Method for producing semiconductor nanoparticle composite

By coordinating semiconductor nanoparticles with an organic acid metal salt and ligand, the method enhances fluorescence quantum efficiency and weather resistance, addressing the deterioration issues of semiconductor nanoparticles.

WO2026235040A1PCT designated stage Publication Date: 2026-11-12SHOEI CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/016648
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-27
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Semiconductor nanoparticles face issues of high surface activity, reactivity with moisture and oxygen, leading to deterioration and decreased fluorescence quantum efficiency when protected by ligand exchange methods.

Method used

A method involving the coordination of semiconductor nanoparticles with a ligand and an organic acid metal salt, specifically using a saturated aliphatic carboxylic acid, under controlled heating and stirring conditions, to form a semiconductor nanoparticle composite with enhanced fluorescence quantum efficiency and weather resistance.

Benefits of technology

The method produces semiconductor nanoparticle composites with high fluorescence quantum efficiency and improved weather resistance, maintaining optical properties even in the presence of oxygen and moisture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A method for producing a semiconductor nanoparticle composite in which semiconductor nanoparticles are coordinated by ligands, said method including: a first mixing step for mixing the semiconductor nanoparticles, the ligand, and an organic acid metal salt and obtaining a first reaction raw material mixture; and a first reaction step for reacting the first reaction raw material mixture to obtain a first reaction product. According to the present invention, it is possible to provide a method for producing a semiconductor nanoparticle composite having high fluorescence quantum efficiency and high weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing semiconductor nanoparticle composite

[0001] The present invention relates to a method for producing a semiconductor nanoparticle composite.

[0002] Semiconductor nanoparticles (quantum dots, QD) that are small enough to exhibit the quantum confinement effect have a band gap dependent on their particle size. Excitons formed inside semiconductor nanoparticles by means such as photoexcitation and charge injection emit photons with energy corresponding to the band gap through recombination. Therefore, light emission at a desired wavelength can be obtained by appropriately selecting the composition and particle size of the semiconductor nanoparticles.

[0003] In the early stage of research, studies on semiconductor nanoparticles focused mainly on elements containing Cd and Pb. However, since Cd and Pb are regulated substances subject to restrictions such as the Restriction of the Use of Certain Hazardous Substances, non-Cd and non-Pb semiconductor nanoparticles have been studied in recent years.

[0004] Semiconductor nanoparticles have a problem of high surface activity, and tend to easily react with moisture and oxygen in the atmosphere to deteriorate. In order to solve these problems, many studies have been conducted to protect the surface of semiconductor nanoparticles.

[0005] As a method for protecting the surface of semiconductor nanoparticles and imparting weather resistance thereto, forming a semiconductor nanoparticle composite in which a ligand for imparting weather resistance to the semiconductor nanoparticles is coordinated has been carried out.

[0006] Takashi Jin, "Semiconductor Quantum Dots, Their Synthesis Methods and Applications in Life Science", Production and Technology, Vol. 63, No. 2, p. 58-63, 2011

[0007] A ligand exchange method is known as a method for obtaining a semiconductor nanoparticle composite by coordinating a desired ligand to semiconductor nanoparticles. The ligand exchange method is a method of replacing the ligand already coordinated on the surface of the synthesized semiconductor nanoparticles with a different ligand. The semiconductor nanoparticle composite obtained thereby can be dispersed in a dispersion medium different from that for the post-synthesis ligand. However, although the semiconductor nanoparticle composite disclosed in the non-patent document can be dispersed in dispersion media with different polarities, it has a problem that the luminous efficiency decreases.

[0008] In other words, even when attempting to protect the surface of semiconductor nanoparticles and impart weather resistance by coordinating new ligands to semiconductor nanoparticles through ligand exchange, there was a problem that the fluorescence quantum efficiency of the semiconductor nanoparticles decreased, even before considering the imparting of weather resistance.

[0009] Therefore, an object of the present invention is to provide a method for producing semiconductor nanoparticle composites that have high fluorescence quantum efficiency and high weather resistance.

[0010] As a result of diligent research, the inventors of this invention discovered the following and completed the present invention.

[0011] In other words, the present invention (1) provides a method for producing a semiconductor nanoparticle composite in which a ligand is coordinated to semiconductor nanoparticles, comprising: a first mixing step of mixing semiconductor nanoparticles, a ligand and an organic acid metal salt to obtain a first reaction material mixture; and a first reaction step of reacting the first reaction material mixture to obtain a first reactant.

[0012] Furthermore, the present invention (2) provides a method for producing the semiconductor nanoparticle composite of (1), wherein the organic acid metal salt is a metal salt of a carboxylic acid.

[0013] Furthermore, the present invention (3) provides a method for producing the semiconductor nanoparticle composite of (2), wherein the carboxylic acid is a saturated aliphatic carboxylic acid.

[0014] Furthermore, the present invention (4) provides a method for producing any of the semiconductor nanoparticle composites described in (1) to (3), wherein the metal element constituting the organic acid metal salt includes one or more of Zn, Cd, Ag, In, Ga, and Te.

[0015] Furthermore, the present invention (5) provides a method for producing any of the semiconductor nanoparticle composites according to (1) to (4), wherein in the first reaction step, the first reaction raw material mixture is heated to 50°C or higher to cause the reaction.

[0016] Furthermore, the present invention (6) provides a method for producing any of the semiconductor nanoparticle composites according to (1) to (5), wherein the molar ratio of the organic acid metal salt to the ligand is 0.01 or more.

[0017] Furthermore, the present invention (7) provides a method for producing semiconductor nanoparticle composites according to (1) to (6), wherein, after performing the first reaction step, a mixing step for additional reaction raw materials is performed to obtain a mixture of raw materials for an additional reaction containing the first reactant, a ligand, and an organic acid metal salt, and a reaction step is performed to react the mixture of raw materials for the additional reaction to obtain a reactant.

[0018] Furthermore, the present invention (8) provides a method for producing a semiconductor nanoparticle composite according to any of (1) to (6), wherein, after performing the first reaction step, a mixing step for additional reaction raw materials is performed to obtain a mixture of raw materials for an additional reaction containing the reactant obtained in the previous reaction step, a ligand, and an organic acid metal salt, and a reaction step is performed to react the mixture of raw materials for the additional reaction to obtain a reactant, and these steps are repeated two or more times.

[0019] Furthermore, the present invention (9) provides a method for producing any of the semiconductor nanoparticle composites (1) to (8), wherein the ligand has an organic group and a coordinating group, and the coordinating group comprises at least one of a thiol group, a carboxyl group, an amino group, a phosphine group, a phosphone group, and a phosphine oxide group.

[0020] According to the present invention, it is possible to provide a method for producing semiconductor nanoparticles that have high fluorescence quantum efficiency and high weather resistance.

[0021] The present invention relates to a method for producing semiconductor nanoparticle composites in which ligands are coordinated to the surface of semiconductor nanoparticles. The semiconductor nanoparticle composites obtained by the present invention have high fluorescence quantum efficiency and high weather resistance. In particular, the semiconductor nanoparticle composites obtained by the present invention have high weather resistance even when the amount of ligand coordination is small. The coordination referred to herein means that the ligand is chemically bonded to the surface of the semiconductor nanoparticle.

[0022] The present invention relates to a method for producing a semiconductor nanoparticle composite in which a ligand is coordinated to semiconductor nanoparticles, and is characterized by comprising: a first mixing step of mixing semiconductor nanoparticles, a ligand and an organic acid metal salt to obtain a first reaction material mixture; and a first reaction step of reacting the first reaction material mixture to obtain a first reactant.

