Separator for alkaline water electrolysis, alkaline water electrolysis cell, and alkaline water electrolysis device

By controlling the thermal expansion coefficients in the separator's fabric and polymer layer to a ratio of 1.5 or less, the separator addresses misalignment and deformation issues, enhancing stability and reducing damage during alkaline water electrolysis.

WO2026234973A1PCT designated stage Publication Date: 2026-11-12FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015634
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-17
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing alkaline water electrolysis separators face issues such as misalignment and deformation due to mismatched thermal expansion coefficients between the separator and electrodes, leading to scratches and potential damage during operation.

Method used

The separator is designed with a woven or nonwoven fabric support base material embedded with a porous polymer layer, where the linear thermal expansion coefficients in different directions are carefully controlled to maintain a ratio of 1.5 or less, reducing anisotropy and minimizing scratches.

Benefits of technology

This design effectively suppresses scratches and damage to the separator during alkaline water electrolysis, ensuring stable operation and reducing the risk of misalignment and deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015634_12112026_PF_FP_ABST
    Figure JP2026015634_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a separator for alkaline water electrolysis including: a support substrate which is a woven fabric or a nonwoven fabric; and a porous polymer layer in which at least part of the support substrate is embedded. In the in-plane direction of the separator for alkaline water electrolysis, the ratio of T1 to T2 is 1.5 or less, where T1 is the linear thermal expansion coefficient in a direction t1 in which the linear thermal expansion coefficient becomes the maximum, and T2 is the linear thermal expansion coefficient in a direction t2 in which the linear thermal expansion coefficient becomes the minimum. Also provided is a use of said separator for alkaline water electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Separator for alkaline water electrolysis, alkaline water electrolysis cell, and alkaline water electrolysis apparatus

[0001] The present disclosure relates to a separator for alkaline water electrolysis, an alkaline water electrolysis cell, and an alkaline water electrolysis apparatus.

[0002] Hydrogen is a clean energy source that does not emit carbon dioxide, and is used, for example, as fuel for fuel cell vehicles and household fuel cells. As a method for producing hydrogen, alkaline water electrolysis using a high-concentration alkaline aqueous solution as an electrolyte is known. If alkaline water electrolysis is performed using a power generation system that utilizes renewable energy as a power source, hydrogen can be produced without emitting carbon dioxide, and thus hydrogen is attracting increasing attention as a fundamental energy source for a sustainable society.

[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H generated at the cathode 2 O + 2e - →H 2 + 2OH - ) is prevented from moving to the anode side, and the bubble-like oxygen (4OH generated at the anode - →O 2 + 2H 2 O + 4e - ) is prevented from moving to the cathode side, a gas barrier separator (diaphragm) is disposed between the cathode and the anode.

[0004] Patent Document 1 discloses a bipolar electrolytic cell in which a plurality of elements including an anode and a cathode are stacked with a diaphragm interposed therebetween, and the diaphragm is in contact with the anode and the cathode to form a zero-gap structure, wherein in the zero-gap structure, the difference ΔH (|Ha-Hc|) between the heat generation coefficient Ha [K / sec] of the anode defined by the formula (1) and the heat generation coefficient Hc [K / sec] of the cathode defined by the formula (2) is 0.18 to 10.11 K / sec, and the linear expansion coefficient of the diaphragm is 0.5 × 10 -5 [1 / K] or more and 2.0 × 10 -5A bipolar electrolytic cell is described, characterized in that it is [1 / K] or less. Patent Document 2 describes an electrolytic cell separator, characterized in that it has a residual non-aqueous solvent amount of less than 5% by mass relative to the total dry weight of the separator.

[0005] Patent Document 1: Japanese Patent No. 6782796 Patent Document 2: International Publication No. 2023 / 118088

[0006] Conventionally, a configuration is known in which an alkaline water electrolysis separator and an electrode are used in combination. In this configuration, when alkaline water electrolysis is performed, there was a risk of damage to the alkaline water electrolysis separator due to misalignment between the separator and the electrode, or deformation of the separator.

[0007] The object of one embodiment of this disclosure is to provide an alkaline water electrolysis separator in which the occurrence of scratches during alkaline water electrolysis is suppressed. The object of another embodiment of this disclosure is to provide an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator.

[0008] This disclosure includes the following embodiments: <1> An alkaline water electrolysis separator comprising a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embeds at least a portion of the support base material, wherein, in the in-plane direction of the alkaline water electrolysis separator, when the linear thermal expansion coefficient in direction t1 where the linear thermal expansion coefficient is maximum is T1, and the linear thermal expansion coefficient in direction t2 where the linear thermal expansion coefficient is minimum is T2, the ratio of T1 to T2 is 1.5 or less. <2> The alkaline water electrolysis separator according to <1>, wherein the ratio of T1 to T2 is 1.3 or less. <3> The alkaline water electrolysis separator according to <1> or <2>, wherein the angle between direction t1 and direction t2 is 40 degrees to 50 degrees. <4> The alkaline water electrolysis separator according to any one of <1> to <3>, wherein the supporting base material is a woven fabric and has fibers that intersect each other and extend in two directions, and the angle between the direction t2 in which the linear thermal expansion coefficient is minimized and one of the two directions in which the fibers extend is 5 degrees or less. <5> The alkaline water electrolysis separator according to <4>, wherein the angle between direction t1 and one of the two directions in which the fibers extend is 40 degrees to 50 degrees. <6> An alkaline water electrolysis separator comprising a woven fabric having fibers extending in two directions that intersect each other, and a porous polymer layer embedding at least a portion of the woven fabric, wherein, in the in-plane direction of the alkaline water electrolysis separator, when the linear thermal expansion coefficient in the direction m2 in which the linear thermal expansion coefficient is relatively small is M2, and the maximum value of the linear thermal expansion coefficient in the direction in which the angle with direction m2 is in the range of 40 to 50 degrees is M1, the maximum ratio of M1 to M2 is 1.5 or less. <7> An alkaline water electrolysis cell comprising the alkaline water electrolysis separator according to any one of <1> to <6>. <8> An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell according to <7>.

