more and less than 45 at%, further preferably 30 at% or more and less than 45 at%, and particularly preferably 34 at% or more and less than 45 at%. It is preferable that the metal element ratio by depth direction analysis on both surfaces of the separator of the present invention satisfies the numerical ranges mentioned above (preferable range, more preferable range, further preferable range, particularly preferable range). The metal element ratio by depth direction analysis can be adjusted to fall within the above range by separator production conditions such as the ratio of hydrophilic inorganic particles to the total of the organic polymer and hydrophilic inorganic particles in the film-forming solution, the type of solvent in the film-forming solution (coating liquid), and the coagulation bath temperature, which will be described later. The metal element ratio by depth direction analysis of the separator is a value measured and determined as follows. The thickness of the separator will be described later. <Metal Element Ratio by Depth Direction Analysis> A measurement sample is cut out from the separator, one surface of the measurement sample is etched using an Ar+ ion gun under the conditions described below, and then X-ray photoelectron spectroscopy analysis is performed in the same manner as described in the above <Metal Element Ratio on Surface> (X-ray photoelectron spectroscopy analysis in the depth direction is performed) to determine the metal element ratio. (Etching conditions using Ar+ ion gun) Acceleration voltage: 4 kV Etching area: square with a side length of 2 mm Etching time: 30 minutes Etching rate: 22 nm / min (SiO 2 conversion rate)

[0016] In the separator of the present invention, a preferred combination of the metal element ratio obtained by depth analysis from at least one surface of the separator and the thickness of the separator is that the thickness of the separator is 100 to 400 μm, and the metal element ratio obtained by depth analysis from at least one surface of the separator of the present invention is 20 at% or more and less than 45 at%. The preferred range of the metal element ratio obtained by depth analysis from at least one surface of the separator described above and the preferred range of the thickness of the separator described below can be appropriately combined. In this combination, the numerical range of the metal element ratio obtained by depth analysis from at least one surface of the separator can be appropriately selected from the preferred range, more preferred range, even more preferred range, and particularly preferred range described above, and the numerical range of the thickness of the separator can be appropriately selected from the preferred range, more preferred range, even more preferred range described below, and the lower limit values ​​of these numerical ranges can be appropriately selected from the preferred values, more preferred values, and even more preferred values ​​described below.

[0017] In the surface metal element ratio and the metal element ratio obtained by depth profiling, the metal element refers to the transition metal elements (transition metal elements of groups 3 to 12) and typical metal elements (alkali metal elements, alkaline earth metal elements, and typical metal elements of groups 13 to 16 (Al, Ga, In, Tl, Ge, Sn, Pb, Sb, Bi, Po)) of the periodic table. Preferably, these are the transition metal elements of groups 3 to 12, alkaline earth metal elements, and typical metal elements of groups 13 to 16 of the periodic table, respectively. More preferably, these are Ti, Mg, Zr, Al, Zn, Ca, Ba, Sr, Pb, Ta, Bi, and Ce, and even more preferably Zr. When two or more metal elements are measured by XPS, the surface metal element ratio and the metal element ratio obtained by depth profiling refer to the total ratio of the two or more metal elements.

[0018] <Thickness> The thickness (film thickness) of the separator of the present invention is not particularly limited and can be appropriately determined considering properties such as mechanical strength and alkali durability. For example, it can be 100 to 550 μm, and within this thickness range, the effect of thickness on gas barrier properties is not observed. From the viewpoint of keeping ion resistance low, 100 to 400 μm is preferred, 100 to 350 μm is more preferred, and 100 to 300 μm is even more preferred. The lower limit is also preferably 120 μm or more, more preferably 140 μm or more, and even more preferably 160 μm or more. The lower limit of the above numerical range of separator thickness (100 to 550 μm, preferred range, more preferred range, even more preferred range) can be appropriately adopted from the preferred, more preferred, and even more preferred values ​​of the lower limit mentioned above. The thickness of the separator is determined by taking a cross-sectional SEM (scanning electron microscope) image of a cross-section cut from the separator of the present invention with a razor blade at a magnification (e.g., 400x) that allows the entire cross-section of the separator to fit in a single field of view, assuming that no pores exist in the obtained cross-sectional SEM image (assuming that the pores are filled with organic polymer), measuring the thickness at 20 equally spaced points, calculating the arithmetic mean of the 20 obtained measurements, and rounding the value to the first decimal place in μm.

[0019] In the separator of the present invention, as a preferable combination of the metal element ratio on at least one surface of the separator, the metal element ratio obtained by depth direction analysis from at least one surface of the separator, and the thickness of the separator, the metal element ratio on at least one surface of the separator is 5 at% or more, the thickness of the separator is 100 to 400 μm, and the metal element ratio obtained by depth direction analysis from at least one surface of the separator is 20 at% or more and less than 45 at%, and the above-mentioned preferable values or ranges can be appropriately combined with each other. In this combination, for the numerical range of the metal element ratio on at least one surface of the separator (5 at% or more), a range that appropriately adopts the above-mentioned preferable lower limit value or more, more preferable lower limit value or more, still more preferable lower limit value or more, the above-mentioned preferable range, more preferable range, still more preferable range, most preferable range, and further, in these numerical ranges (at least one of the upper limit value and the lower limit value), the preferable value, more preferable value, still more preferable value of the above-mentioned lower limit value, and / or the preferable value, more preferable value of the above-mentioned upper limit value can be appropriately adopted. For the numerical range of the metal element ratio obtained by depth direction analysis from at least one surface of the separator, the above-mentioned preferable range, more preferable range, still more preferable range, and particularly preferable range can be appropriately adopted. For the numerical range of the thickness of the separator, the above-mentioned preferable range, more preferable range, still more preferable range, and further, a range that appropriately adopts the above-mentioned preferable value, more preferable value, still more preferable value for the lower limit values in these numerical ranges can be appropriately adopted.

[0020] Furthermore, in the separator of the present invention, a preferred combination of the metal element ratio on both surfaces of the separator, the metal element ratio obtained by depth analysis from at least one surface of the separator, and the thickness of the separator is such that the metal element ratio on both surfaces of the separator is 5 at% or more, the thickness of the separator is 100 to 400 μm, and the metal element ratio obtained by depth analysis from at least one surface of the separator is 20 at% or more and less than 45 at%, and the above preferred values ​​or ranges can be appropriately combined. In this combination, the numerical range (5 at% or more) of the metal element ratio on both surfaces of the separator can be any range that appropriately adopts the preferred lower limit, a more preferred lower limit, an even more preferred lower limit, the preferred range, a more preferred range, an even more preferred range, the most preferred range, and even a range in which the preferred, more preferred, and / or preferred upper limits are appropriately adopted within these numerical ranges (at least one of the upper and lower limits). The numerical range of the metal element ratio obtained by depth analysis from at least one surface of the separator can appropriately adopt the preferred range, a more preferred range, an even more preferred range, and a particularly preferred range. The numerical range of the thickness of the separator can appropriately adopt the preferred range, a more preferred range, an even more preferred range, and even a range in which the preferred, more preferred, and even more preferred values ​​are appropriately adopted for the lower limits within these numerical ranges.

