Zirconia powder, zirconia sintered body, and method for producing zirconia sintered body
A zirconia powder formulation with controlled Li content, pore distribution, and particle size allows for efficient production of high-density zirconia sintered bodies at lower temperatures and shorter times, addressing inefficiencies in existing methods.
Patent Information
- Application Number
- PCT/JP2026/017113
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing zirconia sintered bodies require high sintering temperatures and prolonged holding times, leading to inefficiencies in production and increased energy consumption.
A zirconia powder formulation containing a specific range of Li compound content, pore distribution, and particle size, allowing for sintering at lower temperatures and shorter times, with a controlled specific surface area and stabilizer content to achieve high relative density and strength.
The solution enables the production of zirconia sintered bodies with high relative density and strength at reduced sintering temperatures and times, improving production efficiency and reducing energy consumption.
Smart Images

Figure JP2026017113_12112026_PF_FP_ABST
Abstract
Description
Zirconia powder, zirconia sintered body, and method for manufacturing a zirconia sintered body
[0001] This invention relates to zirconia powder, zirconia sintered bodies, and methods for producing zirconia sintered bodies.
[0002] It has been known that the sintering temperature can be lowered by adding a sintering aid (e.g., alumina) to zirconia.
[0003] Patent Document 1 discloses zirconia powder containing 0.1 to 1 wt% crystalline lithium aluminosilicate as a sintering aid (Claim 1). Patent Document 1 also discloses that the relative density of zirconia powder reaches 99.7% by holding it at 1100°C for 10 hours (Paragraph
[0021] ).
[0004] Japanese Patent Publication No. 2015-093813
[0005] Patent Document 1 describes how a sintered body with a high relative density of 99.7% can be obtained at a low temperature of 1100°C. However, as mentioned above, it is necessary to hold the body at 1100°C for a long period of 10 hours, which is not optimal in terms of production efficiency or energy consumption during production.
[0006] The present invention has been made in view of the above-mentioned problems, and its object is to provide a zirconia powder that can produce a zirconia sintered body having high relative density at a low sintering temperature and in a short sintering time. It also aims to provide a zirconia sintered body obtained by sintering the zirconia powder. Furthermore, it aims to provide a method for producing a zirconia sintered body using the zirconia powder.
[0007] The inventors of this invention conducted extensive research on zirconia powder. As a result, they discovered that by adopting the following configuration, it is possible to obtain a zirconia sintered body with high relative density at a low sintering temperature and in a short sintering time, thus completing the present invention.
[0008] The present invention provides the following: [1] A material comprising zirconia and a Li compound containing Li, wherein the content of the Li compound is such that, when the zirconia powder is considered as a whole, Li 2Zirconia powder characterized by having an O content of 0.050% to 0.200% by mass in terms of O equivalent, and in the pore distribution based on the mercury intrusion method, having a peak top diameter of 35 nm to 80 nm in the range of 10 nm to 200 nm, and a pore volume of 0.20 ml / g to 0.50 ml / g.
[0009] According to the above configuration, the content of the Li compound is Li 2 Because it contains 0.050% by mass or more and 0.200% by mass or less in terms of oxygen, densification is possible even at low sintering temperatures (for example, 1150°C, 1100°C, etc.).
[0010] The "range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method" is the range in which pores as primary particle gaps can exist in the zirconia powder. According to the above configuration, in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method, the peak top diameter of the pore volume distribution is 35 nm to 80 nm, and the size of each pore (each primary particle gap) is small. Therefore, each primary particle constituting the secondary particle is densely aggregated, and there are no large pores. Here, zirconia particles (including primary and secondary particles) have the characteristic that they are difficult to sinter if the pore volume is large. In other words, in order to sinter at low temperatures, it is necessary not only to reduce the size of pores originating from the primary particle gaps within the secondary particles, but also to simultaneously reduce the pore volume originating from the primary particle gaps. Therefore, in the present invention, the pore volume in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method is set to 0.20 ml / g to 0.50 ml / g. As a result, the pore volume derived from the primary particle gaps is small, and there are no large pores, making it possible to obtain a sintered body with high sintering density even at low sintering temperatures.
[0011] In particular, in the above configuration, the Li compound is Li 2Contained in a range of 0.050 mass% or more and 0.200 mass% or more in terms of O, and by setting the pore distribution to the specific state described above, the sintering temperature can be lowered and the sintering time can be shortened. Although the reason is not clear, the present inventors infer that, by adjusting the peak top diameter to 35 nm or more and 80 nm or less and the pore volume to 0.20 ml / g or more and 0.50 ml / g or less in the pore size distribution (10 to 200 nm) of the zirconia powder, the liquid phase of the Li compound remains in the pores during the sintering step, and segregation and elution are suppressed. That is, it is inferred that even if the sintering time is shortened by increasing the temperature rising rate up to the sintering temperature or shortening the holding time at the sintering temperature, sintering proceeds uniformly within the molded body, and a sintered body with high sintered density can be obtained.
[0012] As described above, according to the above configuration, the Li compound is converted to Li 2 Contained in a range of 0.050 mass% or more and 0.200 mass% or less in terms of O, and by setting the pore distribution to a specific state, the sintering temperature can be lowered and the sintering time can be shortened.
[0013] Furthermore, the present invention provides the following. [2] The zirconia powder according to the above [1], wherein the specific surface area is 20 m 2 / g or more and 40 m 2 / g or less.
[0014] When the specific surface area is more than 20 m 2 / g and 40 m 2 / g or less, the low-temperature sinterability is more excellent. This point will be explained below. In order to sinter zirconia powder at a temperature as low as about 1050°C to 1150°C, which is lower than conventional temperatures, increasing the specific surface area is effective. However, conventionally, it is difficult to control the grain growth rate during the production of zirconia powder, and in order to prevent pores from remaining as much as possible in the zirconia powder, it has been considered preferable to set the specific surface area to 20 m 2 / g or less. On the other hand, according to the present invention, since the gaps between primary particles are controlled, a large number of pores do not remain in the zirconia powder even when the specific surface area is more than 20 m 2 / g. Therefore, even when the specific surface area is more than 20 m 2By exceeding the weight per gram, low-temperature sinterability can be further improved. Furthermore, the specific surface area is 20 m². 2 / g over 40m 2 If the concentration is below / g, segregation of Li can be further suppressed.
[0015] Furthermore, the present invention provides the following: [3] Particle size D 50 The zirconia powder according to [1] or [2], characterized in that the particle size is 0.1 μm or more and 0.6 μm or less.
[0016] Particle size D 50 When the particle size is 0.6 μm or less, the particle size of the secondary particles is relatively small, which allows for a smaller gap between secondary particles. As a result, it exhibits superior low-temperature sinterability. Furthermore, because the gap between secondary particles is small, a sintered body with a higher sintering density can be obtained.
[0017] Furthermore, the present invention provides the following: [4] The zirconia comprises a stabilizer, the stabilizer being Y 2 O 3 , CEO 2 , Sc 2 O 3 , CaO, Er 2 O 3 , and Yb 2 O 3 The zirconia powder according to any one of [1] to [3] above, characterized in that it is one or more selected from the group consisting of the above.
[0018] Y as a stabilizer 2 O 3 , CEO 2 , Sc 2 O 3 , CaO, Er 2 O 3 , and Yb 2 O 3 Including one or more selected from the group makes it possible to obtain a zirconia sintered body with higher strength. In this specification, high strength refers to a large value of flexural strength (three-point bending strength).
[0019] Furthermore, the present invention provides the following: [5] The zirconia powder according to [4], characterized in that the content of the stabilizer is 1.5 mol% or more and 15 mol% or less when the total amount of zirconia and stabilizer is considered.
[0020] When the content of the stabilizer is 1.5 mol% or more and 15 mol% or less, it becomes possible to obtain a zirconia sintered body with higher strength.
[0021] Furthermore, the present invention provides the following: [6] A zirconia body comprising a Li compound containing Li, wherein the content of the Li compound is such that, when the zirconia sintered body is as a whole, 2 A zirconia sintered body characterized by having an O content of 0.050% by mass or more and 0.200% by mass or less, and a relative density of 98.5% or more.
[0022] Li compounds volatilize at high temperatures. Furthermore, the amount of volatilization increases when exposed to high temperatures for a long period of time. According to the above configuration, Li compounds are Li 2 Since it contains 0.050% by mass or more and 0.200% by mass or less in terms of oxygen, it can be said that it was sintered in a short time and at a low temperature (sintered at 1150°C or below). Furthermore, since the relative density is 98.5% or more, it can be said to have a high relative density. In other words, according to the above configuration, it can be said that it is a zirconia sintered body with a high relative density that was sintered at a low sintering temperature and in a short time.
[0023] Furthermore, the present invention provides the following: [7] The zirconia sintered body according to [6], characterized in that the zirconia does not contain a stabilizer, or the total amount of zirconia and stabilizer is less than 1.5 mol%.