[0009] According to one embodiment of the present disclosure, an alkaline water electrolysis separator is provided in which the occurrence of scratches during alkaline water electrolysis is suppressed. According to another embodiment of the present disclosure, an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator are provided.

[0010] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.

[0011] The contents of this disclosure will be described in detail below. The descriptions of constituent elements described below may be based on representative embodiments of this disclosure, but this disclosure is not limited to such embodiments. In this specification, the "~" indicating a numerical range is used to mean that the numbers described before and after it are the lower and upper limits. In numerical ranges described in stages in this disclosure, the upper or lower limit described in one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with the values ​​shown in the examples. Furthermore, the term "process" in this specification is included not only in the case of an independent process, but also in the case of a process that is not clearly distinguishable from other processes, as long as the intended purpose of that process is achieved. Furthermore, in this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.

[0012] [Separator for Alkaline Water Electrolysis] The separator for alkaline water electrolysis of this disclosure (hereinafter also referred to as "separator") is a separator used in alkaline water electrolysis. Alkaline water electrolysis refers to the electrolysis of water using an alkaline aqueous solution as an electrolyte to produce hydrogen and oxygen.

[0013] In the first embodiment of the present disclosure, the separator comprises a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embeds at least a portion of the support base material, wherein, in the in-plane direction of the alkaline water electrolysis separator, when the linear thermal expansion coefficient in direction t1 where the linear thermal expansion coefficient is maximum is defined as T1, and the linear thermal expansion coefficient in direction t2 where the linear thermal expansion coefficient is minimum is defined as T2, the ratio of T1 to T2 is 1.5 or less.

[0014] The statement that a porous polymer layer embeds at least a portion of the supporting substrate means that it is sufficient for at least a portion of the supporting substrate to be embedded in the porous polymer layer.

[0015] In alkaline water electrolysis apparatuses, an alkaline water electrolysis cell in which an electrode and a separator are bonded together may be used. Conventionally, during alkaline water electrolysis, misalignment may occur between the separator and the electrode, or the separator may be deformed, which in some cases causes scratches on the separator. In response to this, the separator of the present disclosure has a ratio of T1 to T2 of 1.5 or less, where T1 is the linear thermal expansion coefficient in the direction t1 in which the linear thermal expansion coefficient is maximum in the in-plane direction of the separator, and T2 is the linear thermal expansion coefficient in the direction t2 in which the linear thermal expansion coefficient is minimum. That is, the separator of the present disclosure has low anisotropy of the linear thermal expansion coefficient in the in-plane direction. Therefore, the occurrence of scratches during alkaline water electrolysis can be suppressed.

[0016] Patent Document 1 has no description focusing on the anisotropy of the linear thermal expansion coefficient in the in-plane direction of the separator.

[0017] (Support Substrate) The support substrate is a woven fabric or a nonwoven fabric. The open area ratio of the support substrate is preferably 30% to 80%, more preferably 40% to 70%. The open area ratio refers to the proportion of the area of voids occupying a unit area when the support substrate is viewed in plan.

[0018] Examples of the polymer constituting the support substrate include polypropylene, polyethylene, polysulfone, polyphenylene sulfide, polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyether ether ketone, sulfonated polyether ether ketone, monochlorotrifluoroethylene, copolymers of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid.

[0019] Above all, the polymer constituting the support substrate preferably contains at least one selected from the group consisting of polypropylene, polyphenylene sulfide, and polyether ether ketone, and more preferably contains at least one selected from the group consisting of polyphenylene sulfide and polyether ether ketone.

[0020] The thickness of the support substrate is preferably 30 μm to 150 μm, more preferably 30 μm to 100 μm, and even more preferably 30 μm to 75 μm.

[0021] The thickness of the support substrate is a value measured by a constant-pressure thickness measuring instrument in accordance with JIS (Japanese Industrial Standards) K6250 (2019). Regarding the thickness of the support substrate in the separator, the support substrate is taken out from the separator using a solvent that dissolves components other than the support substrate constituting the separator, and the measurement is performed on the taken-out support substrate.

[0022] (Porous Polymer Layer) The porous polymer layer has a function of blocking permeation of hydrogen gas and oxygen gas, and allowing hydroxide ions to permeate therethrough.

[0023] The porous polymer layer contains a polymer. As the polymer contained in the porous polymer layer, various polymers applicable to the wet phase separation described later can be adopted.

[0024] Examples of the polymer include fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, polysulfone, polyethersulfone, polyphenylene sulfide, polyphenylsulfone, polyacrylate, polyetherimide, polyimide, polyamideimide, and the like. The fluororesin is preferably at least one selected from the group consisting of polyvinylidene fluoride and polytetrafluoroethylene. The olefin resin is preferably polypropylene. The polyester resin is preferably at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate and polybutylene naphthalate. The aromatic hydrocarbon resin is preferably polystyrene.

[0025] The polymers may be used alone, or two or more types may be used in combination.

[0026] In particular, the polymer preferably contains at least one selected from the group consisting of polyvinylidene fluoride, polysulfone, polyethersulfone, and polyphenylsulfone, and more preferably contains at least one selected from the group consisting of polysulfone, polyethersulfone, and polyphenylsulfone.

[0027] The weight-average molecular weight (Mw) of the polymer is not particularly limited. However, from the viewpoint of the handling properties of the doping solution described later and the mechanical strength of the separator, the weight-average molecular weight (Mw) of the polymer is preferably 10,000 to 500,000, and more preferably 20,000 to 300,000.

