Rubber modifier, rubber composition, molded article, automotive member, and hose

A polyester modifier with specific structural components addresses poor filler dispersibility in high nitrile acrylonitrile butadiene rubber compositions, enhancing mixing efficiency and improving the physical properties of molded articles.

WO2026234977A1PCT designated stage Publication Date: 2026-11-12DIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015717
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-20
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing rubber compositions with high nitrile acrylonitrile butadiene rubber face poor filler dispersibility, necessitating high energy consumption during mixing, which is inefficient and costly.

Method used

A polyester modifier with specific structural components, such as aliphatic and aromatic diol and dicarboxylic acid residues, enhances filler dispersibility through π-π interactions, improving mixing efficiency.

Benefits of technology

The polyester modifier significantly reduces energy consumption and improves the dispersibility of fillers, leading to better physical properties in molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015717_12112026_PF_FP_ABST
    Figure JP2026015717_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a rubber modifier capable of enhancing dispersibility of a rubber filler. Specifically, the rubber modifier is a polyester represented by the following general formula (1) (wherein A1 is an aromatic dicarboxylic acid residue having 8 to 14 carbon atoms).
Need to check novelty before this filing date? Find Prior Art

Description

Rubber modifiers, rubber compositions, molded articles, automotive components, and hoses

[0001] The present invention relates to rubber modifiers, rubber compositions, molded articles, automotive components, and hoses.

[0002] Rubber hose manufacturers enhance the physical properties of their rubber hoses, such as strength and abrasion resistance, by adding reinforcing materials like carbon black to diene-based rubber. The physical properties of a rubber hose are greatly influenced by the degree of dispersion of the reinforcing material within the hose, and it is necessary to sufficiently disperse the reinforcing material during the mixing process that prepares the rubber composition, which is the raw material for rubber hoses.

[0003] Poor dispersibility of the filler necessitates significant energy consumption during the mixing process; therefore, ensuring the dispersibility of the filler is crucial from the standpoint of manufacturing efficiency and energy conservation. For these reasons, a method has been proposed to ensure the dispersibility of the filler by adding a rubber modifier separately (for example, Patent Document 1).

[0004] Japanese Patent Application Publication No. 10-087901

[0005] Among diene rubbers, acrylonitrile butadiene rubber (NBR) has excellent physical properties, and in particular, "high-nitrile acrylonitrile butadiene rubber" and "ultra-high-nitrile acrylonitrile butadiene rubber," which have a high acrylonitrile content, can greatly improve the physical properties such as oil resistance and heat resistance of the resulting molded articles.

[0006] On the other hand, acrylonitrile butadiene rubber, which has a high nitrile group content, has particularly poor compatibility with fillers, and even when using the modifier described in Patent Document 1, sufficient dispersibility of the filler cannot be obtained. Thus, in the mixing process of rubber compositions containing fillers, there was a problem that a large amount of energy was required to disperse the filler.

[0007] The problem that this invention aims to solve is to provide a rubber modifier that can improve the dispersibility of rubber fillers.

[0008] The present inventors conducted intensive studies to solve the above problems, and as a result, found that a polyester having a specific structure can enhance the dispersibility of a rubber filler, thereby completing the present invention.

[0009] That is, the present invention relates to the following rubber modifier and the like. 1. A rubber modifier which is a polyester represented by the following general formula (1). (In the general formula (1), G 1 is an aliphatic diol residue having 2 to 12 carbon atoms or an aromatic diol residue having 6 to 18 carbon atoms, A 1 is an aromatic dicarboxylic acid residue having 8 to 14 carbon atoms, B 1 and B 2 are each independently a hydrogen atom, an aliphatic monocarboxylic acid residue having 1 to 8 carbon atoms, or an aromatic monocarboxylic acid residue having 6 to 12 carbon atoms, and n represents the number of repetitions. However, G for each repetition 1 may be the same as or different from each other, and A for each repetition 1 may be the same as or different from each other.) 2. The rubber modifier according to 1, wherein G in the general formula (1) 1 is an aliphatic diol residue having 2 to 12 carbon atoms. 3. The rubber modifier according to 1 or 2, wherein G in the general formula (1) 1 is one or more glycol residues selected from the group consisting of ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol, and A 11. A rubber modifier according to 1 or 2, wherein the compound is one or more dicarboxylic acid residues selected from the group consisting of phthalic acid, terephthalic acid, and isophthalic acid. 4. A rubber modifier according to any one of 1 to 3, wherein the number average molecular weight of the polyester is 350 to 2,000. 5. A rubber composition containing a diene rubber, a rubber filler, and a rubber modifier according to any one of 1 to 4. 6. The rubber composition according to 5, wherein the diene rubber is one or more selected from natural rubber, isoprene rubber, chloroprene rubber, acrylonitrile butadiene rubber, styrene butadiene rubber, and butadiene rubber. 7. The rubber composition according to 5 or 6, wherein the diene rubber contains acrylonitrile butadiene rubber with an acrylonitrile content of 36% by mass or more. 8. The rubber composition according to any one of 5 to 7, wherein the rubber filler is one or more carbon fillers selected from carbon black, graphite, carbon fiber, carbon nanotubes, and graphene. 9. A molded article of the rubber composition according to any one of 5 to 8. Automotive components using the rubber composition described in any of sections 10.5 to 8. Hose using the rubber composition described in any of sections 11.5 to 8.