[0021] <Average Pore Diameter> The average pore diameter in the surface region of the separator of the present invention can be appropriately adjusted within the range that satisfies the metal element ratio of the surface described above. For example, on at least one surface of the separator of the present invention, it can be 0.05 to 1.0 μm, preferably 0.1 to 0.8 μm, and more preferably 0.1 to 0.5 μm. The average pore diameter in the surface region is a value measured and calculated as follows: The separator of the present invention is impregnated with methanol and frozen in liquid nitrogen. A cross section is cut from the separator using a microtome (for example, Leica Corporation, product name: EM UC6). The arithmetic mean of the pore diameter in the region from the surface to 10% of the separator's thickness (for example, in the case of a separator with a thickness of 200 μm, the region from the surface to 20 μm) is placed in one field of view, and the value rounded to the second decimal place is defined as the "average pore diameter in the film surface region".

[0022] <Porosity> The porosity of the separator of the present invention can be appropriately adjusted within the range that satisfies the metal element ratio of the surface described above. For example, from the viewpoint of ion permeability and gas barrier properties, it is preferably 30 to 70%, and more preferably 40 to 60%. This porosity is the value of porosity calculated from the insertion curve by the mercury intrusion method.

[0023] <Bubble Point> The separator of the present invention can be appropriately adjusted within the range that satisfies the above-mentioned surface metal element ratio. For example, from the viewpoint of gas barrier properties required for porous separators for water electrolysis, it is preferable that the bubble point exceeds 1 bar, and more preferably exceeds 2 bar. The bubble point is determined by measuring using a palm porometer based on the bubble point method described in ASMT (American Society for Testing and Materials) F316-86, and the pressure at which the first bubble is generated in the resulting wet curve is defined as the bubble point.

[0024] <Ion Resistance> The separator of the present invention has an ion resistance of 0.30 Ω·cm, from the viewpoint of ion permeability required for porous separators for water electrolysis. 2 Preferably less than 0.25 Ω·cm2 Less than 0.20 Ω·cm is more preferable. 2 Less than 0.18 Ω·cm is even more preferable. 2 A value less than 0.15 Ω·cm is particularly preferred. 2 Less than 0.01 Ω·cm is most preferable. However, a practical lower limit is 0.01 Ω·cm. 2 The above is true, and a preferred range is 0.01 Ω·cm. 2 0.30Ω・cm or more 2 A more preferable range is less than 0.01 Ω·cm. 2 0.15Ω・cm or more 2 Examples include those less than the specified value. Ion resistance is a value measured by the AC impedance method at 30°C with the separator of the present invention, punched out in a circular shape, set in a cell. Details are as described in the examples below.

[0025] <Structure of the Separator of the Present Invention> The separator of the present invention is a porous separator for water electrolysis comprising a porous structure (porous material) containing an organic polymer and hydrophilic inorganic particles. In the separator of the present invention, the porous material containing the organic polymer and hydrophilic inorganic particles may further contain other components other than the organic polymer and hydrophilic inorganic particles. Furthermore, the separator of the present invention may or may not contain a porous support other than the porous material containing the organic polymer and hydrophilic inorganic particles. When the separator of the present invention contains a porous support, the separator of the present invention is not a structure in which the porous support and the porous material are simply stacked, but rather a structure in which the porous support and the porous material are inseparable (i.e., a composite). For example, as shown in the examples described later, the separator of the present invention is a composite (or a composite with a structure equivalent to the composite obtained by this method) formed by impregnating the porous support with a film-forming solution constituting the porous material and subjecting it to wet phase separation while encompassing the porous support. As described above, in the present invention, a composite formed by impregnating a porous support with a film-forming solution constituting a porous material and subjecting the porous support to wet phase separation is referred to as a "structure in which a porous support is embedded in a porous material." Furthermore, when the separator of the present invention contains a porous support, the separator of the present invention is not limited to those manufactured by the wet phase separation method described above, but also includes those manufactured by other methods, as long as they are a "structure in which a porous support is embedded in a porous material."

[0026] The specific configuration of the separator of the present invention is not particularly limited, as long as it is a porous separator for water electrolysis containing an organic polymer and hydrophilic inorganic particles, and the ratio of metal elements on the surface of at least one surface of the separator is 5 at% or more. For example, if the separator of the present invention contains a porous support, it is preferable that the separator of the present invention has a configuration in which the porous support and the porous material are arranged on at least one of the outer surface and voids of the porous support. The "outer surface of the porous support" means the surface when the porous support is viewed from a macroscopic perspective as a film-like support having a single thickness, and the "voids of the porous support" means the holes (voids between the framework (e.g., fibers, metals, ceramics) constituting the porous support) that the porous support has. The structure in which the porous material is arranged on at least one of the outer surface and voids of the porous support can be appropriately adjusted within the range that satisfies the above-mentioned ratio of metal elements on the surface, and for example, the porous material may be arranged only on the outer surface of the porous support. In this case, the porous material may be arranged on only one side of the porous support, which is a film-like support, or on both sides. Furthermore, in a structure in which the porous material is disposed on one or both sides of the outer surface, the porous material may be disposed on at least a portion of each surface, or on the entire surface. Alternatively, the porous material may be disposed only in at least a portion of the voids of the porous support. Furthermore, the porous material may be disposed on at least a portion of the outer surface and at least a portion of the voids of the porous support. In the present invention, such forms are also included in a structure in which the porous material is disposed on at least one of the outer surface and voids of the porous support. Among these, a structure in which the porous material is disposed on the entire outer surface and the entire voids of the porous support is preferred. The porous support, porous material, organic polymer and hydrophilic inorganic particles which are constituent materials of the porous material will be described in detail below.

[0027] <Porous Support> The porous support is not particularly limited as long as it is applicable to porous separators for water electrolysis, but it is preferably applicable to porous separators for alkaline water electrolysis, and usually a porous cloth can be used. The opening ratio of the porous support is preferably 30 to 80%, more preferably 40 to 70%. The opening ratio is the ratio of the area of ​​voids to the unit area when the porous support is viewed in a planar manner. The porous support is preferably a porous cloth, and more preferably a porous polymer cloth. The porous polymer cloth is a woven or nonwoven fabric.

[0028] The polymers constituting the porous polymer fabric are not particularly limited, and examples include polypropylene, polyethylene, polysulfone (PSU), polyphenylene sulfide (PPS), polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyetheretherketone (PEEK), sulfonated polyetheretherketone, monochlorotrifluoroethylene, copolymer of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid. Among the above, it is preferable that the polymer constituting the porous polymer fabric contains at least one of polypropylene, polyphenylene sulfide, and polyetheretherketone, more preferably at least one of polyphenylene sulfide and polyetheretherketone, and even more preferably polyetheretherketone.

[0029] The thickness of the porous support is preferably 30 to 150 μm, more preferably 30 to 130 μm, and even more preferably 30 to 110 μm. The thickness of the porous support is measured using a dot-type thickness gauge. The thickness of the porous support in the separator can be measured and calculated by removing the porous support from the separator using a solvent that dissolves the organic polymer contained in the porous material, and then measuring the thickness of the porous support using the method described above.

[0030] <Porous Material> The porous material only needs to be able to realize a separator that satisfies the above-mentioned ratio of metal elements on the surface. As a porous separator for water electrolysis, it is preferable that it has the function of blocking the permeation of gases (preferably hydrogen gas and oxygen gas) and allowing ions (preferably hydroxyl ions) to permeate.

[0031] As described above, the porous material contains at least an organic polymer and hydrophilic inorganic particles, and may further contain other components.

[0032] (Organic Polymers) The organic polymer contained in the porous material is not particularly limited as long as it is applicable to porous separators for water electrolysis, and it is preferable to use various organic polymers applicable to the wet phase separation described later, as this makes it easier to adjust the metal element ratio on the surface.