[0024] Normally, zirconia without a stabilizer undergoes a phase transition accompanied by volume change at temperatures above 1150°C, leading to cracking and other damage. Therefore, conventionally, zirconia without a stabilizer cannot be sintered at temperatures above 1150°C. On the other hand, even if conventional zirconia without a stabilizer is attempted to be sintered at temperatures below 1150°C, it is not possible to obtain a sintered body with high relative density due to the low sintering temperature. However, as explained in the section on zirconia sintered bodies described in [6], the zirconia sintered body described in [7] is a zirconia sintered body sintered at a low sintering temperature (for example, below 1150°C), and therefore, even if it does not contain a stabilizer, or if the total amount of zirconia and stabilizer is less than 1.5 mol%, cracking and other damage are suppressed. In other words, the zirconia sintered body is a zirconia sintered body in which cracking and other damage are suppressed, even though it does not contain a stabilizer, or if the total amount of zirconia and stabilizer is less than 1.5 mol%. Such a zirconia sintered body can be said to be novel.
[0025] Furthermore, the present invention provides the following: [8] A method for producing a zirconia sintered body, comprising: step X of molding zirconia powder according to any one of [1] to [5] above to obtain a molded body; and step Y of sintering the molded body after step X under the following <sintering conditions>. <Sintering conditions> (a) Heating from room temperature to sintering temperature takes no more than 40 minutes. (b) Sintering temperature is 1050°C or higher and 1150°C or lower. (c) Holding time after reaching the sintering temperature is 1 minute or more.
[0026] According to the above configuration, since the zirconia powder described in any one of [1] to [5] above is used, a zirconia sintered body with high relative density can be obtained even when sintered under the above <sintering conditions>. In particular, because the sintering temperature is low, between 1050°C and 1150°C, it becomes possible to co-sinter stabilizers, pigments, etc., which could not be used under conventional sintering conditions (e.g., above 1150°C) due to heat resistance. Furthermore, since the heating time from room temperature to the sintering temperature is within 40 minutes, and the time from room temperature to the sintering temperature is shortened compared to conventional methods, production efficiency is high and energy consumption during production can be reduced.
[0027] Furthermore, the present invention provides the following: [9] A method for producing a zirconia sintered body according to [8], characterized in that the holding time is 30 minutes or less.
[0028] If the holding time is 30 minutes or less, the holding time after reaching the sintering temperature is shortened compared to conventional methods, resulting in higher production efficiency and a greater reduction in energy consumption during production.
[0029] According to the present invention, it is possible to provide a zirconia powder that can be used to obtain a zirconia sintered body having high relative density at a low sintering temperature and in a short sintering time. Furthermore, it is possible to provide a zirconia sintered body obtained by sintering the zirconia powder. Furthermore, it is possible to provide a method for manufacturing a zirconia sintered body using the zirconia powder.
[0030] This is a schematic diagram illustrating the method for producing zirconia powder according to this embodiment. This shows the pore distribution of the zirconia powder of Example 1. This shows the pore distribution of the zirconia powder of Example 2. This shows the pore distribution of the zirconia powder of Comparative Example 3.
[0031] Embodiments of the present invention will be described below. However, the present invention is not limited to these embodiments. In this specification, zirconia (zirconium oxide) is a general term and includes impurity metal compounds, including hafnia, in an amount of 10% by mass or less. In this specification, the expressions "contains" and "includes" include the concepts of "contains," "includes," "substantially consists of," and "consists only of."
[0032] The maximum and minimum values of the content of each component shown below are, independently of the content of other components, the preferred minimum and preferred maximum values of the present invention. Similarly, the maximum and minimum values of the various parameters (measured values, etc.) shown below are, independently of the content (composition) of each component, the preferred minimum and preferred maximum values of the present invention.
[0033] [Zirconia Powder] The zirconia powder according to this embodiment comprises zirconia and a Li compound containing Li, wherein the content of the Li compound is such that, when the zirconia powder is considered as a whole, Li 2 The O equivalent is within the range of 0.050% to 0.200% by mass, and in the pore distribution based on the mercury intrusion method, the peak top diameter of the pore volume distribution is between 35 nm and 80 nm in the range of 10 nm to 200 nm, and the pore volume is between 0.20 ml / g and 0.50 ml / g.
[0034] The zirconia powder contains zirconia. The zirconia is contained in the zirconia powder in the form of unaggregated primary particles and secondary particles formed by the aggregation of primary particles. However, the amount of primary particles that do not become secondary particles and exist in the form of unaggregated primary particles is very small, for example, less than 1% by mass of the total primary particles (the sum of unaggregated primary particles and primary particles that have aggregated into secondary particles). In other words, the zirconia may contain a very small amount of unaggregated primary particles, but the majority is in the form of secondary particles.
[0035] <Pore Distribution> 1. Peak Top Diameter of Primary Particle Gap The zirconia powder has a peak top diameter of pore volume distribution of 35 nm to 80 nm in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method.
[0036] The peak top diameter is preferably 40.0 nm or more, more preferably 45.0 nm or more. The peak top diameter is preferably 70.0 nm or less, more preferably 60.0 nm or less. The peak top diameter is preferably 40.0 nm or more and 70.0 nm or less, more preferably 45.0 nm or more and 60.0 nm or less. When multiple peaks exist in the range of 10 nm to 200 nm of the pore distribution, "the peak top diameter of the pore volume distribution is 20 nm or more and 85 nm or less" as used herein means that all peak top diameters in the range of 10 nm to 200 nm of the pore distribution are within the range of 35 nm to 80 nm.
[0037] 2. Pore volume of primary interparticle gaps The zirconia powder has a pore volume of 0.20 ml / g or more and 0.50 ml / g or less in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method.
[0038] The total pore volume is preferably 0.23 cm³. 3 / g or more, more preferably 0.25 cm 3 It is 1 / g or more. The total pore volume is preferably 0.40 cm³. 3 The amount is less than or equal to / g, more preferably 0.30 or less. The total pore volume is preferably 0.23 cm³. 3 / g or more 0.40cm 3 / g or less, more preferably 0.25 cm 3 / g or more 0.30cm 3 It is less than or equal to / g.
[0039] 3. Pore distribution width of primary particle gaps The zirconia powder has a pore distribution width of 40 nm to 105 nm in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method. The pore distribution width is preferably 43 nm or more, more preferably 46 nm or more, even more preferably 50 nm or more, and particularly preferably 55 nm or more. The pore distribution width is preferably 100 nm or less, more preferably 95 nm or less, even more preferably 90 nm or less, particularly preferably 85 nm or less, and especially preferably 80 nm or less. Here, the pore distribution width refers to the width of the peak where the log differential pore volume (see, for example, Figure 2) is 0.1 ml / g or more. Furthermore, if multiple peaks exist in the pore distribution range of 10 nm to 200 nm, the phrase "pore distribution width is 40 nm to 105 nm" as used herein means that, in a graph showing the pore distribution with the horizontal axis representing pore diameter and the vertical axis representing log differential pore volume (see, for example, Figure 2), the point where the graph first intersects with the log differential pore volume of 0.1 mL / g (the point where it intersects while rising) is defined as the minimum diameter, and the point where it intersects with the log differential pore volume of 0.1 mL / g again (the point where it intersects while descending) is defined as the maximum diameter, and the difference between the maximum and minimum diameters is 40 nm to 105 nm.
[0040] The "range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method" is the range in which pores as primary particle gaps may exist in the zirconia powder. In the zirconia powder according to this embodiment, in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method, the peak top diameter of the pore volume distribution is 35 nm to 80 nm, and the size of each pore (each primary particle gap) is small. Therefore, each primary particle constituting the secondary particle is densely aggregated, and there are no large pores. Here, zirconia particles (including primary and secondary particles) have the characteristic that they are difficult to sinter if the pore volume is large. In other words, in order to sinter at low temperatures, it is necessary not only to reduce the size of pores originating from the primary particle gaps within the secondary particles, but also to simultaneously reduce the pore volume originating from the primary particle gaps. Therefore, in the zirconia powder according to this embodiment, the pore volume in the range of 10 nm to 200 nm in the pore distribution based on the mercury intrusion method is set to 0.20 ml / g to 0.50 ml / g. As a result, the pore volume derived from the primary particle gaps is small, and there are no large pores, making it possible to obtain a sintered body with high sintering density even at low sintering temperatures.
[0041] Furthermore, in the pore distribution based on the mercury intrusion method, if the pore distribution width is between 40 nm and 105 nm within the range of 10 nm to 200 nm, the pore distribution can be said to be uniform (sharp). In this case, each primary particle constituting the secondary particle is uniformly and densely aggregated, and large pores do not exist. Therefore, if the pore distribution width is between 40 nm and 105 nm, it becomes possible to obtain a sintered body with a higher sintering density even at a lower sintering temperature.
[0042] The peak top diameter, pore volume, and pore distribution width refer to the values obtained by the method described in the examples.
[0043] <Specific Surface Area> The specific surface area of the zirconia powder is 20 m². 2 / g over 40m 2 It is preferable that the specific surface area is 20 m² or less. 2 / g over 40m 2If the amount is less than / g, it exhibits superior low-temperature sintering properties. Furthermore, if the specific surface area is 20 m², 2 / g over 40m 2 If the concentration is below / g, segregation of Li can be further suppressed.
[0044] The specific surface area is more preferably 21.0 m². 2 / g or more, more preferably 22.0m 2 It is 1 / g or more. The specific surface area is more preferably 38.0 m². 2 / g or less, more preferably 36.0m 2 It is less than or equal to / g. The specific surface area is more preferably 21.0 m². 2 / g or more 38.0m 2 / g or less, more preferably 22.0m 2 / g or more 36.0m 2 It is less than or equal to / g. The specific surface area refers to the value obtained by the method described in the examples.