[0010] The present invention provides a rubber modifier that can improve the dispersibility of rubber fillers.

[0011] One embodiment of the present invention will be described below. The present invention is not limited to the following embodiments, and can be implemented with appropriate modifications without impairing the effects of the present invention. The compounds used herein may be derived from fossil resources or from biological resources.

[0012] [Rubber Modifier] The rubber modifier of the present invention is a polyester represented by the following general formula (1). Hereinafter, the polyester represented by general formula (1) may be referred to as "the polyester of the present invention."

[0013] (In the above general formula (1), G 1 A is an aliphatic diol residue having 2 to 12 carbon atoms or an aromatic diol residue having 6 to 18 carbon atoms. 1 B is an aromatic dicarboxylic acid residue having 8 to 14 carbon atoms.1 and B 2 Each of these is independently a hydrogen atom, an aliphatic monocarboxylic acid residue with 1 to 8 carbon atoms, or an aromatic monocarboxylic acid residue with 7 to 13 carbon atoms, and n represents the number of repetitions. However, G is used for each repetition. 1 They may be the same or different from each other, and each time A 1 They may be the same or different from each other.

[0014] It is hypothesized that the polyester of the present invention can improve the dispersibility of rubber fillers through π-π interactions of aromatic rings in the repeating units.

[0015] In this invention, "carboxylic acid residue" refers to the organic group remaining after removing the hydroxyl group from a carboxylic acid. In this invention, "alcohol residue" refers to the organic group remaining after removing the hydrogen atom from an alcohol. In this invention, "diol residue" refers to the organic group remaining after removing the hydrogen atom from a diol. In this invention, "glycol residue" refers to the organic group remaining after removing the hydrogen atom from a glycol.

[0016] G 1 The fatty chain of aliphatic diol residues having 2 to 12 carbon atoms may be linear or branched, and may contain alicyclic structures and / or ether bonds. Also, G 1 The fatty acid chain of the aliphatic diol residue may be a saturated fatty acid chain or an unsaturated fatty acid chain having carbon-carbon unsaturated bonds.

[0017] G 1 Preferably, this is an alkylene glycol residue having 2 to 12 carbon atoms or an oxyalkylene glycol residue having 2 to 12 carbon atoms.

[0018] G 1Examples of alkylene glycol residues having 2 to 12 carbon atoms include ethylene glycol residues, 1,2-propylene glycol residues, 1,3-propanediol residues, 1,2-butanediol residues, 1,3-butanediol residues, 2-methyl-1,3-propanediol residues, 1,4-butanediol residues, 1,5-pentanediol residues, 2,2-dimethyl-1,3-propanediol (neopentyl glycol) residues, and 2,2-diethyl-1,3-propanediol (3,3-dimethyl- Examples include benzoyl phosphate residues, 2-n-butyl-2-ethyl-1,3-propanediol (3,3-dimethylolheptane) residues, 3-methyl-1,5-pentanediol residues, 1,6-hexanediol residues, 2,2,4-trimethyl-1,3-pentanediol residues, 2-ethyl-1,3-hexanediol residues, 2-methyl-1,8-octanediol residues, 1,9-nonanediol residues, 1,10-decanediol residues, 1,12-dodecanediol residues, and 1,2-dodecanediol residues.

[0019] G 1 The alkylene glycol residue having 2 to 12 carbon atoms may include an alicyclic structure. Examples of aliphatic diol residues having 2 to 12 carbon atoms that include such an alicyclic structure include 1,3-cyclopentanediol residue, 1,2-cyclohexanediol residue, 1,3-cyclohexanediol residue, 1,4-cyclohexanediol residue, 1,2-cyclohexanedimethanol residue, and 1,4-cyclohexanedimethanol residue.

[0020] G 1 The oxyalkylene glycol residue having 2 to 12 carbon atoms is an alkylene glycol residue containing one or more ether bonds (-O-). Examples of such oxyalkylene glycol residues having 2 to 12 carbon atoms include diethylene glycol residues, triethylene glycol residues, tetraethylene glycol residues, dipropylene glycol residues, and tripropylene glycol residues.