[0028] In this disclosure, the weight-average molecular weight is measured under the following conditions. Instrument: HLC-8220GPC (Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARD COLUMN HXL-L 6mm x 40mm (Tosoh Corporation) Sample-side column: The following three columns are directly connected in order (all Tosoh Corporation): ・TSK-GEL GMHXL 7.8mm x 300mm ・TSK-GEL G4000HXL 7.8mm x 300mm ・TSK-GEL G2000HXL 7.8mm x 300mm Reference-side column: TSK-GEL G1000HXL 7.8mm x 300mm Oven temperature: 40℃ Mobile phase: THF (Tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1% by mass Sample injection volume: 100 μL Data acquisition time: 5 to 45 minutes after sample injection Sampling pitch: 300 milliseconds

[0029] The polymer content is preferably 5% to 50% by mass, more preferably 5% to 40% by mass, even more preferably 7% to 30% by mass, and particularly preferably 9% to 25% by mass, relative to the total amount of the porous polymer layer.

[0030] Furthermore, the polymer content is preferably 15% to 65% by volume, more preferably 25% to 60% by volume, even more preferably 35% to 55% by volume, and particularly preferably 35% to 50% by volume, relative to the total volume of the porous polymer layer.

[0031] The porous polymer layer preferably contains at least one inorganic particle in addition to the polymer.

[0032] From the viewpoint of hydrophilicity in alkaline solutions, the inorganic particles are preferably at least one type of particle selected from the group consisting of metal oxides and metal hydroxides.

[0033] Examples of metal oxides include zirconium oxide, titanium oxide, bismuth oxide, cerium oxide, and magnesium oxide.

[0034] Examples of metal hydroxides include zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide, and magnesium hydroxide.

[0035] The inorganic particles may also be barium sulfate particles.

[0036] The median diameter (D50) of the inorganic particles is preferably 0.05 μm to 2.00 μm, more preferably 0.1 μm to 1.50 μm, even more preferably 0.15 μm to 1.00 μm, and particularly preferably 0.20 μm to 1.00 μm. The median diameter (D50) refers to the particle size at which the total volume of the particles is 100% and the cumulative volume is 50%. In this disclosure, the median diameter (D50) is measured using a dynamic image analysis device.

[0037] If the porous polymer layer contains inorganic particles, the inorganic particle content is preferably 50% to 95% by mass, more preferably 60% to 95% by mass, even more preferably 70% to 93% by mass, and particularly preferably 75% to 91% by mass, based on the total amount of the porous polymer layer.

[0038] When the porous polymer layer contains inorganic particles, the inorganic particle content is usually 35% by volume or more, preferably 40% by volume or more, more preferably 45% by volume or more, and even more preferably 50% by volume or more, relative to the total volume of the porous polymer layer. The inorganic particle content is preferably 85% by volume or less, more preferably 75% by volume or less, and even more preferably 65% ​​by volume or less, relative to the total volume of the porous polymer layer. In other words, the inorganic particle content is preferably 35% to 85% by volume, more preferably 40% to 75% by volume, even more preferably 45% to 65% by volume, and particularly preferably 50% to 65% by volume, relative to the total volume of the porous polymer layer.

[0039] The inorganic particle content in the porous polymer layer is measured by the following method: The porous polymer layer is scraped from the separator, and the mass of organic matter and inorganic matter (inorganic particles) is quantified by thermal analysis. The inorganic particle content can be calculated using the densities of organic and inorganic matter described in publicly available data.

[0040] When the porous polymer layer contains inorganic particles, the ratio of inorganic particles to polymer content (inorganic particles / polymer) is preferably 10 / 1 to 1 / 1 by mass, more preferably 9 / 1 to 2 / 1, even more preferably 8 / 1 to 3 / 1, particularly preferably 7 / 1 to 4 / 1, and most preferably 6.5 / 1 to 4 / 1.

[0041] When a separator is manufactured using the doping solution described later, a certain amount of good solvent contained in the doping solution inevitably remains in the porous polymer layer. The total content of good solvent in the porous polymer layer is usually between 0.01% by mass and 5.00% by mass.

[0042] The porous polymer layer in which the support substrate is embedded may be a single layer, or it may be a multilayer structure having a first porous polymer layer disposed on one side of the support substrate and a second porous polymer layer disposed on the other side of the support substrate. The first porous polymer layer and the second porous polymer layer are different layers, and they may be layers with different types or amounts of constituent components.

[0043] (Linear thermal expansion coefficient) In the first embodiment of the present disclosure, the separator has a ratio of T1 to T2 of 1.5 or less, where T1 is the linear thermal expansion coefficient in the direction t1 in which the linear thermal expansion coefficient is maximum, and T2 is the linear thermal expansion coefficient in the direction t2 in which the linear thermal expansion coefficient is minimum.

[0044] The in-plane direction of the separator is the direction perpendicular to the thickness direction of the separator.

[0045] The linear thermal expansion coefficient in the in-plane direction of the separator is measured using a thermomechanical analyzer in the following manner. First, a strip-shaped reference sample with a width of 4 mm and a length of 40 mm is cut from the separator. Using the reference sample as a reference, a sample of the same size as the reference sample is cut in a direction rotated 10 degrees clockwise. Subsequently, samples of the same size as the reference sample are cut in directions rotated 10 degrees clockwise increments. A total of 10 sample pieces are obtained.

[0046] The coefficient of linear thermal expansion will be measured for 10 sample specimens under the following conditions: • Sample width: 4 mm • Chuck distance at 25°C: 15 mm • Heating rate: 3°C / min • Measurement range: 25°C to 150°C • Tension: 50 mN

[0047] The average value of the expansion rate in the range of 50°C to 150°C is obtained from the following formula and adopted as the coefficient of linear expansion: Coefficient of linear expansion = 1 / 15 mm x [(distance between chucks at 150°C - distance between chucks at 50°C) / (150°C - 50°C)] The unit of the coefficient of linear expansion is " / °C".

[0048] Among the 10 measurement samples, the direction in which the maximum value of the linear thermal expansion coefficient was obtained is defined as direction t1. Among the 10 measurement samples, the direction in which the minimum value of the linear thermal expansion coefficient was obtained is defined as direction t2. Furthermore, the linear thermal expansion coefficient in direction t1 is defined as T1, and the linear thermal expansion coefficient in direction t2 is defined as T2. The ratio of T1 to T2 is calculated.