[0033] The organic polymer can be selected from, for example, fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, etc. As the fluororesin, a resin selected from polyvinylidene fluoride and polytetrafluoroethylene is preferred. As the olefin resin, polypropylene resin is preferred. As the polyester resin, a resin selected from polyethylene terephthalate, polybutylene terephthalate, and polybutylene naphthalate is preferred. As the aromatic hydrocarbon resin, polystyrene resin is preferred.

[0034] Other preferred organic polymers include polysulfone (PSU), polyethersulfone, polyphenylene sulfide, polyphenylsulfone, polyacrylate, polyetherimide, polyimide, and polyamideimide.

[0035] Organic polymers may be used individually or in combination of two or more types.

[0036] The organic polymer more preferably contains at least one of polyvinylidene fluoride, polysulfone, polyethersulfone, and polyphenylsulfone, even more preferably contains at least one of polysulfone, polyethersulfone, and polyphenylsulfone, and even more preferably contains polysulfone.

[0037] The mass-average molecular weight (Mw) of the organic polymer is not particularly limited. Considering the handling properties of the film-forming solution described later and the mechanical strength of the resulting separator, it can be, for example, 10,000 to 500,000, and preferably 20,000 to 300,000. Mw can be determined under the following conditions. Instrument: HLC-8220GPC (Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARD COLUMN HXL-L 6mm x 40mm (Tosoh Corporation) Sample-side column: The following three columns are directly connected in order (all Tosoh Corporation): ・TSK-GEL GMHXL 7.8mm x 300mm ・TSK-GEL G4000HXL 7.8mm x 300mm ・TSK-GEL G2000HXL 7.8mm x 300mm Reference-side column: TSK-GEL G1000HXL 7.8mm x 300mm Oven temperature: 40℃ Mobile phase: THF (Tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1% by mass Sample injection volume: 100 μL Data acquisition time: 5 to 45 minutes after sample injection Sampling pitch: 300 milliseconds

[0038] The content of the organic polymer in the porous material is not particularly limited, but it is preferably 5 to 45% by mass, more preferably 5 to 40% by mass, even more preferably 7 to 30% by mass, particularly preferably 9 to 25% by mass, and most preferably 12 to 19% by mass, as this makes it easier to set the surface metal element ratio within the above range.

[0039] (Hydrophilic Inorganic Particles) The hydrophilic inorganic particles contained in the porous material can be any particles of an inorganic compound that contains a metal element as a constituent element and exhibits hydrophilicity. Note that an inorganic compound that contains a metal element as a constituent element is not a compound that is itself a metal, but rather one that contains a metal element as a constituent element, and examples of metal oxides, metal hydroxides, and metal sulfates are preferred. The metal elements contained in the inorganic compound constituting the hydrophilic inorganic particles can be the metal elements listed in the metal element ratio of the surface and the metal element ratio obtained by depth profiling described above. Therefore, as metal oxides, metal hydroxides, or metal sulfates constituting the hydrophilic inorganic particles, oxides, hydroxides, or sulfates of Ti, Mg, Zr, Al, Zn, Ca, Ba, Sr, Pb, Ta, Bi, or Ce are preferred, and oxides or hydroxides of Zr are more preferred.

[0040] The above metal oxides are preferably selected from zirconium oxide, titanium oxide, bismuth oxide, cerium oxide, and magnesium oxide.

[0041] The above metal hydroxides are preferably selected from zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide, and magnesium hydroxide.

[0042] The above metal sulfate is preferably selected from calcium sulfate and barium sulfate.

[0043] Hydrophilic inorganic particles may be used individually or in combination of two or more types.

[0044] The particle size of the hydrophilic inorganic particles is preferably 0.05 to 2.00 μm, more preferably 0.1 to 1.50 μm, even more preferably 0.15 to 1.00 μm, and particularly preferably 0.20 to 1.00 μm. This particle size is the median diameter (D50), and is determined by measuring the particle size distribution using laser diffraction and scattering methods, representing the particle size at which the cumulative distribution reaches 50% when the total volume of the particles is considered 100%.

[0045] The content of hydrophilic inorganic particles in the porous material is preferably 50 to 94% by mass, more preferably 60 to 93% by mass, even more preferably 70 to 92% by mass, particularly preferably 75 to 91% by mass, and most preferably 81 to 88% by mass, as this makes it easier to set the surface metal element ratio within the above range.

[0046] In porous materials, the ratio of the content of hydrophilic inorganic particles to the content of organic polymer (content of hydrophilic inorganic particles / content of organic polymer) is preferably 10.0 / 1 to 1.0 / 1 by mass, more preferably 9.0 / 1 to 2.0 / 1, even more preferably 8.0 / 1 to 3.0 / 1, even more preferably 7.0 / 1 to 4.0 / 1, and even more preferably 6.9 / 1 to 5.3 / 1.

[0047] (Other components) Other components that the porous material may contain include, for example, components that control pore formation in wet phase separation, specifically the other components listed in the film-forming solution described later. The total content of other components in the porous material is preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and even more preferably 0.1 to 1% by mass.

[0048] The separator of the present invention can be used as a separator placed between the cathode electrode and the anode electrode in a method for producing hydrogen by electrolyzing an alkaline aqueous solution using an electrolytic cell. Furthermore, the separator of the present invention can also be used as a separator in an anion exchange membrane type water electrolysis system. In particular, it can be suitably used as a porous separator for water electrolysis in the alkaline water electrolysis apparatus described below.

[0049] The separator of the present invention may be in the form of a long sheet wound into a roll, or it may be pre-cut into a predetermined shape according to its intended use, equipment, etc. From the viewpoint of manufacturing efficiency, it is also preferable that the separator of the present invention is in the form of a long sheet and has a thickness distribution in at least one of the width and length directions in which the thickness in the center of the sheet is greater than the thickness at both ends of the sheet. Furthermore, the separator of the present invention may be stored by immersing it in a preservation solution such as pure water. Furthermore, the separator of the present invention may be stored as a dry film without being immersed in a preservation solution.

[0050] [Method for Manufacturing Separator] The method for manufacturing the separator of the present invention is not particularly limited as long as the resulting separator contains a porous material containing an organic polymer and hydrophilic inorganic particles and satisfies the surface metal element ratio specified in the present invention. The separator of the present invention is preferably manufactured by a method that includes forming a porous material containing an organic polymer and hydrophilic inorganic particles by wet phase separation, as this makes it easier to set the surface metal element ratio within the above range. This wet phase separation step makes it possible to obtain the separator of the present invention composed of a porous material containing an organic polymer and hydrophilic inorganic particles. Furthermore, by performing the formation of the porous material by wet phase separation integrally with a porous support, it is possible to obtain the separator of the present invention composed of a porous support and a porous material. The separator of the present invention can be obtained by performing steam induction phase separation and / or liquid induction phase separation as wet phase separation. Specifically, it is preferably manufactured by a method that includes performing water vapor induction phase separation on a laminate consisting of a coating film containing the constituent materials of the porous material, and / or immersing the laminate (the laminate after water vapor induction phase separation if the above water vapor induction phase separation is performed) in a condensation bath. In the present invention, it is preferable to perform the above-mentioned vapor-induced phase separation and / or liquid-induced phase separation using a film-forming support. For example, the separator of the present invention can be obtained by casting a film-forming solution containing the constituent materials of the porous material onto a film-forming support to form a coating film, and then performing wet phase separation with the film-forming support attached or with the film-forming support removed. Furthermore, by including a step of further impregnating the coating film with a porous support, a porous film of the present invention containing a porous support and a porous material can be obtained. In the present invention, performing wet phase separation with the film-forming support attached is particularly preferable because it makes it easier to set the surface metal element ratio within the above range.

