Method for producing multicore optical fiber preform and set for forming multicore optical fiber preform
By preparing clad tubes with specific diameter differences and using vapor-phase etching, the method facilitates easy glass rod insertion and reduces misalignment in multi-core optical fiber preform manufacturing, enhancing efficiency and cost-effectiveness.
Patent Information
- Application Number
- PCT/JP2026/016544
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-24
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing multi-core optical fiber preforms face challenges in easily inserting glass rods into clad tubes with multiple holes of varying diameters and preventing misalignment after integration, leading to manufacturing inefficiencies and increased costs.
The method involves preparing clad tubes with specific diameter differences between holes and glass rods, allowing for easy insertion and reducing misalignment by adjusting hole diameters through vapor-phase etching, and using a dummy tube to stabilize the clad tube during heating.
This approach enables efficient insertion of glass rods into clad tubes with varying diameters and minimizes misalignment, thereby improving manufacturing efficiency and reducing costs.
Smart Images

Figure JP2026016544_12112026_PF_FP_ABST
Abstract
Description
Method for producing multi-core optical fiber preform and set for forming multi-core optical fiber preform
[0001] The present disclosure relates to a method for producing a multi-core optical fiber preform and a set for forming a multi-core optical fiber preform. This application claims priority based on Japanese Application No. 2025-078079 filed on May 8, 2025, and the entire contents described in the aforementioned Japanese application are incorporated herein by reference.
[0002] Patent Document 1 and Patent Document 2 describe methods for producing an optical fiber preform by the rod-in-tube (hereinafter referred to as RIT) method. The RIT method is, for example, a method of preparing a glass material to be the cladding of an optical fiber, forming holes at positions where cores are desired to be arranged, inserting core rods into the holes, and integrating the cladding tube and the core rods using a heat source. The heat source is an induction furnace, a resistance furnace, or an oxyhydrogen burner.
[0003] JP 2000-128559 A JP 2023-146915 A
[0004] The method for producing an MCF preform according to the present disclosure includes a step of preparing a cladding tube provided with a plurality of holes and a plurality of glass rods, and a step of inserting a corresponding one of the plurality of glass rods into each of the plurality of holes, the plurality of glass rods including a first glass rod and a second glass rod having a smaller diameter than the first glass rod, the plurality of holes including a first hole into which the first glass rod is inserted and a second hole into which the second glass rod is inserted, and in the preparing step, the cladding tube is prepared such that the difference between the diameter of the second hole and the diameter of the second glass rod is larger than the difference between the diameter of the first hole and the diameter of the first glass rod.
[0005] Figure 1 is a cross-sectional view perpendicular to the central axis of the MCF base material manufactured by the manufacturing method of the MCF base material according to the embodiment. Figure 2 is a flowchart of the manufacturing method of the MCF base material according to the embodiment. Figure 3 is a cross-sectional view perpendicular to the central axis of the clad tube prepared in the preparation step. Figure 4 is a cross-sectional view of the clad tube and dummy tube connected in the connection step. Figure 5 is a cross-sectional view for explaining the insertion step. Figure 6 is a cross-sectional view showing the state in which glass rods have been inserted into all of the multiple holes of the clad tube.
[0006] In the RIT method described above, to reduce manufacturing costs, a relatively inexpensive dummy tube may be connected to the clad tube, and the dummy tube may be used to grip the clad tube and integrate it with the glass rod. The clad tube and dummy tube are connected using a heat source such as an induction furnace, resistance furnace, or oxyhydrogen burner. In this case, the end of the clad tube may be heated, causing the hole in the clad tube to contract, which may prevent the glass rod from being inserted.
[0007] Therefore, sulfur hexafluoride (SF 6 One possible method is to enlarge the holes in the clad tube by vapor-phase etching the inner surface of the holes using a vapor-phase etching device. In clad tubes with multiple holes of different diameters, sulfur hexafluoride does not flow as easily into the smaller holes as it does into the larger holes. Therefore, vapor-phase etching may not enlarge the smaller holes, and it may not be possible to insert a glass rod into the smaller holes.