[0049] In the first embodiment of this disclosure, the separator has a ratio of T1 to T2 of 1.5 or less, preferably 1.3 or less, and more preferably 1.1 or less. A ratio of T1 to T2 of 1.0 is most preferable for suppressing the occurrence of scratches during alkaline water electrolysis. Therefore, the ratio of T1 to T2 is preferably 1.0 to 1.5, more preferably 1.0 to 1.3, and even more preferably 1.0 to 1.1.

[0050] Methods for setting the ratio of T1 to T2 to 1.5 or less include, for example, selecting polyetheretherketone as the support substrate, and reducing the tension applied to the support substrate when forming the porous polymer layer using the manufacturing method described later.

[0051] To prevent displacement of electrodes, seals, and separators when the electrolytic cell is in operation, and to prevent leakage of electrolyte and damage to the separator due to displacement, the maximum value of the linear thermal expansion coefficient, T1, is set to 0.01 × 10⁻⁶. -5 ~30 x 10 -5 Preferably, 0.1 × 10 -5 ~10 x 10 -5 It is more preferable that this is the case. From the same viewpoint as above for T1, T2, which is the minimum value of the linear thermal expansion coefficient, is 0.01 × 10 -5 ~30 x 10 -5 Preferably, 0.1 × 10 -5 ~10 x 10 -5 It is preferable that it be so.

[0052] In the first embodiment of this disclosure, the separator is preferably 30 to 60 degrees, and more preferably 40 to 50 degrees, between direction t1 and direction t2. The angle between direction t1 and direction t2 is calculated based on the angle rotated from a reference sample for measurement.

[0053] By satisfying the above range, the anisotropy of the linear thermal expansion coefficient in the in-plane direction of the separator is reduced, and the occurrence of damage to the separator during alkaline water electrolysis can be further suppressed.

[0054] In the first embodiment of this disclosure, the support base material is preferably a woven fabric having fibers extending in two directions that intersect each other, and the angle between the direction t2 in which the linear thermal expansion coefficient is minimized and one of the two directions in which the fibers extend is preferably 5 degrees or less, more preferably 3 degrees or less, and most preferably 0 degrees. Furthermore, the angle between the direction t1 in which the linear thermal expansion coefficient is maximized and one of the two directions in which the fibers extend is preferably 40 degrees to 50 degrees.

[0055] Woven fabrics typically have fibers (warp and weft) that extend in two directions perpendicular to each other.

[0056] Directions t1 and t2 can be determined by the measurement method described above. For example, when calculating the angle between the direction in which the warp threads extend and direction t2, and the angle between the direction in which the weft threads extend and direction t2, it is preferable that one of the angles is 5 degrees or less. That is, it is preferable that the warp threads or weft threads and direction t2 are approximately on the same line.

[0057] Furthermore, if the angle between the direction in which the warp threads extend and direction t2 is 5 degrees or less, it is preferable that the angle between the direction in which the weft threads extend and direction t1 is 40 to 50 degrees. Similarly, if the angle between the direction in which the weft threads extend and direction t2 is 5 degrees or less, it is preferable that the angle between the direction in which the warp threads extend and direction t1 is 40 to 50 degrees.

[0058] By satisfying the above range, the anisotropy of the linear thermal expansion coefficient in the in-plane direction of the separator is reduced, and the occurrence of damage to the separator during alkaline water electrolysis can be further suppressed.

[0059] The angle between direction t2 and the direction in which the fiber extends is measured by the following method.

[0060] To obtain direction t2, the cut-out sample is placed on a light table. The angle between the end face along the longitudinal direction of the sample and the direction in which the fibers extend is measured using a protractor.

[0061] In a second embodiment of the present disclosure, the separator comprises a woven fabric having fibers extending in two directions intersecting each other, and a porous polymer layer embedding at least a portion of the woven fabric, wherein, in the in-plane direction of the separator, when M2 is the coefficient of linear thermal expansion in direction m2, which has a relatively small coefficient of linear thermal expansion among the two directions in which the fibers extend, and M1 is the maximum value of the coefficient of linear thermal expansion in the direction whose angle with direction m2 is in the range of 40 to 50 degrees, the ratio of M1 to M2 is 1.5 or less.

[0062] Preferred embodiments of the woven fabric and porous polymer layer are the same as in the first embodiment.

[0063] The method for measuring the linear thermal expansion coefficient is as described above. In a woven fabric, for example, measurement samples are prepared in the direction in which the warp threads extend and in the direction in which the weft threads extend, and the linear thermal expansion coefficient is measured under the same conditions as described above. The direction in which the linear thermal expansion coefficient is relatively small is defined as direction m2. The linear thermal expansion coefficient in direction m2 is defined as M2.

[0064] The direction whose angle with direction m2 is in the range of 40 to 50 degrees is the region that includes the direction rotated 40 to 50 degrees clockwise from direction m2 and the direction rotated 40 to 50 degrees counterclockwise from direction m2. Let M1 be the maximum value of the linear thermal expansion coefficient in this region.

[0065] Specifically, cut out a sample of the same size as the reference sample in a direction rotated 40 degrees clockwise with respect to direction m2. Then, cut out another sample of the same size as the reference sample in a direction rotated 10 degrees clockwise in increments. Next, cut out another sample of the same size as the reference sample in a direction rotated 40 degrees counterclockwise with respect to direction m2. Then, cut out another sample of the same size as the reference sample in a direction rotated 10 degrees counterclockwise in increments. A total of 10 samples are obtained. Measure the coefficient of thermal expansion of each of the 10 samples under the same conditions as described above.

[0066] Among the 10 measurement samples, the direction in which the maximum value of the linear thermal expansion coefficient was obtained is defined as direction m1. The linear thermal expansion coefficient in direction m1 is defined as M1.