[0021] G 1Examples of aromatic diol residues having 6 to 18 carbon atoms include alkylene oxide adducts such as hydroquinone, resorcinol, bisphenol A, and bisphenol A; alkylene oxide adducts such as bisphenol F and bisphenol F; and alkylene oxide adduct residues such as biphenol and biphenol.

[0022] A 1 Examples of aromatic dicarboxylic acid residues having 8 to 14 carbon atoms include phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, and 1,8-naphthalenedicarboxylic acid.

[0023] A 1 The aromatic dicarboxylic acid residue having 8 to 14 carbon atoms is preferably an aromatic dicarboxylic acid residue having 8 to 12 carbon atoms. Also, A 1 The aromatic dicarboxylic acid residue having 8 to 14 carbon atoms may be further substituted with substituents (for example, alkyl groups having 1 to 6 carbon atoms), and residues of dimethyl terephthalic acid are examples of this.

[0024] B 1 and B 2 Examples of aliphatic monocarboxylic acid residues with 1 to 8 elementary atoms include residues of acetic acid, propionic acid, butanoic acid, hexanoic acid, and cyclohexanecarboxylic acid.

[0025] B 1 and B 2 Examples of aromatic monocarboxylic acid residues having 6 to 12 carbon atoms include benzoic acid, dimethylbenzoic acid, trimethylbenzoic acid, tetramethylbenzoic acid, ethylbenzoic acid, propylbenzoic acid, butylbenzoic acid, cumic acid, para-tert-butylbenzoic acid, orthotoluic acid, metatoluic acid, paratoluic acid, ethoxybenzoic acid, propoxybenzoic acid, naphthoic acid, and anisic acid residues. 1 and B 2 The aromatic monocarboxylic acid residue having 6 to 12 carbon atoms is preferably an aromatic monocarboxylic acid residue having 7 to 12 carbon atoms.

[0026] The polyester that is the rubber modifier of the present invention may be any polyester satisfying the aforementioned general formula (1), and for example, may be two or more types of polyesters having different structures from each other.

[0027] The repeating number n is, for example, an integer in the range of 0 to 20. The average value of the repeating number n is preferably in the range of 0.5 to 10.0, more preferably in the range of 0.6 to 8.0, and still more preferably in the range of 0.8 to 7.0. The average value of the repeating number n can be calculated from the number average molecular weight of the polyester of the present invention.

[0028] The number average molecular weight (Mn) of the polyester of the present invention is, for example, in the range of 100 to 5,000, preferably in the range of 300 to 2,000, and more preferably in the range of 350 to 1,500. The above number average molecular weight (Mn) is a value converted in terms of polystyrene based on gel permeation chromatography (GPC) measurement, and is measured by the method described in the Examples.

[0029] The acid value of the polyester of the present invention is, for example, 10 mgKOH / g or less, preferably 5 mgKOH / g or less, more preferably 3 mgKOH / g or less, and still more preferably 1 mgKOH / g or less. The lower limit of the acid value of the polyester of the present invention is not particularly limited, and is, for example, 0 mgKOH / g. The acid value of the above polyester is confirmed by the method described in the Examples.

[0030] The properties of the polyester of the present invention vary depending on the number average molecular weight, composition and the like, but are usually liquid, solid, paste-like or the like at normal temperature.

[0031] The polyester of the present invention can be obtained, for example, by using diols, dicarboxylic acids, and any monocarboxylic acids that constitute each residue as reaction raw materials. Therefore, the polyester of the present invention is a polyester that uses as reaction raw materials one or more diols selected from aliphatic diol residues having 2 to 12 carbon atoms and aromatic diols having 6 to 18 carbon atoms, a dicarboxylic acid which is an aromatic dicarboxylic acid having 6 to 12 carbon atoms, and one or more monocarboxylic acids selected from any aliphatic monocarboxylic acids having 1 to 8 carbon atoms and aromatic monocarboxylic acids having 6 to 12 carbon atoms. Here, "reaction raw materials" means raw materials that constitute the polyester, and does not include solvents or catalysts that do not constitute the polyester.

[0032] The method for producing polyester according to the present invention is not particularly limited and can be produced by known methods, or by the production method described later.