[0051] <Film-forming solution> The film-forming solution can be any dissolving solution containing an organic polymer and hydrophilic inorganic particles that constitute the porous material, and may contain an organic polymer, hydrophilic inorganic particles and a solvent, as well as other components. It is preferable to prepare the film-forming solution by mixing the organic polymer and other components first, and then adding the hydrophilic inorganic particles, from the viewpoint of adjusting the metal element ratio on the surface to the above range.

[0052] (Solvent) The film-forming solution in wet phase separation can be any solvent (good solvent) that can dissolve the above organic polymer, and is preferably a solvent miscible with water, or a mixed solvent of water and a water-miscible solvent. The water-miscible solvent is preferably selected from N-methyl-2-pyrrolidone (NMP), N-ethyl-pyrrolidone (NEP), N-butyl-pyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, γ-valerolactone, compound (2), compound (3) shown below, and mixtures thereof, with at least one of NMP, NBP, DMF, γ-valerolactone, compound (2), and compound (3) shown below being more preferred, and DMF being even more preferred.

[0053] In particular, using a mixed solvent of water and a miscible solvent is preferred as the solvent, from the viewpoint of easily adjusting the metal element ratio on the surface to the above range, a mixed solvent of water and at least one of NMP, NBP, DMF, γ-valerolactone, and the compounds (2) and (3) shown above is more preferred, and a mixed solvent of water and DMF is even more preferred. The amount of water mixed in this mixed solvent can be appropriately determined, for example, it can be 0.1 to 1.5% by mass, and it is preferable to have an amount of 0.6 to 1.2% by mass in terms of easily adjusting the metal element ratio on the surface.

[0054] The solvent content in the above film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 25 to 70% by mass, even more preferably 30 to 65% by mass, even more preferably 32 to 60% by mass, and even more preferably 35 to 50% by mass.

[0055] (Organic Polymers) The description of organic polymers in the film-forming solution can be applied to the organic polymers in the separator described above. The content of organic polymers in the film-forming solution is preferably 2 to 30% by mass, more preferably 4 to 20% by mass, even more preferably 5 to 15% by mass, and particularly preferably 6 to 12% by mass.

[0056] (Hydrophilic inorganic particles) The description of hydrophilic inorganic particles in the separator described above can be applied to the hydrophilic inorganic particles contained in the film-forming solution. Although hydrophilic inorganic particles are particles that exist dispersed in the film-forming solution without dissolving, in this invention, such a dispersion state is also referred to as the film-forming solution. That is, the "solution" in the film-forming solution refers to the state in which the organic polymer is dissolved in the solvent. The content of hydrophilic inorganic particles in the above film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 20 to 70% by mass, and particularly preferably 25 to 60% by mass.

[0057] In the film-forming solution, the ratio of the content of hydrophilic inorganic particles to the content of organic polymer (content of hydrophilic inorganic particles / content of organic polymer) is preferably 10.0 / 1 to 1.0 / 1 by mass, more preferably 9.0 / 1 to 2.0 / 1, even more preferably 8.0 / 1 to 3.0 / 1, even more preferably 7.0 / 1 to 4.0 / 1, and even more preferably 6.9 / 1 to 5.3 / 1. As shown in Comparative Example 2 described later, when the ratio of the content of hydrophilic inorganic particles to the content of organic polymer in the film-forming solution becomes large, hydrophilic inorganic particles may fall off on or near the surface of the separator, but this does not affect the total content of hydrophilic inorganic particles in the separator.

[0058] (Other Components) The above film-forming solution may contain components other than those described above (solvent, organic polymer, and hydrophilic inorganic particles). For example, in order to control pore formation in wet phase separation, it may contain polyethylene glycol, polyethylene oxide, polypropylene glycol, ethylene glycol, tripropylene glycol, glycerol, polyhydric alcohol, dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid, neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, and lithium chloride. These components (also referred to as additives) are thought to be able to control pore formation by at least one action, such as adjusting the viscosity of the film-forming solution (coating solution) which serves as the starting point for pore formation in the wet phase separation step described later, or adjusting the hydrophilicity of the inner wall of the formed pores. In the present invention, additives can be selected considering gas barrier properties and ionic resistance, and among them, polyvinylpyrrolidone is preferred. In the above film-forming solution, the total content of other components is preferably 0.1 to 15% by mass, more preferably 0.2 to 10% by mass, and even more preferably 0.5 to 5% by mass.

[0059] <Formation of Porous Material by Wet Phase Separation> (Water Vapor Induced Phase Separation) In a preferred method for manufacturing the separator of the present invention, water vapor induced phase separation may be performed on the coating-side surface (hereinafter also simply referred to as "the coating-side surface of the laminate") of a laminate consisting of a film-forming support and a coating film containing the constituent materials of the separator of the present invention formed on the film-forming support (this laminate may also be a laminate in which a porous support is impregnated into the coating film). The laminate can be formed, for example, by dissolving the organic polymer and casting a film-forming solution containing the hydrophilic inorganic particles onto the film-forming support, and then appropriately drying the surface to form a coating film. When impregnating the porous support with the film-forming solution, the porous support may be pre-placed on the film-forming support from which the film-forming solution is cast, or it may be impregnated by immersing the porous support in the coating film obtained by casting.

[0060] In water vapor induction phase separation, it is preferable to use high-temperature, high-humidity water vapor as the poor solvent vapor in the water vapor induction phase separation. The relative humidity in the region where water vapor induction phase separation is performed can be, for example, 50 to 99%, more preferably 60 to 99%, and even more preferably 70 to 99%. The temperature in the region where water vapor induction phase separation is performed is, for example, preferably 55 to 85°C, more preferably 60 to 80°C, and even more preferably 60 to 75°C. The time for performing water vapor induction phase separation is, for example, preferably 1 to 35 seconds, more preferably 1 to 30 seconds, and even more preferably 1 to 25 seconds. The space in which water vapor induction phase separation is performed is not particularly limited in terms of specific adjustment methods, equipment, etc., as long as it can be a space in which the predetermined temperature and humidity are maintained. It is preferable that the space is provided so as to be continuous with the solidification bath in which liquid induction phase separation is performed after water vapor induction phase separation.

[0061] (Liquid Induction Phase Separation) In a preferred method for manufacturing the separator of the present invention, the separator of the present invention can be manufactured by impregnating the laminate that has undergone the above-mentioned water vapor induction phase separation into a solidification bath with the film-forming support still attached, or with the film-forming support removed, and performing liquid induction phase separation. Alternatively, the separator of the present invention can be manufactured by impregnating the laminate described in the above-mentioned water vapor induction phase separation (the laminate before the above-mentioned water vapor induction phase separation) into a solidification bath with the film-forming support still attached, or with the film-forming support removed, and performing liquid induction phase separation. In the present invention, when the laminate that has undergone the above-mentioned water vapor induction phase separation or the laminate described in the above-mentioned water vapor induction phase separation is impregnated into a solidification bath with the film-forming support still attached, and liquid induction phase separation is performed, it becomes easier to adjust the metal element ratio on the surface to the range described above. Therefore, performing liquid induction phase separation with the film-forming support still attached is preferable in that it is possible to manufacture a separator that satisfies the metal element ratio on the surface.