[0008] When preparing the clad tube, it is possible to make the diameter of all the holes sufficiently large relative to the glass rod. Since it is necessary to make each hole large along the entire length in the longitudinal direction, the gap between each hole and the glass rod will be large except at the ends of the clad tube. As a result, the fixing position of the glass rod after it has been integrated with the clad tube is likely to shift from the design position.
[0009] This disclosure provides a method for manufacturing a multicore optical fiber (hereinafter referred to as MCF) preform and a set for forming an MCF preform, which allows for easy insertion of a glass rod into a clad tube having multiple holes of different diameters and reduces misalignment of the glass rod after it has been integrated with the clad tube.
[0010] According to this disclosure, a glass rod can be easily inserted into a clad tube having multiple holes of different diameters during the manufacturing of the MCF base material, and the displacement of the glass rod in the MCF base material after it has been integrated with the clad tube can be reduced.
[0011] Embodiments of the present disclosure will be described. (1) A method for manufacturing an MCF base material according to a first aspect of the present disclosure comprises the steps of preparing a clad tube having a plurality of holes and a plurality of glass rods, and inserting a corresponding glass rod from the plurality of glass rods into each of the plurality of holes, wherein the plurality of glass rods include a first glass rod and a second glass rod having a smaller diameter than the first glass rod, and the plurality of holes include a first hole into which the first glass rod is inserted and a second hole into which the second glass rod is inserted, and in the preparation step, the clad tube is prepared such that the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod. In the above method for manufacturing an MCF base material, the diameter of the second hole is smaller than the diameter of the first hole, but the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod. Therefore, even when the clad tube is heated and the second hole shrinks, the second hole can maintain a diameter that allows the second glass rod to be inserted. Thus, the glass rod can be easily inserted into the second hole. The diameter of the first hole is larger than the diameter of the second hole, but the difference between the diameter of the first hole and the diameter of the first glass rod is smaller than the difference between the diameter of the second hole and the diameter of the second glass rod. Therefore, the gap between the first hole and the first glass rod is small. Thus, displacement of the first glass rod after it has been integrated with the clad tube can be reduced.
[0012] (2) In (1) above, the first glass rod may have the largest diameter among the multiple glass rods, and the second glass rod may have the smallest diameter among the multiple glass rods. In this case as well, the glass rod can be easily inserted into the second hole, and displacement of the first glass rod after it has been integrated with the clad tube can be reduced.
[0013] (3) In (1) or (2) above, the ratio a1 / b1 of the diameter of the first glass rod to the diameter b1 of the first hole may be 0.93 or more and 1.15 or less. In this case, the displacement of the first glass rod after it has been integrated with the clad tube can be further reduced.
[0014] (4) In any of (1) to (3) above, the ratio a2 / b2 of the diameter of the second glass rod to the diameter b2 of the second hole may be 0.67 or more and 0.92 or less. In this case, the glass rod can be inserted into the second hole more easily.
[0015] (5) In any of (1) to (4) above, the diameter of the first glass rod may be larger than the diameter of the first hole, and the diameter of the second glass rod may be smaller than the diameter of the second hole. In this case, the first glass rod can be easily inserted into the first hole by enlarging the diameter of the first hole by vapor phase etching of the inner surface of the first hole.
[0016] (6) The MCF base material forming set according to a first aspect of the present disclosure comprises a clad tube having a plurality of holes and a plurality of glass rods inserted into the plurality of holes, wherein the plurality of glass rods include a first glass rod and a second glass rod having a smaller diameter than the first glass rod, and the plurality of holes include a first hole into which the first glass rod is inserted and a second hole into which the second glass rod is inserted, wherein the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod. In the above MCF base material forming set, the diameter of the second hole is smaller than the diameter of the first hole, but the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod. Therefore, even when the clad tube is heated and the second hole shrinks, the second hole can maintain a diameter that allows the second glass rod to be inserted. Thus, the glass rod can be easily inserted into the second hole. The diameter of the first hole is larger than the diameter of the second hole, but the difference between the diameter of the first hole and the diameter of the first glass rod is smaller than the difference between the diameter of the second hole and the diameter of the second glass rod. Therefore, the gap between the first hole and the first glass rod is small. Thus, the displacement of the first glass rod after it has been integrated with the clad tube can be reduced.
