Surface-treated copper foil, copper-clad laminate using said surface-treated copper foil, and printed wiring board
A surface-treated copper foil with specific conductivity and impedance stability addresses the challenge of maintaining signal integrity in high-frequency transmission by ensuring homogeneous conductivity and reduced impedance mismatch.
Patent Information
- Application Number
- PCT/JP2026/017197
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Existing copper foils fail to maintain excellent signal integrity characteristics for high-frequency signal transmission due to insufficient consideration of surface conductivity and impedance variations, despite surface treatments aimed at improving conductor loss.
A surface-treated copper foil with a surface specific conductivity of 0.5 or more and a standard deviation of measured characteristic impedance of 0.3 or less, ensuring homogeneous conductivity and reduced impedance mismatch.
The copper foil maintains superior signal integrity characteristics by ensuring consistent conductivity and reduced signal reflection, suitable for high-frequency signal transmission.
Smart Images

Figure JP2026017197_12112026_PF_FP_ABST
Abstract
Description
Surface-treated copper foil, copper-clad laminates using said surface-treated copper foil, and printed circuit boards
[0001] This invention relates to surface-treated copper foil. More specifically, the present invention relates to surface-treated copper foil that has excellent effective conductivity and is therefore suitable for use in printed circuit boards for high-frequency signal transmission.
[0002] Conventionally, printed circuit boards (PCBs) have been used in various communication devices, computers, and mobile phones, in which conductive copper wiring patterns are formed on an insulating resin substrate such as epoxy resin or polyimide resin.
[0003] In recent years, various devices using radio waves with frequencies exceeding 3 GHz, and even extremely high frequencies of 30 GHz or more, known as millimeter waves, have been developed to facilitate the widespread adoption of services utilizing fifth-generation mobile communication systems (5G) and automobiles equipped with advanced driver-assistance systems (ADAS). Consequently, there is a growing demand for printed circuit boards that can handle high-frequency signal transmission.
[0004] When a printed circuit board transmits a high-frequency signal, the attenuation increases as the signal frequency increases, resulting in a decrease in signal integrity characteristics (hereinafter referred to as "SI characteristics").
[0005] In SI characteristics, the degree of signal loss during transmission is called insertion loss, and generally, the threshold insertion loss required for signal transmission without problems is said to be -3 dB.
[0006] Insertion losses are broadly classified into dielectric losses and conductor losses.
[0007] In copper-clad laminates and printed circuit boards, dielectric loss is related to the insulating resin substrate, while conductor loss is related to the copper foil.
[0008] Regarding conductor loss, the so-called skin effect is known, in which the transmitted AC signal current concentrates near the surface of the copper foil as the frequency increases. To improve SI characteristics, improvements have been made, such as reducing the surface irregularities of the copper foil to shorten the transmission distance.
[0009] However, regarding the improvement of SI characteristics in high-frequency signal transmission, from the perspective of the skin effect, reducing the irregularities on the copper foil surface can be a necessary condition but not a sufficient condition.
[0010] This is because the region where alternating current concentrates due to the skin effect, that is, the skin depth, is affected by the electrical conductivity σ and the magnetic permeability μ, as shown in the following [Equation 1].
[0011]
[0012] The electrical conductivity σ and magnetic permeability μ in Equation 1 are effective values that vary depending on the range of the skin depth and the high-frequency frequency, and are different from the electrical conductivity and magnetic permeability under direct current.
[0013] The surface shape is only one of the factors that affect this effective electrical conductivity.
[0014] For copper foils for printed wiring boards, surface treatments such as roughening treatment to ensure adhesion to the insulating resin base material, and dissimilar metal plating treatment to impart heat resistance, chemical resistance, and rust resistance are essential.
[0015] However, the effective electrical conductivity in the vicinity of the surface (hereinafter referred to as "surface electrical conductivity") is affected not only by the surface shape of the roughened treatment layer, but also by the dissimilar metals and the like in the dissimilar metal plating treatment layer.
[0016] Accordingly, there is a demand for the development of a surface-treated copper foil having excellent effective electrical conductivity, which can be suitably used for printed wiring boards for high-frequency signal transmission.