[0045] <Particle size D 50 > Particle size D of the zirconia powder 50 The particle size is preferably 0.1 μm or more and 0.6 μm or less. 50 When the particle size is 0.6 μm or less, the particle size of the secondary particles is relatively small, which allows for a smaller gap between secondary particles. As a result, it exhibits superior low-temperature sinterability. Furthermore, because the gap between secondary particles is small, a sintered body with a higher sintering density can be obtained.
[0046] The particle size D 50 The particle size D is more preferably 0.15 μm or larger, and even more preferably 0.20 μm or larger. 50 The particle size D is more preferably 0.56 μm or less, and even more preferably 0.52 μm or less. 50 The particle size D is more preferably 0.15 μm or more and 0.56 μm or less, and even more preferably 0.20 μm or more and 0.52 μm or less. 50 This refers to the value obtained by the method described in the examples. Note that the particle size D 50When measuring, the measurement may include not only secondary particles but also unaggregated primary particles, however the amount of unaggregated primary particles that may be contained in the zirconia powder is very small. Therefore, the particle size D 50 This refers to the particle size D of secondary particles. 50 In other words, it can be considered to represent the average particle diameter of secondary particles.
[0047] Preferably, the relative density of the sintered product obtained by heating the zirconia powder from room temperature to 1100°C (sintering temperature) in 11 minutes and holding it for 10 minutes after reaching 1100°C (sintering temperature) is 98.5% or higher. If the relative density of the sintered product obtained by heating the zirconia powder from room temperature to 1100°C (sintering temperature) in 11 minutes and holding it for 10 minutes after reaching 1100°C (sintering temperature) is 98.5% or higher, it can be said that it is easier to obtain a zirconia sintered body with high relative density at a low sintering temperature and in a short sintering time.
[0048] The relative density is more preferably 98.7% or higher, and even more preferably 99.0% or higher. The relative density is preferably high, for example, 99.9% or less, 99.8% or less, etc. The relative density is more preferably 98.7% or higher and 99.9% or lower, and even more preferably 99.0% or higher and 99.8% or lower.
[0049] Preferably, the zirconia powder contains a stabilizer, and the amount of the stabilizer is 1.5 mol% or more when considering the total amount of zirconia and stabilizer, and the sintered product obtained by raising the temperature from room temperature to 1100°C (sintering temperature) in 11 minutes and holding it for 10 minutes after reaching 1100°C (sintering temperature) has a three-point bending strength of 400 MPa or more and 1400 MPa or less.
[0050] If the zirconia contains a stabilizer, and the content of the stabilizer is 1.5 mol% or more when the zirconia and stabilizer are combined, the three-point bending strength is more preferably 500 MPa or more, and even more preferably 600 MPa or more. If the zirconia contains a stabilizer, and the content of the stabilizer is 1.5 mol% or more when the zirconia and stabilizer are combined, the three-point bending strength is preferably higher, for example, 1200 MPa or less, 1000 MPa or less, etc. If the zirconia contains a stabilizer, and the content of the stabilizer is 1.5 mol% or more when the zirconia and stabilizer are combined, the three-point bending strength is more preferably 500 MPa or more and 1200 MPa or less, and even more preferably 600 MPa or more and 1000 MPa or less. The method for determining the three-point bending strength is by the method described in the examples.
[0051] <Composition> The zirconia powder contains zirconia. The zirconia is contained in the zirconia powder in the form of primary particles that have not aggregated and secondary particles in which the primary particles have aggregated.
[0052] The zirconia content is preferably 86.00% by mass or more, more preferably 87.00% by mass or more, when considering the total zirconia powder. The zirconia content is preferably 98.45% by mass or less, more preferably 98.40% by mass or less, when considering the total zirconia powder. The zirconia content is preferably 86.00% by mass or more, 98.45% by mass or less, when considering the total zirconia powder, more preferably 87.00% by mass or more, 98.40% by mass or less.
[0053] The zirconia may contain a stabilizer. If the zirconia contains a stabilizer, the stabilizer is included in the zirconia in a form such as solid solution.
[0054] When the zirconia contains a stabilizer, the amount of the stabilizer is preferably 1.5 mol% to 15 mol% of the total zirconia powder. When the zirconia contains a stabilizer, and the amount of the stabilizer is 1.5 mol% to 15 mol% of the total zirconia powder, it becomes possible to obtain a zirconia sintered body with higher strength.
[0055] If the zirconia contains a stabilizer, the content of the stabilizer is more preferably 1.55% by mass or more, and even more preferably 1.60% by mass or more, when considering the total zirconia powder. If the zirconia contains a stabilizer, the content of the stabilizer is more preferably 14.00% by mass or less, and even more preferably 13.00% by mass or less, when considering the total zirconia powder. If the zirconia contains a stabilizer, the content of the stabilizer is more preferably 1.55% by mass or more and 14.00% by mass or less, and even more preferably 1.60% by mass or more and 13.00% by mass or less, when considering the total zirconia powder.
[0056] The stabilizer is not particularly limited, but Y 2 O 3 , CEO 2 , Sc 2 O 3 , CaO, Er 2 O 3 , and Yb 2 O 3 It is preferable that it be one or more selected from the group consisting of the following.
[0057] The aforementioned stabilizer varies depending on the application, but from the viewpoint of cost and coloration, Y 2 O 3 , CEO 2 CaO, Yb 2 O 3 More preferable, Y 2 O 3 , CEO 2 CaO is more preferably Y 2 O 3 , CEO 2 , is particularly preferred, Y 2 O 3 That is particularly preferable.
[0058] As the stabilizer, Y 2 O 3 is used, the content of the Y 2 O 3 is preferably 1.50 mol% or more and 10.00 mol% or less, based on the total of zirconia and the stabilizer. The Y 2 O 3 content being 1.50 mol% or more and 10.00 mol% or less allows the zirconia sintered body obtained by sintering the zirconia powder to have more excellent mechanical strength.
[0059] The Y 2 O 3 content is more preferably 1.55 mol% or more, and still more preferably 1.60 mol% or more. The Y 2 O 3 content is more preferably 8.00 mol% or less, and still more preferably 6.00 mol% or less. The Y 2 O 3 content is more preferably 1.55 mol% or more and 8.00 mol% or less, and still more preferably 1.60 mol% or more and 6.00 mol% or less.
[0060] When CeO is used as the stabilizer 2 , the content of the CeO 2 is preferably 6.00 mol% or more and 15.00 mol% or less, based on the total of zirconia and the stabilizer. The CeO 2 content being 6.00 mol% or more and 15.00 mol% or less allows the zirconia sintered body obtained by sintering the zirconia powder to have more excellent mechanical strength.
[0061] The CeO 2 content is more preferably 8.00 mol% or more, and still more preferably 10.00 mol% or more. The CeO 2 content is more preferably 14.00 mol% or less, and still more preferably 13.00 mol% or less. The CeO 2The content is more preferably 8.00 mol% to 14.00 mol%, and even more preferably 10.00 mol% to 13.00 mol%.
[0062] As the stabilizing agent, Sc 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is preferably 1.50 mol% or more and 10.00 mol% or less when considering zirconia and stabilizers as a whole. 2 O 3 Er 2 O 3 Yb 2 O 3 When either of these is used, if the content is 1.50 mol% or more and 10.00 mol% or less, the zirconia sintered body obtained by sintering the zirconia powder has superior mechanical strength.
[0063] Said Sc 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is more preferably 1.55 mol% or more, and even more preferably 1.60 mol% or more. 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is more preferably 8.00 mol% or less, and even more preferably 6.00 mol% or less. 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of these, the content is more preferably 1.55 mol% to 8.00 mol%, and even more preferably 1.60 mol% to 6.00 mol%.
[0064] When CaO is used as the stabilizer, its content is preferably 2.00 mol% to 12.00 mol% when considering the total amount of zirconia and stabilizer. When the CaO content is 2.00 mol% to 12.00 mol%, the zirconia sintered body obtained by sintering the zirconia powder has superior mechanical strength.
[0065] The CaO content is more preferably 3.00 mol% or more, and even more preferably 4.00 mol% or more. The CaO content is more preferably 10.00 mol% or less, and even more preferably 8.00 mol% or less. The CaO content is more preferably 3.00 mol% or more and 10.00 mol% or less, and even more preferably 4.00 mol% or more and 8.00 mol% or less.
[0066] The zirconia described above does not need to contain a stabilizer. "Substantially free of a stabilizer" means that it does not contain a stabilizer, or that it contains less than 1.5 mol% of a stabilizer when the zirconia and stabilizer are considered as a whole. Normally, zirconia that does not contain a stabilizer (or substantially does not contain one) undergoes a phase transition accompanied by volume change at temperatures above 1150°C, resulting in cracking and other damage. Therefore, conventionally, zirconia that does not contain a stabilizer cannot be sintered at temperatures above 1150°C. On the other hand, even if conventional zirconia that does not contain a stabilizer is attempted to be sintered at temperatures below 1150°C, a sintered body with high relative density cannot be obtained due to the low sintering temperature. However, the zirconia powder described above has the pore distribution described above and, as will be described later, contains a specific amount of Li compound. Therefore, even if it does not contain a stabilizer, the resulting sintered body is less prone to cracking and other damage.
[0067] If the zirconia is substantially free of stabilizers, the content of the stabilizer is more preferably 0.80 mol% or less, and even more preferably 0.50 mol% or less.