[0017] [Details of Embodiments of the Disclosure] Specific examples of the method for manufacturing the MCF base material and the MCF base material forming set of the Disclosure will be described below with reference to the drawings. The Disclosure is not limited to these examples, and is intended to include all changes within the meaning and scope of the claims, as indicated by the claims. In the description of the drawings, the same elements are denoted by the same reference numerals, and redundant descriptions are omitted.
[0018] Figure 1 is a cross-sectional view perpendicular to the central axis of an MCF base material manufactured by the manufacturing method of the MCF base material according to the embodiment. As shown in Figure 1, the MCF base material 1 comprises a plurality of core portions 2, a cladding portion 3, and marker portions 4 for identifying each core portion 2.
[0019] Multiple core portions 2 extend along the central axis A1 of the MCF base material 1. The number of core portions 2 is not limited as long as it is two or more. In this embodiment, the number of core portions 2 is four, and the MCF base material 1 is a base material for a 4-core optical fiber. Multiple core portions 2 are provided at positions that are separated from each other. Multiple core portions 2 are provided at positions that are rotationally symmetric with respect to the central axis A1 in a cross section perpendicular to the central axis A1. The cross-sectional shapes of the multiple core portions 2 are all the same circular shape. The refractive index of the multiple core portions 2 is higher than the refractive index of the cladding portion 3.
[0020] The clad portion 3 is a common clad portion that surrounds multiple core portions 2 and marker portions 4. The clad portion 3 is provided in contact with the outer circumferential surfaces of each of the multiple core portions 2 and marker portions 4. The central axis A1 is also the central axis of the clad portion 3. The clad portion 3 has an outer circumferential surface 3a.
[0021] The marker portion 4 is positioned away from the central axis A1. The distance between the center of the marker portion 4 and the central axis A1 is longer than the distance between the center of the core portion 2 and the central axis A1. The marker portion 4 is positioned away from each core portion 2. The marker portion 4 is positioned in a location that is not symmetrical with respect to the arrangement of the core portions 2. That is, the marker portion 4 is positioned in a location that breaks the rotational symmetry of the cross-sectional structure perpendicular to the central axis A1. The diameter of the marker portion 4 is, for example, smaller than the diameter of the core portion 2. The marker portion 4 is distinguished from the core portion 2 by, for example, coloring. The refractive index of the marker portion 4 is different from the refractive index of the cladding portion 3. For this reason, if the marker is positioned close to the core or if the diameter of the marker is large, the marker may affect the properties of the core. Therefore, the marker is usually positioned far away from the core by making the distance between the center of the marker and the central axis longer than the distance between the center of the core and the central axis. In addition, the marker is formed with a smaller diameter than the core.
[0022] Multiple core parts 2, cladding parts 3, and marker parts 4 contain quartz glass as the main component. Multiple core parts 2, cladding parts 3, and marker parts 4 contain 50% or more quartz glass. Multiple core parts 2, cladding parts 3, and marker parts 4 contain dopants for adjusting the refractive index. Examples of dopants that increase the refractive index include germanium. Examples of dopants that decrease the refractive index include fluorine or boron. Marker parts 4 contain, for example, dopants for coloring.
[0023] Figure 2 is a flowchart illustrating a method for manufacturing an MCF base material according to an embodiment. As shown in Figure 2, the method for manufacturing the MCF base material 1 includes a preparation step S10, a connection step S20, a determination step S30, an insertion step S40, an etching step S50, and an integration step S60. The MCF base material 1 is manufactured, for example, by performing the preparation step S10, the connection step S20, the determination step S30, the insertion step S40, the etching step S50, and the integration step S60 in this order. The MCF base material 1 is manufactured by the RIT method.
[0024] Figure 3 is a cross-sectional view perpendicular to the central axis of the clad tube prepared in the preparation step. Preparation step S10 is a step of preparing the clad tube 10 provided with a plurality of holes 11 as shown in Figure 3, and a plurality of glass rods 30 (see Figure 6) described later. In preparation step S10, a dummy tube 20 (see Figure 4) described later may also be prepared. The clad tube 10 and the plurality of glass rods 30 prepared in preparation step S10 constitute an MCF base material forming set 100.