[0023] The present invention provides a method for producing a semiconductor nanoparticle composite, comprising a first mixing step and a first reaction step.

[0024] The first mixing step involves mixing semiconductor nanoparticles, a ligand, and an organic acid metal salt to obtain a first reaction raw material mixture.

[0025] The semiconductor nanoparticles involved in the first mixing step are mixed with the ligand and the organic acid metal salt in the first mixing step and are reaction materials that react in the first reaction step. The semiconductor nanoparticles involved in the first mixing step may be particles having one type of semiconductor, or particles having two or more different types of semiconductors. In the case of particles having two or more different types of semiconductors, they may constitute a core-shell structure.

[0026] The semiconductor nanoparticles involved in the first mixing step preferably have luminescence properties. For example, the semiconductor nanoparticles are particles that absorb light in the 340 nm to 480 nm range and emit light with an emission peak wavelength of 400 nm to 750 nm. As mentioned above, such semiconductor nanoparticles are deactivated by oxygen in the atmosphere, so by coordinating ligands using the semiconductor nanoparticle composite manufacturing method of the present invention, the benefits of improved weather resistance can be more fully enjoyed.

[0027] When the semiconductor nanoparticles involved in the first mixing step are particles having one type of semiconductor, examples of the composition include InP, InZnP, ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnSeS, CdSe, CdS, CdSeS, CdSeZn, AgGaS, AgInGaS, etc. From the viewpoint of environmental impact, a composition containing InP, InZnP, ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnSeS, AgGaS, AgInGaS, etc. is preferred.

[0028] When the semiconductor nanoparticles involved in the first mixing step constitute a core-shell structure made up of two or more types of semiconductors, examples of the composition forming the core include InP, InZnP, ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnSeS, CdSe, CdS, CdSeS, CdSeZn, AgGaS, AgInGaS, etc. From the viewpoint of environmental impact, a composition containing InP, InZnP, ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnSeS, AgGaS, AgInGaS, etc. is preferred.

[0029] Examples of compositions for forming the shell include group II-VI element semiconductors, specifically ZnSe, ZnS, ZnSeS, ZnSeTe, ZnSTe, and ZnTe. In particular, when the shell has a structure containing Zn, the weather resistance can be further improved by the method for producing the semiconductor nanoparticle composite of the present invention.

[0030] The semiconductor nanoparticles involved in the first mixing step are, from the viewpoint of having high optical properties, core-shell type semiconductor nanoparticles comprising core particles and a shell covering at least a portion of the surface of the core particles, wherein the core particles preferably contain In and P, and the shell preferably contains at least one element from Zn, Se, and S.

[0031] As long as the effects of the present invention are not impaired, the composition for forming semiconductor nanoparticles does not necessarily have to be a stoichiometric composition and may contain trace elements as appropriate. Examples of trace elements include Si, Ge, B, Al, Tl, N, P, As, Sb, Bi, Te, and Po.

[0032] In the present invention, the method for producing semiconductor nanoparticles is not particularly limited, and any method may be used, such as conventional methods including hot injection molding, homogeneous solvent methods, reverse micelle methods, and CVD methods.

[0033] In the first mixing step, the semiconductor nanoparticles may be the synthesized semiconductor nanoparticles as they are, or purified semiconductor nanoparticles may be used. Generally, the synthesized semiconductor nanoparticles often have the initial ligands added during synthesis coordinated to them. Examples of initial ligands added during synthesis include ligands having coordinating groups such as thiol groups, carboxyl groups, amino groups, phosphine groups, phosphone groups, and phosphine oxide groups. Typical examples include alkylthiols such as dodecanethiol and octanthiol, carboxylic acids such as oleic acid and stearic acid, alkylamines such as octylamine, dioctylamine, and trioctylamine, alkylphosphines such as trioctylphosphine, and alkylphosphine oxides such as trioctylphosphine oxide. Even if the initial ligands are coordinated to the semiconductor nanoparticles after synthesis, according to the present invention, it is possible to coordinate any ligand described later.

[0034] In the first mixing step, if the synthesized semiconductor nanoparticles are used as is, there is no need to go through a purification step, thus simplifying the equipment required to obtain the semiconductor nanoparticle composite. Furthermore, if purified semiconductor nanoparticles are used in the first mixing step, excess additives added during synthesis can be removed, making it less likely for impurities to be incorporated when obtaining the semiconductor nanoparticle composite, and thus stabilizing the properties of the resulting semiconductor nanoparticle composite, which is preferable.

[0035] The ligand involved in the first mixing step is a reaction material that is mixed with semiconductor nanoparticles and an organic acid metal salt in the first mixing step and reacts in the first reaction step. The ligand is preferably an organic ligand. The organic ligand has a coordinating group that coordinates to the semiconductor nanoparticles and an organic group consisting of an organic chain. The coordinating group of the ligand contributes to binding to the semiconductor nanoparticles.

[0036] The ligand's coordinating group preferably contains at least one of the following: a thiol group, a carboxyl group, an amino group, a phosphine group, a phosphone group, and a phosphine oxide group. Having at least one of these coordinating groups allows the ligand to coordinate to the semiconductor nanoparticles, suppressing the deterioration of the semiconductor nanoparticle's optical properties. It is more preferable that the ligand's coordinating group be a thiol group, a carboxyl group, or an amino group. Having a thiol group, a carboxyl group, or an amino group allows for strong coordination to the surface of the semiconductor nanoparticles, thereby improving the weather resistance of the semiconductor nanoparticle composite. In particular, when the surface of the semiconductor nanoparticles is composed of Zn, it is even more preferable that the coordinating group be a thiol group, as this allows for strong coordination to the Zn and further improves weather resistance.

[0037] The organic group of the ligand is not particularly limited and can be appropriately selected depending on the application of the semiconductor nanoparticle composite. When the semiconductor nanoparticle composite is dispersed in a nonpolar solvent, it is preferable that the organic group is a hydrocarbon group. There is no particular limitation as long as it is a hydrocarbon group, and the presence or absence of saturated or unsaturated bonds does not matter. Also, the hydrocarbon group may be linear or branched. There is no particular limit to the number of carbon atoms, but it is preferable that it be between 1 and 30. On the other hand, when the semiconductor nanoparticle composite is dispersed in a polar dispersion medium, it is preferable that the organic group has a hydrophilic functional group. Examples of hydrophilic functional groups include hydroxyl groups, carboxyl groups, carbonyl groups, mercapto groups, amino groups, ether bonds, ester bonds, siloxane bonds, etc., and it is preferable that the organic group has at least one of these.

[0038] Ligands are not limited to these, but examples include dodecanethiol, octanthiol, acetic acid, propionic acid, myristic acid, stearic acid, octylamine, dioctylamine, trioctylamine, oleic acid, oleylamine, PEGthiol, etc.

[0039] The number-average molecular weight of the ligand is preferably 600 or less, more preferably 500 or less, and even more preferably 400 or less. By setting the number-average molecular weight of the ligand within the above range, the volume of the semiconductor nanoparticle composite can be reduced, allowing for a higher concentration of semiconductor nanoparticles when dispersed in a dispersion medium or product, and further suppressing the discrepancy between the optical density of a dispersion containing semiconductor nanoparticles and a dispersion containing the semiconductor nanoparticle composite. The lower limit of the ligand's molecular weight is not particularly limited, but is preferably 50 or more.

