Separator roll for alkaline water electrolysis, alkaline water electrolysis cell, and alkaline water electrolysis device
The alkaline water electrolysis separator roll with a core and porous polymer layer addresses the issue of separator adhesion and deformation, maintaining cell stability by loose winding and core support.
Patent Information
- Application Number
- PCT/JP2026/015635
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-17
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional alkaline water electrolysis separators tend to stick together or deform when stored for a period of time, leading to malfunctions in alkaline water electrolysis cells.
The development of an alkaline water electrolysis separator roll with a core diameter of 7.5 cm to 30.0 cm, incorporating a woven or nonwoven fabric support base material and a porous polymer layer, which suppresses adhesion and deformation by allowing loose winding.
The separator roll effectively prevents adhesion and deformation of separators, ensuring stable operation of alkaline water electrolysis cells and apparatuses.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure 00000032_0000
Abstract
Description
Separator rolls for alkaline water electrolysis, alkaline water electrolysis cells, and alkaline water electrolysis apparatus
[0001] This disclosure relates to a separator roll for alkaline water electrolysis, an alkaline water electrolysis cell, and an alkaline water electrolysis apparatus.
[0002] Hydrogen is a clean energy source that does not emit carbon dioxide and is used, for example, as fuel for fuel cell vehicles and household fuel cells. Alkaline water electrolysis, which uses a highly concentrated alkaline aqueous solution as an electrolyte, is a known method for producing hydrogen. By using a renewable energy power generation system as the power source for alkaline water electrolysis, hydrogen can be produced without emitting carbon dioxide, and therefore hydrogen is attracting increasing attention as a fundamental energy source for a sustainable society.
[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H) generated at the cathode is produced. 2 O + 2e - →H 2 +2OH - This prevents the oxygen (4OH) from moving to the anode, and also prevents the bubble-like oxygen (4OH) generated at the anode from moving to the anode. - →O 2 +2H 2 O+4e - To prevent the gas from moving towards the cathode, a gas barrier separator is placed between the cathode and the anode.
[0004] Patent Document 1 describes an alkali hydrolysis-resistant separator comprising a porous support, a first porous polymer layer adjacent to one side of the support, and a second porous polymer layer adjacent to the opposite side of the support, characterized in that the maximum pore diameter of the outer surface of the first porous polymer layer (PDmax(1)) and the maximum pore diameter of the outer surface of the second porous polymer layer (PDmax(2)) are different from each other, and the ratio of PDmax(2) / PDmax(1) is 1.25 to 10.
[0005] Patent Document 1: Japanese Patent Publication No. 2020-527193
[0006] Conventionally, when long alkaline water electrolysis separators were wound up and stored for a certain period of time, the separators would sometimes stick together or deform, such as being crushed.
[0007] The object of one embodiment of this disclosure is to provide an alkaline water electrolysis separator roll that can suppress adhesion between alkaline water electrolysis separators or deformation of alkaline water electrolysis separators. The object of another embodiment of this disclosure is to provide an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator roll.
[0008] This disclosure includes the following embodiments: <1> An alkaline water electrolysis separator roll comprising a winding core and a roll-shaped alkaline water electrolysis separator wound around the winding core, wherein the diameter of the winding core is 7.5 cm to 30.0 cm, and the alkaline water electrolysis separator includes a support base material which is a woven or nonwoven fabric and a porous polymer layer which embeds at least a portion of the support base material. <2> The alkaline water electrolysis separator roll according to <1>, wherein the outer diameter is 7.6 cm to 100.0 cm. <3> The alkaline water electrolysis separator roll according to <1> or <2>, wherein the roll-shaped alkaline water electrolysis separator has a Shore A hardness of 30 to 70 at the outermost surface of the roll. <4> The alkaline water electrolysis separator roll according to any one of <1> to <3>, wherein the roll-shaped alkaline water electrolysis separator has an uneven shape on the end face of the roll, and the width between the concave end and the convex end in a direction perpendicular to the longitudinal direction is in the range of 1 mm to 30 mm. <5> The alkaline water electrolysis separator roll according to any one of <1> to <4>, wherein a through hole with a hole diameter of 0.3 mm to 3 mm is formed at a position 1 mm to 30 mm from at least one end in the width direction toward the center. <6> The alkaline water electrolysis separator roll according to any one of <1> to <5>, wherein the support substrate is exposed at the end in the width direction. <7> An alkaline water electrolysis separator roll according to any one of <1> to <6>, wherein the roll-shaped alkaline water electrolysis separator has pores on one surface and on the other surface, and the average pore diameter of the pores on one surface is different from that of the other surface. <8> An alkaline water electrolysis separator roll according to any one of <1> to <7>, wherein the porous polymer layer contains hydrophilic inorganic particles. <9> An alkaline water electrolysis cell comprising the alkaline water electrolysis separator in the alkaline water electrolysis separator roll according to any one of <1> to <8>. <10> An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell according to <9>.
[0009] According to one embodiment of the present disclosure, an alkaline water electrolysis separator roll is provided that can suppress adhesion between alkaline water electrolysis separators or deformation of alkaline water electrolysis separators. According to another embodiment of the present disclosure, an alkaline water electrolysis cell and an alkaline water electrolysis apparatus using the above-mentioned alkaline water electrolysis separator roll are provided.
[0010] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.