[0025] The multiple glass rods 30 include multiple core rods 30A and one marker rod 30B (see Figure 6). The core rods 30A are glass rods that form the core portion 2. The marker rod 30B is a glass rod that forms the marker portion 4. The core rods 30A and marker rod 30B have a circular cross-section. The diameter of the core rods 30A is, for example, 15 mm to 50 mm. The diameter of the marker rods 30B is, for example, 5 mm to 20 mm. The diameter of the marker rods 30B is smaller than the diameter of the core rods 30A.
[0026] The multiple core rods 30A have equivalent diameters to each other. Therefore, each of the multiple core rods 30A has the largest diameter among the multiple glass rods 30. The marker rod 30B has the smallest diameter among the multiple glass rods 30. In this embodiment, "equivalent" may include slight differences or manufacturing tolerances within a predetermined range. For example, if multiple values fall within ±5% of the average value of those multiple values, then those multiple values are defined as equivalent.
[0027] The clad pipe 10 is a common clad pipe that forms the clad section 3. The clad pipe 10 has two end faces, a first end 10a and a second end 10b, which are aligned with the central axis A2 of the clad pipe 10. The clad pipe 10 has an outer circumferential surface 10c. The multiple holes 11 penetrate the clad pipe 10 along the central axis A2 and open at the first end 10a and the second end 10b, respectively. The multiple holes 11 have a circular cross-section.
[0028] The multiple holes 11 include multiple first holes 11A and one second hole 11B. The first holes 11A are located in positions corresponding to the core portion 2. A core rod 30A is inserted into the first holes 11A. The second holes 11B are located in positions corresponding to the marker portion 4. A marker rod 30B is inserted into the second holes 11B. The diameter (inner diameter) of the first holes 11A is, for example, 15.1 mm or more and 51.0 mm or less. The diameter (inner diameter) of the second holes 11B is, for example, 5.2 mm or more and 20.2 mm or less. The diameter of the second holes 11B is smaller than the diameter of the first holes 11A.
[0029] In preparation step S10, the clad tube 10 is prepared such that the difference between the diameter of the second hole 11B and the diameter of the marker rod 30B (the gap for the marker) is greater than the difference between the diameter of the first hole 11A and the diameter of the core rod 30A (the gap for the core). In other words, in this embodiment, the following equation (1) holds: b2 - a2 > b1 - a1 (1) Here, a1 is the diameter of the core rod 30A. b1 is the diameter of the first hole 11A. a2 is the diameter of the marker rod 30B. b2 is the diameter of the second hole 11B. All of these diameters are the diameters before connection step S20.
[0030] In this embodiment, the value calculated by the following formula (2) is between 0.93 and 1.15. a1 / b1 (2)
[0031] In this embodiment, the value calculated by the following formula (3) is between 0.67 and 0.92. a² / b² (3)
[0032] Preparation step S10 includes a drilling step S11 in which a plurality of holes 11 are formed in a cylindrical glass rod, for example, by drilling. In drilling step S11, the first hole 11A and the second hole 11B are formed such that the difference between the diameter of the second hole 11B and the diameter of the marker rod 30B is greater than the difference between the diameter of the first hole 11A and the diameter of the core rod 30A.
[0033] The diameter of the core rod 30A (a1) is smaller than the diameter of the first hole 11A (b1) (a1 < b1). The diameter of the marker rod 30B (a2) is smaller than the diameter of the second hole 11B (b2) (a2 < b2). The diameter of the core rod 30A may be equal to the diameter of the first hole 11A (a1 = b1), or it may be larger than the diameter of the first hole 11A (a1 > b1).