[0017] JP 2022-085378 A JP 2023-134352 A JP 2023-163171 A WO 2023 / 190833
[0018] Patent Documents 1 and 2 disclose copper foils in which the arithmetic mean height Sa and the developed area ratio Sdr are controlled as parameters of the surface shape.
[0019] However, controlling only the surface shape is insufficient for improving the SI characteristics.
[0020] Patent Document 2 discloses the surface conductivity measured by the balanced circular disk resonator method (BCDR method), but the results are for rolled copper foil, and the effect of surface treatment is not described.
[0021] Patent Document 3 discloses a copper foil with controlled conductivity, but according to the measurement method (the four-point probe method described in JIS K 7194), the conductivity is direct current conductivity, which is different from the surface conductivity in the region where alternating current concentrates due to the skin effect.
[0022] Patent Document 4 discloses an etching factor, which is an index indicating the rectangularity of a circuit.
[0023] The etching factor is also important for SI characteristics, but the etching factor determined from the cross-sectional shape is extremely local information, not information on the entire circuit.
[0024] The present inventors set out to solve the aforementioned problems as a technical challenge, and as a result of numerous repeated trial productions and evaluations, found that for a surface-treated copper foil having at least one surface subjected to surface treatment, wherein the surface specific conductivity of the treated surface of the surface-treated copper foil is 0.5 or more, and the standard deviation of the actually measured characteristic impedance of a circuit formed from the surface-treated copper foil is 0.3 or less, since this reflects not only the surface shape but also the influence of the surface treatment, the effective conductivity is excellent, and the circuit formed from the surface-treated copper foil according to the present invention has small characteristic variation as a circuit and improved SI characteristics, thereby completing the present invention to achieve the aforementioned technical challenge.
[0025] The aforementioned technical problem can be solved by the present invention as described below.
[0026] The surface specific conductivity in the present specification refers to the ratio of the surface conductivity to the direct current conductivity. The "direct current conductivity" refers to the conductivity measured with direct current by a four-terminal method, a four-point probe method, or the like.
[0027] The present invention relates to a surface-treated copper foil in which at least one surface is surface-treated, wherein the surface conductivity of the surface-treated copper foil surface, represented by the following formula (Formula 1), is 0.5 or more, and the standard deviation of the measured characteristic impedance of a circuit formed with the surface-treated copper foil is 0.3 or less. (Formula 1) Surface conductivity of the surface-treated copper foil surface / 5.8 × 10 7
[0028] Furthermore, the present invention relates to the surface-treated copper foil, wherein the surface conductivity is the surface conductivity at frequencies of 67 GHz or lower.
[0029] Furthermore, the present invention relates to a copper-clad laminate using the surface-treated copper foil described above.
[0030] Furthermore, the present invention relates to a printed circuit board using the surface-treated copper foil described above.
[0031] Furthermore, the present invention relates to a printed circuit board using the aforementioned copper-clad laminate.
[0032] Surface conductivity is a value that reflects the effects of surface treatment in addition to surface shape.
[0033] This invention relates to a surface-treated copper foil with a surface specific conductivity of 0.5 or higher, resulting in excellent effective conductivity and superior SI characteristics with low conductor loss.
[0034] The measured characteristic impedance represents the overall result of the influence of not only the cross-sectional shape of the entire circuit, but also factors such as the thickness of the copper foil, surface roughness, and surface treatment.
[0035] Large fluctuations (variations) in the measured characteristic impedance result in a larger proportion of the signal being reflected at impedance mismatch points and a smaller proportion of the signal being transmitted, ultimately leading to a deterioration of the signal-to-signal (SI) characteristics.
[0036] Small fluctuations in the measured characteristic impedance indicate that the various characteristics of the copper foil are also small, meaning the copper foil is homogeneous.
[0037] Since the standard deviation of the measured characteristic impedance of the circuit formed with the surface-treated copper foil in this invention is 0.3 or less, the surface-treated copper foil in this invention is a homogeneous copper foil and is a surface-treated copper foil with excellent SI characteristics.