[0062] In liquid-induced phase separation, the above-mentioned organic polymer is not dissolved, and a solvent (poor solvent) that is compatible (miscible) with the solvent (good solvent) of the film-forming solution is used as the solidification bath. By immersing the laminate that has undergone the above-mentioned water vapor-induced phase separation, or the laminate described in the above-mentioned water vapor-induced phase separation, in the solidification bath, the proportion of good solvent in the coating film of the film-forming solution decreases, the organic polymer and the solvent undergo phase separation (liquid-induced phase separation), the organic polymer gels (solidifies), a porous material containing the organic polymer is formed, and the separator of the present invention can be obtained.

[0063] In the wet phase separation described above, the poor solvent used in the coagulation bath can be, for example, water, a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water), a mixed solvent of water and a water-soluble polymer, or a mixed solvent of water, a hydrophilic organic solvent, and a water-soluble polymer. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAC), and alcoholic solvents such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among the above, water or a mixed solvent of water and a hydrophilic organic solvent is preferred as the poor solvent, and water or a mixed solvent of water and an aprotic solvent (particularly preferably DMF) is more preferred in that it is easier to set the surface metal element ratio within the above range, and a mixed solvent of water and an aprotic solvent (particularly preferably DMF) is even more preferred. The amount of water mixed in the mixed solvent can be appropriately determined considering the state of phase separation, and can be, for example, 10 to 99% by mass, but it is preferable to set it to 70 to 95% by mass, as this makes it easier to adjust the ratio of metal elements on the surface.

[0064] The temperature of the solidification bath can be appropriately determined according to the components of the film-forming solution, and is usually preferably 5 to 60°C. From the viewpoint of easily adjusting the ratio of metal elements on the surface to the above range, a lower temperature is preferable, specifically 5 to 55°C is more preferable, 5 to 35°C is even more preferable, and 5 to 15°C is particularly preferable. From the viewpoint of controlling the pore size of the coating film on the film-forming support side and easily adjusting the ratio of metal elements on the surface to the above range, the time for performing the solidification bath is preferably 1 to 15 minutes, more preferably 1 to 12 minutes, and even more preferably 3 to 10 minutes.

[0065] From the viewpoint of easily setting the surface metal element ratio within the above range, it is preferable that the solvent in the film-forming solution and the temperature of the solidification bath in wet phase separation satisfy the following relationship, for example: When the solvent in the film-forming solution in wet phase separation is a solvent miscible with water (does not contain water), the temperature of the solidification bath is preferably 5 to 35°C, and more preferably 5 to 15°C. When the solvent in the film-forming solution in wet phase separation is a mixed solvent of water and a solvent miscible with water, the temperature of the solidification bath is preferably 5 to 60°C, and more preferably 5 to 35°C.

[0066] In the above liquid derivative phase separation, after immersing the laminate in the poor solvent to form a porous material, it may be immersed in glycols such as ethylene glycol and diethylene glycol, and water, or washed with the aforementioned glycols and water. This step can remove any remaining solvent from the porous material. The conditions for immersion and washing are not particularly limited and can be determined as appropriate.

[0067] In the separator obtained by the above-described method for manufacturing separators, a certain amount of good solvent from the film-forming solution used in its manufacture inevitably remains. As a result, a separator is provided in which the total content of good solvent in the porous material is 0.01 to 5.00% by mass. The amount of residual solvent is determined by gas chromatography or after pre-drying the separator at 40°C for 12 hours. 1 The amount can be quantified as a mass percentage of 100% by mass of the dried separator using 1H-NMR (nuclear magnetic resonance) measurement.

[0068] [Alkaline Water Electrolysis] The separator of the present invention can be used, for example, by placing it between the cathode and the anode in alkaline water electrolysis. Preferred embodiments of an alkaline water electrolysis apparatus to which the separator of the present invention is applied (also referred to as "the alkaline water electrolysis apparatus of the present invention") will be described, but the alkaline water electrolysis of the present invention is not limited to these embodiments.

[0069] Figure 1 schematically shows a preferred embodiment of the alkaline water electrolysis apparatus of the present invention. In the alkaline water electrolysis apparatus (10) shown in Figure 1, a cathode electrode (12) is arranged on one side of the separator (11) of the present invention, and an anode electrode (13) is arranged on the other side. The separator (11) and each electrode (12, 13) are immersed in a high-concentration alkaline aqueous solution (14, preferably a potassium hydroxide aqueous solution or a sodium hydroxide aqueous solution). When an electric current flows between the electrodes, electrons are supplied to the cathode side, and bubble-like hydrogen (H) is produced from the water. 2 ) occurs (2H 2 O + 2e - →H 2 +2OH - ). Along with the generation of hydrogen, a hydroxyl ion (OH) is produced. - ) passes through the separator (11) and moves to the anode side, where electrons are removed and bubble-shaped oxygen (O 2 ) occurs (4OH - →O 2 +2H 2 O+4e - ). The cathode electrode (12) and anode electrode (13) described above are preferably composed of an electrode substrate (conductive material) and a catalyst layer on the electrode substrate. When a catalyst layer is included, the catalyst species may be the same or different between the cathode electrode (12) and the anode electrode (13). In the alkaline water electrolysis apparatus (10) shown in Figure 1, the separator (11) and each electrode (12, 13) are far apart, so the distance traveled by hydroxyl ions is long, which limits the improvement of ion conduction efficiency.

[0070] Figure 2 schematically shows another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (20) shown in Figure 2 is a zero-gap type in which the separator (11) and each electrode (12, 13) are arranged in contact with each other in the alkaline water electrolysis apparatus (10) shown in Figure 1. Because the separator (11) and each electrode (12, 13) are in contact in the alkaline water electrolysis apparatus (20) shown in Figure 2, the distance traveled by hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency. In addition, from the viewpoint of imparting suitability for renewable energy, pressurized alkaline water electrolysis apparatuses that are operated under a pressure of 10 bar or more relative to atmospheric pressure (approximately 1 bar) are also known. As an example of such a pressurized alkaline water electrolysis apparatus, an example is the alkaline water electrolysis apparatus shown in Figure 2, in which the configuration, components, etc. of the alkaline water electrolysis apparatus are appropriately adjusted to be able to handle pressurized operation (for example, operation under pressurized conditions of 10 bar or more).

[0071] Figure 3 schematically shows yet another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (30) shown in Figure 3 is a configuration that includes a membrane electrode assembly. That is, a cathode catalyst layer (32) is arranged on one side of the separator (31) of the present invention, and an anode catalyst layer (33) is arranged on the other side. These catalyst layers are composed of a catalyst and its binder. Furthermore, a gas diffusion layer (34) is formed on the outer surface of these catalyst layers (the surface opposite to the side on which the separator (33) is arranged) to constitute a membrane electrode assembly. In Figure 3, a bipolar plate (35) is formed further outside the membrane electrode assembly. When an alkaline aqueous solution is supplied to the cathode catalyst layer (32) and the anode catalyst layer (33) of this membrane electrode assembly, and the cathode catalyst layer (32) and the anode catalyst layer (33) are electrically connected and current is passed, bubble-like hydrogen is generated from the cathode catalyst layer (32) and bubble-like oxygen is generated from the anode catalyst layer (33).

[0072] In the above-described alkaline water electrolysis apparatus, the components other than the separator, such as the cathode electrode, cathode catalyst layer, anode electrode, and anode catalyst layer, are not particularly limited, and ordinary components used in alkaline water electrolysis apparatuses can be appropriately applied.