[0067] To prevent displacement of electrodes, seals, and separators when the electrolytic cell is in operation, and to prevent leakage of electrolyte and damage to the separator due to displacement, the linear thermal expansion coefficient M1 in direction m1 is 0.01 × 10⁻⁶. -5 ~30 x 10 -5 Preferably, 0.1 × 10 -5 ~10 x 10 -5 It is more preferable that the linear thermal expansion coefficient M2 in direction m2 is 0.01 × 10⁻¹⁰. This is from the viewpoint of preventing displacement of electrodes, seals, and separators when the electrolytic cell is in operation, and preventing damage to the separator due to electrolyte leakage or displacement. -5 ~30 x 10 -5 Preferably, 0.1 × 10 -5 ~10 x 10 -5 It is preferable that it be so.

[0068] In the second embodiment of this disclosure, the separator has a ratio of M1 to M2 of 1.5 or less, preferably 1.3 or less, and more preferably 1.1 or less. Since it is optimal for there to be no anisotropy in the coefficient of linear thermal expansion to suppress the occurrence of scratches during alkaline water electrolysis, the ratio of M1 to M2 is most preferably 1.0. Therefore, the ratio of M1 to M2 is preferably 1.0 to 1.5, more preferably 1.0 to 1.3, and even more preferably 1.0 to 1.1.

[0069] Methods for setting the ratio of M1 to M2 to 1.5 or less include, for example, selecting polyetheretherketone as the woven fabric, and reducing the tension applied to the woven fabric when forming the porous polymer layer using the manufacturing method described later.

[0070] By satisfying the above range, the anisotropy of the linear thermal expansion coefficient in the in-plane direction of the separator is small, and the occurrence of damage to the separator during alkaline water electrolysis can be suppressed.

[0071] The following describes matters common to the first and second embodiments of this disclosure.

[0072] The separator of this disclosure preferably has a thickness of 600 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less. The thickness can usually be 30 μm or more, preferably 50 μm or more, and more preferably 100 μm or more. That is, the thickness is preferably 30 μm to 600 μm, more preferably 50 μm to 300 μm, and even more preferably 100 μm to 250 μm.

[0073] The thickness of the separator is measured by the following method.

[0074] Samples are taken at five arbitrary points, and cross-sections are cut out with a razor. A cross-sectional SEM (scanning electron microscope) image is acquired at a magnification (e.g., 400x) that allows the separator cross-section to fit in a single field of view. In the obtained cross-sectional SEM image, assuming that no pores exist (for example, assuming that the pores are filled with polymer), the thickness is measured at 20 equally spaced points at each sampling point, and the arithmetic mean of the total of 100 measurements is adopted.

[0075] From the viewpoint of gas barrier properties required for porous separators for alkaline water electrolysis, the separator of this disclosure preferably has a bubble point greater than 1 bar, and more preferably greater than 2 bar. The pore diameter and porosity of the pores in the separator of this disclosure should be adjusted to a range that satisfies the above-mentioned bubble point. The bubble point is determined by measuring using a palm porometer based on the bubble point test method described in ASTM (American Society for Testing and Materials) F316-86, and the pressure at which the first bubble is generated in the resulting wet curve is defined as the bubble point.

[0076] The pore diameter of the separator in this disclosure is preferably 10 nm to 1000 nm, more preferably 20 nm to 700 nm, and even more preferably 30 nm to 500 nm, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The pore diameter is determined by obtaining the pore diameter distribution from the insertion curve by the mercury intrusion method and taking the average value thereof.

[0077] The separator of this disclosure preferably has pores on one surface and on the other surface, and the average pore diameter of the pores on one surface is different from that of the pores on the other surface.

[0078] The porosity of the separator in this disclosure is preferably 30% to 70%, more preferably 40% to 60%, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The porosity is a value calculated from the insertion curve by the mercury intrusion method.

[0079] The separator of this disclosure has an ionic resistance of 0.01 Ω·cm from the viewpoint of hydroxyl ion permeability. 2 ~0.30 Ω·cm 2 Preferably, 0.01 Ω·cm 2 ~0.15Ω·cm 2 This is more preferable. Ion resistance is a value measured by AC impedance method at 90°C with a circularly punched separator set in a cell.

[0080] The separator of this disclosure has a water permeability of 100 mL / (h·m) from the viewpoint of mass balance between the cathode and anode sides of the electrolyte. 2 ・bar)~2000mL / (h・m 2 A water permeability of 100 mL / (h·m) is preferred. Furthermore, from the viewpoint of not requiring operational modifications to the alkaline water electrolysis cell, such as changing the permeability of the electrolyte on the anode and cathode sides, a water permeability of 100 mL / (h·m) is preferred. 2 ・bar)~1000mL / (h・m 2 A pressure of 1 bar is more preferable. The permeability is calculated by setting a circularly punched separator in a filter holder and measuring the volume of liquid (mL) when a 30% potassium hydroxide aqueous solution is passed through the circular separator for 30 seconds under conditions of 90°C and a gauge pressure of 1 bar.

[0081] The separator of this disclosure can be preferably used as a separator in a pressurized alkaline water electrolysis system (separator for pressurized alkaline water electrolysis). The separator of this disclosure can also be used as a separator in an alkaline water electrolysis system used under normal pressure (separator for alkaline water electrolysis). The separator of this disclosure may be in the form of a long sheet wound into a roll, or it may be pre-cut into a predetermined shape according to the intended use, equipment, etc. Furthermore, the separator of this disclosure may be stored immersed in a preservation solution such as pure water. Alternatively, the separator of this disclosure may be stored as a dry film without being immersed in a preservation solution.

[0082] The method for manufacturing the separator of this disclosure is not particularly limited. The separator of this disclosure can be manufactured, for example, by forming a porous polymer layer by wet phase separation. For example, one method (hereinafter referred to as "manufacturing method I") includes forming the porous polymer layer by wet phase separation while the support substrate is placed in a coating film formed with a dope solution obtained by dissolving the polymer. This step yields a separator comprising a support substrate and a porous polymer layer that embeds at least a portion of the support substrate.

[0083] (Doping solution) The doping solution may contain, for example, the polymer contained in the porous polymer layer and a solvent, and may also contain inorganic particles. Details of the polymer contained in the porous polymer layer are as described above. Details of the inorganic particles that may be contained in the doping solution are as described above.