[0033] The dicarboxylic acid used in the production of the polyester of the present invention is A 1 The dicarboxylic acid is the dicarboxylic acid corresponding to the dicarboxylic acid residue, and the dicarboxylic acid used may be used alone or in combination of two or more. The diol used in the production of the polyester of the present invention is G 1 The diol corresponds to the diol residue of the diol, and the diol used may be used alone or in combination of two or more. The monocarboxylic acid used in the production of the polyester of the present invention is B 1 and B 2 The monocarboxylic acid corresponds to the monocarboxylic acid residue, and the monocarboxylic acid used may be used alone or in combination of two or more.

[0034] The dicarboxylic acids, diols, and monocarboxylic acids used in the production of the polyester of the present invention can all be derivatives thereof. Examples of such derivatives include esterified products, acid chlorides, and cyclic esters.

[0035] Specific examples of the polyester production method of the present invention include the following methods 1 and 2. Method 1: A method of charging dicarboxylic acids, diols, and any monocarboxylic acids that constitute each residue of the polyester all at once and reacting them. Method 2: A method of reacting dicarboxylic acids and diols that constitute each residue of the polyester under conditions in which the equivalent amount of hydroxyl groups is greater than the equivalent amount of carboxyl groups to obtain a polyester having hydroxyl groups at the ends of the main chain, and then reacting the obtained polyester resin with monocarboxylic acids that constitute monocarboxylic acid residues.

[0036] In the production of polyester according to the present invention, the reaction of the reaction raw materials may be carried out in the presence of an esterification catalyst as needed, for example, at a temperature range of 170 to 250°C for 10 to 25 hours. The temperature, time, and other conditions of the esterification reaction are not particularly limited and may be set as appropriate.

[0037] Examples of the esterification catalysts include titanium-based catalysts such as tetraisopropyl titanate and tetrabutyl titanate; zinc-based catalysts such as zinc acetate; tin-based catalysts such as tin octoate and dibutyltin oxide; and organic sulfonic acid-based catalysts such as p-toluenesulfonic acid.

[0038] The amount of esterification catalyst used can be set as appropriate, but it is usually used in the range of 0.0001 to 0.1 parts by mass per 100 parts by mass of the total amount of reaction raw materials.

[0039] [Rubber Composition] The rubber composition of the present invention contains a diene rubber, a rubber filler, and the rubber modifier of the present invention. By containing the rubber modifier of the present invention in the rubber composition, the dispersibility of the rubber filler can be improved, and the physical properties of the resulting molded article can be improved.

[0040] The content of the rubber modifier of the present invention in the rubber composition of the present invention is, for example, in the range of 1.0 to 50 parts by mass, preferably in the range of 5.0 to 50 parts by mass, and more preferably in the range of 5.0 to 30 parts by mass, per 100 parts by mass of the rubber filler.

[0041] (Diene rubber) The diene rubber in the rubber composition of the present invention is one or more selected from, for example, natural rubber, isoprene rubber, chloroprene rubber, acrylonitrile butadiene rubber, styrene butadiene rubber, and butadiene rubber. The diene rubber may be used alone or in combination of two or more types.

[0042] Among diene rubbers, acrylonitrile butadiene rubber (NBR) is classified according to its acrylonitrile (-C-C(CN)-) content. Specifically, it is classified into low-nitrile NBR with an acrylonitrile content of less than 24% by mass, medium-nitrile NBR with an acrylonitrile content of 24% to less than 30%, medium-high nitrile NBR with an acrylonitrile content of 30% to less than 36%, high-nitrile NBR with an acrylonitrile content of 36% to less than 43%, and very high-nitrile NBR with an acrylonitrile content of 43% or more. The upper limit of the acrylonitrile content for the aforementioned very high-nitrile NBR is, for example, 80% by mass.

[0043] Acrylonitrile butadiene rubber tends to exhibit improved physical properties such as oil resistance, heat resistance, and abrasion resistance as the acrylonitrile content increases. Therefore, the diene rubber preferably includes acrylonitrile butadiene rubber with an acrylonitrile content of 36% by mass or more (the diene rubber preferably includes high-nitrile NBR and / or very high-nitrile NBR).

[0044] If the diene rubber includes acrylonitrile butadiene rubber with an acrylonitrile content of 36% by mass or more, the proportion of acrylonitrile butadiene rubber with an acrylonitrile content of 36% by mass or more in the diene rubber may be, for example, 50% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 100% by mass.

[0045] The lower limit of the diene rubber content in the rubber composition of the present invention may be, for example, 25% by mass or more, 30% by mass or more, 35% by mass or more, or 40% by mass or more of the total amount of the rubber composition. The upper limit of the diene rubber content in the rubber composition of the present invention may be, for example, 80% by mass or less, 70% by mass or less, 55% by mass or less, or 50% by mass or less of the total amount of the rubber composition.