[0038] By using copper-clad laminates or printed circuit boards using surface-treated copper foil according to the present invention, or by using printed circuit boards using copper-clad laminates according to the present invention, it is possible to manufacture copper-clad laminates or printed circuit boards that maintain good SI characteristics even in high-frequency signal transmission.
[0039] This is an example of a surface-treated copper foil according to the present invention.
[0040] (Copper foil) The copper foil used in the surface-treated copper foil of the present invention is not particularly limited, and copper foil or copper alloy foil formed by rolling or electrolytic methods can be used.
[0041] The thickness of the copper foil is not particularly limited and can be selected appropriately depending on the application, but it is preferably 2 μm to 70 μm, and more preferably 9 μm to 35 μm.
[0042] The thickness of the surface-treated copper foil affects the design characteristic impedance along with the circuit width of the signal layer, so it should be selected appropriately depending on the circuit pattern of the signal layer and the dielectric properties of the insulating resin substrate used.
[0043] (Surface-treated copper foil) The surface treatment in the present invention is not particularly limited, and examples include roughening treatment to ensure adhesion, dissimilar metal plating treatment to provide heat resistance, chemical resistance, and rust prevention, and chemical conversion treatment to provide chemical adhesion and rust prevention, which can be appropriately selected depending on the application and purpose (Figure 1).
[0044] In the present invention, the surface-treated copper foil only needs to have surface treatment on at least one side, or it may be treated on both sides (Figure 2).
[0045] In the present invention, the surface-treated copper foil preferably has a surface conductivity of 0.5 or higher, more preferably 0.7 or higher, and even more preferably 0.8 or higher.
[0046] In the case of treated copper foil with surface treatment on both sides, it is preferable that the surface conductivity ratio of the treated surfaces on both sides is 0.5 or higher, more preferably 0.7 or higher, and even more preferably 0.8 or higher.
[0047] A surface conductivity ratio of less than 0.5 indicates low surface conductivity at the interface with the insulating resin substrate, which may prevent the maintenance of good SI characteristics in high-frequency signal transmission.
[0048] The surface conductivity is determined by measuring the surface conductivity (S / m) of the surface-treated copper foil surface as shown in (Equation 1) below, and is equal to the conductivity of the international standard soft copper, which is 5.8 × 10⁻⁶. 7 It can be calculated by dividing by S / m.
[0049] (Equation 1) Surface conductivity of the surface-treated copper foil surface / 5.8 × 10 7
[0050] Furthermore, if the surface conductivity is 0.5 or higher at 67 GHz or below, it can be suitably used as a printed circuit board for high-frequency signal transmission.
[0051] In the present invention, the surface-treated copper foil preferably has a standard deviation of 0.3 or less in the measured characteristic impedance when a circuit is formed, and more preferably 0.2 or less.
[0052] If the standard deviation of the measured characteristic impedance is greater than 0.3, the proportion of signals reflected due to impedance mismatch increases, while the proportion of signals transmitted decreases, which may make it impossible to maintain good SI characteristics.
[0053] Examples and comparative examples of the present invention are shown below, but the present invention is not limited thereto, and can be selected without limitation within the scope described herein.
[0054] (Surface-treated copper foil) <Example 1> Using an aqueous solution of 280 g / L copper sulfate pentahydrate, 100 g / L sulfuric acid, 20 mg / L polyethylene glycol (average molecular weight: 20000, manufactured by Sanyo Chemical Industries, Ltd.), 20 mg / L polyethyleneimine (product name: Epomin®, product number: PP-061, average molecular weight: 1200, manufactured by Nippon Shokubai Co., Ltd.), 6 μmol / L sodium 3-mercapto-1-propanesulfonate, and 20 mg / L chloride ions, at a bath temperature of 40°C, with a current density of 50 A / dm 2, a titanium plate was used as the cathode for treatment, to obtain an untreated electrolytic copper foil with a nominal thickness of 18 μm. An insoluble electrode made of titanium coated with a platinum group oxide was used as the anode. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each subsequent treatment was performed.