[0040] The amount of ligand that coordinates to the semiconductor nanoparticles is appropriately adjusted by the amount of ligand mixed when preparing the first reaction raw material mixture in the first mixing step. There is no particular lower limit to the amount of ligand mixed in the first mixing step, but it is preferably 0.0001 or more by mass ratio with respect to the semiconductor nanoparticles, more preferably 0.0005 or more, and even more preferably 0.001 or more. By keeping the amount of ligand mixed in the first mixing step within the above range, the fluorescence quantum efficiency and weather resistance of the semiconductor nanoparticles can be improved. There is no particular upper limit to the amount of ligand mixed in the first mixing step, but it is preferably 1000 or less by mass ratio with respect to the semiconductor nanoparticles, more preferably 900 or less, and even more preferably 800 or less. By keeping the amount of ligand mixed in the first mixing step within the above range, it is possible to simplify the process when removing excess ligand.

[0041] The organic acid metal salt involved in the first mixing step is a reaction raw material that is mixed with semiconductor nanoparticles and ligands in the first mixing step and reacts in the first reaction step. The organic acid metal salt is a metal salt of an organic acid and is composed of an organic acid anion and a metal cation. For example, zinc acetate, a type of organic acid metal salt, is composed of two organic acid anions CH 3 COO - and metal cation Zn 2+It is composed of and . In particular, the metal salt of the organic acid is preferably a metal salt of a carboxylic acid. Examples of carboxylic acids related to the metal salt of the organic acid include saturated aliphatic carboxylic acids and unsaturated aliphatic carboxylic acids. The organic chain constituting the carboxylic acid may be a straight chain or may have a branched chain. Examples of carboxylic acids related to the metal salt of the organic acid include acetic acid, propionic acid, butyric acid, hexanoic acid, octanoic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, oleic acid, neodecanoic acid, 2-ethylhexanoic acid, and 3,5,5-trimethylhexanoic acid. It is more preferable that the carboxylic acid related to the metal salt of the organic acid is a saturated aliphatic carboxylic acid and / or a carboxylic acid having a branched chain. Although the mechanism is not clear, by having the carboxylic acid related to the metal salt be a saturated aliphatic carboxylic acid and / or a carboxylic acid having a branched chain, it is possible to obtain a semiconductor nanoparticle composite with high fluorescence quantum efficiency and high weather resistance.

[0042] The metal elements constituting the organic acid metal salt preferably include elements that constitute semiconductor nanoparticles. If the semiconductor nanoparticles have a core-shell structure, the metal elements preferably include elements that constitute the shell. It is thought that the inclusion of elements that constitute semiconductor nanoparticles in the organic acid metal salt promotes strong coordination of the organic acid metal salt to the surface of the semiconductor nanoparticles together with the ligand. Examples of metal elements constituting the organic acid metal salt include Zn, Cd, Ag, In, Ga, Te, etc.

[0043] While the effects are not particularly limited, for example, the following combinations are preferable for the semiconductor nanoparticles and the organic acid metal salt used in the first mixing step. The same applies to the combination of the semiconductor nanoparticles used in the first mixing step and the organic acid metal salt used in the mixing step for the additional reaction raw material described later. When a ligand is coordinated to semiconductor nanoparticles containing Zn to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains Zn. When a ligand is coordinated to semiconductor nanoparticles containing Cd to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains Cd. When a ligand is coordinated to semiconductor nanoparticles containing Ag to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains Ag. When a ligand is coordinated to semiconductor nanoparticles containing In to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains In. When a ligand is coordinated to semiconductor nanoparticles containing Ga to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains Ga. When a ligand is coordinated to semiconductor nanoparticles containing Te to obtain a semiconductor nanoparticle composite, the metal element of the organic acid metal salt used preferably contains Te. Further, for example, when the semiconductor nanoparticles have a core-shell structure, the metal element of the organic acid metal salt used is preferably a component constituting the shell. The same applies to the combination of the semiconductor nanoparticles having a core-shell structure used in the first mixing step and the organic acid metal salt used in the mixing step for the additional reaction raw material described later. For example, when the core / shell of the semiconductor nanoparticles having a core-shell structure used in the first mixing step has a structure such as InP / ZnSe, InP / ZnS, InP / ZnSe / ZnS, CdSe / ZnSe, CdSe / ZnSe / ZnS, ZnSe / ZnS, or ZnTeSe / ZnS, the metal element of the organic acid metal salt used preferably contains Zn.

[0044] The mixing amount of the organic acid metal salt mixed in the first mixing step is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.1 or more, in terms of molar ratio relative to the ligand mixed in the first mixing step. When the mixing amount of the organic acid metal salt mixed in the first mixing step is within the above range, a semiconductor nanoparticle composite with higher weather resistance can be obtained. In addition, the upper limit of the mixing amount of the organic acid metal salt mixed in the first mixing step is not particularly limited, but depending on the application of the semiconductor nanoparticle composite, it is necessary to remove excess organic acid metal salt, so the mixing amount of the organic acid metal salt mixed in the first mixing step is preferably 1000 or less, more preferably 800 or less, in terms of molar ratio to the ligand mixed in the first mixing step.

[0045] Examples of the method for preparing the first reaction raw material mixture in the first mixing step include a method of preparing a non-aqueous first reaction raw material mixture by mixing semiconductor nanoparticles, a ligand, and an organic acid metal salt in a non-aqueous dispersion medium such as a non-polar organic solvent such as aliphatic hydrocarbons and aromatic hydrocarbons, or a polar organic solvent such as alcohols, ketones, esters, and ethers, and a method of preparing an aqueous first reaction raw material mixture by mixing semiconductor nanoparticles, a ligand, and an organic acid metal salt in an aqueous dispersion medium such as water or a mixed system of water and a water-soluble organic solvent.

[0046] Although the mechanism is not clear, it is considered that by mixing the semiconductor nanoparticles, the ligand, and the organic acid metal salt, and reacting the obtained first reaction raw material mixture in the first reaction step, the organic acid metal salt promotes the coordination of the ligand to the surface of the semiconductor nanoparticles, whereby a semiconductor nanoparticle composite with high fluorescence quantum efficiency and high weather resistance can be obtained.

[0047] The first reaction step is a step of reacting the first reaction raw material mixture obtained by performing the first mixing step to obtain a first reaction product. That is, in the first reaction step, the semiconductor nanoparticles, the ligand, and the organic acid metal salt are reacted.

[0048] In the first reaction step, it is preferable to heat the first reaction raw material mixture as a method for reacting it. The heating temperature (reaction temperature) of the first reaction raw material mixture is preferably 50°C or higher and 200°C or lower, more preferably 60°C or higher and 180°C or lower, and even more preferably 100°C or higher and 150°C or lower. By heating the first reaction raw material mixture (reaction temperature) within the above range, the ligand is mixed with the semiconductor nanoparticles and organic acid metal salt in a stable state, and the reactivity of the semiconductor nanoparticles, ligand and organic acid metal salt is further enhanced, making it possible to obtain a semiconductor nanoparticle composite with higher weather resistance. Conventional ligand exchange has avoided actively heating, but in the present invention, by performing it under heating conditions, it is possible to effectively exchange ligands without impairing the properties.

[0049] In the first reaction step, the first reaction raw material mixture is reacted, preferably with stirring. Any known stirring method is acceptable. Furthermore, heating and stirring the first reaction raw material mixture in the first reaction step can further enhance the reactivity of the semiconductor nanoparticles, ligands, and organic acid metal salts. Since semiconductor nanoparticles may be deactivated by oxygen in the atmosphere, it is preferable to heat and / or stir the first reaction raw material mixture in a low oxygen concentration environment during the first reaction step.