[0046] (Rubber fillers) Known rubber fillers can be used as rubber fillers, such as carbon fillers, silica, calcium carbonate, and magnesium silicate. Rubber fillers may be used individually or in combination of two or more types.

[0047] The rubber filler is preferably a carbon filler, more preferably one or more carbon fillers selected from carbon black, graphite, carbon fiber, carbon nanotubes, and graphene, and even more preferably carbon black.

[0048] When using rubber fillers and carbon black, various types of carbon black exist, such as furnace blacks (furnace carbon blacks) like SAF, ISAF, HAF, MAF, FEF, SRF, GPF, APF, FF, CF, SCF, and ECF; acetylene blacks (acetylene carbon blacks); thermal blacks (thermal carbon blacks) like FT and MT; and channel blacks (channel carbon blacks) like EPC, MPC, and CC. The appropriate carbon black should be selected based on its suitable properties for the intended application.

[0049] The content of the rubber filler in the rubber composition of the present invention is, for example, in the range of 10 to 200 parts by mass, preferably in the range of 20 to 180 parts by mass, more preferably in the range of 30 to 150 parts by mass, and even more preferably in the range of 30 to 120 parts by mass, per 100 parts by mass of diene rubber.

[0050] The rubber composition of the present invention may optionally further contain components known in the rubber industry, such as plasticizers, vulcanizing agents, vulcanization accelerators, vulcanization aids, processing aids, antioxidants, process oils, and silane coupling agents, to the extent that they do not impair the effects of the present invention. Note that any of the above components may be used individually or in combination of two or more.

[0051] (Plasticizer) Examples of the plasticizer include polyester-based plasticizers, phthalate-based plasticizers, and adipic acid ether ester-based plasticizers (e.g., bis[2-(2-butoxyethoxy)ethyl] adipate).

[0052] When the rubber composition of the present invention contains a plasticizer, the amount of plasticizer is, for example, in the range of 10 to 60 parts by mass, preferably in the range of 20 to 50 parts by mass, per 100 parts by mass of diene rubber.

[0053] (Vulcanizing agent) Examples of the vulcanizing agent include sulfur, sulfur-containing compounds, and peroxide vulcanizing agents, and sulfur is preferred from the viewpoint of storage stability and cost.

[0054] When the rubber composition of the present invention contains sulfur as a vulcanizing agent, the sulfur content is, for example, in the range of 0.1 to 15 parts by mass, preferably in the range of 0.3 to 5.0 parts by mass, per 100 parts by mass of diene rubber.

[0055] (Sulfurization accelerator) Examples of the aforementioned sulfurization accelerators include thiazole-based sulfurization accelerators, sulfenamide-based sulfurization accelerators, thiram-based sulfurization accelerators, aldehyde ammonia-based sulfurization accelerators, aldehyde amine-based sulfurization accelerators, guanidine-based sulfurization accelerators, and thiourea-based sulfurization accelerators, with sulfenamide-based sulfurization accelerators and thiram-based sulfurization accelerators being preferred.

[0056] Examples of the thiazole-based vulcanization accelerators include dibenzothiazyl disulfide (DM), 2-mercaptobenzothiazole (M), 2-mercaptobenzothiazole sodium salt (NaMBT), and 2-mercaptobenzothiazole zinc salt (ZnMBT).

[0057] Examples of the sulfenamide-based vulcanization accelerators include N-oxydiethylene-2-benzothiazolylsulfenamide (NOBS), N-cyclohexyl-2-benzothiazolylsulfenamide (CM), N-t-butyl-2-benzothiazoylsulfenamide (BBS), and N,N'-dicyclohexyl-2-benzothiazoylsulfenamide.

[0058] Examples of the thiram-based vulcanization accelerators include tetramethylthiram disulfide (TT), tetraethylthiram disulfide (TET), tetrabutylthiram disulfide (TBTD), tetrakis(2-ethylhexyl)thiram disulfide (TOT), and tetrabenzylthiram disulfide (TBZTD).

[0059] When the rubber composition of the present invention contains a vulcanization accelerator, the amount of the vulcanization accelerator is, for example, in the range of 0.1 to 10 parts by mass, preferably in the range of 0.5 to 6.0 parts by mass, per 100 parts by mass of diene rubber.

[0060] (Vulcanization aids) Examples of vulcanization aids include triallyl isocyanurate, N,N'-m-phenylenebismaleimide, methacrylic acid, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, sec-butyl methacrylate, t-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, isodecyl methacrylate, lauryl methacrylate, tridecyl methacrylate, stearyl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monomethacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, allyl methacrylate, glycidyl methacrylate, benzyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate Examples include acrylate, methacryloxyethyl phosphate, 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, trimethylolethane trimethacrylate, trimethylolpropane trimethacrylate, allyl glycidyl ether, N-methylol methacrylamide, 2,2-bis(4-methacryloxypolyethoxyphenyl)propane, aluminum methacrylate, zinc methacrylate, calcium methacrylate, magnesium methacrylate, 3-chloro-2-hydroxypropyl methacrylate, zinc oxide, magnesium oxide, etc.