[0068] The zirconia powder contains a Li compound containing Li. The Li compound is not particularly limited as long as it is a compound containing the element Li. Preferably, the Li compound does not contain any metal elements other than Li. Preferably, the Li compound does not contain the element Al. Examples of the Li compound include LiOH, Li 2 CO 3 , LINO 3 Li 2 O, LiCl, Li 2 SO 4 These are some examples.
[0069] The content of the Li compound is such that, when considering the zirconia powder as a whole, Li 2 The content of the Li compound is within the range of 0.050% by mass or more and 0.200% by mass or less in terms of O. 2 Because it contains 0.050% by mass or more and 0.200% by mass or less in terms of oxygen, densification is possible even at low sintering temperatures (for example, 1150°C, 1100°C, etc.).
[0070] The content of the Li compound is preferably 0.06% by mass or more, more preferably 0.08% by mass or more. The content of the Li compound is preferably 0.18% by mass or less, more preferably 0.16% by mass or less. The content of the Li compound is preferably 0.06% by mass or more and 0.18% by mass or less, more preferably 0.08% by mass or more and 0.16% by mass or less.
[0071] In particular, the zirconia powder contains Li compounds. 2 By including it in an amount of 0.050% to 0.200% by mass in terms of O, and by setting the pore distribution to the specific state described above, the sintering temperature can be lowered and the sintering time can be shortened.
[0072] The zirconia powder may contain additives. In this specification, additives refer to substances added as a mixture to zirconia (zirconia particles) and Li compounds. Examples of such additives include sintering aids other than Li compounds, colorants, etc. Some additives function only as sintering aids, some function only as colorants, and some function as both sintering aids and colorants. Sintering aids other than Li compounds and colorants will be described below.
[0073] The zirconia powder may contain sintering aids other than Li compounds in an amount of 0.005% by mass or more and 2% by mass or less. Examples of sintering aids other than Li compounds include oxides of aluminum, iron, germanium, cobalt, chromium, and zinc. Including sintering aids other than Li compounds within the above numerical range allows them to function as sintering aids, resulting in superior low-temperature sintering performance. Furthermore, the zirconia powder may contain sintering aids other than Li compounds in an amount of less than 0.005% by mass.
[0074] Furthermore, the zirconia powder may be configured as a sintering agent that does not contain any sintering aids other than the Li compound.
[0075] The zirconia powder has a peak top diameter of 35 nm to 80 nm and a pore volume of 0.20 ml / g to 0.50 ml / g in the pore distribution range of 10 nm to 200 nm based on the mercury intrusion method, and therefore can be sintered at low temperatures. For this reason, low-temperature sintering is possible even if the composition does not include sintering aids other than the Li compound.
[0076] The zirconia powder may also contain sinterable ceramics, thermosetting resins, and other materials in addition to the sintering aids other than the Li compound, for the purpose of improving properties such as strength.
[0077] The zirconia powder may contain one or more elements selected from the group consisting of Fe, V, Mn, Co, Cr, Tb, Zn, Cu, and Ti. Including one or more elements selected from the group consisting of Fe, V, Mn, Co, Cr, Tb, Zn, Cu, and Ti as coloring elements allows for suitable coloring of the zirconia sintered body obtained by sintering the zirconia powder.
[0078] The form of the coloring element is not particularly limited and can be added in the form of oxides, chlorides, etc. Specific examples of colorants containing the coloring element include Fe 2 O 3 , V 2 O 5 MnO 2 CoO, Cr 2 O 3 , Tb 4 O 7 , ZnO, CuO, TiO 2 Examples include the above. Preferably, the coloring agent is added to the zirconia powder as a mixture.
[0079] Fe as the coloring agent 2 O 3 When the coloring agent is included, the content of the coloring agent is preferably 0.005% by mass or more and 1% by mass or less, and more preferably 0.05% by mass or more and 1.0% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0080] V as the aforementioned coloring agent 2 O 5 When the coloring agent is included, the amount is preferably 0.005% by mass or more and 0.1% by mass or less, and more preferably 0.01% by mass or more and 0.05% by mass or less, when the total amount of zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0081] As the coloring agent, MnO 2When the coloring agent is included, the amount is preferably 0.005% by mass or more and 2% by mass or less, and more preferably 0.03% by mass or more and 1.1% by mass or less, when the total amount of zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0082] As the aforementioned coloring agent, Cr 2 O 3 When the coloring agent is included, the amount is preferably 0.005% by mass or more and 2% by mass or less, and more preferably 0.1% by mass or more and 1.5% by mass or less, when the total amount of zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0083] When the coloring agent contains CoO, the content of the coloring agent is preferably 0.005% by mass or more and 2% by mass or less, and more preferably 0.01% by mass or more and 1.5% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended coloring is easily obtained. In other words, the color tone can be easily adjusted.
[0084] As the coloring agent, Tb 4 O 7 When the coloring agent is included, the content of the coloring agent is preferably 0.005% by mass or more and 5% by mass or less, and more preferably 0.1% by mass or more and 3% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0085] When the coloring agent contains ZnO, the content of the coloring agent is preferably 0.005% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 0.5% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended coloring is easily obtained. In other words, the color tone can be easily adjusted.
[0086] When CuO is included as the coloring agent, the content of the coloring agent is preferably 0.005% by mass or more and 1% by mass or less, more preferably 0.05% by mass or more and 0.6% by mass or less, and even more preferably 0.1% by mass or more and 0.3% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended coloring is easily obtained. In other words, the color tone can be easily adjusted.
[0087] As the coloring agent, TiO 2 When the coloring agent is included, the content of the coloring agent is preferably 0.005% by mass or more and 2% by mass or less, and more preferably 0.01% by mass or more and 1% by mass or less, when the total zirconia powder is considered to be 100% by mass. When the content of the coloring agent is 0.005% by mass or more, the intended color is easily obtained. In other words, the color tone can be easily adjusted.
[0088] The zirconia powder according to this embodiment has been described above.
[0089] [Method for Manufacturing Zirconia Powder] An example of a method for manufacturing zirconia powder is described below. However, the method for manufacturing zirconia powder is not limited to the example below.
[0090] The method for producing zirconia powder according to this embodiment includes: Step 1: Heating a zirconium salt solution and a sulfated chloride solution separately to 95°C or higher and 100°C or lower; Step 2: Contacting the heated zirconium salt solution and the heated sulfated chloride solution so that the concentration of the mixture does not change from the start to the end of contact, thereby obtaining a reaction solution containing basic zirconium sulfate as a mixture; Step 3: Aging the reaction solution containing basic zirconium sulfate obtained in Step 2 at 95°C or higher for 3 hours or more; Step 4: Adding a stabilizer to the aged reaction solution containing basic zirconium sulfate obtained in Step 3; Step 5: Adding alkali to the reaction solution containing basic zirconium sulfate obtained in Step 4 to obtain a zirconium-containing hydroxide; Step 6: Heat treating the zirconium-containing hydroxide obtained in Step 5 to obtain powder (zirconia); and Step 7: Mixing the powder obtained in Step 6 with a Li compound, wherein in Step 2, from the start to the end of contact, SO4 in the mixture is...4 2- / ZrO 2 Maintain the weight ratio within the range of 0.3 to 0.8, and maintain the temperature of the mixture at 95°C or higher. The process will be explained in detail below.
[0091] <Step 1> In Step 1, the starting materials, a zirconium salt solution and a sulfated chlorine solution, are heated separately to a temperature of 95°C to 100°C. The zirconium salt used to prepare the zirconium salt solution can be any salt that supplies zirconium ions, such as zirconium oxynitrate, zirconium oxychloride, zirconium nitrate, etc. One or more of these can be used. Among these, zirconium oxychloride is preferred because it offers high productivity on an industrial scale.
[0092] The solvent used to prepare the zirconium salt solution can be selected according to the type of zirconium salt, etc. Water (pure water, deionized water, etc.) is generally preferred.
[0093] The concentration of the zirconium salt solution is not particularly limited, but generally it is zirconium oxide (ZrO) per 1000 g of solvent. 2 It is preferable that the amount contained is 5 to 250 g in terms of conversion, and more preferably 20 to 150 g.
[0094] Any sulfated agent that reacts with zirconium ions to produce sulfates (i.e., a sulfated reagent) can be used, and examples include sodium sulfate, potassium sulfate, ammonium sulfate, potassium bisulfate, sodium bisulfate, potassium disulfate, sodium disulfate, and sulfur trioxide. The sulfated agent may be in powder or solution form, but a solution (especially an aqueous solution) is preferred. As for the solvent, the same solvent used to prepare the zirconium salt solution can be used.
[0095] The acid concentration of the zirconium salt solution is preferably 0.1 to 2.0 N. By setting the acid concentration within this range, the aggregation state of the particles constituting the zirconia powder can be controlled to a suitable state. The acid concentration can be adjusted, for example, by using hydrochloric acid, nitric acid, sodium hydroxide, etc.
[0096] The concentration of the sulfated chloride (the sulfated chloride solution) is not particularly limited, but it is generally preferable to use 5 to 250 g of sulfated chloride per 1000 g of solvent, and more preferably 20 to 150 g.
[0097] The material of the containers used to prepare the zirconium salt solution and the sulfated chloride solution is not particularly limited, as long as they have a capacity to sufficiently stir each of the solutions. However, it is preferable to have equipment that can appropriately heat each solution so that its temperature does not fall below 95°C. The heating temperature of the zirconium salt solution and the sulfated chloride solution should be between 95°C and 100°C, and preferably 97°C or higher. If step 2 is carried out while the temperature of the zirconium salt solution and the sulfated chloride solution is below 95°C, the zirconium salt solution and the sulfated chloride will not react sufficiently, and the yield will decrease.