[0050] In the method for producing semiconductor nanoparticle composites of the present invention, the first reactant obtained by the first reaction step can be washed, purified, separated, etc., as appropriate to obtain a semiconductor nanoparticle composite as the target product.

[0051] Furthermore, in the method for producing the semiconductor nanoparticle composite of the present invention, after the first reaction step, additional mixing and reaction steps may be performed using the first reactant obtained in the first reaction step.

[0052] Even at the stage where the reactant is obtained by the first reaction step described above, a semiconductor nanoparticle composite in which the ligand is coordinated to the surface of the semiconductor nanoparticle can be obtained. However, by performing additional mixing and reaction steps, the final semiconductor nanoparticle composite can have higher weather resistance.

[0053] In other words, the present invention provides a method for producing a semiconductor nanoparticle composite, which includes, after the first reaction step, a mixing step for additional reaction raw materials to obtain a mixture of raw materials for an additional reaction containing the first reactant, a ligand, and an organic acid metal salt, and a reaction step to react the mixture of raw materials for the additional reaction to obtain a reactant (hereinafter also referred to as Method A). Here, if the mixture of raw materials for the additional reaction is aqueous, that is, if an aqueous dispersion medium is used as the dispersion medium, the organic acid metal salt in the mixture of raw materials for the additional reaction may be contained in a state in which part or all consists of an organic acid anion and a metal cation. This Method A for producing a semiconductor nanoparticle composite of the present invention is a method in which the mixing step for additional reaction raw materials and the reaction step are performed once after the first reaction step.

[0054] Furthermore, as a method for producing the semiconductor nanoparticle composite of the present invention, there is a form (hereinafter also referred to as form B) in which, after performing the first reaction step, a mixing step for additional reaction raw materials is performed to obtain a mixture of raw materials for an additional reaction containing the reactant obtained in the previous reaction step, a ligand, and an organic acid metal salt, and a reaction step is performed to react the mixture of raw materials for the additional reaction to obtain a reactant, and this process is repeated two or more times.Here, if the mixture of raw materials for the additional reaction is aqueous, that is, if an aqueous dispersion medium is used as the dispersion medium, the organic acid metal salt in the mixture of raw materials for the additional reaction may be contained in a state in which part or all consists of an organic acid anion and a metal cation.Form B of the method for producing the semiconductor nanoparticle composite of the present invention is a form in which, after performing the first reaction step, the mixing step for additional reaction raw materials and the reaction step are repeated two or more times.

[0055] In embodiments A and B of the present invention for the method of producing semiconductor nanoparticle composites, a step of purifying the reactants can be included between the preceding reaction step and the step of mixing additional reaction raw materials to prepare a mixture of raw materials for the additional reaction. For example, after the reaction step to obtain the reactants, purification can be performed to extract the phase containing the semiconductor nanoparticle composite, and then the ligand and organic acid metal salt can be added again to the phase containing the semiconductor nanoparticle composite to prepare a mixture of additional reaction raw materials. The purification method is not particularly limited, and known purification methods such as centrifugation or purification methods using filters can be used as appropriate.

[0056] The additional reaction raw material mixing step is a step in which a mixture of additional reaction raw materials is obtained, which includes the reactant obtained in the previous reaction step (or, in the case of the additional reaction raw material mixing step performed immediately after the first reaction step, the first reactant obtained in the first reaction step), a ligand, and an organic acid metal salt.

[0057] In the additional reaction raw material mixing step, the additional reaction raw material mixture is a mixture in which the reactants from the previous reaction step (or, in the case of the additional reaction raw material mixing step performed immediately after the first reaction step, the first reactants obtained from the first reaction step), a ligand, and an organic acid metal salt are dispersed or dissolved in a dispersion medium. Examples of dispersion media used in the additional reaction raw material mixing step include non-aqueous dispersion media such as non-polar organic solvents such as aliphatic hydrocarbons and aromatic hydrocarbons, polar organic solvents such as alcohols, ketones, esters, and ethers, and aqueous dispersion media such as water and a mixture of water and water-soluble organic solvents. In this invention, the statement that the raw material mixture for the additional reaction contains the reactants from the previous reaction step (or, in the case of a mixing step of additional reaction raw materials performed immediately after the first reaction step, the first reactants obtained from the first reaction step), a ligand, and an organic acid metal salt means that in the raw material mixture for the additional reaction, the reactants from the previous reaction step (or, in the case of a mixing step of additional reaction raw materials performed immediately after the first reaction step, the first reactants obtained from the first reaction step), a ligand, and an organic acid metal salt are dispersed or dissolved in the dispersion medium.

[0058] The ligand and organic acid metal salt used in the mixing step of the additional reaction raw materials are the same as those used in the first mixing step.

[0059] In the mixing step of additional reaction raw materials, the organic acid metal salt included in the mixture of additional reaction raw materials may be excess organic acid metal salt remaining in the system after obtaining the reactant in the previous reaction step, or it may be a newly mixed organic acid metal salt. When a ligand is newly mixed in the mixing step of additional reaction raw materials, the amount of ligand mixed is appropriately selected according to the coordination amount of the ligand to be newly mixed. When a ligand and an organic acid metal salt are newly mixed in the mixing step of additional reaction raw materials, the amount of newly added organic acid metal salt mixed is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.1 or more in molar ratio with respect to the newly mixed ligand. By having the amount of organic acid metal salt newly mixed in the mixing step of additional reaction raw materials within the above range, a semiconductor nanoparticle composite with higher weather resistance can be obtained. Furthermore, when a ligand and an organic acid metal salt are newly mixed in the additional reaction material mixing step, there is no particular upper limit to the amount of organic acid metal salt mixed in the additional reaction material mixing step. However, depending on the application of the semiconductor nanoparticle composite, it may be necessary to remove excess organic acid metal salt. Therefore, the amount of organic acid metal salt newly mixed in the additional reaction material mixing step is preferably 1000 or less, and more preferably 800 or less, in terms of molar ratio to the newly mixed ligand.

[0060] In the mixing step for additional reaction materials, the organic acid metal salt newly mixed may be the same organic acid metal salt as the one mixed in the first mixing step, or it may be a different organic acid metal salt. Furthermore, if the mixing step for additional reaction materials is performed multiple times, the organic acid metal salt newly mixed in each additional reaction material mixing step may be the same organic acid metal salt, or it may be a different organic acid metal salt.

[0061] In the mixing step of the additional reaction raw materials, the ligand included in the mixture of raw materials for the additional reaction may be excess ligand remaining in the system after obtaining the reactant in the previous reaction step, or it may be newly mixed ligand. There is no particular lower limit to the amount of ligand mixed in the mixing step of the additional reaction raw materials, but it is preferably 0.0001 or more, more preferably 0.0005 or more, and even more preferably 0.001 or more, in mass ratio with respect to the semiconductor nanoparticles mixed in the first mixing step. By having the amount of ligand mixed in the mixing step of the additional reaction raw materials within the above range, the fluorescence quantum efficiency and weather resistance of the semiconductor nanoparticles can be improved. Furthermore, there is no particular upper limit to the amount of ligand mixed in the mixing step of the additional reaction raw materials, but it is preferably 1000 or less, more preferably 900 or less, and even more preferably 800 or less, in mass ratio with respect to the semiconductor nanoparticles mixed in the first mixing step. By having the amount of ligand mixed in the mixing step of the additional reaction raw materials within the above range, it is possible to simplify the process when removing excess ligand.