[0061] When the rubber composition of the present invention contains a vulcanization aid, the amount of the vulcanization aid is, for example, in the range of 0.05 to 15 parts by mass, preferably in the range of 0.1 to 10 parts by mass, and more preferably in the range of 1 to 8 parts by mass, per 100 parts by mass of diene rubber.

[0062] (Processing aids) Examples of processing aids include fatty acids such as oleic acid, palmitic acid, and stearic acid; fatty acid metal salts such as zinc laurate, zinc stearate, barium stearate, and calcium stearate; fatty acid esters; alkylene glycols such as ethylene glycol and polyethylene glycol, with stearic acid being preferred.

[0063] If the rubber composition of the present invention contains a processing aid, the amount of the processing aid is, for example, in the range of 0.2 to 10 parts by mass, preferably in the range of 0.3 to 5.0 parts by mass, per 100 parts by mass of diene rubber.

[0064] (Anti-aging agents) Examples of anti-aging agents include amine / ketone-based anti-aging agents, imidazole-based anti-aging agents, amine-based anti-aging agents, phenol-based anti-aging agents, sulfur-based anti-aging agents, and phosphorus-based anti-aging agents.

[0065] When the rubber composition of the present invention contains an anti-aging agent, the amount of processing aid is, for example, in the range of 1.0 to 10 parts by mass, preferably in the range of 2.0 to 8.0 parts by mass, per 100 parts by mass of diene rubber.

[0066] Examples of process oils include aromatic oils, naphthenic oils, and paraffinic oils.

[0067] When the rubber composition of the present invention contains process oil, the content of the processing aid is, for example, in the range of 0.1 to 10 parts by mass, preferably in the range of 1.0 to 5.0 parts by mass, per 100 parts by mass of diene rubber.

[0068] [Method for Producing Rubber Composition] The rubber composition of the present invention can be produced using known methods. For example, it can be prepared by blending diene rubber, a rubber filler, the rubber modifier of the present invention, and any other components (plasticizer, vulcanizing agent, vulcanization accelerator, vulcanization aid, processing aid, antioxidant, process oil, silane coupling agent, etc.) and kneading them using a kneader, Banbury mixer, rolls, or other kneading machine. In the rubber composition of the present invention, the rubber modifier of the present invention can improve the dispersibility of the rubber filler, thus reducing the kneading energy and kneading time. This makes it possible to prepare the rubber composition with energy savings.

[0069] [Molded Articles of Rubber Composition] Molded articles obtained by molding the rubber composition of the present invention have well-dispersed rubber fillers due to the rubber modifier of the present invention, and can be made into molded articles with excellent physical properties such as abrasion resistance. The applications of the molded articles of the present invention are not particularly limited and can be used, for example, in hoses, tires, vibration-damping rubber, rubber belts, seismic isolation rubber, golf balls, rubber rollers, and footwear components (e.g., shoe soles).

[0070] For example, when manufacturing a hose using the rubber composition of the present invention, the rubber composition can be prepared by the method described above, extruded into a tube shape using a single-screw extruder, and then the resulting tube can be heated under predetermined conditions to vulcanize (crosslink) it to manufacture the hose. The hose is not limited to a single-layer structure, and a resin layer, a reinforcing yarn layer, a layer made of another rubber composition, etc., may be formed on the outer circumference of the single-layer hose as needed.

[0071] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples.

[0072] In the embodiments of this application, the values ​​of acid value and hydroxyl value were evaluated by the following methods. [Method for measuring acid value] Measured according to the method in accordance with JIS K0070-1992. [Method for measuring hydroxyl value] Measured according to the method in accordance with JIS K0070-1992.

[0073] In the embodiments of this invention, the number-average molecular weight of the polyester is a value converted to polystyrene based on GPC measurement, and the measurement conditions are as follows. [GPC Measurement Conditions] Measurement device: Tosoh Corporation high-speed GPC device "HLC-8420GPC" Column: Tosoh Corporation "TSKgel guardcolumn SuperMP (HZ)-N" x 1 + Tosoh Corporation "TSKgel SuperMultipore HZ-N" x 4 Detector: RI (differential refractometer) Data processing: Tosoh Corporation "GPC workstation EcoSEC Elite-WS" Column temperature: 40°C Developing solvent: Tetrahydrofuran Flow rate: 0.35 mL / min Sample: 20 mg of the sample was dissolved in 10 ml of tetrahydrofuran, and the resulting solution was filtered through a microfilter to be used as the sample. Sample injection volume: 10 μl Standard sample: In accordance with the measurement manual for the "HLC-8420GPC" described above, the following monodisperse polystyrene with known molecular weight was used.