[0098] <Step 2> In Step 2, the heated zirconium salt solution and the heated sulfated chloride solution are brought into contact so that the concentration of the mixture does not change from the start to the end of contact, thereby obtaining a reaction solution containing basic zirconium sulfate as a mixture. Here, from the start to the end of contact, the SO in the mixture 4 2- / ZrO 2 Maintain the weight ratio within the range of 0.3 to 0.8, and maintain the temperature of the mixture at 95°C or higher. Step 2 will now be explained with reference to the drawings.
[0099] Figure 1 is a schematic diagram illustrating the method for producing zirconia powder according to this embodiment. As shown in Figure 1, container 10 is connected to one upper end (left side in Figure 1) of the T-tube 20 via valve 12. Container 30 is connected to the other upper end (right side in Figure 1) of the T-tube 20 via valve 32. Container 10 stores a zirconium solution heated to 95°C or higher and 100°C or lower. Container 30 stores a sulfated chloride solution heated to 95°C or higher and 100°C or lower. In step 2, the zirconium solution and the sulfated chloride solution are brought into contact by opening valve 12 and valve 32. The resulting mixture (basic zirconium sulfate-containing reaction solution) flows immediately into the aging container 40 from the bottom of the T-tube 20. In step 2, this method ensures that the concentration of the reaction solution (concentration of the reaction solution in the T-tube 20) does not change from the start to the end of contact between the zirconium solution and the sulfated chloride solution. In step 2, SO4 is used from the start to the end of contact. 4 2- / ZrO 2 Because the concentration change is suppressed, a uniform reactant can be obtained. By employing such a process (step 2), the peak top diameter, pore volume, and pore distribution width of the primary particles can be controlled. In other words, the size of the pores originating from the interparticle gaps within the secondary particles can be made smaller and the distribution sharper, and furthermore, the pore volume originating from the interparticle gaps can also be made smaller. SO in the mixed liquid in step 2 4 2- / ZrO 2 The weight ratio is preferably in the range of 0.3 to 0.8, more preferably 0.4 to 0.7, and even more preferably 0.45 to 0.65. 4 2- / ZrO 2 By setting the weight ratio to 0.3 or higher, the yield of the reaction product, basic zirconium sulfate, can be increased. Also, the SO in the mixture 4 2- / ZrO 2By setting the weight ratio to 0.8 or less, the formation of soluble zirconium sulfate salts can be suppressed, and the decrease in the yield of basic zirconium sulfate can be suppressed. In step 2, it is preferable to install heaters in the piping (for example, the T-joint 20) that supplies each solution in order to maintain the temperature of the mixed solution at 95°C or higher.
[0100] The following is a detailed explanation of an example of step 2. As the T-tube 20, a T-tube with a diameter L1 of 10 mm at one upper end (left side in Figure 1), a diameter L2 of 10 mm at the other upper end (right side in Figure 1), and a diameter L3 of 15 mm at the bottom is used, and 213 g of 25% by mass sodium sulfate aqueous solution and ZrO 2 When contacting 450 g of a 16% by mass aqueous solution of zirconium oxychloride, the time from the start of contact to the end of contact (until the zirconium chloride aqueous solution in container 10 and the sulfated chloride solution in container 30 are gone) (contact time) is preferably 30 to 300 seconds, more preferably 60 to 200 seconds, and even more preferably 90 to 150 seconds.
[0101] <Step 3> In Step 3, the reaction solution containing basic zirconium sulfate obtained in Step 2 is aged at 95°C or higher for 3 hours or more. In Step 3, for example, the reaction solution containing basic zirconium sulfate that flows into the aging container 40 is stirred with a stirrer 42 and aged at 95°C or higher for 3 hours or more. There is no particular upper limit to the aging time, but for example, it is 7 hours or less. The temperature (aging temperature) of the mixed solution (reaction solution containing basic zirconium sulfate) in Step 3 is preferably 95°C or higher, more preferably 97°C or higher and 100°C or lower. By setting the aging temperature to 95°C or higher and the aging time to 3 hours or more, sufficient basic zirconium sulfate can be produced and the yield can be increased. The above mixed solution contains basic zirconium sulfate as its main component and is a basic zirconium sulfate slurry.
[0102] <Step 4> In Step 4, a stabilizer is added to the aged basic zirconium sulfate-containing reaction solution obtained in Step 3.
[0103] <Step 5> In Step 5, an alkali is added to the reaction solution containing basic zirconium sulfate obtained in Step 4 to carry out a neutralization reaction. By neutralization, zirconium-containing hydroxide is produced. The alkali is not limited and examples include caustic soda, sodium carbonate, ammonia, hydrazine ammonium bicarbonate, etc. The concentration of the alkali is not particularly limited, but it is diluted with water and usually a concentration of 5 to 30% is used. There are two methods for adding the alkali: (1) adding the alkali solution to the reaction solution containing basic zirconium sulfate, and (2) adding the reaction solution containing basic zirconium sulfate to the alkali solution, but neither method is particularly limited and either method may be used. After neutralization, the slurry is filtered to obtain zirconium-containing hydroxide. It is preferable to remove impurities from this zirconium-containing hydroxide by washing it with pure water, etc., as needed. After washing, drying may be carried out as needed.
[0104] <Step 6> In Step 6, the zirconium-containing hydroxide obtained in Step 5 is heat-treated (calcined) to oxidize the zirconium-containing hydroxide and obtain zirconia powder. The heat treatment temperature (calcination temperature) and heat treatment time (calcination time) of the zirconium-containing hydroxide are not particularly limited, but are usually performed at around 600 to 1050°C for 1 to 10 hours. The calcination temperature is more preferably 650°C to 1000°C, and even more preferably 700°C to 980°C. The calcination time is more preferably 2 to 6 hours, and even more preferably 2 to 4 hours. By setting the heat treatment temperature to 600°C to 1000°C, the specific surface area of the obtained zirconia powder can be set to a suitable range. Also, by setting the heat treatment temperature to 600°C to 1050°C, the pore distribution of the obtained zirconia powder can be set to a suitable range. The heat treatment atmosphere is not particularly limited, but is usually in the air or an oxidizing atmosphere.
[0105] <Step 7> In Step 6, the powder obtained in Step 6 is mixed with the Li compound. This yields zirconia powder.
[0106] <Step 8> After Step 7, the obtained zirconia powder may be pulverized to form a slurry if necessary. In this case, a binder may be added to improve moldability. If slurrying is not performed (pulverization is not performed), the binder and zirconia powder may be uniformly mixed in a kneader. An organic binder is preferred as the binder. An organic binder is easily removed from the molded body in a heating furnace with an oxidizing atmosphere, and a degreased body can be obtained, so that impurities are less likely to remain in the sintered body in the end. Examples of the organic binder include those that dissolve in alcohol, or those that dissolve in a mixture of two or more selected from the group consisting of alcohol, water, aliphatic ketones, and aromatic hydrocarbons. Examples of the organic binder include at least one selected from the group consisting of polyethylene glycol, glycol fatty acid ester, glycerin fatty acid ester, polyvinyl butyral, polyvinyl methyl ether, polyvinyl ethyl ether, and vinyl propionate. The organic binder may further contain one or more thermoplastic resins that are insoluble in alcohol or the above mixture. After adding the organic binder, the desired zirconia powder can be obtained by drying, grinding, and other processes using known methods. The particle size D of the zirconia powder is obtained by grinding in step 8. 50 This allows for control of the particle size D of the zirconia powder obtained in step 5. For example, grinding is performed according to the state of the zirconia powder obtained in step 5. 50 This can be controlled to a range of 0.1 μm to 0.6 μm.
[0107] When adding colorants, etc., zirconia powder containing the colorants can be obtained by adding and mixing them after step 6. A more detailed method of mixing is to disperse the colorants in pure water or the like to form a slurry and then wet mix them. Also, when performing step 8, the colorants may be added at the time of step 8. For example, when mixing the powder and the Li compound in step 7, the colorants may be mixed at the same time.
[0108] The zirconia powder according to this embodiment has been described above.
[0109] [Zirconia Sintered Body] An example of a zirconia sintered body according to this embodiment will be described below. However, the zirconia sintered body of the present invention is not limited to the following examples.
[0110] The zirconia sintered body according to this embodiment comprises zirconia and a Li compound containing Li, wherein the content of the Li compound, when considering the zirconia sintered body as a whole, is 2 The oxygen content is within the range of 0.050% by mass or more and 0.200% by mass or less, and the relative density is 98.5% or higher.
[0111] <Composition> The zirconia sintered body according to this embodiment contains zirconia.
[0112] The zirconia content of the zirconia sintered body is preferably 86.00% by mass or more, more preferably 87.00% by mass or more. The zirconia content of the zirconia sintered body is preferably 98.45% by mass or less, more preferably 98.40% by mass or less. The zirconia content of the zirconia sintered body is preferably 86.00% by mass or more and 98.45% by mass or less, more preferably 87.00% by mass or more and 98.40% by mass or less.
[0113] The zirconia may contain a stabilizer.