[0084] The solvent contained in the doping solution in the wet phase separation can be any solvent that can dissolve the above polymer (a good solvent), and is preferably miscible with water. The solvent is preferably selected from N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N-butylpyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, and mixtures thereof, with at least one of NMP and NBP being more preferred.

[0085] If the doped solution contains inorganic particles, the solvent content in the doped solution is preferably 20% to 95% by mass, more preferably 25% to 90% by mass, even more preferably 30% to 80% by mass, even more preferably 30% to 70% by mass, even more preferably 32% to 60% by mass, and even more preferably 35% to 50% by mass. If the doped solution does not contain inorganic particles, the solvent content in the doped solution is preferably 20% to 95% by mass, more preferably 25% to 90% by mass, even more preferably 30% to 80% by mass, even more preferably 40% to 80% by mass, even more preferably 45% to 75% by mass, and even more preferably 50% to 75% by mass.

[0086] If the doping solution contains inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 20% by mass, even more preferably 5% to 15% by mass, and still more preferably 6% to 15% by mass. If the doping solution does not contain inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 30% by mass, even more preferably 6% to 25% by mass, and still more preferably 8% to 20% by mass.

[0087] In this disclosure, inorganic particles are particles that exist dispersed in the dope solution without dissolving, and this dispersion state is also referred to as the dope solution. That is, the "solution" in dope solution refers to the state in which the polymer is dissolved in the solvent. When the dope solution contains inorganic particles, the content of inorganic particles in the dope solution is preferably 20% to 95% by mass, more preferably 25% to 92% by mass, even more preferably 30% to 90% by mass, and particularly preferably 35% to 88% by mass.

[0088] The doping solution may contain components other than the solvent, polymer, and inorganic particles. For example, in wet phase separation, to control the formation of pores in the porous polymer layer, the doping solution may contain polyhydric alcohols such as polyethylene glycol, polypropylene glycol, ethylene glycol, tripropylene glycol, and glycerol; dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid or neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, lithium chloride, etc.

[0089] If the doping solution contains other components and inorganic particles, the total content of the other components in the doping solution is preferably 0.1% to 15% by mass, more preferably 0.2% to 10% by mass, and even more preferably 0.5% to 5% by mass. If the doping solution contains other components but does not contain inorganic particles, the total content of the other components in the doping solution is preferably 1% to 25% by mass, more preferably 5% to 25% by mass, and even more preferably 7% to 20% by mass.

[0090] -Manufacturing Method I- In Manufacturing Method I, a separator can be manufactured that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate by wet phase separation while a support substrate is placed in a coating film formed with a doped solution obtained by dissolving a polymer. In wet phase separation, the support substrate is placed on a coating film formed by casting the doped solution onto a substrate, and the support substrate is immersed in the coating film to impregnate the support substrate with the doped solution. Next, the support substrate, which has been impregnated with the doped solution, is immersed in a solvent (poor solvent, coagulation bath) that does not dissolve the polymer and is miscible with the good solvent. When the proportion of the good solvent in the coating film of the doped solution decreases due to this immersion, the polymer and the solvent undergo phase separation (liquid-induced phase separation), the polymer gels (coagulates), and a porous polymer layer is formed. A separator is then obtained that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate.

[0091] As a poor solvent, for example, water, or a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water) or a water-soluble polymer can be used. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAC), and alcohols such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among these, water is preferred as the poor solvent.

[0092] The temperature of the coagulation bath is preferably 20°C to 90°C, more preferably 40°C to 70°C.

[0093] It is also preferable to expose the coating film to the vapor of the poor solvent before immersing it in the poor solvent to induce vapor-induced phase separation (vapor-induced phase separation). By performing vapor-induced phase separation, it is possible to suppress the formation of a dense skin layer on the surface. Therefore, in the above wet phase separation, vapor-induced phase separation and liquid-induced phase separation can also be performed in combination. Furthermore, it is preferable to perform a washing step with pure water or the like after wet phase separation, preferably after liquid-induced phase separation.

[0094] In vapor induction phase separation, the support substrate coated with the dope solution is exposed to a non-solvent vapor, preferably humid air. As a method for performing vapor induction phase separation, for example, the description of Figure 2 and its explanation in Japanese Patent Publication No. 2023-531792 can be appropriately referred to and applied in accordance with this disclosure. The poor solvent vapor used in vapor induction phase separation is preferably humid air. The space for performing vapor induction phase separation can be, for example, provided between the step of coating the support substrate with the dope solution and the step of performing liquid induction phase separation, continuous with the apparatus for each step, and further shielded from the external environment using insulating metal plates. The degree and speed of water movement in the vapor induction phase separation step can be adjusted by adjusting the air velocity, relative humidity and temperature of the air, and exposure time. The relative humidity within the vapor induction phase separation region can be adjusted by the temperature of the solidification bath and shielding the vapor induction phase separation region from the environment. Vapor-induced phase separation performed on a support substrate coated with a doping solution may be carried out under the same conditions on both sides or under different conditions. The relative humidity and temperature in the region where vapor-induced phase separation is performed can be adjusted using an insulating metal plate, for example, when using the apparatus described in Figure 2 of Japanese Patent Publication No. 2023-531792. If the metal plate completely shields the region from the external environment, the relative humidity and temperature are determined by the temperature of the solidification bath used in the subsequent liquid-induced phase separation. The higher the relative humidity in the region where vapor-induced phase separation is performed, and the higher the air velocity, the larger the maximum pores in the resulting porous material. The relative humidity in the region where vapor-induced phase separation is performed can be, for example, in the range of 50% to 99%, preferably 60% to 98%, and more preferably 70% to 98%.

[0095] In the separator obtained by the above manufacturing method, a certain amount of good solvent from the doping solution used in the manufacturing inevitably remains. The amount of residual solvent can be determined by gas chromatography or by pre-drying the separator at 40°C for 12 hours. 1 The amount can be quantified using H-NMR as a mass percentage in 100% by mass of the above-mentioned dried porous separator for alkaline water electrolysis.