[0011] The contents of this disclosure will be described in detail below. The descriptions of constituent elements described below may be based on representative embodiments of this disclosure, but this disclosure is not limited to such embodiments. In this specification, the "~" indicating a numerical range is used to mean that the numbers described before and after it are the lower and upper limits. In numerical ranges described in stages in this disclosure, the upper or lower limit described in one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with the values shown in the examples. Furthermore, the term "process" in this specification is included not only in the case of an independent process, but also in the case of a process that is not clearly distinguishable from other processes, as long as the intended purpose of that process is achieved. Furthermore, in this disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.
[0012] In this disclosure, “longitudinal direction” means the longitudinal direction of a separator roll manufactured in an elongated shape. “Width direction” means the direction perpendicular to the longitudinal direction of the separator roll. In this disclosure, “width” of the separator roll means the length of the separator roll in the width direction.
[0013] [Alkaline Water Electrolysis Separator Roll] The alkaline water electrolysis separator roll of this disclosure is a separator roll used for alkaline water electrolysis. Specifically, the alkaline water electrolysis separator is unwound from the alkaline water electrolysis separator roll and cut to the desired size for use. Alkaline water electrolysis refers to the electrolysis of water using an alkaline aqueous solution as an electrolyte to produce hydrogen and oxygen.
[0014] The separator roll of this disclosure (hereinafter also referred to as "separator roll") comprises a winding core and a roll-shaped alkaline water electrolysis separator (hereinafter also referred to as "separator") wound around the winding core, wherein the winding core has a diameter of 7.5 cm to 30.0 cm, and the separator includes a support base material which is a woven or nonwoven fabric and a porous polymer layer which embeds at least a portion of the support base material.
[0015] The statement that a porous polymer layer embeds at least a portion of the supporting substrate means that it is sufficient for at least a portion of the supporting substrate to be embedded in the porous polymer layer.
[0016] In alkaline water electrolysis devices, alkaline water electrolysis cells are sometimes used in which electrodes and separators are bonded together. Conventionally, sheet-shaped separators have been used. In order to manufacture alkaline water electrolysis cells at a lower cost, it is necessary to use long-length separators. However, when long-length separators are wound and stored for a certain period of time, this can lead to malfunctions or deformation where the separators adhere to each other. In contrast, in the separator roll of this disclosure, the separator is wound around a core, and because the diameter of the core is relatively large, ranging from 7.5 cm to 30.0 cm, it is possible to wind the separator loosely, which suppresses adhesion between separators and also suppresses deformation of the separators.
[0017] Patent Document 1 does not contain any description focusing on the adhesion of separators to each other or the deformation of separators, nor does it describe any specific means for doing so.
[0018] <Core> The separator roll of this disclosure includes a core. The core is used to wind the separator and typically has a circular cross-section.
[0019] The shape of the core can be cylindrical or columnar, and may be cylindrical or cylindrical.
[0020] The material of the core is not particularly limited and can include, for example, paper, rubber, plastic, metals such as aluminum, or composite materials thereof.
[0021] The diameter of the core is 7.5 cm to 30.0 cm, preferably 10.0 cm to 25.0 cm, and more preferably 10.0 cm to 20.0 cm.
[0022] By having a core diameter of 7.5 cm to 30.0 cm, the separators can be wound loosely, which suppresses adhesion between separators and also suppresses deformation of the separators. The core diameter is measured using a measuring tape or similar tool.
[0023] <Separator> The separator includes a support base material which is a woven or nonwoven fabric, and a porous polymer layer which embeds at least a portion of the support base material.
[0024] Since the support substrate has voids, the porous polymer layer may be formed inside the support substrate. Alternatively, the porous polymer layer may cover at least a portion of the outer surface of the support substrate. In the separator, at least a portion of the support substrate may be exposed on the surface. Alternatively, the support substrate may be embedded in the separator without being exposed.
[0025] From the viewpoint of improving the shape of the separator roll, it is preferable that the support substrate is exposed at the ends in the width direction of the separator. That is, it is preferable that the width of the support substrate is wider than the width of the porous polymer layer. From the viewpoint of gas barrier properties, it is preferable that the ratio of the ends where the support substrate is exposed is 0.1% to 5% of the width of the support substrate.
[0026] (Supporting material) The supporting material is a woven or nonwoven fabric. The opening ratio of the supporting material is preferably 30% to 80%, more preferably 40% to 70%. The opening ratio is the ratio of the area of voids to the area of a unit area when the supporting material is viewed from above.
[0027] Examples of the polymer constituting the support substrate include polypropylene, polyethylene, polysulfone, polyphenylene sulfide, polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyether ether ketone, sulfonated polyether ether ketone, monochlorotrifluoroethylene, copolymers of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid.
[0028] Among these, the polymer constituting the support substrate preferably comprises at least one selected from the group consisting of polypropylene, polyphenylene sulfide, and polyether ether ketone, and more preferably comprises at least one selected from the group consisting of polyphenylene sulfide and polyether ether ketone.
[0029] The thickness of the support substrate is preferably 30 μm to 150 μm, more preferably 30 μm to 100 μm, and even more preferably 30 μm to 75 μm.
[0030] The thickness of the support substrate is a value measured by a constant-pressure thickness measuring instrument in accordance with JIS (Japanese Industrial Standards) K6250 (2019). Regarding the thickness of the support substrate in the separator, the support substrate is taken out from the separator using a solvent that dissolves components other than the support substrate constituting the separator, and the measurement is performed on the taken-out support substrate.
[0031] (Porous Polymer Layer) The porous polymer layer has a function of blocking permeation of hydrogen gas and oxygen gas and allowing permeation of hydroxide ions.
[0032] The porous polymer layer contains a polymer. As the polymer contained in the porous polymer layer, various polymers applicable to the wet phase separation described later can be adopted.