[0073] Thus, in one embodiment, the present invention provides an alkaline water electrolysis apparatus in which the separator of the present invention is incorporated as a separator in the alkaline water electrolysis apparatus. Furthermore, in one embodiment, the present invention provides a method for manufacturing an alkaline water electrolysis apparatus, which includes incorporating the separator of the present invention as a separator in the alkaline water electrolysis apparatus.

[0074] [Alkaline Water Electrolysis Member] The alkaline water electrolysis member of the present invention includes the separator of the present invention. Specifically, the alkaline water electrolysis member of the present invention includes the separator of the present invention and at least one of a catalyst, an anode electrode, and a cathode electrode. The form including the separator of the present invention, an anode electrode, and a cathode electrode will be classified as the alkaline water electrolysis cell of the present invention, as described later. Forms in which the alkaline water electrolysis member of the present invention does not include an electrode but includes a catalyst include a form in which the catalyst is located on only one side of the separator of the present invention, and a form in which the catalyst is located on both sides of the separator of the present invention. Forms in which the alkaline water electrolysis member of the present invention does not include a cathode electrode but includes an anode electrode include a form in which the anode electrode is located on one side of the separator of the present invention. In this form, the catalyst may or may not be present. If a catalyst is present, the catalyst may be located on only one side of the separator of the present invention, or the catalyst may be located on both sides of the separator of the present invention. In the present invention, an alkaline water electrolytic member does not include an anode electrode but includes a cathode electrode. This configuration includes having a cathode electrode on one side of the separator. In this configuration, a catalyst may or may not be present. If a catalyst is present, the catalyst may be present on only one side of the separator, or on both sides of the separator.

[0075] [Alkaline Water Electrolysis Cell] The alkaline water electrolysis cell of the present invention includes the separator of the present invention or the alkaline water electrolysis component of the present invention. The "alkaline water electrolysis cell" includes the separator and two electrodes separated by the separator (anode electrode and cathode electrode). In this embodiment, an alkaline aqueous solution may be present as an electrolyte between both electrodes (including the separator of the present invention), and the anode electrode and cathode electrode may each further contain a catalyst. For example, if the alkaline water electrolysis cell of the present invention includes the separator of the present invention, the alkaline water electrolysis cell of the present invention can be made by combining the separator of the present invention with the anode electrode and cathode electrode. In this case, the anode electrode and cathode electrode may each independently contain a catalyst. Also, if the alkaline water electrolysis cell of the present invention does not include electrodes and includes the separator and catalyst of the present invention, the alkaline water electrolysis cell of the present invention can be made by combining them with the anode electrode and cathode electrode. In this case, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the anode electrode or cathode electrode. In the alkaline water electrolytic cell of the present invention, the catalyst may be included on at least one side of the separator of the present invention, or it may be included on both sides. Furthermore, if the alkaline water electrolytic cell of the present invention does not include a cathode electrode but includes the separator and anode electrode of the present invention, it can be made into the alkaline water electrolytic cell of the present invention by combining it with a cathode electrode. In this case, the anode electrode and cathode electrode may each independently contain the catalyst. Furthermore, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the cathode electrode. Furthermore, if the alkaline water electrolytic cell of the present invention does not include an anode electrode but includes the separator and cathode electrode of the present invention, it can be made into the alkaline water electrolytic cell of the present invention by combining it with an anode electrode. In this case, the anode electrode and cathode electrode may each independently contain the catalyst.Furthermore, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the anode electrode.

[0076] [Method for Producing Hydrogen] The method for producing hydrogen according to the present invention is the same as a conventional method for producing hydrogen (water electrolysis), except that it includes electrolysis of water using the alkaline water electrolysis apparatus of the present invention. In particular, a preferred method for producing hydrogen according to the present invention is one which includes using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as the electrolyte solution and electrolyzing water at 70 to 95°C. Examples of metal hydroxides include sodium hydroxide and potassium hydroxide, and potassium hydroxide is preferred from the viewpoint of having a higher specific conductivity of the aqueous solution of the metal hydroxide. The content of the metal hydroxide (electrolyte) in the alkaline aqueous solution is 10 to 35% by mass, preferably 25 to 35% by mass, and more preferably 28 to 32% by mass. The temperature of the alkaline aqueous solution used when operating the alkaline water electrolysis apparatus and producing hydrogen by electrolyzing water is 70 to 95°C, preferably 70 to 90°C. This temperature may also be 75 to 85°C or 78 to 82°C. Thus, the separator of the present invention can be suitably used in the method for producing hydrogen according to the present invention that uses a high-temperature, high-concentration alkaline aqueous solution.

[0077] The present invention will be described in more detail below based on examples, but the present invention is not to be construed as being limited thereto. The water used is deionized water. "rpm" means revolutions per minute.

[0078] [Example 1] 8.5 g of polysulfone (product name: Udel P-3500 LCD MB7, Mw: approximately 80,000, manufactured by Solvay) was added to 41.3 g of DMF (dimethylformamide, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and stirred overnight at 50°C to completely dissolve it. Next, 2.4 g of PVP K90 (product name: polyvinylpyrrolidone, manufactured by Merck) was added and stirred at 60°C for 1 hour, after which ZrO 247.9 g of particles (product name: E101, particle size 0.8 μm, manufactured by Luxfer Mel Technologies) were added, and the mixture was then stirred and defoamed using an Awatori Rentaro (product name, manufactured by THINKY, model: ARV-310LED) (orbital speed: 1200 rpm, vacuum value: 30 kPa, stirring time: 4 minutes) to obtain coating solution A. The obtained coating solution A was cast onto a PET (polyethylene terephthalate) film on which a polyether ether ketone (PEEK) woven fabric (product name: RIBONS MADE OF SEFAR PEEKTEX IEM-17-240 / 62, thickness approximately 100 μm, manufactured by Sefar) was placed as a porous support, using an applicator with a clearance set to 500 μm, and the woven fabric was completely impregnated with coating solution A. Next, the material was gently immersed in a condensation bath cooled to 10°C (a mixture of 10% by mass of DMF (dimethylformamide) and 90% by mass of pure water) and left immersed for 5 minutes (solidification time) to form a porous polysulfone structure (referred to as "PSU porous structure") (phase separation step in the condensation bath). Furthermore, it was washed with water at 60°C for 5 minutes, and the woven fabric and the PSU porous structure were peeled off from the PET film as a single unit to obtain the separator of Example 1.

[0079] [Example 2] The separator of Example 2 was obtained in the same manner as in Example 1, except that the temperature of the coagulation bath was set to 30°C.

[0080] [Example 3] The separator of Example 3 was obtained in the same manner as in Example 1, except that in addition to 41.3 g of DMF, 0.41 g of water was used as the solvent for preparing the polysulfone solution.

[0081] [Example 4] The separator of Example 4 was obtained in the same manner as in Example 3, except that the temperature of the coagulation bath was set to 30°C.

[0082] [Example 5] The separator of Example 5 was obtained in the same manner as in Example 3, except that the temperature of the coagulation bath was set to 50°C.

[0083] [Example 6] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 49.3 g, and ZrO 2The separator of Example 6 was obtained in the same manner as in Example 2, except that the amount of particles was changed from 47.9 g to 39.9 g.

[0084] [Example 7] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 45.3 g, and ZrO 2 The separator of Example 7 was obtained in the same manner as in Example 2, except that the particle size was changed from 47.9 g to 43.9 g.

[0085] [Example 8] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 37.3 g, and ZrO 2 The separator of Example 8 was obtained in the same manner as in Example 2, except that the amount of particles was changed from 47.9 g to 51.9 g.