[0096] The separator of this disclosure can be used as a separator in a method for producing hydrogen by electrolyzing an alkaline aqueous solution using an electrolytic cell. In particular, it can be suitably used as an alkaline water electrolysis separator in the alkaline water electrolysis system described below.

[0097] Furthermore, the separator of this disclosure may be provided with a catalyst layer on at least one surface to serve as an alkaline water electrolysis member. Since the separator of this disclosure has excellent discriminability on both sides, the catalyst layer can be appropriately provided.

[0098] [Alkaline Water Electrolysis Cell] The alkaline water electrolysis cell of the present disclosure includes the separator of the present disclosure. Specifically, the alkaline water electrolysis cell of the present disclosure preferably includes the separator of the present disclosure and at least one of an anode electrode and a cathode electrode, and more preferably includes the separator of the present disclosure and an anode electrode and a cathode electrode.

[0099] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.

[0100] In the alkaline water electrolysis system 20 shown in Figure 1, the alkaline water electrolysis cell 10 includes a separator 11, a cathode electrode 12 positioned on one surface of the separator 11, and an anode electrode 13 positioned on the other surface of the separator 11. The alkaline water electrolysis cell 10 is immersed in a high-concentration alkaline aqueous solution 14.

[0101] The alkaline aqueous solution 14 is, for example, an aqueous solution of potassium hydroxide or an aqueous solution of sodium hydroxide.

[0102] When an electric current flows between the electrodes, electrons are supplied to the cathode side, causing water to produce bubble-like hydrogen (H₂). 2 ) occurs (2H 2 O + 2e - →H 2 +2OH - ). Hydroxyl ions (OH) generated along with the generation of hydrogen. - ) moves to the anode side after passing through the separator 11, and electrons are removed at the anode to form bubble-shaped oxygen (O 2 ) occurs (4OH- →O 2 +2H 2 O+4e - ).

[0103] Since the separator 11 is in contact with the cathode electrode 12 and the anode electrode 13, the distance traveled by the hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency.

[0104] In the above-described alkaline water electrolysis system, the components other than the separator, such as the cathode electrode and anode electrode, are not particularly limited, and ordinary components used in alkaline water electrolysis systems can be applied as appropriate.

[0105] [Alkaline Water Electrolysis Apparatus] The alkaline water electrolysis apparatus of this disclosure includes the alkaline water electrolysis cell of this disclosure. The alkaline water electrolysis apparatus of this disclosure can produce hydrogen by supplementing the necessary components, components, etc., depending on the configuration of the alkaline water electrolysis cell of this disclosure.

[0106] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples unless it exceeds the spirit of the disclosure.

[0107] <Example 1> 8.5 g of polysulfone (product name "Udel P-3500 LCD MB7", manufactured by Solvay) was added to 41.3 g of dimethylformamide (manufactured by Wako), and stirred at 60°C for 5 hours to completely dissolve it. Next, 2.4 g of polyvinylpyrrolidone (product name "PVP K90", manufactured by Merck) was added, and stirred at 60°C for 1 hour, after which ZrO 2 47.9 g of particles (product name "E101", manufactured by Luxfer) were added and stirred for a further 3 hours to obtain a coating solution. The obtained coating solution was cast onto a PET (polyethylene terephthalate) film with an applicator clearance of 200 μm. A woven fabric (PEEKTEX; Sefar), which serves as a support substrate, was then placed on top and impregnated with the coating solution. Subsequently, it was gently immersed in a solidification bath (pure water) cooled to 10°C to form a porous structure. Further washing at 50°C for 10 minutes removed the separator from the PET film. Subsequently, washing at 90°C for 1 hour obtained the separator.

[0108] <Example 2> A separator was obtained in the same manner as in Example 1, except that the applicator clearance was changed to 300 μm and the woven fabric was immersed in a coagulation bath while a tension of 49 N per meter was applied to it.

[0109] <Comparative Example 1> A separator was obtained in the same manner as in Example 2, except that the woven fabric was immersed in a coagulation bath while a tension of 98 N per meter was applied to it.

[0110] (Linear Thermal Expansion Coefficient) First, the method for calculating the linear thermal expansion coefficients T1 and T2 will be explained. The linear thermal expansion coefficient in the in-plane direction of the separator was measured using a thermomechanical analyzer. First, a strip-shaped reference sample with a width of 4 mm and a length of 40 mm was cut from the separator. Using the reference sample as a reference, a sample of the same size as the reference sample was cut in a direction rotated 10 degrees clockwise. Subsequently, samples of the same size as the reference sample were cut in directions rotated in 10-degree increments. A total of 10 sample pieces were obtained.

[0111] The coefficient of linear thermal expansion was measured for 10 sample specimens under the following conditions: • Sample width: 4 mm • Chuck distance: 15 mm • Heating rate: 3°C / min • Measurement range: 25°C to 150°C • Tension: 50 mN

[0112] The average value of the expansion rate in the range of 50°C to 150°C was adopted as the coefficient of linear expansion.

[0113] Among the 10 measurement samples, the direction in which the maximum value of the linear thermal expansion coefficient was obtained was defined as direction t1. Among the 10 measurement samples, the direction in which the minimum value of the linear thermal expansion coefficient was obtained was defined as direction t2. Furthermore, the linear thermal expansion coefficient in direction t1 was defined as T1, and the linear thermal expansion coefficient in direction t2 was defined as T2. The ratio of T1 to T2 was calculated. The angle between direction t1 and direction t2 was calculated based on the angle rotated from the reference sample used for measurement.

[0114] Next, we will explain the method for calculating the angle between the direction in which the fibers extend and direction t2. A measurement sample corresponding to direction t2 was placed on a light table, and the light intensity was adjusted so that the fibers of the woven fabric could be seen. Using a protractor, the angle between the direction in which the fibers of the woven fabric extend (the direction in which the warp threads extend and the direction in which the weft threads extend) and the end face along the longitudinal direction of the measurement sample corresponding to direction t2 was measured.