[0033] Examples of polymers include fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, polysulfones, polyethersulfones, polyphenylene sulfide, polyphenylsulfone, polyacrylates, polyetherimides, polyimides, and polyamideimides. The fluororesin is preferably at least one selected from the group consisting of polyvinylidene fluoride and polytetrafluoroethylene. The olefin resin is preferably polypropylene. The polyester resin is preferably at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, and polybutylene naphthalate. The aromatic hydrocarbon resin is preferably polystyrene.
[0034] The polymer may be used individually or in combination of two or more types.
[0035] In particular, the polymer preferably contains at least one selected from the group consisting of polyvinylidene fluoride, polysulfone, polyethersulfone, and polyphenylsulfone, and more preferably contains at least one selected from the group consisting of polysulfone, polyethersulfone, and polyphenylsulfone.
[0036] The weight-average molecular weight (Mw) of the polymer is not particularly limited. However, from the viewpoint of the handling properties of the doping solution described later and the mechanical strength of the separator, the weight-average molecular weight (Mw) of the polymer is preferably 10,000 to 500,000, and more preferably 20,000 to 300,000.
[0037] In this disclosure, the weight-average molecular weight is measured under the following conditions. Instrument: HLC-8220GPC (Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARD COLUMN HXL-L 6mm x 40mm (Tosoh Corporation) Sample-side column: The following three columns are directly connected in order (all Tosoh Corporation): ・TSK-GEL GMHXL 7.8mm x 300mm ・TSK-GEL G4000HXL 7.8mm x 300mm ・TSK-GEL G2000HXL 7.8mm x 300mm Reference-side column: TSK-GEL G1000HXL 7.8mm x 300mm Oven temperature: 40℃ Mobile phase: THF (Tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1% by mass Sample injection volume: 100 μL Data acquisition time: 5 to 45 minutes after sample injection Sampling pitch: 300 milliseconds
[0038] The polymer content is preferably 5% to 50% by mass, more preferably 5% to 40% by mass, even more preferably 7% to 30% by mass, and particularly preferably 9% to 25% by mass, relative to the total amount of the porous polymer layer.
[0039] Furthermore, the polymer content is preferably 15% to 65% by volume, more preferably 25% to 60% by volume, even more preferably 35% to 55% by volume, and particularly preferably 35% to 50% by volume, relative to the total volume of the porous polymer layer.
[0040] The porous polymer layer preferably contains at least one inorganic particle in addition to the polymer, and more preferably contains hydrophilic inorganic particles. Hydrophilic inorganic particles refer to particles composed of an inorganic material that exhibits dispersibility in water. Hydrophilic inorganic particles may be composed of a single inorganic material, or they may have a core-shell structure in which the shell portion is composed of a hydrophilic inorganic material. Normally, when a porous polymer layer contains hydrophilic inorganic particles, the separators tend to adhere to each other due to the interaction between the hydrophilic inorganic particles, but adhesion is suppressed with the separator roll of this disclosure.
[0041] From the viewpoint of hydrophilicity in alkaline solutions, the inorganic particles are preferably at least one type of particle selected from the group consisting of metal oxides and metal hydroxides.
[0042] Examples of metal oxides include zirconium oxide, titanium oxide, bismuth oxide, cerium oxide, and magnesium oxide.
[0043] Examples of metal hydroxides include zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide, and magnesium hydroxide.
[0044] The inorganic particles may also be barium sulfate particles.
[0045] The median diameter (D50) of the inorganic particles is preferably 0.05 μm to 2.00 μm, more preferably 0.1 μm to 1.50 μm, even more preferably 0.15 μm to 1.00 μm, and particularly preferably 0.20 μm to 1.00 μm. The median diameter (D50) refers to the particle size at which the total volume of the particles is 100% and the cumulative volume is 50%. In this disclosure, the median diameter (D50) is measured using a dynamic image analysis device.
[0046] If the porous polymer layer contains inorganic particles, the inorganic particle content is preferably 50% to 95% by mass, more preferably 60% to 95% by mass, even more preferably 70% to 93% by mass, and particularly preferably 75% to 91% by mass, based on the total amount of the porous polymer layer.
[0047] When the porous polymer layer contains inorganic particles, the inorganic particle content is usually 35% by volume or more, preferably 40% by volume or more, more preferably 45% by volume or more, and even more preferably 50% by volume or more, relative to the total volume of the porous polymer layer. The inorganic particle content is preferably 85% by volume or less, more preferably 75% by volume or less, and even more preferably 65% by volume or less, relative to the total volume of the porous polymer layer. In other words, the inorganic particle content is preferably 35% to 85% by volume, more preferably 40% to 75% by volume, even more preferably 45% to 65% by volume, and particularly preferably 50% to 65% by volume, relative to the total volume of the porous polymer layer.
[0048] The inorganic particle content in the porous polymer layer is measured by the following method: The porous polymer layer is scraped from the separator, and the mass of organic matter and inorganic matter (inorganic particles) is quantified by thermal analysis. The inorganic particle content can be calculated using the densities of organic and inorganic matter described in publicly available data.
[0049] When the porous polymer layer contains inorganic particles, the ratio of inorganic particles to polymer content (inorganic particles / polymer) is preferably 10 / 1 to 1 / 1 by mass, more preferably 9 / 1 to 2 / 1, even more preferably 8 / 1 to 3 / 1, particularly preferably 7 / 1 to 4 / 1, and most preferably 6.5 / 1 to 4 / 1.
[0050] When a separator is manufactured using the doping solution described later, a certain amount of good solvent contained in the doping solution inevitably remains in the porous polymer layer. The total content of good solvent in the porous polymer layer is usually between 0.01% by mass and 5.00% by mass.