[0086] [Example 9] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 33.3 g, and ZrO 2 The separator of Example 9 was obtained in the same manner as in Example 2, except that the particle size was changed from 47.9 g to 55.9 g.

[0087] [Example 10] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 29.3 g, and ZrO 2 The separator of Example 10 was obtained in the same manner as in Example 2, except that the amount of particles was changed from 47.9 g to 59.9 g.

[0088] [Example 11] The separator of Example 11 was obtained in the same manner as in Example 1, except that coating solution B described below was used instead of coating solution A. (Preparation of coating solution B) 11 g of polysulfone (product name: Udel P-3500 LCD MB7, Mw: approximately 80,000, manufactured by Solvay) was added to 40 g of NBP (N-butylpyrrolidone, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and stirred overnight at 50°C to completely dissolve it. Next, 5 g of glycerin was added and stirred at 60°C for 1 hour, and then ZrO 244 g of particles (product name: E101, particle size 0.8 μm, manufactured by Luxfer Mel Technologies) were added, and then the mixture was stirred and defoamed using an Awatori Rentaro (product name, manufactured by THINKY, model: ARV-310LED) (orbital speed: 1200 rpm, vacuum value: 30 kPa, stirring time: 4 minutes) to obtain coating solution B.

[0089] [Example 12] The separator of Example 12 was obtained in the same manner as in Example 4, except that the clearance setting of the applicator was changed to 400 μm.

[0090] [Example 13] The separator of Example 13 was obtained in the same manner as in Example 4, except that the clearance setting of the applicator was changed to 1000 μm.

[0091] [Comparative Example 1] A separator for Comparative Example 1 was obtained in the same manner as in Example 1, except that the temperature of the coagulation bath was set to 50°C.

[0092] [Comparative Example 2] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 25.3 g, and ZrO 2 A separator for Comparative Example 2 was obtained in the same manner as in Example 2, except that the amount of particles was changed from 47.9 g to 63.9 g.

[0093] [Comparative Example 3] In Example 2, the amount of DMF used to prepare the polysulfone solution was changed from 41.3 g to 53.3 g, and ZrO 2 A separator for Comparative Example 3 was obtained in the same manner as in Example 2, except that the amount of particles was changed from 47.9 g to 35.9 g.

[0094] [Evaluation of Separators] The following measurements and evaluations were performed on each separator fabricated as described above. The results are shown in Tables 1-1 and 1-2 (hereinafter referred to as Table 1). Unless otherwise specified, the separators used for each evaluation were those that had been cut to the desired shape for the evaluation described later.

[0095] <Thickness of the Separator> A cross-section cut from the separator with a razor blade was scanned using a cross-sectional SEM (scanning electron microscope) at a magnification that allowed the entire separator cross-section to fit in a single field of view (e.g., 200x). Assuming that no pores exist in the obtained cross-sectional SEM image (assuming that the pores are filled with organic polymer), the thickness was measured at 20 equally spaced points. The arithmetic mean of the 20 measurements was calculated and rounded to the first decimal place in μm, and this value is shown in Table 1 as the thickness of the separator. The following equipment was used for the cross-sectional SEM observation. Conductive processing device: Meiwa Forsis Co., Ltd., Model: HPC-1SW osmium coater / Source: Os / Thickness: 5 nm CIS device: JEOL Ltd., Model: IB-09060CIS / Acceleration voltage: 4 kV / Processing temperature: -130°C / Pre-treatment The sample cut with a razor blade was attached to a Si wafer (100 μm thick) with epoxy resin and fixed. FE-SEM (Field Emission Scanning Electron Microscope) observation system: Carl Zeiss, Model: Ultra5, Measurement conditions: Secondary / backscattered electron image, Acceleration voltage 2kV, Aperture 30μm, Working distance 3.0mm (cross-section)

[0096] <Surface Metal Element Ratio> Samples for measurement were cut from the separator, and X-ray photoelectron spectroscopy (XPS) was performed on the surface of each sample that was in contact with the PET film (substrate surface) and the surface that was not in contact with the PET film (Air surface) under the conditions described below. Specifically, Wide Scan (Survey) measurements were performed under the conditions described below, and for the elements (S, C, O, Zr, and N) for which peaks were observed, Narrow Scan measurements were performed under the conditions described below to obtain X-ray photoelectron spectra. Peak separation was performed on each obtained X-ray photoelectron spectrum, and the abundance ratio (at%) of each element was calculated to determine the metal element ratio. - XPS Measurement Conditions - Equipment: Quantera SXM type XPS (product name) manufactured by Ulvac-PHI X-ray source: Monochromatic Al-Kα rays X-ray beam diameter: 100 μmφ (X-ray output: 25 W, accelerating voltage: 15 kV) Measurement area: Square with sides of 300 μm Photoelectron extraction angle: 45° Charge correction (charge neutralization) mechanism: Use of low-energy electron gun and low-energy ion gun (Wide Scan (Survey) measurement conditions) Time per step: 20 ms (Survey) Pass Energy: 280.0 eV Step: 1.0 eV (Narrow Scan measurement conditions) Time per step: 50 ms (narrow) Pass Energy: 55.0 eV Step: 0.05 eV Number of cumulative steps: 10

[0097] <Metal element ratios by depth profiling> Samples for measurement were cut from the separator, and each surface of the sample, both the side in contact with the PET film (substrate surface) and the side not in contact with the PET film (Air surface), was etched using an Ar+ ion gun under the conditions described below. Then, X-ray photoelectron spectroscopy analysis was performed in the same manner as described in <Surface metal element ratios> above (depth profiling X-ray photoelectron spectroscopy analysis was performed) to determine the metal element ratios. (Etching conditions using an Ar+ ion gun) Acceleration voltage: 4kV Etching area: 2mm square Etching time: 30 minutes Etching rate: 22nm / min (SiO 2 conversion speed)

[0098] <Ionic Resistance> A two-chamber cell, having nickel electrodes at the current control terminal and a Lugin tube filled with 3M-KCl at the voltage control terminal, was subjected to a 30% potassium hydroxide aqueous solution as the electrolyte, and maintained at 30°C. In galvanostat mode, the current density was 10 mA / cm². 2 The ion resistance was measured under the conditions described above to obtain a blank value for measurement. Next, a sample punched out in a circular shape with a diameter of 10 mm was placed between each of the separators prepared above, and a 30% potassium hydroxide aqueous solution was filled in the same manner as the blank value measurement, and the ion resistance was measured under the same conditions as the blank value measurement. The difference between the obtained resistance value of each separator and the blank value (i.e., the value calculated by [separator resistance value] - [blank value]) was taken as the ion resistance value of that separator, and the ion resistance was evaluated according to the following evaluation criteria. - Evaluation Criteria - A: Ion resistance value of 0.15 Ω・cm 2 It is less than B. + Ionic resistance value: 0.15 Ω·cm 2 0.18Ω・cm or more 2 It is less than B. - Ionic resistance value: 0.18 Ω·cm 2 0.20Ω・cm or more 2 It is less than . C: Ionic resistance is 0.20 Ω·cm 2 0.25Ω・cm or more 2 It is less than . D: Ionic resistance is 0.25 Ω·cm 2 0.30Ω・cm or more 2 It is less than.