[0062] In the mixing step of additional reaction materials, the ligand newly mixed may be the same ligand as the ligand mixed in the first mixing step, or it may be a different ligand. Furthermore, if the mixing step of additional reaction materials is performed multiple times, the ligand newly mixed in each additional reaction material mixing step may be the same ligand or it may be a different ligand.

[0063] The reaction step for reacting the raw material mixture for the additional reaction is a step in which the raw material mixture for the additional reaction obtained by the mixing step of the additional reaction raw materials is reacted to obtain the reactant. In other words, in the reaction step for reacting the raw material mixture for the additional reaction, the reactant obtained from the previous reaction step (or the first reactant obtained from the first reaction step if it is a reaction step performed immediately after the first reaction step), the ligand, and the organic acid metal salt are reacted.

[0064] In the reaction step of reacting the raw material mixture for the additional reaction, it is preferable to heat the raw material mixture for the additional reaction. The heating temperature (reaction temperature) of the raw material mixture for the additional reaction is preferably 50°C or higher and 200°C or lower, more preferably 80°C or higher and 180°C or lower, and even more preferably 100°C or higher and 150°C or lower. By heating the raw material mixture for the additional reaction within the above range, the ligand is mixed with the semiconductor nanoparticles and organic acid metal salt in a stable state, and the reactivity of the semiconductor nanoparticles, ligand and organic acid metal salt is further enhanced, resulting in a semiconductor nanoparticle composite with higher weather resistance.

[0065] In the reaction step in which the raw material mixture for the additional reaction is reacted, it is preferable to stir the raw material mixture for the additional reaction. Any known method of stirring is acceptable. Furthermore, in the reaction step in which the raw material mixture for the additional reaction is reacted, the reactivity of the semiconductor nanoparticles, ligands, and organic acid metal salts can be further enhanced by heating and stirring the raw material mixture for the additional reaction. Since semiconductor nanoparticles may be deactivated by oxygen in the atmosphere, it is preferable to heat and / or stir the raw material mixture for the additional reaction in an environment with a low oxygen concentration during the reaction step in which the raw material mixture for the additional reaction is reacted.

[0066] In the method for producing semiconductor nanoparticle composites of the present invention, a final reaction step is performed in which a mixture of raw materials for an additional reaction is reacted, and the resulting reaction product can be washed, purified, separated, etc. as appropriate to obtain a semiconductor nanoparticle composite as the target product.

[0067] In the semiconductor nanoparticle composite manufacturing method of the present invention, ligands can be strongly coordinated to the surface of semiconductor nanoparticles. Therefore, the semiconductor nanoparticle composite manufacturing method of the present invention can produce semiconductor nanoparticle composites with high fluorescence quantum efficiency and high weather resistance.

[0068] In the semiconductor nanoparticle composite obtained by the semiconductor nanoparticle composite manufacturing method of the present invention, the amount of ligand coordinated to the semiconductor nanoparticles is appropriately adjusted by the amount of ligand mixed in the first mixing step, and, if an additional reaction material mixing step is performed, by the amount of ligand mixed in the first mixing step and the mixing step of all additional reaction materials. In the semiconductor nanoparticle composite manufacturing method of the present invention, by adjusting the total amount of ligand mixed, it is also possible to coordinate ligand to the semiconductor nanoparticles in an amount of 30.0% by mass or less in terms of mass ratio to the semiconductor nanoparticle composite. When the mass ratio of ligand to the obtained semiconductor nanoparticle composite is 30.0% by mass or less, it is possible to promote greater absorption of blue light by the semiconductor nanoparticles and increase the external quantum efficiency. Furthermore, by having a mass ratio of ligand to the semiconductor nanoparticle composite of 30.0% by mass or less, the content of semiconductor nanoparticles in products such as ink compositions and films can be increased when the semiconductor nanoparticles are applied to products such as ink compositions and films. In the method for producing semiconductor nanoparticle composites of the present invention, from the viewpoint of improving the weather resistance of the semiconductor nanoparticle composites, the total amount of ligand to be mixed is adjusted so that the amount of ligand coordinating to the semiconductor nanoparticle composite is preferably 1.0% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, in terms of mass ratio to the semiconductor nanoparticle composites. Conventionally, methods have been used to improve the weather resistance of semiconductor nanoparticle composites by increasing the amount of ligand coordination or by coordinating ligands with large molecular weights. However, by using the method for producing semiconductor nanoparticle composites of the present invention, it is possible to obtain semiconductor nanoparticle composites with high weather resistance even when relatively small molecular weight ligands are used and the amount of ligand coordination is small.

[0069] In the semiconductor nanoparticle composite obtained by the method for producing the semiconductor nanoparticle composite of the present invention, the mass ratio of ligand to the semiconductor nanoparticle composite is measured by thermogravimetric analysis (TG). When performing thermogravimetric analysis, dry powder of the semiconductor nanoparticle composite is used. Dry powder of the semiconductor nanoparticle composite is prepared and heated in a nitrogen atmosphere from room temperature to 10°C / min, and thermogravimetric analysis (DTA-TG) is performed. Then, from the thermogravimetric analysis results obtained by the thermogravimetric analysis, the mass ratio of ligand to the semiconductor nanoparticle composite is determined by the following formula from the mass of the semiconductor nanoparticle composite at a heating temperature of 100°C (y1) and the mass of the semiconductor nanoparticle composite when the mass loss rate per 10°C becomes less than 0.1% (y2). Mass ratio of ligand to semiconductor nanoparticle composite (%) = ((y1 - y2) / y1) × 100 In the present invention, the mass ratio of ligand to the semiconductor nanoparticle composite obtained using thermogravimetric analysis (DTA-TG) is used as an indicator of the coordination amount of the ligand.

[0070] When measuring the mass ratio of ligands to semiconductor nanoparticle composites, the semiconductor nanoparticle composites are first added to a poor solvent to precipitate, then centrifuged, redispersed in the solvent, dried, and measured from the dry powder state. This pretreatment removes excess ligands that are not coordinated to the semiconductor nanoparticles, allowing for accurate measurement of the mass ratio of ligands to the semiconductor nanoparticle composites. In this invention, all ligands were desorbed from the semiconductor nanoparticle composites upon heating up to 600°C, so the measurement temperature range was set from room temperature (25°C) to 600°C. However, it is preferable to adjust the maximum measurement temperature depending on the type of ligand coordinated to the semiconductor nanoparticle composites.

[0071] In this application, the retention rate of fluorescence quantum efficiency in heat and humidity resistance tests is used as an indicator of the weather resistance of the semiconductor nanoparticle composite. The higher the retention rate of fluorescence quantum efficiency in the heat and humidity resistance tests, the better the weather resistance. Specifically, the semiconductor nanoparticle composite is dispersed in chloroform at a weight percent concentration to form a chloroform dispersion, and the resulting dispersion is kept in a constant temperature and humidity chamber at 60°C and 90% relative humidity for a certain period of time (100 hours in this application). The retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test is evaluated by the retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test. The retention rate of fluorescence quantum efficiency before and after the heat and humidity resistance test is calculated using the fluorescence quantum efficiency before the heat and humidity resistance test (QYa) and the fluorescence quantum efficiency after the heat and humidity resistance test (QYb) using the following formula (1): Weather resistance (retention rate of fluorescence quantum efficiency) (%) = (QYb / QYa) × 100 (1)

[0072] The fluorescence quantum efficiency of the semiconductor nanoparticle composite obtained by the semiconductor nanoparticle composite manufacturing method of the present invention in heat resistance and humidity resistance tests is 80% or more, preferably 90% or more, and more preferably 92% or more.