[0034] Figure 4 is a cross-sectional view of the clad tube and dummy tube connected by the connection process. Figure 4 is a cross-sectional view along the central axis A2. The dummy tube 20 is a cylindrical glass tube with a hole 21. The dummy tube 20 is used to grip the clad tube 10. In this embodiment, the dummy tube 20 and the clad tube 10 have equivalent outer diameters. In this embodiment, "equivalent" may include slight differences or manufacturing tolerances within a predetermined range. For example, if a plurality of values are within ±5% of the average value of the plurality of values, then the plurality of values are defined as equivalent. Viewed along the central axis A2, the outer circumferential surface 20c of the dummy tube 20 coincides with the outer circumferential surface 10c of the clad tube 10. The outer diameter of the dummy tube 20 may be smaller than the outer diameter of the clad tube 10 in the range in which the hole 21 communicates with the hole 11.
[0035] The connection step S20 is the step of connecting the dummy tube 20 to the first end 10a of the clad tube 10. The clad tube 10 and the dummy tube 20 are connected so that they are coaxial with each other. The dummy tube 20 is connected to the first end 10a such that, when viewed along the central axis A2, all of the multiple holes 11 overlap with the holes 21. The clad tube 10 and the dummy tube 20 are fused together using a heat source. The heat source is, for example, an induction furnace, a resistance furnace, or an oxyhydrogen burner. Although not shown in the figures, in the connection step S20 of this embodiment, the dummy tube 20 is also connected to the second end 10b of the clad tube 10.
[0036] In connection step S20, the end of the clad pipe 10 is heated, causing the hole 11 at the end of the clad pipe 10 to contract. Therefore, the diameter of the hole 11 at the end of the clad pipe 10 after connection step S20 may be smaller than the diameter before connection step S20.
[0037] The determination step S30 is a step to determine whether or not the insertion step S40 can be performed. For each of the multiple holes 11 after the connection step S20, it is determined whether or not the corresponding glass rod 30 from among the multiple glass rods 30 can be inserted. If it is determined to be possible (S30: Yes), the insertion step S40 is performed. If it is determined to be impossible (S30: No), the etching step S50 is performed.
[0038] Figure 5 is a cross-sectional view illustrating the insertion process. Figure 5 is a cross-sectional view along the central axis A2. Insertion process S40 is the process of inserting a corresponding glass rod 30 from among the multiple glass rods 30 into each of the multiple holes 11. The multiple glass rods 30 are inserted one by one into the holes 11.
[0039] The insertion step S40 is performed with the pair of dummy tubes 20 being gripped in the direction of the central axis A2 by the gripping part (not shown) of the glass lathe. In this embodiment, the glass rod 30 passes through the hole 21 of the dummy tube 20 and is inserted into the hole 11 from the opening of the first end 10a. The glass rod 30 may also be inserted into the hole 11 from the opening of the second end 10b.
[0040] The insertion step S40 is performed using a jig 40 that lifts the glass rod 30 away from the inner surface of the hole 21 in the dummy tube 20. The jig 40 is inserted into the hole 21 and positioned in contact with the inner surface of the hole 21. The jig 40 is a glass rod with a rectangular cross-section. The jig 40 has a contact surface 40a and a mounting surface 40b that face opposite directions. The contact surface 40a is the surface that contacts the inner surface of the hole 21. The mounting surface 40b is the surface on which the glass rod 30 is placed. The jig 40 is positioned such that the mounting surface 40b is an extension of the part of the inner surface of the hole 11 that is furthest from the central axis A2. The mounting surface 40b may also be parallel to the part of the inner surface of the hole 11 that is furthest from the central axis A2. If the clad tube 10 and the dummy tube 20 are horizontal, the mounting surface 40b may also be horizontal.
[0041] In the insertion step S40, first, the clad tube 10 is rotated by rotating the shaft of a glass lathe, so that the hole 11 to be inserted is arranged at the lowermost position. Next, the jig 40 and the glass rod 30 placed on the placement surface 40b are inserted together into the hole 21 of the dummy tube 20.
[0042] Subsequently, the glass rod 30 placed on the placement surface 40b is pushed with a rod-shaped member (not illustrated), so that the glass rod 30 is inserted into the hole 11 of the clad tube 10. The rod-shaped member is formed of, for example, a heat-resistant resin such as a fluorine-based resin. Finally, the jig 40 and the rod-shaped member are taken out from the dummy tube 20. In the insertion step S40, these operations are repeated until the glass rods 30 are inserted into all of the plurality of holes 11.