[0115] Next, the method for calculating the linear thermal expansion coefficients M1 and M2 will be explained. A separator was placed on a light table, and the light intensity was adjusted so that the fibers of the woven fabric could be seen. Measurement samples were cut out along the direction in which the fibers of the woven fabric extend (the direction in which the warp threads extend, and the direction in which the weft threads extend). Here, a measurement sample along the direction in which the threads extend refers to a sample in which the angle between the thread and the end face of the measurement sample is between 0 and 5 degrees. The linear thermal expansion coefficient was measured under the same conditions as above. Of the directions in which the warp threads extend and the weft threads extend, the direction in which the linear thermal expansion coefficient was relatively small was defined as direction m2. The linear thermal expansion coefficient in direction m2 was defined as M2.

[0116] A sample of the same size as the reference sample was cut out in a direction rotated 40 degrees clockwise with respect to direction m2. Subsequently, samples of the same size as the reference sample were cut out in directions rotated 10 degrees clockwise in increments. Furthermore, a sample of the same size as the reference sample was cut out in a direction rotated 40 degrees counterclockwise with respect to direction m2. Subsequently, samples of the same size as the reference sample were cut out in directions rotated 10 degrees counterclockwise in increments. A total of 10 samples were obtained. The coefficient of thermal expansion was measured for each of the 10 samples under the same conditions as described above.

[0117] Among the 10 measurement samples, the direction in which the maximum value of the linear thermal expansion coefficient was obtained was defined as direction m1. The linear thermal expansion coefficient in direction m1 was defined as M1. The ratio of M1 to M2 was calculated.

[0118] The following evaluation of damage after alkaline water electrolysis was performed using a separator.

[0119] A separator was sandwiched between two porous electrodes and set in an electrolytic cell. 30% potassium hydroxide was used as the electrolyte at 85°C and 1 A / cm². 2 The system was operated for three consecutive weeks under the specified conditions. After the operation ended, the separator was removed. The surface of the separator was visually inspected on a light table, and the number of scratches was calculated. Scratches are visible as bright spots on the light table. -Evaluation Criteria- A: There are 5 or fewer scratches in a 50cm square area. B: There are 6 to 20 scratches in a 50cm square area. C: There are 21 or more scratches in a 50cm square area.

[0120]

[0121] As shown in Table 1, in Examples 1 and 2, the separator included a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embedded at least a portion of the support base material. In the in-plane direction of the separator, when the linear thermal expansion coefficient in direction t1 where the linear thermal expansion coefficient is maximum is defined as T1, and the linear thermal expansion coefficient in direction t2 where the linear thermal expansion coefficient is minimum is defined as T2, the ratio of T1 to T2 is 1.5 or less, so that the occurrence of damage to the separator during alkaline water electrolysis could be suppressed. On the other hand, in Comparative Example 1, the ratio of T1 to T2 was greater than 1.5, and many scratches occurred on the separator during alkaline water electrolysis.

[0122] Furthermore, in Examples 1 and 2, the separator included a woven fabric having fibers extending in two directions that intersect each other, and a porous polymer layer embedding at least a portion of the woven fabric. In the in-plane direction of the separator, when the linear thermal expansion coefficient in direction m2, where the linear thermal expansion coefficient is relatively small among the two directions in which the fibers extend, is defined as M2, and the maximum value of the linear thermal expansion coefficient in the direction where the angle with direction m2 is in the range of 40 to 50 degrees is defined as M1, the maximum ratio of M1 to M2 is 1.5 or less, thus suppressing the occurrence of damage to the separator during alkaline water electrolysis. In Comparative Example 1, the ratio of M1 to M2 was greater than 1.5, and many scratches occurred on the separator during alkaline water electrolysis.

[0123] Furthermore, the disclosure of Japanese Patent Application No. 2025-078884, filed on 9 May 2025, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.

[0124] 10 Alkaline water electrolysis cell 11 Separator 12 Cathode electrode 13 Anode electrode 14 Alkaline aqueous solution 20 Alkaline water electrolysis system O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH - Hydroxy ion e - electronic

Claims

1. An alkaline water electrolysis separator comprising a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embeds at least a portion of the support base material, wherein, in the in-plane direction of the alkaline water electrolysis separator, when the linear thermal expansion coefficient in the direction t1 where the linear thermal expansion coefficient is maximum is defined as T1, and the linear thermal expansion coefficient in the direction t2 where the linear thermal expansion coefficient is minimum is defined as T2, the ratio of T1 to T2 is 1.5 or less.

2. The alkaline water electrolysis separator according to claim 1, wherein the ratio of T1 to T2 is 1.3 or less.

3. The alkaline water electrolysis separator according to claim 1 or claim 2, wherein the angle between the direction t1 and the direction t2 is 40 degrees to 50 degrees.

4. The alkaline water electrolysis separator according to claim 1 or claim 2, wherein the supporting substrate is a woven fabric and has fibers extending in two directions that intersect each other, and the angle between the direction t2 in which the linear thermal expansion coefficient is minimized and one of the two directions in which the fibers extend is 5 degrees or less.

5. The alkaline water electrolysis separator according to claim 4, wherein the angle between the direction t1 and one of the two directions in which the fibers extend is 40 to 50 degrees.

6. An alkaline water electrolysis separator comprising a woven fabric having fibers extending in two directions that intersect each other, and a porous polymer layer embedding at least a portion of the woven fabric, wherein, in the in-plane direction of the alkaline water electrolysis separator, when the linear thermal expansion coefficient in the direction m2 in which the linear thermal expansion coefficient is relatively small is M2, and the maximum value of the linear thermal expansion coefficient in the direction in which the angle with direction m2 is in the range of 40 to 50 degrees is M1, the ratio of M1 to M2 is 1.5 or less.

7. An alkaline water electrolysis cell comprising the alkaline water electrolysis separator described in claim 1 or claim 6.

8. An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell described in claim 7.