[0074] (Monodisperse polystyrene) Tosoh Corporation "F-4" Tosoh Corporation "A-5000" Tosoh Corporation "A-500"

[0075] (Synthesis Example 1: Synthesis of Ester Compound (1)) In a 2 L four-necked glass flask, 1046.62 g of terephthalic acid as the dibasic acid component, 697.29 g of propylene glycol and 29.93 g of ethylene glycol as glycol components, and 0.1064 g of tetraisopropyl titanate as the catalyst were charged. The mixture was heated stepwise to 230°C while stirring under a nitrogen stream, and the reaction was continued until the acid value fell below 1.0. After confirming that the acid value was below 1.0, the temperature was lowered to 160°C, and 0.071 g of phosphoric acid was charged and stirred for about 1 hour. Then, the mixture was reduced in pressure to remove unreacted raw materials and other residues to obtain ester compound (1). The obtained ester compound (1) was a pale yellow solid with an acid value of 0.4, a hydroxyl value of 147, and a number-average molecular weight (Mn) of 870.

[0076] (Synthesis Example 2: Synthesis of Ester Compound (2)) In a 2 L four-necked glass flask, 1587.63 g of dimethyl 2,6-naphthalenedicarboxylate as the dibasic acid component, 803.76 g of propylene glycol and 34.51 g of ethylene glycol as glycol components, and 0.1456 g of tetraisopropyl titanate as the catalyst were charged. The mixture was gradually heated to 230°C while stirring under a nitrogen stream, and the reaction was continued until the acid value fell below 1.0. After confirming that the acid value was below 1.0, the temperature was lowered to 160°C, and 0.097 g of phosphoric acid was charged and stirred for about 1 hour. Then, the mixture was reduced in pressure to remove unreacted raw materials and obtain ester compound (2). The obtained ester compound (2) was a pale yellow solid with an acid value of 0.2, a hydroxyl value of 146, and a number-average molecular weight (Mn) of 850.

[0077] (Synthesis Comparative Example 1: Synthesis of Ester Compound (3)) In a 3 L four-necked glass flask, 1373.72 g of adipic acid as the dibasic acid component, 1057.91 g of propylene glycol and 45.41 g of ethylene glycol as glycol components, and 0.149 g of tetraisopropyl titanate as the catalyst were charged. The temperature was gradually raised to 230°C while stirring under a nitrogen stream, and the reaction was continued until the acid value fell to 1.0 or less. After confirming that the acid value was 1.0 or less, the temperature was lowered to 140°C, and 0.099 g of phosphoric acid was charged and stirred for about 1 hour. Then, ester compound (2) was obtained by removing unreacted raw materials under reduced pressure. The obtained ester compound (2) was a pale yellow liquid with an acid value of 0.2, a hydroxyl value of 150, and a number-average molecular weight (Mn) of 890.

[0078] (Example 1: Preparation and Evaluation of Rubber Composition) A rubber composition was prepared by kneading using a kneader ("Laboplastmill Micro" manufactured by Toyo Seiki Seisakusho Co., Ltd.) in the following order (1) to (7): (1) The mixer of the kneader was heated to 130°C and rotated at 5 rpm, and 10 parts by mass of ultra-high nitrile acrylonitrile butadiene rubber ("JSR N215SL" manufactured by JSR Corporation) and 10 parts by mass of high nitrile acrylonitrile butadiene rubber ("JSR N220S" manufactured by JSR Corporation) were added. After adding the acrylonitrile butadiene rubber, the rotation speed was increased to 20 rpm and kneaded for 2 minutes. (2) 5.0 parts by mass of rubber plasticizer ("Monosizer W-260" manufactured by DIC Corporation) was added as a plasticizer and kneaded for a further 2 minutes and 30 seconds. (3) Add 4.4 parts by mass of ester compound (1) as a modifier and knead for a further 1 minute. (4) Add 22 parts by mass of carbon black (Asahi Carbon Co., Ltd. "Asahi #70") and knead for 4 minutes. (5) Add 1.0 part by mass of zinc oxide as a vulcanization aid and 0.3 parts by mass of stearic acid as a processing aid and knead for 1 minute. (6) Add 0.3 parts by mass of 4-isopropylaminodiphenylamine as an antioxidant and knead for 1 minute. (7) Knead for a further 10 minutes to prepare the rubber composition.