[0114] If the zirconia contains a stabilizer, the amount of the stabilizer is preferably 1.5 mol% to 15 mol% of the zirconia sintered body as a whole. When the zirconia contains a stabilizer, if the amount of the stabilizer is 1.5 mol% to 15 mol% of the zirconia sintered body as a whole, a zirconia sintered body with higher strength is obtained.
[0115] If the zirconia contains a stabilizer, the content of the stabilizer is more preferably 1.55% by mass or more, and even more preferably 1.60% by mass or more, when considering the entire zirconia sintered body. If the zirconia contains a stabilizer, the content of the stabilizer is 14.00% by mass or less, and even more preferably 13.00% by mass or less, when considering the entire zirconia sintered body. If the zirconia contains a stabilizer, the content of the stabilizer is more preferably 1.55% by mass or more and 14.00% by mass or less, and even more preferably 1.60% by mass or more and 13.00% by mass or less, when considering the entire zirconia sintered body.
[0116] The stabilizer is not particularly limited, but Y 2 O 3 , CEO 2 , Sc 2 O 3 , CaO, Er 2 O 3 , and Yb 2 O 3 It is preferable that it be one or more selected from the group consisting of the following.
[0117] The aforementioned stabilizer varies depending on the application, but from the viewpoint of cost and coloration, Y 2 O 3 , CEO 2 CaO, Yb 2 O 3 More preferable, Y 2 O 3 , CEO 2 CaO is more preferably Y 2 O 3 CaO is particularly preferred, Y 2 O 3 That is particularly preferable.
[0118] Y as the aforementioned stabilizer 2 O 3 When using the above Y 2 O 3 The content of is preferably 1.50 mol% or more and 10.00 mol% or less when considering zirconia and stabilizers as a whole. 2 O 3When the content is between 1.50 mol% and 10.00 mol%, the mechanical strength is superior.
[0119] The aforementioned Y 2 O 3 The content of is more preferably 1.55 mol% or more, and even more preferably 1.60 mol% or more. 2 O 3 The content of is more preferably 8.00 mol% or less, and even more preferably 6.00 mol% or less. 2 O 3 The content is more preferably 1.55 mol% to 8.00 mol%, and even more preferably 1.60% to 6.00 mol%.
[0120] As the stabilizing agent, CeO 2 When using the CeO 2 The content of is preferably 6.00 mol% to 15.00 mol% when considering zirconia and stabilizers as a whole. 2 When the content is between 6.00 mol% and 15.00 mol%, the mechanical strength is superior.
[0121] The aforementioned Co 2 The content of is more preferably 8.00 mol% or more, and even more preferably 10.00 mol% or more. 2 The content of is more preferably 14.00 mol% or less, and even more preferably 13.00 mol% or less. 2 The content is more preferably 8.00 mol% to 14.00 mol%, and even more preferably 10.00 mol% to 13.00 mol%.
[0122] As the stabilizing agent, Sc 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is preferably 1.50 mol% or more and 10.00 mol% or less when considering zirconia and stabilizers as a whole. 2 O 3Er 2 O 3 Yb 2 O 3 When using either of these, a content of 1.50 mol% to 10.00 mol% results in superior mechanical strength.
[0123] Said Sc 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is more preferably 1.55 mol% or more, and even more preferably 1.60 mol% or more. 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of the above, the content is more preferably 8.00 mol% or less, and even more preferably 6.00 mol% or less. 2 O 3 Er 2 O 3 Yb 2 O 3 When using either of these, the content is more preferably 1.55 mol% to 8.00 mol%, and even more preferably 1.60 mol% to 6.00 mol%.
[0124] When CaO is used as the stabilizer, its content is preferably 2.00 mol% to 12.00 mol% when considering the total amount of zirconia and the stabilizer. A CaO content of 2.00 mol% to 12.00 mol% results in superior mechanical strength.
[0125] The CaO content is more preferably 3.00 mol% or more, and even more preferably 4.00 mol% or more. The CaO content is more preferably 10.00 mol% or less, and even more preferably 8.00 mol% or less. The CaO content is more preferably 3.00 mol% or more and 10.00 mol% or less, and even more preferably 4.00 mol% or more and 8.00 mol% or less.
[0126] The zirconia described above does not need to contain a stabilizer substantially. "Substantially free of a stabilizer" means that it does not contain a stabilizer, or that it contains less than 1.5 mol% of a stabilizer when the zirconia and stabilizer are considered as a whole. Normally, zirconia that does not contain a stabilizer (substantially free) undergoes a phase transition accompanied by volume change at temperatures above 1150°C, resulting in cracking and other damage. Therefore, conventionally, zirconia that does not contain a stabilizer cannot be sintered at temperatures above 1150°C. On the other hand, even if conventional zirconia that does not contain a stabilizer is attempted to be sintered at temperatures below 1150°C, it is not possible to obtain a sintered body with high relative density due to the low sintering temperature. However, as will be described later, the zirconia sintered body described above is a zirconia sintered body sintered at a low sintering temperature (for example, below 1150°C), so even if it does not contain a stabilizer substantially, the occurrence of cracking and other damage is suppressed.
[0127] If the zirconia is substantially free of stabilizers, the content of the stabilizer is more preferably 0.80 mol% or less, and even more preferably 0.50 mol% or less.
[0128] The zirconia sintered body contains a Li compound containing Li. The Li compound is not particularly limited as long as it is a compound containing the element Li. Preferably, the Li compound does not contain any metal elements other than Li. Preferably, the Li compound does not contain the element Al. Examples of the Li compound include LiOH, Li 2 Co 3 , LINO 3 Li 2 O, LiCl, Li 2 SO 4 These are some examples.
[0129] The content of the Li compound is such that, when considering the zirconia sintered body as a whole, Li 2 The amount is in the range of 0.050% by mass or more and 0.200% by mass or less in terms of oxygen. Li compounds volatilize at high temperatures. Furthermore, the amount of volatilization increases when exposed to high temperatures for a long time. According to the zirconia sintered body, the Li compound is Li 2Since it contains in the range of 0.050% to 0.200% by mass in terms of O, it can be said that the Li compound is not volatile. In other words, according to the zirconia sintered body, the Li compound is Li 2 Since it contains 0.050% by mass or more and 0.200% by mass or less in terms of oxygen, it can be said that it was sintered in a short time and at a low temperature (sintered at 1150°C or below).
[0130] The content of the Li compound is preferably 0.06% by mass or more, more preferably 0.08% by mass or more. The content of the Li compound is preferably 0.18% by mass or less, more preferably 0.16% by mass or less. The content of the Li compound is preferably 0.06% by mass or more and 0.18% by mass or less, more preferably 0.08% by mass or more and 0.16% by mass or less.
[0131] The content of the Li compound (Li 2 The value (in O equivalent) is obtained by crushing the zirconia sintered body with a hammer to form a powder, and then performing a compositional analysis (ICP measurement) on the resulting powder.
[0132] The zirconia sintered body may contain additives. The same additives as those described in the section on zirconia powder may be used.
[0133] <Relative Sintering Density (Relative Density)> The zirconia sintered body has a relative sintering density (relative density) of 98.5% or higher. Since the relative sintering density is 98.5% or higher, it can be said to have a high relative density. In other words, the zirconia sintered body can be said to be a high relative density zirconia sintered body that is sintered at a low sintering temperature and in a short time.
[0134] The relative density is preferably 98.7% or higher, and more preferably 99.0% or higher. The relative density is preferably high, for example, 99.9% or lower, 99.8% or lower, etc. The relative density is preferably 98.7% or higher and 99.9% or lower, and more preferably 99.0% or higher and 99.8% or lower.
[0135] <Method for measuring the relative sintering density of a zirconia sintered body> The relative sintering density refers to the relative sintering density expressed by the following formula (1). Relative sintering density (%) = (sintering density / theoretical sintering density) × 100 ... (1) Here, the theoretical sintering density (ρ 0 ρz is the value calculated by the following formula (2-1): ρ0 = 100 / [(Y / 3.987) + (Z / 2.013) + (100 - Y - Z) / ρz] ... (2-1) However, ρz is the value calculated by the following formula (2-2): ρz = [124.25(100 - X) + [molecular weight of stabilizer] × X] / [150.5(100 + X)A] 2 C]...(2-2) Here, the molecular weight of the stabilizer is Y 2 O 3 In this case, 225.81, Er 2 O 3 In this case, 382.52, Yb 2 O 3 In this case, use 394.11. Also, X, Y, and Z are the stabilizer concentration (mol%), Al 2 O 3 (Weight %) and Li 2 O (weight %). Also, A and C are values calculated by the following formulas (2-3) and (2-4), respectively. A = 0.5080 + 0.06980X / (100 + X) ... (2-3) C = 0.5195 - 0.06180X / (100 + X) ... (2-4) In formula (1), the theoretical sintering density varies depending on the powder composition. For example, the theoretical sintering density of yttria-containing zirconia is 6.117 g / cm³ if the yttria content is 2 mol%. 3 If it's 3 mol%, then it's 6.098 g / cm³. 3 If it's 5.5 mol%, then it's 6.051 g / cm³. 3 (Al 2 O 3 =0% by weight, Li 2 (When O = 0% by weight) Stabilizer is Sc 2 O 3 In this case, ρz is the value calculated by the following formula (3): ρz = -0.0402 (Sc 2 O 3(Molar concentration of CaO) + 6.1294 ... (3) When the stabilizer is CaO, ρz is the value calculated by the following formula (3-1): ρz = -0.0400 (molar concentration of CaO) + 6.1700 ... (3-1) Also, the theoretical sintering density (let's call it ρ1) when a coloring agent is included is: ρ1 = 100 / [(Z / V) + (100 - Z) / ρ0] ... (2-5) Also, Z is the coloring agent concentration (weight %) and V is the theoretical density of the coloring agent (g / cm³) 3 ) The theoretical density of the colorant is Fe 2 O 3 5.24 g / cm³ 3 ZnO is 5.61 g / cm³ 3 MnO 2 5.03 g / cm³ 3 CoO is 6.10 g / cm³ 3 , Cr 2 O 3 5.22 g / cm³ 3 , TiO 2 4.23 g / cm³ 3 , Tb 4 O 7 7.80 g / cm 3 CuO is 6.31 g / cm³ 3 , V 2 O 5 3.36 g / cm³ 3 The sintering density will be measured using the Archimedes method.