[0051] The porous polymer layer in which the support substrate is embedded may be a single layer, or it may be a multilayer structure having a first porous polymer layer disposed on one side of the support substrate and a second porous polymer layer disposed on the other side of the support substrate. The first porous polymer layer and the second porous polymer layer are different layers, and they may be layers with different types or amounts of constituent components.
[0052] The separator preferably has a Shore A hardness of 30 to 70 at the outermost surface of the roll, and more preferably 30 to 60. A Shore A hardness of 30 or higher results in excellent separator roll shape. A Shore A hardness of 70 or lower further suppresses adhesion between separators.
[0053] By adjusting the tension applied to the separator when winding it onto the core, the Shore A hardness of the separator wound onto the core can be adjusted.
[0054] Shore hardness is determined by measuring the central part of the separator's width direction at the outermost surface of the separator roll using a Shore hardness durometer.
[0055] The separator is preferably 600 μm or less in thickness, more preferably 300 μm or less, and even more preferably 250 μm or less. The thickness can usually be 30 μm or more, preferably 50 μm or more, and more preferably 100 μm or more. In other words, the thickness is preferably 30 μm to 600 μm, more preferably 50 μm to 300 μm, and even more preferably 100 μm to 250 μm.
[0056] The thickness of the separator is measured by the following method.
[0057] Samples are taken at five arbitrary points, and cross-sections are cut out with a razor. A cross-sectional SEM (scanning electron microscope) image is acquired at a magnification (e.g., 400x) that allows the separator cross-section to fit in a single field of view. In the obtained cross-sectional SEM image, assuming that no pores exist (for example, assuming that the pores are filled with polymer), the thickness is measured at 20 equally spaced points at each sampling point, and the arithmetic mean of the total of 100 measurements is adopted.
[0058] From the viewpoint of gas barrier properties required for porous separators for alkaline water electrolysis, the bubble point of the separator is preferably greater than 1 bar, and more preferably greater than 2 bar. The pore diameter and porosity of the pores in the separator should be adjusted to a range that satisfies the above bubble point. The bubble point is determined by measuring using a palm porometer based on the bubble point test method described in ASTM (American Society for Testing and Materials) F316-86, and the pressure at which the first bubble appears in the resulting wet curve is defined as the bubble point.
[0059] The pore size of the separator is preferably 10 nm to 1000 nm, more preferably 20 nm to 700 nm, and even more preferably 30 nm to 500 nm, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The pore size is determined by obtaining the pore size distribution from the insertion curve by the mercury intrusion method and taking the average value. Note that the pore size referred to here refers to the pore size of the pores contained in the entire separator and is distinct from the pore size of the pores on the separator surface, which will be described later.
[0060] The separator preferably has pores on one surface and on the other surface, with different average pore diameters for each surface. By individually controlling the average pore diameters of both surfaces, ion permeability and gas barrier properties can be improved. Furthermore, when the average pore diameters of the pores on one surface and the other surface are different, when the separator is wound, the surface with a relatively smaller average pore diameter will come into contact with the surface with a relatively larger average pore diameter. By bringing the surface with a relatively smaller average pore diameter into contact with the surface with a relatively larger average pore diameter, adhesion between the separators can be further suppressed. For example, the pores on the separator surface are the pores on the surface of the porous polymer layer.
[0061] From the viewpoint of further suppressing adhesion between separators, the difference between the average pore diameter of the pores on one surface and the average pore diameter of the pores on the other surface is preferably 0.5 μm to 5 μm, and more preferably 1 μm to 4 μm.
[0062] The average pore diameter of the pores on the separator surface is determined by observing SEM images of 10 μm square fields of view on the separator surface in five different fields, determining the maximum Ferret diameter obtained by binary analysis for the pores present in each 10 μm square area, and taking the average value of these values.
[0063] The porosity of the separator is preferably 30% to 70%, more preferably 40% to 60%, from the viewpoint of exhibiting excellent ion permeability and excellent gas barrier properties. The porosity is the value of the porosity calculated from the insertion curve by the mercury intrusion method.
[0064] The separator preferably has through holes with a diameter of 0.3 mm to 3 mm formed at positions 1 mm to 30 mm from at least one end toward the center in the width direction, more preferably has through holes with a diameter of 0.3 mm to 3 mm formed at positions 3 mm to 15 mm from at least one end toward the center in the width direction, and even more preferably has through holes with a diameter of 0.5 mm to 2 mm formed at positions 3 mm to 15 mm from at least one end toward the center in the width direction. The formation of through holes at the above positions makes it easier to grip the separator before winding it onto the core, and the shape of the separator roll is excellent. It is more preferable that through holes with a diameter of 0.3 mm to 3 mm are formed at positions 1 mm to 30 mm from both ends in the width direction toward the center, more preferably that through holes with a diameter of 0.3 mm to 3 mm are formed at positions 3 mm to 15 mm from at least one end in the width direction toward the center, and even more preferably that through holes with a diameter of 0.5 mm to 2 mm are formed at positions 3 mm to 15 mm from at least one end in the width direction toward the center. It is preferable that multiple through holes are formed at regular intervals along the longitudinal direction of the separator. The interval between through holes along the longitudinal direction is, for example, 5 cm to 30 cm.
[0065] The through-holes are formed, for example, using a processing device such as a pin tenter.
[0066] The position of the through-hole is determined by the distance from the end of the separator in the width direction to the center of the through-hole. The diameter of the through-hole is measured using a digital caliper.