[0043] The etching step S50 is a step of subjecting the inner surface of the hole 11 of the clad tube 10 to vapor phase etching. The holes 11 can be enlarged by vapor phase etching. As an etching gas, for example, sulfur hexafluoride is used. As a carrier gas, for example, chlorine gas is used. The etching gas and the carrier gas pass through the holes 21 of the dummy tube 20 and are supplied to the plurality of holes 11 of the clad tube 10. The etching step S50 is performed by heating the clad tube 10 by traversing a heat source. The heat source is, for example, an induction furnace, a resistance furnace, or an oxy-hydrogen burner. After the holes 11 are enlarged to a size that allows the glass rods 30 to be inserted therethrough by the etching step S50, the insertion step S40 is performed.
[0044] FIG. 6 is a cross-sectional view illustrating a state in which glass rods are inserted into all of the plurality of holes of the clad tube. FIG. 6 is a cross-sectional view orthogonal to the central axis A2.
[0045] The integration step S60 is a step of melting the clad tube 10 and the plurality of glass rods 30 by heating using the RIT method, so as to integrate them with each other. As a heat source, an induction furnace, a resistance furnace, or an oxy-hydrogen burner is used. The integration step S60 is also referred to as a collapse step. The MCF preform 1 (see FIG. 1) is obtained by the integration step S60.
[0046] The embodiments have been described above, but the present disclosure is not necessarily limited to the above-described embodiments, and various modifications are possible without departing from the gist of the present disclosure.
[0047] For example, the hole 11 does not need to penetrate the clad tube 10. The hole 11 only needs to be open at least at the first end 10a.
[0048] Hereinafter, the results of evaluation tests using Examples and Comparative Examples according to the present disclosure will be shown to describe the present disclosure in further detail. The present disclosure is not limited to these Examples.
[0049] (Test Example 1 to Test Example 5) As Test Example 1 to Test Example 5, MCF base materials were manufactured by changing the diameter a1 of the core rod. The diameter b1 of the hole for the core rod was fixed to 20.0 mm, the diameter b2 of the hole for the marker rod was fixed to 6.0 mm, and the diameter a2 of the marker rod was fixed to 4.0 mm. The outer diameter of the dummy tube was set to φ100 mm, the inner diameter to φ80 mm, the thickness to 10 mm, and the length to 1000 mm. The outer diameter of the clad tube was set to φ100 mm, and the length to 1000 mm. The openings of the clad tube were 4 holes for core rods and 1 hole for a marker rod. Each hole position corresponds to the example shown in Figure 3.
[0050] The connection of the clad tube and the dummy tube was performed under the same applied temperature and time conditions in all test examples. In some test examples, an etching step was performed. As the etching gas and carrier gas, sulfur hexafluoride and chlorine gas were each flowed at 1000 sccm together. The traverse speed was set to 30 mm / min to traverse the external heat source of the induction furnace, and vapor phase etching was performed while heating the clad tube.
[0051] Table 1 summarizes the test conditions and test results for Test Examples 1 to 5. It shows the diameter b1 (mm) of the hole for the core rod, the diameter a1 (mm) of the core rod, the diameter b2 (mm) of the hole for the marker rod, the diameter a2 (mm) of the marker rod, whether or not the glass rod can be inserted into the clad tube, the ratio a1 / b1 of the diameter of the core rod to the diameter b1 of the hole for the core rod, and the ratio a2 / b2 of the diameter a2 of the marker rod to the diameter b2 of the hole for the marker rod. The hole diameters shown in Table 1 are the diameters of the holes in the clad tube at the time of opening (before the connection process).
[0052] "Possible 1" under "Insertable" indicates that all glass rods could be inserted into the holes without gas-phase etching. "Possible 2" indicates that the core rods could not be inserted into the holes before gas-phase etching, but all glass rods could be inserted after gas-phase etching. The number of gas-phase etching traverses for "Possible 2" is 1 or 2. "Abnormal" indicates that there was a large displacement of the core after integration.