[0073] The full width at half maximum (FWHM) of the emission spectrum of the semiconductor nanoparticle composite obtained by the method for producing the semiconductor nanoparticle composite of the present invention is preferably 40 nm or less, and more preferably 35 nm or less. Having the FWHM of the emission spectrum within this range allows the semiconductor nanoparticle composite to emit light with high color purity when applied to displays or the like.

[0074] The fluorescence quantum efficiency (QY) of the semiconductor nanoparticle composite obtained by the semiconductor nanoparticle composite manufacturing method of the present invention is preferably 88% or higher, and more preferably 90% or higher. A fluorescence quantum efficiency within this range allows for efficient color conversion in response to absorbed light. While conventional ligand exchange methods for manufacturing semiconductor nanoparticle composites have resulted in low fluorescence quantum efficiency, the semiconductor nanoparticle composite obtained by the present invention exhibits a high fluorescence quantum efficiency.

[0075] In this invention, the full width at half maximum (FWHM) and fluorescence quantum efficiency of the semiconductor nanoparticle composite can be measured using a quantum efficiency measurement system. An emission spectrum is obtained by irradiating a dispersion of semiconductor nanoparticles in a dispersion medium with excitation light. From the emission spectrum obtained here, the peak wavelength (λmax), fluorescence quantum efficiency (QY), and FWHM are calculated from the re-excitation corrected emission spectrum, which excludes the re-excitation fluorescence emission spectrum of the nanoparticles that have been re-excited and emitted fluorescence. Examples of dispersion mediums include n-hexane, octadecene, toluene, acetone, and PGMEA (propylene glycol monomethyl ether acetate). The excitation light used for measurement is a single light of 450 nm, and the dispersion is prepared by adjusting the concentration of semiconductor nanoparticles so that the absorption rate is 20-30%.

[0076] The semiconductor nanoparticle composite obtained by the method for producing the semiconductor nanoparticle composite of the present invention can be applied to a wide range of uses. Depending on the application, it can be used in the form of a dispersion liquid dispersed in a dispersion medium, an ink composition mixed with monomers or prepolymers, or an optical film dispersed within a film.

[0077] Furthermore, the configurations, methods, procedures, and processes described herein are illustrative and do not limit the present invention; numerous variations are applicable within the scope of the present invention.

[0078] The present invention will be described below based on specific experimental examples, but the present invention is not limited to these.

[0079] [Preparation of Precursors and Ligands] <Preparation of Precursors> 40 mmol of zinc oleate and 75 mL of octadecene were mixed and heated under vacuum at 110°C for 1 hour to prepare a Zn precursor solution with [Zn] = 0.4 M. 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain selenized trioctylphosphine with [Se] = 2.2 M. 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain sulfurized trioctylphosphine with [S] = 2.2 M. <Preparation of Ligands> Preparation method for PEG-SH (number average molecular weight 430) 210 g of methoxyPEG-OH (number average molecular weight 400) and 93 g of triethylamine were placed in a flask and dissolved in 420 mL of THF (tetrahydrofuran). The solution was cooled to 0°C, and 51 g of methanesulfonic acid chloride was gradually added dropwise under a nitrogen atmosphere, taking care to ensure that the temperature of the reaction solution did not exceed 5°C due to the heat of reaction. The reaction solution was then raised to room temperature and stirred for 2 hours. This solution was extracted with a chloroform-aqueous system, and the organic phase was recovered. The obtained solution was dried over magnesium sulfate, and after removing the magnesium sulfate by filtration, the filtrate was concentrated by evaporation to obtain an oily intermediate. This was transferred to another flask, and 400 mL of 1.3 M aqueous thiourea solution was added under a nitrogen atmosphere. The solution was refluxed for 2 hours, then 21 g of NaOH was added, and refluxing continued for another 1.5 hours. The reaction solution was cooled to room temperature, and neutralized by adding 1 M aqueous HCl solution until the pH reached 7. The obtained solution was extracted with a chloroform-aqueous system to obtain the target ligand (PEG-SH, number average molecular weight 430).

[0080] <Preparation of Semiconductor Nanoparticles> <Production of Semiconductor Nanoparticles (Green)> Indium acetate (0.28 mmol) and zinc oleate (0.56 mmol) were added to a mixture of oleic acid (0.8 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated to 120°C under vacuum (<20 Pa) and reacted for 1 hour. The mixture reacted under vacuum (<20 Pa) was brought to 25°C under a nitrogen atmosphere, tris(trimethylsilyl)phosphine (0.23 mmol) was added, and the mixture was heated to 270°C and reacted for 8 minutes. The reaction solution was then cooled to 25°C, octanoic acid chloride (0.50 mmol) was injected, and the mixture was heated to 230°C and reacted for 25 minutes, after which it was cooled to 25°C to obtain a core particle dispersion solution. The core particle dispersion solution was heated to 250°C. At 250°C, 6.0 mL of Zn precursor solution and 2.0 mL of selenite trioctylphosphine were added and reacted for 30 minutes to form ZnSe shells on the surface of InP-based semiconductor nanoparticles. Furthermore, 4.0 mL of Zn precursor solution and 1.8 mL of sulfide trioctylphosphine were added, and the temperature was raised to 280°C for 1 hour to form ZnS shells. The reaction solution was then added to acetone, mixed thoroughly, and centrifuged at a centrifugal acceleration of 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This procedure was repeated several times to obtain purified semiconductor nanoparticles.

[0081] <Production of Semiconductor Nanoparticles (Red)> Indium acetate (0.3 mmol) and zinc oleate (0.05 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated to 120°C under vacuum (<20 Pa) and reacted for 1 hour. The mixture reacted under vacuum (<20 Pa) was brought to 25°C under a nitrogen atmosphere, tris(trimethylsilyl)phosphine (0.15 mmol) was added, and the mixture was heated to 300°C and reacted for 10 minutes. The reaction mixture was then cooled to 25°C, octanoic acid chloride (0.60 mmol) was injected, and the mixture was heated to 240°C and reacted for 30 minutes, after which it was cooled to 25°C to obtain a core particle dispersion solution. The core particle dispersion solution was heated to 250°C. At 250°C, 4.3 mL of Zn precursor solution and 1.5 mL of selenite trioctylphosphine were added and reacted for 30 minutes to form ZnSe shells on the surface of InP-based semiconductor nanoparticles. Furthermore, 3.8 mL of Zn precursor solution and 0.5 mL of sulfide trioctylphosphine were added, and the temperature was raised to 280°C and reacted for 1 hour to form ZnS shells. The reaction solution of the obtained semiconductor nanoparticles was added to acetone, mixed well, and then centrifuged. The centrifugal acceleration was set to 4000 G. The precipitate was collected, and n-hexane was added to the precipitate to prepare a dispersion. This operation was repeated several times to obtain purified semiconductor nanoparticles.

[0082] [Example 1] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of this dispersion was placed in the flask, and 1.02 g of dodecanethiol (Sigma-Aldrich, DDT) and 0.09 g of zinc acetate were added to prepare the mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing the reactants was recovered. 5.0 mL of n-hexane was added to the obtained reaction phase to make a dispersion, and then 50 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain a semiconductor nanoparticle composite.