[0067] From the viewpoint of hydroxide ion permeability, the separator preferably has an ionic resistance of 0.01 Ω·cm 2 to 0.30 Ω·cm 2 , more preferably 0.01 Ω·cm 2 to 0.15 Ω·cm 2 . The ionic resistance is a value measured by an AC impedance method at 90°C with a separator punched into a circular shape set in a cell.
[0068] From the viewpoint of mass balance between the cathode side and the anode side of the electrolytic solution, the separator preferably has a water permeation rate of 100 mL / (h·m 2 ·bar) to 2000 mL / (h·m 2 ·bar). In addition, from the viewpoint of eliminating the need for operational contrivances for alkaline water electrolysis cells such as varying the permeation amount of the electrolytic solution on the anode side and the cathode side, the water permeation rate is more preferably 100 mL / (h·m 2 ·bar) to 1000 mL / (h·m 2 ·bar). The water permeation rate is a value calculated by setting a separator punched into a circular shape in a filter holder, and measuring the liquid volume (mL) when a 30 mass% potassium hydroxide aqueous solution is permeated through the circular separator for 30 seconds under conditions of 90°C and a gauge pressure of 1 bar.
[0069] The separator can be preferably used as a separator in a pressurized alkaline water electrolysis system (a separator for pressurized alkaline water electrolysis). The separator can also be used as a separator in an alkaline water electrolysis system used under normal pressure (a separator for alkaline water electrolysis).
[0070] The separator roll of the present disclosure has an uneven shape on the roll end face, and the width dimension between the concave end portion and the convex end portion in the direction perpendicular to the longitudinal direction is preferably in the range of 1 mm to 30 mm, more preferably in the range of 5 mm to 25 mm. The separator is wound around a winding core. For example, as the number of windings increases, the separators are wound while being displaced from each other in the width direction, whereby concave end portions and convex end portions are formed on the roll end face to form an uneven shape.
[0071] It is preferable to perform an oscillation treatment when winding the separator onto the core. Oscillation is the process of moving the separator back and forth in the width direction relative to the core while winding the separator to form a roll. The uneven shape on the side can be adjusted by controlling the rotation speed of the core, the speed of movement of the separator in the width direction, and the amount of movement when winding the separator onto the core.
[0072] The shape of the separator roll is superior when the width between the concave end and the convex end is 1 mm or more. When the width between the concave end and the convex end is 30 mm or less, adhesion between separators can be further suppressed.
[0073] The width between the concave and convex ends in the direction perpendicular to the longitudinal direction of the separator (i.e., the width direction) represents the misalignment between the stacked separators. The width between the concave and convex ends is measured with a metal ruler.
[0074] The separator roll of this disclosure preferably has an outer diameter of 7.6 cm to 100.0 cm, and more preferably 30 cm to 100 cm, from the viewpoint of further suppressing adhesion between separators. The outer diameter refers to the outer diameter of the separator roll. The outer diameter of the roll is measured using a measuring tape.
[0075] The method for manufacturing the separator is not particularly limited. The separator can be manufactured, for example, by forming a porous polymer layer by wet phase separation. For example, one method (hereinafter referred to as "manufacturing method I") involves forming the porous polymer layer by wet phase separation while the support substrate is placed in a coating film formed with a dope solution obtained by dissolving the polymer. This process yields a separator comprising a support substrate and a porous polymer layer that embeds at least a portion of the support substrate.
[0076] (Doping solution) The doping solution may contain, for example, the polymer contained in the porous polymer layer and a solvent, and may also contain inorganic particles. Details of the polymer contained in the porous polymer layer are as described above. Details of the inorganic particles that may be contained in the doping solution are as described above.
[0077] The solvent contained in the doping solution in the wet phase separation can be any solvent that can dissolve the above polymer (a good solvent), and is preferably miscible with water. The solvent is preferably selected from N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N-butylpyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, and mixtures thereof, with at least one of NMP and NBP being more preferred.
[0078] If the doped solution contains inorganic particles, the solvent content in the doped solution is preferably 10% to 85% by mass, more preferably 15% to 80% by mass, even more preferably 25% to 70% by mass, even more preferably 30% to 65% by mass, even more preferably 32% to 60% by mass, and even more preferably 35% to 50% by mass. If the doped solution does not contain inorganic particles, the solvent content in the doped solution is preferably 20% to 95% by mass, more preferably 25% to 90% by mass, even more preferably 30% to 80% by mass, even more preferably 40% to 80% by mass, even more preferably 45% to 75% by mass, and even more preferably 50% to 75% by mass.
[0079] If the doping solution contains inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 20% by mass, even more preferably 5% to 15% by mass, and still more preferably 6% to 15% by mass. If the doping solution does not contain inorganic particles, the polymer content in the doping solution is preferably 2% to 30% by mass, more preferably 4% to 30% by mass, even more preferably 6% to 25% by mass, and still more preferably 8% to 20% by mass.
[0080] In this disclosure, inorganic particles are particles that exist dispersed in the dope solution without dissolving, and this dispersion state is also referred to as the dope solution. That is, the "solution" in dope solution refers to the state in which the polymer is dissolved in the solvent. When the dope solution contains inorganic particles, the content of inorganic particles in the dope solution is preferably 10% to 85% by mass, more preferably 15% to 80% by mass, even more preferably 20% to 70% by mass, and particularly preferably 25% to 60% by mass.
[0081] The doping solution may contain components other than the solvent, polymer, and inorganic particles. For example, in wet phase separation, to control the formation of pores in the porous polymer layer, the doping solution may contain polyhydric alcohols such as polyethylene glycol, polypropylene glycol, ethylene glycol, tripropylene glycol, and glycerol; dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid or neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, lithium chloride, etc.