[0136] <Three-point bending strength> The zirconia sintered body preferably has a three-point bending strength of 400 MPa or more and 1400 MPa or less. A three-point bending strength of 400 MPa or more indicates higher strength.
[0137] The three-point bending strength is more preferably 500 MPa or more, and even more preferably 600 MPa or more. The three-point bending strength is preferable as it is greater, but for example, it is 1200 MPa or less, 1000 MPa or less, etc. The three-point bending strength is more preferably 500 MPa or more and 1200 MPa or less, and even more preferably 600 MPa or more and 1000 MPa or less. The method for determining the three-point bending strength is by the method described in the examples.
[0138] The zirconia sintered body according to this embodiment can be used, for example, as an industrial component, an aesthetic component, or a dental material. More specifically, it can be used in jewelry, watch components, watch dials, artificial teeth, molding components, wear-resistant components, chemical-resistant components, and the like.
[0139] [Method for Manufacturing Zirconia Sintered Bodies] An example of a method for manufacturing zirconia sintered bodies will be described below. However, the method for manufacturing zirconia sintered bodies of the present invention is not limited to the following example.
[0140] The method for manufacturing a zirconia sintered body according to this embodiment comprises: step X of molding the zirconia powder to obtain a molded body; and step Y of sintering the molded body after step X under the following <sintering conditions>. <Sintering conditions> (a) Heating from room temperature to sintering temperature takes no more than 40 minutes. (b) Sintering temperature is 1050°C or higher and 1150°C or lower. (c) Holding time after reaching the sintering temperature is 1 minute or more.
[0141] In the method for manufacturing a zirconia sintered body according to this embodiment, first, zirconia powder is prepared. As the zirconia powder, the one described in the section on [Zirconia Powder] can be used.
[0142] Next, the zirconia powder is molded to obtain a molded body (step X). Molding can be done using a commercially available mold molding machine or cold isostatic pressing (CIP). Alternatively, the zirconia powder may be pre-molded using a mold molding machine, and then the final molding may be performed by press molding. Press molding is typically performed at 0.1t to 3t / cm. 2 It can be within this range. Preferably, 0.5t to 2.5t / cm 2 More preferably 0.8t to 2.2t / cm 2 More preferably 1t to 2t / cm 2 That is the case.
[0143] Next, the molded body is sintered under the following <sintering conditions> (step Y). <Sintering conditions> (a) The temperature rise from room temperature to the sintering temperature is within 40 minutes. (b) The sintering temperature is between 1050°C and 1150°C. (c) The holding time after reaching the sintering temperature is 1 minute or more.
[0144] In this embodiment, since the zirconia powder is used, a zirconia sintered body with high relative density can be obtained even when sintered under the above-mentioned <sintering conditions>. In particular, because the sintering temperature is low, between 1050°C and 1150°C, it becomes possible to co-sinter stabilizers, pigments, etc., which could not be used under conventional sintering conditions (e.g., above 1150°C) due to heat resistance. Furthermore, since the heating time from room temperature to the sintering temperature is within 40 minutes, and the time from room temperature to the sintering temperature is shortened compared to conventional methods, production efficiency is high and energy consumption during production can be reduced.
[0145] The heating from room temperature to the sintering temperature is preferably within 30 minutes, more preferably within 15 minutes. The heating from room temperature to the sintering temperature is preferably 1 minute or more, more preferably 5 minutes or more. The heating from room temperature to the sintering temperature is preferably 1 minute or more and within 30 minutes, more preferably within 5 minutes or more and within 15 minutes.
[0146] The heating rate is preferably constant, except immediately after the start of heating (for example, from the start of heating to 1 minute after the start of heating) and immediately before the completion of heating (for example, from 1 minute before reaching the sintering temperature to the completion of heating). The constant heating rate is preferably 30°C / min or more, more preferably 50°C / min or more, and even more preferably 100°C / min or more. The constant heating rate is preferably 200°C / min or less, more preferably 150°C / min or less, and even more preferably 120°C / min or less. The constant heating rate is preferably 30°C / min or more and 200°C / min or less, more preferably 50°C / min or more and 150°C / min or less, and even more preferably 100°C / min or more and 120°C / min or less.
[0147] The sintering temperature is preferably 1130°C or lower, more preferably 1110°C or lower. The sintering temperature is preferably 1070°C or higher, more preferably 1090°C or higher. The sintering temperature is preferably 1070°C or higher and 1130°C or lower, more preferably 1090°C or higher and 1110°C or lower.
[0148] The holding time is preferably 30 minutes or less. When the holding time is 30 minutes or less, the holding time after reaching the sintering temperature is shortened compared to conventional methods, thus increasing production efficiency and further reducing energy consumption during production.
[0149] The holding time is preferably 1 minute or more, more preferably 5 minutes or more. The holding time is more preferably 20 minutes or less, even more preferably 15 minutes or less. The holding time is preferably 1 minute or more and 30 minutes or less, more preferably 5 minutes or more and 20 minutes or less.
[0150] The sintering atmosphere can be in the atmosphere or an oxidizing atmosphere. Sintering can be carried out under normal pressure, and pressurization is not particularly necessary.
[0151] The method for manufacturing a zirconia sintered body according to this embodiment has been described above.
[0152] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples unless it exceeds the gist of the invention. The zirconia powder and zirconia sintered bodies in the examples and comparative examples contain hafnium oxide as an unavoidable impurity at a concentration of 1.3 to 2.5% by mass relative to the zirconium oxide (calculated by the following formula (X)). <Formula (X)> ([Mass of hafnium oxide] / ([Mass of zirconium oxide] + [Mass of hafnium oxide])) × 100 (%)
[0153] The maximum and minimum values of the content of each component shown in the following examples should be considered as the preferred minimum and preferred maximum values of the present invention, regardless of the content of other components. Furthermore, the maximum and minimum values of the measured values shown in the following examples should be considered as the preferred minimum and maximum values of the present invention, regardless of the content (composition) of each component.
[0154] [Preparation of Zirconia Powder] (Example 1) 213 g of 25% by mass sodium sulfate aqueous solution and ZrO 2 450 g each of 16% by mass of zirconium oxychloride aqueous solution (acid concentration: 1N) was heated separately to 95°C (Step 1). Then, the SO2 mixture was heated. 4 2- / ZrO 2 The heated aqueous solutions were brought into contact with each other over a period of 2 minutes so that the mass ratio was 0.50 (Step 2). Next, the resulting reaction solution containing basic zirconium sulfate was aged at 95°C for 4 hours to obtain basic zirconium sulfate (Step 3). Next, the aged solution was cooled to room temperature, and then Y 2 O 3 A 10% by mass aqueous solution of yttrium chloride is converted to Y 2 O 3 The solution was added to a total concentration of 3 mol% and mixed uniformly (Step 4). Next, a 25% by mass aqueous sodium hydroxide solution was added to the resulting mixed solution and neutralized until the pH reached 13 or higher to form a hydroxide precipitate (Step 5). Specifically, the above operations were carried out using the apparatus described with reference to Figure 1. The obtained hydroxide precipitate was filtered and thoroughly washed with water, and the obtained hydroxide was heat-treated in air at 950°C (calcination temperature) for 4 hours to obtain powder (zirconia) (Step 6). To the obtained unground powder (zirconia), lithium hydroxide monohydrate powder was added at a concentration of 0.1% by mass relative to the powder (zirconia), and the mixture was ground and mixed for 40 hours in a wet ball mill with water as the dispersion medium (Step 7). Zirconia beads with a diameter of 5 mm were used for grinding. The zirconia slurry obtained after grinding was dried at 110°C to obtain the zirconia powder according to Example 1.
[0155] (Example 2) Zirconia powder according to Example 2 was obtained in the same manner as in Example 1, except that lithium carbonate was used instead of lithium hydroxide monohydrate powder.
[0156] (Example 3) Zirconia powder according to Example 3 was obtained in the same manner as in Example 1, except that lithium nitrate was used instead of lithium hydroxide monohydrate powder.
[0157] (Example 4) Zirconia powder according to Example 4 was obtained in the same manner as in Example 1, except that the calcination temperature of the hydroxide was set to 880°C.
[0158] (Examples 5-11) Zirconia powders according to Examples 5-11 were obtained in the same manner as in Example 1, except that the amount of sintering aid, the amount of stabilizer, and the type of stabilizer were changed as shown in Table 1.