[0099] <Gas Barrier Properties> The separator obtained above was set in a cell for water electrolysis evaluation, and an electrolyte (30% potassium hydroxide aqueous solution) heated to 85°C was supplied to the anode and cathode at a rate of 30 mL / min. The current density was 0.1 A / cm². 2The cell was run continuously for 60 minutes with current applied to stabilize it. After that, it was run continuously for another 60 minutes (main operation), and the extent to which hydrogen gas generated on the cathode side leaked to the anode side during this 60 minutes was evaluated. Specifically, the gas recovered from the anode side flow path during the main operation was cooled to 0°C, water vapor was removed, and then it was analyzed using a gas chromatograph (GC3210G / GL Sciences, column: MS13X) to calculate the hydrogen gas concentration (unit: volume %) in the recovered gas, and the gas barrier properties were evaluated according to the following evaluation criteria. - Evaluation Criteria - A: Hydrogen gas concentration is less than 0.10 volume%. B: Hydrogen gas concentration is 0.10 volume% or more and less than 0.15 volume%. C: Hydrogen gas concentration is 0.15 volume% or more and less than 0.20 volume%. D: Hydrogen gas concentration is 0.20 volume% or more.

[0100]

[0101]

[0102] (Notes in the table) In the "Coating Solution" column, the amount of each component added (in g) is shown, and a blank space indicates that the component is not contained. Also, in the "Manufacturing Conditions" column, ○ indicates the coagulation bath temperature.

[0103] From Table 1 above, the following can be seen. As shown in Comparative Examples 1 to 3, if the ratio of metal elements to total elements (surface metal element ratio), measured by X-ray photoelectron spectroscopy, on at least one surface of the separator does not meet the range defined in the present invention, the gas barrier properties are poor. In Comparative Example 1, since the coating solution (film-forming solution) did not contain water and the temperature of the solidification bath was high at 50°C, the phase separation rate of the wet phase separation was slow, and the formation of a dense film of organic polymer on the separator surface was not suppressed, resulting in a surface metal element ratio of 4 at% or less. In Comparative Example 2, the amount of hydrophilic inorganic particles in the coating solution (film-forming solution) was large, and the hydrophilic inorganic particles fell off the separator surface, resulting in a low surface metal element ratio of 3 at%. In Comparative Example 3, the amount of hydrophilic inorganic particles in the coating solution (film-forming solution) was small to begin with, resulting in a surface metal element ratio of 4 at% or less. In contrast, the separators of Examples 1 to 13, in which the ratio of metal elements on at least one surface of the separator satisfies the range defined in this invention, all exhibit excellent gas barrier properties. In particular, when the ratio of metal elements on at least one surface of the separator is 10 at% or higher, and even higher at 15 at% or higher, even better gas barrier properties are observed (see Examples 1 to 5, 8 and 9 for Examples 6, 7, 10 and 11, and Examples 1, 3 and 4 for Examples 2, 5, 8 and 9, respectively). Furthermore, when the thickness of the separator is 100 to 400 μm, and the ratio of metal elements to total elements (ratio of metal elements by depth profiling) measured by depth profiling analysis by X-ray photoelectron spectroscopy from at least one surface of the separator is 20 at% or more and less than 45 at%, the ion resistance is also kept low (Examples 1 to 12 for Comparative Examples 2 and 3).When the thickness of this separator is 100 to 400 μm, if the ratio of metal elements obtained by depth profiling from at least one surface of the separator is 25 at% or more and less than 45 at% (Examples 1 to 5 and 7 to 12 for Example 6), the ion resistance can be kept even lower if it is 30 at% or more and less than 45 at%, and even 34 at% or more and less than 45 at% (Examples 1 to 5 and 8 to 12 for Example 7, and Examples 1 to 5, 8 to 10 and 12 for Example 11, respectively). Furthermore, while gas barrier properties are usually improved by increasing the thickness of the separator, it can be seen that by making the ratio of metal elements on the surface satisfy the range defined in this invention, the same level of gas barrier properties can be obtained even when the thickness of the separator is thin. This can be seen from the fact that the separators of Examples 5 and 12 (thickness 260 μm and 200 μm, surface metal element ratio 12 at% or 13 at%) and the separator of Example 13 (thickness 500 μm, surface metal element ratio 12 at%) all received a "B" rating for gas barrier performance (hydrogen gas concentration on the anode side is 0.10 volume% or more and less than 0.15 volume%), indicating that the amount of hydrogen gas leaking to the anode side is suppressed to a similar extent.

[0104] Although we have described the present invention along with its embodiments, we do not intend to limit our invention in any detail of the description unless specifically designated, and we believe that it should be interpreted broadly without contradicting the spirit and scope of the invention as set forth in the appended claims.

[0105] This application claims priority based on Japanese Patent Application No. 2025-078740, filed in Japan on 9 May 2025, the contents of which are incorporated herein by reference as part of this specification.

[0106] 10 Alkaline water electrolysis apparatus 11 Separator 12 Cathode electrode 13 Anode electrode 14 High-concentration alkaline aqueous solution 20 Alkaline water electrolysis apparatus 30 Alkaline water electrolysis apparatus 31 Separator 32 Cathode catalyst layer 33 Anode catalyst layer 34 Gas diffusion layer 35 Bipolar plate O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH- Hydroxy ion e - electronic

Claims

1. A porous separator for water electrolysis comprising an organic polymer and hydrophilic inorganic particles, wherein the ratio of metal elements to total elements, as measured by X-ray photoelectron spectroscopy, is 5 at% or more on at least one surface of the porous separator for water electrolysis.

2. The porous separator for water electrolysis according to claim 1, wherein the ratio of metal elements to total elements, as measured by X-ray photoelectron spectroscopy, is 5 at% or more on both surfaces of the porous separator for water electrolysis.

3. The porous separator for water electrolysis according to claim 1, wherein the ratio of metal elements to total elements, as measured by X-ray photoelectron spectroscopy, is 10 at% or more on at least one surface of the porous separator for water electrolysis.

4. The porous separator for water electrolysis according to claim 3, wherein the ratio of metal elements to total elements, as measured by X-ray photoelectron spectroscopy, is 15 at% or more on at least one surface of the porous separator for water electrolysis.

5. The porous separator for water electrolysis according to claim 1, wherein the thickness of the porous separator for water electrolysis is 100 to 400 μm, and the ratio of metal elements to total elements, as measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis, is 20 at% or more and less than 45 at%.

6. The porous separator for water electrolysis according to claim 5, wherein the ratio of metal elements to total elements, as measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis, is 25 at% or more and less than 45 at%.

7. The porous separator for water electrolysis according to claim 6, wherein the ratio of metal elements to total elements, as measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis, is 30 at% or more and less than 45 at%.

8. The porous separator for water electrolysis according to claim 7, wherein the ratio of metal elements to total elements, as measured by depth profiling by X-ray photoelectron spectroscopy from at least one surface of the porous separator for water electrolysis, is 34 at% or more and less than 45 at%.

9. The porous separator for water electrolysis according to claim 1, wherein the metal element is Ti, Mg, Zr, Al, Zn, Ca, Ba, Sr, Pb, Ta, Bi, and Ce.

10. The porous separator for water electrolysis according to claim 9, wherein the metal element is Zr.

11. An alkaline water electrolysis member comprising the porous separator for water electrolysis described in claim 1.

12. An alkaline water electrolysis cell comprising a porous separator for water electrolysis according to any one of claims 1 to 10, or an alkaline water electrolysis member according to claim 11.

13. An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell described in claim 12.

14. A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus described in claim 13.

15. A method for producing hydrogen according to claim 14, comprising using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as an electrolyte solution, and electrolyzing water at 70 to 95°C.