[0082] If the doping solution contains other components and inorganic particles, the total content of the other components in the doping solution is preferably 0.1% to 15% by mass, more preferably 0.2% to 10% by mass, and even more preferably 0.5% to 5% by mass. If the doping solution contains other components but does not contain inorganic particles, the total content of the other components in the doping solution is preferably 1% to 25% by mass, more preferably 5% to 25% by mass, and even more preferably 7% to 20% by mass.
[0083] -Manufacturing Method I- In Manufacturing Method I, a separator can be manufactured that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate by wet phase separation while a support substrate is placed in a coating film formed with a doped solution obtained by dissolving a polymer. In wet phase separation, the support substrate is placed on a coating film formed by casting the doped solution onto a substrate, and the support substrate is immersed in the coating film to impregnate the support substrate with the doped solution. Next, the support substrate, which has been impregnated with the doped solution, is immersed in a solvent (poor solvent, coagulation bath) that does not dissolve the polymer and is miscible with the good solvent. When the proportion of the good solvent in the coating film of the doped solution decreases due to this immersion, the polymer and the solvent undergo phase separation (liquid-induced phase separation), the polymer gels (coagulates), and a porous polymer layer is formed. A separator is then obtained that includes a support substrate and a porous polymer layer that embeds at least a portion of the support substrate.
[0084] As a poor solvent, for example, water, or a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water) or a water-soluble polymer can be used. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAC), and alcohols such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among these, water is preferred as the poor solvent.
[0085] The temperature of the coagulation bath is preferably 20°C to 90°C, more preferably 40°C to 70°C.
[0086] It is also preferable to expose the coating film to the vapor of the poor solvent before immersing it in the poor solvent to induce vapor-induced phase separation (vapor-induced phase separation). By performing vapor-induced phase separation, it is possible to suppress the formation of a dense skin layer on the surface. Therefore, in the above wet phase separation, vapor-induced phase separation and liquid-induced phase separation can also be combined. Furthermore, it is preferable to perform a washing step with pure water or the like after wet phase separation, preferably after liquid-induced phase separation.
[0087] In vapor induction phase separation, the support substrate coated with the dope solution is exposed to a non-solvent vapor, preferably humid air. As a method for performing vapor induction phase separation, for example, the description of Figure 2 and its explanation in Japanese Patent Publication No. 2023-531792 can be appropriately referred to and applied in accordance with this disclosure. The poor solvent vapor used in vapor induction phase separation is preferably humid air. The space for performing vapor induction phase separation can be, for example, provided between the step of coating the support substrate with the dope solution and the step of performing liquid induction phase separation, continuous with the apparatus for each step, and further shielded from the external environment using insulating metal plates. The degree and speed of water movement in the vapor induction phase separation step can be adjusted by adjusting the air velocity, relative humidity and temperature of the air, and exposure time. The relative humidity within the vapor induction phase separation region can be adjusted by the temperature of the solidification bath and shielding the vapor induction phase separation region from the environment. Vapor-induced phase separation performed on a support substrate coated with a doping solution may be carried out under the same conditions on both sides or under different conditions. The relative humidity and temperature in the region where vapor-induced phase separation is performed can be adjusted using an insulating metal plate, for example, when using the apparatus described in Figure 2 of Japanese Patent Publication No. 2023-531792. If the metal plate completely shields the region from the external environment, the relative humidity and temperature are determined by the temperature of the solidification bath used in the subsequent liquid-induced phase separation. The higher the relative humidity in the region where vapor-induced phase separation is performed, and the higher the air velocity, the larger the maximum pores in the resulting porous material. The relative humidity in the region where vapor-induced phase separation is performed can be, for example, in the range of 50% to 99%, preferably 60% to 98%, and more preferably 70% to 98%.
[0088] In the separator obtained by the above manufacturing method, a certain amount of good solvent from the doping solution used in the manufacturing inevitably remains. The amount of residual solvent can be determined by gas chromatography or by pre-drying the separator at 40°C for 12 hours. 1 The amount can be quantified using H-NMR as a mass percentage in 100% by mass of the above-mentioned dried porous separator for alkaline water electrolysis.
[0089] The separator in the separator roll of this disclosure can be used as a separator in a method for producing hydrogen by electrolyzing an alkaline aqueous solution using an electrolytic cell. In particular, it can be suitably used as an alkaline water electrolysis separator in the alkaline water electrolysis system described below.
[0090] Furthermore, the separator in the separator roll of this disclosure may be provided with a catalyst layer on at least one surface to serve as an alkaline water electrolysis member.
[0091] [Alkaline Water Electrolysis Cell] The alkaline water electrolysis cell of the present disclosure includes a separator in the separator roll of the present disclosure. Specifically, the alkaline water electrolysis cell of the present disclosure preferably includes a separator and at least one of an anode electrode and a cathode electrode, and more preferably includes a separator, an anode electrode and a cathode electrode.
[0092] Figure 1 is a schematic diagram illustrating a preferred embodiment of the alkaline water electrolysis system of the present disclosure.
[0093] In the alkaline water electrolysis system 20 shown in Figure 1, the alkaline water electrolysis cell 10 includes a separator 11, a cathode electrode 12 positioned on one surface of the separator 11, and an anode electrode 13 positioned on the other surface of the separator 11. The alkaline water electrolysis cell 10 is immersed in a high-concentration alkaline aqueous solution 14.
[0094] The alkaline aqueous solution 14 is, for example, an aqueous solution of potassium hydroxide or an aqueous solution of sodium hydroxide.