[0053] If a sufficiently large gap is provided for the marker rod, even if the diameter of the hole for the core rod and the diameter of the core rod become close, insertion is possible by performing additional etching as in Test Examples 2 to 4. In Test Example 5, although the MCF base material could be manufactured, the gap for the core (the difference between the diameter of the hole for the core rod and the diameter of the core rod) was large, resulting in significant displacement of the core after integration.
[0054] (Test Examples 6 to 10) In Test Examples 6 to 10, the MCF base material was manufactured under the same conditions as in Test Examples 1 to 5, except that the diameter a1 of the core rod was fixed at 19.0 mm and the diameter a2 of the marker rod was varied.
[0055] Table 2 summarizes the test conditions and test results for Test Examples 6 through 10.
[0056] "Insertable" indicates that the marker rod could not be inserted into the hole both before and after gas-phase etching. In Test Examples 6 to 10, the conditions were such that the core rod could be sufficiently inserted into the hole. In Test Examples 6 to 10, the gap for the marker rod was insufficient. Because the hole for the marker rod was small, the etching gas did not flow easily, and even with 3 traverses, it hardly expanded.
[0057] (Test Examples 11 to 15) In Test Examples 11 to 15, MCF base materials were manufactured by varying the diameter a1 of the core rod. The diameter b1 of the hole for the core rod was fixed at 30.0 mm, the diameter b2 of the hole for the marker rod was fixed at 10.0 mm, and the diameter a2 of the marker rod was fixed at 8.0 mm. The outer diameter of the dummy tube was φ150 mm, the inner diameter at φ130 mm, the thickness at 10 mm, and the length at 1000 mm. The outer diameter of the clad tube was φ150 mm and the length at 1500 mm. The opening of the clad tube had four holes for the core rod and one hole for the marker rod. The positions of each hole correspond to the example shown in Figure 3.
[0058] In all test examples, the connection of the clad tubes and dummy tubes was performed under consistent loading temperature and time conditions. In some test examples, an etching process was carried out. Sulfur hexafluoride and chlorine gas were flowed together at 2000 sccm each as the etching gas and carrier gas, respectively. The external heat source of the induction furnace was traversed at a traverse speed of 30 mm / min, and vapor-phase etching was performed while heating the clad tubes.
[0059] Table 3 summarizes the test conditions and test results for Test Examples 11 to 15.
[0060] If a sufficiently large gap is provided for the marker rod, even if the diameter of the hole for the core rod and the diameter of the core rod become close or reversed, insertion will be possible by performing additional etching as in Test Examples 13 to 15. In Test Example 11, it was possible to manufacture the MCF base material, but because the gap for the core (the difference between the diameter of the hole for the core rod and the diameter of the core rod) was large, there was a large displacement of the core part after integration.
[0061] (Test Examples 16 to 20) In Test Examples 16 to 20, the MCF base material was manufactured under the same conditions as in Test Examples 11 to 15, except that the diameter a1 of the core rod was fixed at 29.0 mm and the diameter a2 of the marker rod was varied.
[0062] Table 4 summarizes the test conditions and test results for Test Examples 16 to 20.
[0063] In Test Examples 16 to 20, the core rods were sufficiently inserted into the holes. However, in Test Examples 16 to 20, the clearance for the marker rods was insufficient. Because the holes for the marker rods were small, the etching gas flowed poorly, and even with two traverses, the holes hardly expanded.
[0064] (Test Examples 21 to 25) In Test Examples 21 to 25, MCF base materials were manufactured by varying the diameter a1 of the core rod. The diameter b1 of the hole for the core rod was fixed at 40.0 mm, the diameter b2 of the hole for the marker rod was fixed at 12.0 mm, and the diameter a2 of the marker rod was fixed at 11.0 mm. The outer diameter of the dummy tube was φ230 mm, the inner diameter at φ200 mm, the thickness at 15 mm, and the length at 1000 mm. The outer diameter of the clad tube was φ230 mm and the length at 1500 mm. The opening of the clad tube had four holes for the core rod and one hole for the marker rod. The positions of each hole correspond to the example shown in Figure 3.