[0083] [Example 2] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that zinc acetate was replaced with 0.31 g of zinc oleate.

[0084] [Example 3] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that zinc acetate was replaced with 0.18 g of zinc octanoate.

[0085] [Example 4] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that zinc acetate was replaced with 0.32 g of zinc stearate.

[0086] [Example 5] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that zinc acetate was replaced with 0.23 g of zinc neodecanoate.

[0087] [Example 6] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that zinc acetate was replaced with 0.18 g of zinc 2-ethylhexanoate.

[0088] [Comparative Example 1] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, without adding zinc acetate.

[0089] [Example 7] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion was prepared. 10.0 g of the prepared 1-octadecene dispersion was placed in a flask, and 2.15 g of PEG-SH and 0.09 g of zinc acetate were added to prepare a mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing the reactants was recovered. 5.0 mL of acetone was added to the obtained reaction phase to make a dispersion, and then 50 mL of n-hexane was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain a semiconductor nanoparticle composite.

[0090] [Example 8] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that zinc acetate was replaced with 0.31 g of zinc oleate.

[0091] [Example 9] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that zinc acetate was replaced with 0.18 g of zinc octanoate.

[0092] [Example 10] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that zinc acetate was replaced with 0.32 g of zinc stearate.

[0093] [Example 11] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that zinc acetate was replaced with 0.20 g of zinc neodecanoate.

[0094] [Example 12] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that zinc acetate was replaced with 0.18 g of zinc 2-ethylhexanoate.

[0095] [Comparative Example 2] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, without adding zinc acetate.

[0096] [Example 13] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the amount of zinc octanoate was 0.90 g.

[0097] [Example 14] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the amount of zinc octanoate was 1.8 g.

[0098] [Example 15] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the amount of zinc octanoate was 0.90 g.

[0099] [Example 16] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the amount of zinc octanoate was 1.8 g.

[0100] [Example 17] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the reaction temperature of the mixture was changed to 50°C.

[0101] [Comparative Example 3] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the reaction temperature of the mixture was changed to 25°C.

[0102] [Example 18] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the reaction temperature of the mixture was changed to 50°C.

[0103] [Comparative Example 4] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the reaction temperature of the mixture was changed to 25°C.

[0104] [Example 19] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion was prepared. 10.0 g of the prepared 1-octadecene dispersion was placed in a flask, and 1.01 g of dodecanethiol (Sigma-Aldrich) and 0.18 g of zinc octanoate were added to prepare a mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing reactant 1 was recovered. Hexane was added to the phase containing reactant 1, and the mixture was placed back into the flask. 1.01 g of dodecanethiol and 0.18 g of zinc octanoate were added to prepare an additional mixture. The additional mixture was stirred and reacted under a nitrogen atmosphere at 110°C for 60 minutes, then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 2. 5.0 mL of n-hexane was added to the obtained reactant 2 phase to form a dispersion, and then 50 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain a semiconductor nanoparticle composite.

[0105] [Example 20] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion was prepared. 10.0 g of the prepared 1-octadecene dispersion was placed in a flask, and 1.01 g of dodecanethiol (Sigma-Aldrich) and 0.18 g of zinc octanoate were added to prepare a mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing reactant 1 was recovered. Hexane was added to the phase containing reactant 1, and the mixture was placed back into the flask. 1.01 g of dodecanethiol and 0.18 g of zinc octanoate were added to prepare an additional mixture. The additional mixture was stirred and reacted under a nitrogen atmosphere at 110°C for 60 minutes, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 2. Hexane was added again to the phase containing reactant 2, and the mixture was placed in a flask. 1.01 g of dodecanethiol and 0.18 g of zinc octanoate were added to prepare the additional mixture. The additional mixture was stirred and reacted under a nitrogen atmosphere at 110°C for 60 minutes, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 3. 5.0 mL of n-hexane was added to the resulting reactant 3 phase to form a dispersion, and then 50 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain the semiconductor nanoparticle composite.

[0106] [Example 21] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion was prepared. 10.0 g of the prepared 1-octadecene dispersion was placed in a flask, and 2.15 g of PEG-SH and 0.18 g of zinc octanoate were added to prepare a mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing reactant 1 was recovered. PGMEA (polypropylene glycol monomethyl ether acetate) was added to the phase containing reactant 1, and the mixture was placed back into the flask. An additional mixture was prepared by adding 2.15 g of PEG-SH and 0.18 g of zinc octanoate. The additional mixture was stirred and reacted under a nitrogen atmosphere at 110°C for 60 minutes, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 2. 5.0 mL of acetone was added to the obtained reactant 2 phase to form a dispersion, and then 50 mL of n-hexane was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain a semiconductor nanoparticle composite.

[0107] [Example 22] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. A 1-octadecene dispersion was prepared. 10.0 g of the prepared 1-octadecene dispersion was placed in a flask, and 2.15 g of PEG-SH and 0.18 g of zinc octanoate were added to prepare a mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing reactant 1 was recovered. PGMEA was added to the phase containing reactant 1, and the mixture was placed back into the flask. 2.15 g of PEG-SH and 0.18 g of zinc octanoate were added to prepare an additional mixture. The additional mixture was stirred and reacted at 110°C for 60 minutes under a nitrogen atmosphere, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 2. PGMEA was added again to the phase containing reactant 2, and the mixture was placed in a flask. 2.15 g of PEG-SH and 0.18 g of zinc octanoate were added to prepare the additional mixture. The additional mixture was stirred and reacted at 110°C for 60 minutes under a nitrogen atmosphere, and then cooled to 25°C. The cooled dispersion was transferred to a centrifuge tube, and the resulting dispersion was centrifuged at 4000 G for 20 minutes to recover the phase containing reactant 3. 5.0 mL of acetone was added to the obtained reactant 3 phase to make a dispersion, and then 50 mL of n-hexane was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain the semiconductor nanoparticle composite.

[0108] [Example 23] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 19, except that zinc acetate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0109] [Example 24] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 20, except that zinc acetate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0110] [Example 25] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 21, except that zinc acetate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0111] [Example 26] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 22, except that zinc acetate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0112] [Example 27] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0113] [Example 28] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 19, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0114] [Example 29] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 20, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0115] [Example 30] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0116] [Example 31] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 21, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0117] [Example 32] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 22, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0118] [Example 33] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 1, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0119] [Example 34] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 23, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0120] [Example 35] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 24, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0121] [Example 36] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 7, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0122] [Example 37] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 25, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0123] [Example 38] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 26, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0124] [Example 39] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 3, except that the amount of zinc octanoate was 9.00 g.

[0125] [Example 40] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 9, except that the amount of zinc octanoate was 9.00 g.

[0126] [Example 41] Semiconductor nanoparticles (red) were dispersed in 1-octadecene in a flask at a mass ratio of 10% by mass. 10.0 g of the dispersion was placed in the flask, and 2.00 g of PEG-COOH and 0.09 g of zinc acetate were added to prepare the mixture. The mixture was stirred at 100°C for 60 minutes under a nitrogen atmosphere to allow it to react, and then cooled to 25°C. The reaction product was transferred to a centrifuge tube and centrifuged at 4000 G for 20 minutes, separating it into a clear 1-octadecene phase and a phase containing the reactants. The 1-octadecene phase was removed, and the phase containing the reactants was recovered. 5.0 mL of n-hexane was added to the obtained reaction phase to make a dispersion, and then 50 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the clear supernatant was removed to obtain a semiconductor nanoparticle composite.