[0095] When an electric current flows between the electrodes, electrons are supplied to the cathode side, causing water to produce bubble-like hydrogen (H₂). 2 ) occurs (2H 2 O + 2e - →H 2 +2OH - ). Hydroxyl ions (OH) generated along with the generation of hydrogen. - ) moves to the anode side after passing through the separator 11, and electrons are removed at the anode to form bubble-shaped oxygen (O 2 ) occurs (4OH - →O2 +2H 2 O+4e - ).
[0096] Since the separator 11 is in contact with the cathode electrode 12 and the anode electrode 13, the distance traveled by the hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency.
[0097] In the above-described alkaline water electrolysis system, the components other than the separator, such as the cathode electrode and anode electrode, are not particularly limited, and ordinary components used in alkaline water electrolysis systems can be applied as appropriate.
[0098] [Alkaline Water Electrolysis Apparatus] The alkaline water electrolysis apparatus of this disclosure includes the alkaline water electrolysis cell of this disclosure. The alkaline water electrolysis apparatus of this disclosure can produce hydrogen by supplementing the necessary components, components, etc., depending on the configuration of the alkaline water electrolysis cell of this disclosure.
[0099] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples unless it exceeds the spirit of the disclosure.
[0100] <Example 1> 119 kg of polysulfone (product name "Udel P-3500 LCD MB7", Mw: approximately 80,000, manufactured by Solvay) is added to 397 kg of N-butylpyrrolidone (manufactured by TCI), and the mixture is stirred at 60°C for 5 hours to completely dissolve it. Next, 10 kg of polyvinylpyrrolidone (product name "PVP K90", manufactured by Merck) is added, and the mixture is stirred at 60°C for 1 hour, after which ZrO 2474 kg of particles (product name "E101", manufactured by Luxfer) are added and stirred for a further 3 hours to obtain the coating solution. Under conditions of 25°C and 60% relative humidity, a 1.5 m wide PET (polyethylene terephthalate) film roll is fed out as a coating support, and the coating solution is cast onto the PET film in a width of 1.3 m so that the final thickness when wound onto the separator is 200 μm. A 1.4 m wide PPS woven fabric (product name: PPS119 / 60, manufactured by NBC Meshtec, polyphenylene sulfide woven fabric, thickness 60 μm, opening ratio 60%) is placed on top of the cast coating solution. The PPS woven fabric is completely impregnated with the coating solution. Next, it is impregnated for 5 minutes in a first coagulation bath (pure water) adjusted to 10°C to form a porous polymer layer. Furthermore, the line speed is adjusted so that the time between impregnating the PPS woven fabric with the coating solution and immersing it in the first coagulation bath is 30 seconds. After washing for 10 minutes in a second coagulation bath (pure water) adjusted to 50°C, the long separator is peeled off the PET film. Next, the separator is gripped with a pin tenter 10 mm from both ends in the width direction toward the center, and through holes with a diameter of 1 mm are made. After drying at 80°C for 5 minutes, the separator is wound onto a winding core (7.5 cm in diameter, made of ABS resin) while performing an oscillation treatment. The oscillation treatment creates an uneven surface on the side of the separator roll, and the width between the concave and convex parts (unevenness width) becomes 10 mm. The separator is wound while tension is applied to it, and the Shore A hardness of the separator wound onto the winding core becomes 50. The roll diameter is 20 cm. The pore size of the PET film side of the separator is 2.2 μm, and the pore size of the other side is 0.1 μm.
[0101] <Examples 2 and 3> Separator rolls are obtained in the same manner as in Example 1, except that the core is changed and the diameter of the core is changed to the value shown in Table 1.
[0102] <Examples 4-7> Separator rolls are obtained in the same manner as in Example 2, except that the winding length is changed and the outer diameter is changed to the value shown in Table 1.
[0103] <Examples 8-11> Separator rolls are obtained in the same manner as in Example 2, except that the tension when winding the separator around the core is changed and the Shore A hardness of the separator is changed to the value shown in Table 1.
[0104] <Examples 12-15> Separator rolls are obtained in the same manner as in Example 2, except that the amount of movement of the separator in the width direction during the oscillation process is changed and the width of the unevenness is changed to the values listed in Table 1.
[0105] <Examples 16-21> Separator rolls are obtained in the same manner as in Example 2, except that the position and diameter of the through holes are changed to the values shown in Table 1.
[0106] <Example 22> A separator roll is obtained in the same manner as in Example 2, except that the coating solution is cast onto a PET film in a width of 1.45 m.
[0107] <Example 23> A separator roll is obtained in the same manner as in Example 2, except that the coating solution is cast onto a PET film in a width of 1.4 m.
[0108] <Example 24> A separator roll is obtained in the same manner as in Example 2, except that the line speed is adjusted so that the time from impregnating the PPS woven fabric with the coating solution to impregnating it in the first coagulation bath is 90 seconds. The pore size of the PET film side of the separator is 2.8 μm, and the pore size of the other side is 2.5 μm.
[0109] <Example 25> A separator roll was obtained in the same manner as in Example 2, except that the coating solution was cast in an environment of 25°C and 10% RH relative humidity. The pore size of the PET film surface of the separator was 0.11 μm, and the pore size of the other surface was 0.21 μm.
[0110] <Comparative Example 1> A separator roll is obtained in the same manner as in Example 1, except that the core is changed and the diameter of the core is changed to the value shown in Table 1.
[0111] (Shore A hardness) The Shore hardness is measured at the center of the separator's width direction on the outermost surface of the separator roll using a Shore durometer.