[0065] In all test examples, the connection of the clad tubes and dummy tubes was performed under consistent loading temperature and time conditions. In some test examples, an etching process was carried out. Sulfur hexafluoride and chlorine gas were flowed together at 2000 sccm each as the etching gas and carrier gas, respectively. The external heat source of the induction furnace was traversed at a traverse speed of 30 mm / min, and vapor-phase etching was performed while heating the clad tubes.
[0066] Table 5 summarizes the test conditions and test results for Test Examples 21 to 25.
[0067] If a sufficiently large gap is provided for the marker rod, even if the diameter of the hole for the core rod and the diameter of the core rod become close or reversed, insertion will be possible by performing additional etching as shown in Test Examples 24 and 25.
[0068] (Test Examples 26 to 30) In Test Examples 26 to 30, the MCF base material was manufactured under the same conditions as in Test Examples 21 to 25, except that the diameter a1 of the core rod was fixed at 39.0 mm and the diameter a2 of the marker rod was varied.
[0069] Table 6 summarizes the test conditions and test results for Test Examples 26 to 30.
[0070] In Test Examples 26 to 30, the core rods were sufficiently inserted into the holes. However, in Test Examples 26 to 30, the clearance for the marker rods was insufficient. Because the holes for the marker rods were small, the etching gas flowed poorly, and even with two traverses, the holes hardly expanded.
[0071] The embodiments disclosed herein should be considered in all respects as illustrative and not restrictive. It should be understood that at least one configuration or feature described in each embodiment and example can be combined with or modified in various ways in other embodiments and examples. The scope of the invention is indicated by the claims and not in the sense described above, and all modifications within the sense and scope equivalent to the claims are intended to be included.
[0072] 1…MCF base material 2…Core part 3…Clad part 3a…Outer surface 4…Marker part 10…Clad tube 10a…First end 10b…Second end 10c…Outer surface 11…Hole 11A…First hole 11B…Second hole 20…Dummy tube 20c…Outer surface 21…Hole 30…Glass rod 30A…Core rod 30B…Marker rod 40…Jig 100…MCF base material forming set A1…Central axis A2…Central axis S10…Preparation process S11…Hole drilling process S20…Connection process S30…Decision process S40…Insertion process S50…Etching process S60…Integration process
Claims
A method for manufacturing a multicore optical fiber preform, comprising:
1. the steps of preparing a clad tube having a plurality of holes and a plurality of glass rods; and 2. inserting a corresponding glass rod from the plurality of glass rods into each of the plurality of holes, wherein the plurality of glass rods include a first glass rod and a second glass rod having a smaller diameter than the first glass rod; and the plurality of holes include a first hole into which the first glass rod is inserted and a second hole into which the second glass rod is inserted; and in the preparation step, the clad tube is prepared such that the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod.
2. The method for manufacturing a multicore optical fiber preform according to claim 1, wherein the first glass rod has the largest diameter among the plurality of glass rods, and the second glass rod has the smallest diameter among the plurality of glass rods.
3. A method for manufacturing a multicore optical fiber preform according to claim 1 or claim 2, wherein the value calculated by the following first formula is 0.93 or more and 1.15 or less. Here, the first formula is a1 / b1, where a1 is the diameter of the first glass rod and b1 is the diameter of the first hole.
4. A method for manufacturing a multicore optical fiber preform according to any one of claims 1 to 3, wherein the value calculated by the following second formula is 0.67 or more and 0.92 or less. Here, the second formula is a2 / b2, where a2 is the diameter of the second glass rod and b2 is the diameter of the second hole.
5. The method for manufacturing a multicore optical fiber preform according to any one of claims 1 to 4, wherein the diameter of the first glass rod is greater than the diameter of the first hole, and the diameter of the second glass rod is smaller than the diameter of the second hole.
6. A set for forming a multicore optical fiber matrix, comprising: a clad tube provided with a plurality of holes; and a plurality of glass rods inserted into the plurality of holes, wherein the plurality of glass rods include a first glass rod and a second glass rod having a smaller diameter than the first glass rod; and the plurality of holes include a first hole into which the first glass rod is inserted and a second hole into which the second glass rod is inserted, wherein the difference between the diameter of the second hole and the diameter of the second glass rod is greater than the difference between the diameter of the first hole and the diameter of the first glass rod.