[0079] The obtained rubber compositions were evaluated as follows. The results are shown in Table 1. (Visual evaluation of rubber compositions) The appearance of the obtained rubber compositions was visually checked and evaluated according to the following criteria: ○: No defects in appearance and a smooth surface △: Some roughness in the appearance and some areas that appear to be under-mixed ×: The entire appearance is rough and under-mixed overall

[0080] (Rheological Properties) A ​​rubber composition was obtained using a 2 mm thick mold under the following conditions: temperature: 100°C, pressure: approximately 6 MPa, press time: 10 min, and cooling time under touch pressure: 5 min. The strain dependence of the complex shear modulus of the obtained rubber sheet was measured using a rheometer (Anton Paar "MCR302") under the following conditions: Strain: 0.01–100% Frequency: 10 rad / s Measurement temperature: 100 deg Atmosphere gas: Air Geometry: 8 mm Dispo parallel plate Temperature control system: Hood Peltier (H-PTD200)

[0081] The obtained strain-dependent data of the complex shear modulus was applied to the following formula (1) to calculate the strain-dependent retention rate by dividing the complex shear modulus at 1.0% strain by the complex shear modulus at 0.1% strain and expressing it as a percentage. This value represents the degree of carbon black dispersibility; a higher value indicates better carbon black dispersibility.

[0082]

[0083] In the above calculation formula (1), each symbol represents the following: |G*|: Strain-dependent retention rate [%] |G(1.0%)|: Complex shear modulus at a strain rate of 1.0% [kPa] |G(0.1%)|: Complex shear modulus at a strain rate of 0.1% [kPa]

[0084] (Examples 2-4 and Comparative Examples 1-5: Preparation and Evaluation of Rubber Compositions) Rubber compositions were prepared and evaluated in the same manner as in Example 1, except that the components shown in Table 1 were used and the mixing conditions in Table 1 were used. The results are shown in Table 1.

[0085]

[0086] In Table 1, the carbon black mixing time x is the mixing time for step (4) in the preparation of the rubber composition, the additive mixing time y is the mixing time for steps (5) and (6) respectively in the preparation of the rubber composition, and the total mixing time z is the mixing time for step (7) in the preparation of the rubber composition.

[0087] Table 1 shows that the carbon black is well dispersed even with a short mixing time, based on the visual evaluation and strain-dependent retention rates of Examples 1-4. On the other hand, Comparative Example 1-5 does not achieve the same level of carbon black dispersion as Example 1-4, even with a longer mixing time.

Claims

1. A rubber modifier that is a polyester represented by the following general formula (1). (In the above general formula (1), G 1 A is an aliphatic diol residue having 2 to 12 carbon atoms or an aromatic diol residue having 6 to 18 carbon atoms. 1 B is an aromatic dicarboxylic acid residue having 8 to 14 carbon atoms. 1 and B 2 Each of these is independently a hydrogen atom, an aliphatic monocarboxylic acid residue having 1 to 8 carbon atoms, or an aromatic monocarboxylic acid residue having 6 to 12 carbon atoms, and n represents the number of repetitions. However, G is used for each repetition. 1 They may be the same or different from each other, and each time A 1 They may be the same or different from each other.

2. G in the general formula (1) 1 The rubber modifier according to claim 1, wherein is an aliphatic diol residue having 2 to 12 carbon atoms.

3. G in the aforementioned general formula (1) 1 is at least one glycol residue selected from the group consisting of ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,2-butanediol, 2-methyl-1,3-propanediol, and 2,2-dimethyl-1,3-propanediol, and A 1 is at least one dicarboxylic acid residue selected from the group consisting of phthalic acid, terephthalic acid and isophthalic acid, the rubber modifier according to claim 1.

4. The rubber modifier according to claim 1, wherein the number average molecular weight of the polyester is 350 to 2,000.

5. A rubber composition comprising a diene rubber, a rubber filler, and a rubber modifier according to any one of claims 1 to 4.

6. The rubber composition according to claim 5, wherein the diene rubber is one or more selected from natural rubber, isoprene rubber, chloroprene rubber, acrylonitrile butadiene rubber, styrene butadiene rubber, and butadiene rubber.

7. The rubber composition according to claim 5, wherein the diene rubber comprises acrylonitrile butadiene rubber having an acrylonitrile content of 36% by mass or more.

8. The rubber composition according to claim 5, wherein the rubber filler is one or more carbon fillers selected from carbon black, graphite, carbon fiber, carbon nanotubes, and graphene.

9. A molded article of the rubber composition according to claim 5.

10. An automotive component using the rubber composition described in claim 5.

11. A hose using the rubber composition described in claim 5.