[0159] (Comparative Example 1) A zirconia powder according to Comparative Example 1 was obtained in the same manner as in Example 1, except that 0.50% by mass of alumina powder was added to the aforementioned powder (zirconia) instead of lithium hydroxide monohydrate powder.
[0160] (Comparative Example 2) Zirconia powder according to Comparative Example 2 was obtained in the same manner as in Example 1, except that the calcination temperature of the hydroxide was set to 1100°C.
[0161] (Comparative Example 3) Zirconia powder according to Comparative Example 3 was obtained in the same manner as in Example 1, except that the calcination temperature of the hydroxide was set to 800°C.
[0162] (Comparative Examples 4-5) Zirconia powders according to Comparative Examples 4-5 were obtained in the same manner as in Example 1, except that the amount of lithium hydroxide monohydrate powder added was changed as shown in Table 1.
[0163] [Specific Surface Area Measurement] The specific surface area of the zirconia powders of the examples and comparative examples was measured using the BET method with a specific surface area meter ("Macsorb," manufactured by Mountec). The results are shown in Table 1.
[0164] [Measurement of Pore Volume] For the zirconia powders of the examples and comparative examples, the pore distribution was obtained using a pore distribution analyzer ("Autopore IV9500" manufactured by Micromeritix) and the mercury intrusion method. The measurement conditions were as follows: <Measurement Conditions> Measurement device: Pore distribution analyzer (Autopore IV9500 manufactured by Micromeritix) Measurement range: 0.0036 to 10.3 μm Number of measurement points: 120 points Mercury contact angle: 140 degrees Mercury surface tension: 480 dyne / cm
[0165] Using the obtained pore distribution, the peak top diameter, pore volume, and pore distribution width were determined in the range of 10 nm to 200 nm. The results are shown in Table 1. Here, the pore distribution width refers to the width of the peak where the log differential pore volume is 0.1 ml / g or more. For reference, Figure 2 shows the pore distribution of the zirconia powder of Example 1, Figure 3 shows the pore distribution of the zirconia powder of Example 2, and Figure 4 shows the pore distribution of the zirconia powder of Comparative Example 3.
[0166] [Composition Measurement] The composition (oxide equivalent) of the zirconia powders in the examples and comparative examples was analyzed using ICP-AES ("ULTIMA-2", manufactured by HORIBA). The results are shown in Table 1.
[0167] [Particle size D 50 [Measurement] 0.15 g of zirconia powder from the examples and comparative examples, along with 40 ml of a 0.2% sodium hexametaphosphate aqueous solution, were placed in a 50 ml beaker. After dispersing for 5 minutes using an ultrasonic homogenizer "Sonifier S-450D" (Emerson Japan Co., Ltd.), the mixture was placed in a device (laser diffraction particle size distribution analyzer ("SALD-2300" manufactured by Shimadzu Corporation)) and measured. The results are shown in Table 1.
[0168] [Preparation of Zirconia Sintered Bodies] First, 8 g of zirconia powder from the examples and comparative examples were pre-formed in a 25 mm diameter mold, and then subjected to cold isostatic pressing (CIP) at 2 t / cm². 2 The molded bodies were formed under the following pressure. Next, the molded bodies were sintered under the following conditions: <Sintering Condition 1>, <Sintering Condition 2>, and <Sintering Condition 3>, respectively, to obtain zirconia sintered bodies. The sintering furnace used was a Denken Heidental Co., Ltd. product name: Zircom Speed.
[0169] <Sintering Conditions 1> Heating time from room temperature to 1100°C (sintering temperature): 37 minutes Holding time after reaching 1100°C (sintering temperature): 10 minutes Cooling down after holding time: Natural cooling
[0170] <Sintering Conditions 2> Heating time from room temperature to 1100°C (sintering temperature): 22 minutes Holding time after reaching 1100°C (sintering temperature): 10 minutes Cooling down after holding time: Natural cooling
[0171] <Sintering Condition 3> Heating time from room temperature to 1100°C (sintering temperature): 11 minutes Holding time after reaching 1100°C (sintering temperature): 10 minutes Cooling down after holding time: Natural cooling
[0172] [Relative Sintering Density] The relative sintering density of the obtained zirconia sintered body was determined as follows. The results are shown in Table 1.
[0173] <Relative Sintering Density> Relative sintering density (%) = (Sintering density / Theoretical sintering density) × 100 ... (1) Here, theoretical sintering density (ρ 0 ρz is the value calculated by the following formula (2-1): ρ0 = 100 / [(Y / 3.987) + (Z / 2.013) + (100 - Y - Z) / ρz] ... (2-1) However, ρz is the value calculated by the following formula (2-2): ρz = [124.25(100 - X) + [molecular weight of stabilizer] × X] / [150.5(100 + X)A] 2 C]...(2-2) Here, the molecular weight of the stabilizer is Y 2 O 3 In this case, 225.81, Er 2 O 3 In this case, 382.52, Yb 2 O 3 In this case, use 394.11. Also, X, Y, and Z are the stabilizer concentration (mol%), Al 2 O 3 (Weight %) and Li 2 O (weight %). Also, A and C are values calculated by the following formulas (2-3) and (2-4), respectively. A = 0.5080 + 0.06980X / (100 + X) ... (2-3) C = 0.5195 - 0.06180X / (100 + X) ... (2-4) In formula (1), the theoretical sintering density varies depending on the powder composition. For example, the theoretical sintering density of yttria-containing zirconia is 6.117 g / cm³ if the yttria content is 2 mol%. 3 If it's 3 mol%, then it's 6.098 g / cm³. 3 If it's 5.5 mol%, then it's 6.051 g / cm³. 3 (Al 2 O 3 =0% by weight, Li 2 (When O = 0% by weight) Stabilizer is Sc 2 O 3 In this case, ρz is the value calculated by the following formula (3): ρz = -0.0402 (Sc 2 O 3(Molar concentration of CaO) + 6.1294 ... (3) When the stabilizer is CaO, ρz is the value calculated by the following formula (3-1): ρz = -0.0400 (molar concentration of CaO) + 6.1700 ... (3-1) Also, the theoretical sintering density (let's call it ρ1) when a coloring agent is included is: ρ1 = 100 / [(Z / V) + (100 - Z) / ρ0] ... (2-5) Also, Z is the coloring agent concentration (weight %) and V is the theoretical density of the coloring agent (g / cm³) 3 ) The theoretical density of the colorant is Fe 2 O 3 5.24 g / cm³ 3 ZnO is 5.61 g / cm³ 3 MnO 2 5.03 g / cm³ 3 CoO is 6.10 g / cm³ 3 , Cr 2 O 3 5.22 g / cm³ 3 , TiO 2 4.23 g / cm³ 3 , Tb 4 O 7 7.80 g / cm 3 CuO is 6.31 g / cm³ 3 , V 2 O 5 3.36 g / cm³ 3 The sintering density was measured using the Archimedes method.
[0174] <Relative molding density> Relative molding density (%) = (molding density / theoretical sintering density) × 100 ... (4) Here, theoretical sintering density (ρ 0 (Let's assume this is the value calculated by the above formula (2-1).
[0175] [Three-point bending strength] The three-point bending strength of the zirconia sintered bodies of the examples and comparative examples obtained above was measured in accordance with the three-point bending strength of JIS R 1601:2008. The results are shown in Table 1.
[0176]
Claims
1. The material contains zirconia and a Li compound containing Li, wherein the content of the Li compound is such that, when the zirconia powder is considered as a whole, Li 2 Zirconia powder characterized by having an O content of 0.050% to 0.200% by mass in terms of O equivalent, and in the pore distribution based on the mercury intrusion method, having a peak top diameter of 35 nm to 80 nm in the range of 10 nm to 200 nm, and a pore volume of 0.20 ml / g to 0.50 ml / g.
2. Specific surface area is 20 m² 2 / g over 40m 2 The zirconia powder according to claim 1, characterized in that it is less than or equal to / g.
3. Particle size D 50 The zirconia powder according to claim 1 or 2, characterized in that the particle size is 0.1 μm or more and 0.6 μm or less.
4. The zirconia contains a stabilizer, and the stabilizer is Y 2 O 3 , CeO 2 , Sc 2 O 3 , CaO, Er 2 O 3 , and Yb 2 O 3 is at least one selected from the group consisting of the above, the zirconia powder according to claim 1 or 2.
5. The zirconia powder according to claim 4, characterized in that the content of the stabilizer is 1.5 mol% or more and 15 mol% or less when the total amount of zirconia and stabilizer is considered.
6. The material comprises zirconia and a Li compound containing Li, wherein the content of the Li compound is such that, when the zirconia sintered body is considered as a whole, 2 A zirconia sintered body characterized by having an O content of 0.050% by mass or more and 0.200% by mass or less, and a relative density of 98.5% or more.
7. The zirconia sintered body according to claim 6, characterized in that the zirconia does not contain a stabilizer, or the total amount of zirconia and stabilizer is less than 1.5 mol%.
8. A method for producing a zirconia sintered body, comprising: step X of molding zirconia powder according to claim 1 or 2 to obtain a molded body; and step Y of sintering the molded body after step X under the following <sintering conditions>. <Sintering conditions> (a) Heating from room temperature to sintering temperature takes no more than 40 minutes. (b) Sintering temperature is 1050°C or higher and 1150°C or lower. (c) Holding time after reaching the sintering temperature is 1 minute or more.
9. The method for producing a zirconia sintered body according to claim 8, characterized in that the holding time is 30 minutes or less.