[0112] (Pore diameter on the separator surface) On both sides of the separator, SEM images of a 10 μm square field of view were observed in five different fields of view. For each 10 μm square area, the maximum Ferret diameter was determined by binary analysis, and the average value was calculated.
[0113] (Through-hole diameter) Three through-holes at the end of the separator are randomly selected, their diameters are measured with a digital caliper, and the average value is calculated.
[0114] The following evaluations of adhesive resistance and shape will be performed using separator rolls.
[0115] (Adhesion Resistance) The separator roll is left for one week in an environment with a temperature of 40°C and a relative humidity of 90% RH. After that, the separator is unwound from the separator roll and the shape of the separator surface is observed visually. -Evaluation Criteria- A: No adhesive residue is observed in any area. B: Adhesion residue is observed in an area that does not affect performance. C: There is some obvious adhesive residue that affects performance, but it can be removed. D: Obvious adhesive residue that affects performance is observed in all areas.
[0116] (Shape) Visually inspect the appearance of the separator roll in a room with a brightness of 10,000 lux. -Evaluation Criteria- A: No cosmetic defects such as wrinkles, dents, or scratches are observed. B: Minor cosmetic defects that do not affect performance are observed on a part of the separator roll. C: Minor cosmetic defects that do not affect performance are observed on the entire surface of the separator roll. D: Obvious cosmetic defects that affect performance are observed.
[0117] In Table 1, the "width of the recess and protrusion" refers to the width between the recess and protrusion formed on the side surface. The "position of the through hole" refers to the distance from both ends of the separator in the width direction to the through hole. The "ends in the width direction" column lists the members located at the ends of the separator in the width direction.
[0118]
[0119] As shown in Table 1, Examples 1 to 25 include a winding core and a separator wound around the winding core, with the diameter of the winding core ranging from 7.5 cm to 30.0 cm. The separator includes a support base material which is a woven or nonwoven fabric and a porous polymer layer which embeds at least a portion of the support base material, thereby suppressing adhesion between the separators.
[0120] In Comparative Example 1, the diameter of the winding core was less than 7.5 cm, the separators were bonded together, and adhesive marks were visible.
[0121] In Example 6, the outer diameter is 100.0 cm or less, and the adhesion between separators is suppressed compared to Example 7.
[0122] In Example 9, the Shore A hardness is 30 or higher, and the shape of the separator roll is superior compared to Example 8.
[0123] In Example 10, the Shore A hardness is 70 or less, and the adhesion between separators is suppressed compared to Example 11.
[0124] In Example 13, the width of the irregularities is 1 mm or more, and the shape of the separator roll is superior to that of Example 12.
[0125] In Example 14, the width of the unevenness is 30 mm or less, and the adhesion between the separators is suppressed compared to Example 15.
[0126] In Example 19, through holes with a diameter of 0.3 mm or more are formed, and the shape of the separator roll is superior to that of Example 18.
[0127] In Example 20, through holes with a diameter of 3 mm or less are formed, and the shape of the separator roll is superior to that of Example 21.
[0128] In Example 2, the support substrate is exposed at the end of the separator in the width direction, and the shape of the separator roll is superior to that of Examples 22 and 23.
[0129] Furthermore, the disclosure of Japanese Patent Application No. 2025-078885, filed on 9 May 2025, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted to be incorporated by reference.
[0130] 10 Alkaline water electrolysis cell 11 Separator 12 Cathode electrode 13 Anode electrode 14 Alkaline aqueous solution 20 Alkaline water electrolysis system O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH - Hydroxy ion e - electronic
Claims
1. An alkaline water electrolysis separator roll comprising a winding core and a roll-shaped alkaline water electrolysis separator wound around the winding core, wherein the diameter of the winding core is 7.5 cm to 30.0 cm, and the alkaline water electrolysis separator includes a support base material which is a woven or nonwoven fabric and a porous polymer layer which embeds at least a portion of the support base material.
2. The alkaline water electrolysis separator roll according to claim 1, wherein the outer diameter is 7.6 cm to 100.0 cm.
3. The alkaline water electrolysis separator roll according to claim 1 or claim 2, wherein the roll-shaped alkaline water electrolysis separator has a Shore A hardness of 30 to 70 at the outermost surface of the roll.
4. The alkaline water electrolysis separator roll according to claim 1 or claim 2, wherein the roll-shaped alkaline water electrolysis separator has an uneven shape on the end face of the roll, and the width between the concave end and the convex end in a direction perpendicular to the longitudinal direction is in the range of 1 mm to 30 mm.
5. The alkaline water electrolysis separator roll according to claim 1 or claim 2, wherein the roll-shaped alkaline water electrolysis separator has through holes with a diameter of 0.3 mm to 3 mm formed at positions 1 mm to 30 mm from at least one end in the width direction perpendicular to the longitudinal direction toward the center.
6. The alkaline water electrolysis separator roll according to claim 1 or 2, wherein the support substrate is exposed at the end of the roll-shaped alkaline water electrolysis separator in the width direction perpendicular to the longitudinal direction.
7. The alkaline water electrolysis separator roll according to claim 1 or 2, wherein the roll-shaped alkaline water electrolysis separator has holes on one surface and on the other surface, and the average pore diameter of the holes on the one surface and the holes on the other surface are different.
8. The separator roll for alkaline water electrolysis according to claim 1 or claim 2, wherein the porous polymer layer contains hydrophilic inorganic particles.
9. An alkaline water electrolysis cell comprising the alkaline water electrolysis separator in the alkaline water electrolysis separator roll according to claim 1 or claim 2.