[0127] [Example 42] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 41, except that zinc acetate was replaced with 0.23 g of zinc neodecanoate.

[0128] [Comparative Example 5] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 41, without adding zinc acetate.

[0129] [Example 43] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 41, except that PEG-COOH was replaced with 0.89 g of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0130] [Example 44] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 43, except that zinc acetate was replaced with 0.23 g of zinc neodecanoate.

[0131] [Comparative Example 6] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 41, without adding zinc acetate.

[0132] [Example 45] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 42, except that the amount of zinc neodecanoate was changed to 1.15 g.

[0133] [Example 46] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 42, except that the amount of zinc neodecanoate was changed to 2.3 g.

[0134] [Example 47] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 42, except that the amount of zinc neodecanoate was changed to 11.5 g.

[0135] [Example 48] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 44, except that the amount of zinc neodecanoate was changed to 1.15 g.

[0136] [Example 49] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 44, except that the amount of zinc neodecanoate was changed to 2.3 g.

[0137] [Example 50] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 44, except that the amount of zinc neodecanoate was changed to 11.5 g.

[0138] [Example 51] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 42, except that the reaction temperature of the mixture was changed to 50°C.

[0139] [Example 52] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 44, except that the reaction temperature of the mixture was changed to 50°C.

[0140] [Example 53] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 19, except that 2.00 g of PEG-COOH was used instead of dodecanethiol when preparing the mixture and the additional mixture, and 0.20 g of zinc neodecanoate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0141] [Example 54] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 19, except that 2.00 g of PEG-COOH was used instead of dodecanethiol when preparing the mixture and the additional mixture, and 0.20 g of zinc neodecanoate was used instead of zinc octanoate when preparing the mixture and the additional mixture.

[0142] [Example 55] A semiconductor nanoparticle composite was obtained in the same manner as in Example 53, except that 0.89 g of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid was used instead of PEG-COOH during the preparation of the mixture and the additional mixture.

[0143] [Example 56] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 54, except that 0.89 g of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid was used instead of PEG-COOH during the preparation of the mixture and the additional mixture.

[0144] [Example 57] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 44, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0145] [Example 58] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 55, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0146] [Example 59] A semiconductor nanoparticle composite was obtained using the same procedure as in Example 56, except that the semiconductor nanoparticles used were changed to semiconductor nanoparticles (green).

[0147] <Method for Characterization> (Optical Properties) The optical properties of the semiconductor nanoparticle composite were measured using a fluorescence quantum efficiency measurement system (Otsuka Electronics, QE-2100). The obtained semiconductor nanoparticle composite was dispersed in toluene to form a dispersion, and the concentration of the dispersion was adjusted so that the absorption rate of 450 nm light was 20-30%. The obtained dispersion was irradiated with a single 450 nm light (excitation light) to obtain an emission spectrum. From the emission spectrum obtained here, the peak wavelength (λmax), fluorescence quantum efficiency (QY), and full width at half maximum (FWHM) were calculated from the re-excitation corrected emission spectrum, which excludes the re-excitation fluorescence emission spectrum of the portion that was re-excited and emitted fluorescence.

[0148] (Weathering Test) After measuring the fluorescence quantum efficiency (QYa) before the weathering test, the semiconductor nanoparticle composite was placed in a constant temperature and humidity chamber (ESPEC Corporation: PHP-2J) set to 60°C and 90% relative humidity and held for 100 hours. After that, the fluorescence quantum efficiency (QYb) of the removed nanoparticle composite was measured again. The weathering resistance of the semiconductor nanoparticle composite was calculated using the fluorescence quantum efficiency (QYa) before the weathering test and the fluorescence quantum efficiency (QYb) after the weathering test using the following formula (1): Weathering resistance (retention rate of fluorescence quantum efficiency) (%) = (QYb / QYa) × 100 (1)

[0149] The weather resistance results of the semiconductor nanoparticle composites of Examples 1 to 59 and Comparative Examples 1 to 6 are shown in Tables 1 to 4.

[0150]

[0151]

[0152]

[0153]

[0154]

[0155]

[0156]

[0157]

[0158] In the table, A-COOH represents 2-[2-(2-methoxyethoxy)ethoxy]acetic acid.

[0159] Tables 1 and 5 show the effect on weather resistance depending on the presence or absence of organic acid metal salts used in preparing the first reaction raw material mixture, and the type of organic acid metal salt used. When organic acid metal salts were used in preparing the first reaction raw material mixture, the resulting semiconductor nanoparticle composite showed a higher fluorescence quantum efficiency of 88% or more and a weather resistance of 90% or more compared to when organic acid metal salts were not used.

[0160] Tables 2 and 6 show the effect of the amount of organic acid metal salt used in preparing the first reaction raw material mixture on weather resistance. When the amount of organic acid metal salt relative to the ligand was 0.1 or higher in molar ratio, the semiconductor nanoparticles showed high weather resistance.

[0161] Tables 3 and 7 show the effect of heating temperature (reaction temperature) on the weather resistance of the first reaction raw material mixture. The first reaction raw material mixture showed a weather resistance of 88.0% or higher at heating temperatures (reaction temperatures) of 50°C or higher, and a weather resistance of over 90.0% at 100°C.

[0162] Tables 4 and 8 show the effect of the number of repetitions of the mixing and reaction processes on weather resistance. Increasing the number of repetitions of the mixing and reaction processes improved weather resistance. In particular, a significant difference of more than 2% in weather resistance was observed between cases where the mixture preparation and reaction were performed once and cases where they were performed two or more times.

Claims

1. A method for producing a semiconductor nanoparticle composite in which a ligand is coordinated to semiconductor nanoparticles, comprising: a first mixing step of mixing semiconductor nanoparticles, a ligand, and an organic acid metal salt to obtain a first reaction material mixture; and a first reaction step of reacting the first reaction material mixture to obtain a first reactant.

2. The method for producing a semiconductor nanoparticle composite according to claim 1, wherein the organic acid metal salt is a metal salt of a carboxylic acid.

3. The method for producing a semiconductor nanoparticle composite according to claim 2, wherein the carboxylic acid is a saturated aliphatic carboxylic acid.

4. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 3, wherein the metal element constituting the organic acid metal salt includes one or more of Zn, Cd, Ag, In, Ga, and Te.

5. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 4, wherein in the first reaction step, the first reaction raw material mixture is heated to 50°C or higher to cause a reaction.

6. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 5, wherein the molar ratio of the organic acid metal salt to the ligand is 0.01 or more.

7. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 6, comprising: a mixing step for additional reaction raw materials to obtain a mixture of raw materials for an additional reaction containing the first reactant, a ligand, and an organic acid metal salt after performing the first reaction step; and a reaction step to react the mixture of raw materials for the additional reaction to obtain a reactant.

8. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 6, wherein, after performing the first reaction step, a mixing step for additional reaction raw materials is performed to obtain a mixture of raw materials for an additional reaction containing the reactant obtained in the previous reaction step, a ligand, and an organic acid metal salt, and a reaction step is performed to react the mixture of raw materials for the additional reaction to obtain a reactant, and these steps are repeated two or more times.

9. A method for producing a semiconductor nanoparticle composite according to any one of claims 1 to 8, wherein the ligand has an organic group and a coordinating group, and the coordinating group includes at least one of a thiol group, a carboxyl group, an amino group, a phosphine group, a phosphone group, and a phosphine oxide group.