[0055] First, an aqueous solution containing 39 g / L of cobalt sulfate heptahydrate, 24 g / L of disodium molybdate dihydrate, 45 g / L of trisodium citrate dihydrate, with a pH of 5.6 and a bath temperature of 30°C was used, at a current density of 7 A / dm 2 , and an electric quantity of 14 C / dm 2 , the deposition surface of the copper foil was treated as the cathode. An insoluble electrode made of titanium coated with a platinum group oxide was used as the anode.
[0056] Next, an aqueous solution containing 10 g / L of sodium dichromate dihydrate, with a pH of 4.2 and a bath temperature of 30°C was used, at a current density of 0.5 A / dm 2 , and an electric quantity of 1 C / dm 2 , the deposition surface of the copper foil was treated as the cathode. An insoluble electrode made of titanium coated with a platinum group oxide was used as the anode.
[0057] Finally, an aqueous solution containing 5 mL / L of γ-aminopropyltriethoxysilane with a bath temperature of 30°C was used, the copper foil was immersed for 15 seconds for treatment, followed by natural drying.
[0058] <Example 2> The same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each subsequent treatment was performed.
[0059] First, an aqueous solution containing 35 g / L of copper sulfate pentahydrate, 100 g / L of pentasodium diethylenetriaminepentaacetate, with a pH of 4.8 and a bath temperature of 30°C was used, at a current density of 5 A / dm 2 , and an electric quantity of 60 C / dm 2 , the deposition surface of the copper foil was treated as the cathode. A copper plate was used as the anode.
[0060] Next, an aqueous solution containing 30 g / L of nickel sulfate hexahydrate, 10 g / L of sodium acetate trihydrate, 2 g / L of sodium hypophosphite monohydrate, with a pH of 4.5 and a bath temperature of 32°C was used, at a current density of 2.5 A / dm 2 , and an electric quantity of 5 C / dm 2The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0061] Next, an aqueous solution containing 12.5 g / L of sodium dichromate dihydrate, 2.5 g / L of zinc ions, pH 12, and a bath temperature of 30°C was used, and the current density was 4 A / dm². 2 Electrical charge 6 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0062] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0063] <Example 3> The same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each treatment was performed.
[0064] First, an aqueous solution containing 35 g / L of copper sulfate pentahydrate and 100 g / L of pentasodium diethylenetriaminepentaacetate, with a pH of 4.8 and a bath temperature of 30°C, was used to measure the current density at 5 A / dm². 2 Electrical charge 30 C / dm 2 The deposited surface of the copper foil was treated as the cathode. A copper plate was used as the anode.
[0065] Next, an aqueous solution containing 30 g / L nickel sulfate hexahydrate, 10 g / L sodium acetate trihydrate, and 2 g / L sodium hypophosphite monohydrate, with a pH of 4.5 and a bath temperature of 32°C, was used to test the current density at 1 A / dm². 2 Electrical charge 1.8 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0066] Next, an aqueous solution containing 12.5 g / L of sodium dichromate dihydrate, 2.5 g / L of zinc ions, pH 12, and a bath temperature of 30°C was used, and the current density was 4 A / dm². 2 Electrical charge 6 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0067] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0068] <Example 4> The same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each treatment was performed.
[0069] First, an aqueous solution containing 30 g / L nickel sulfate hexahydrate, 10 g / L sodium acetate trihydrate, and 2 g / L sodium hypophosphite monohydrate, with a pH of 4.5 and a bath temperature of 32°C, was used to test the current density at 1 A / dm². 2 Electrical charge 1.8 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0070] Next, an aqueous solution containing 12.5 g / L of sodium dichromate dihydrate, 2.5 g / L of zinc ions, pH 12, and a bath temperature of 30°C was used, and the current density was 4 A / dm². 2 Electrical charge 6 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0071] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0072] <Example 5> The same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each treatment was performed.
[0073] First, an aqueous solution containing 45 g / L of copper sulfate pentahydrate, 90 g / L of sulfuric acid, 15 mg / L of tungsten ions, 500 mg / L of titanium ions, and 5 mg / L of chloride ions, with a bath temperature of 40°C, was used to obtain a current density of 25 A / dm². 2 Electrical charge 50 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0074] Next, an aqueous solution of copper sulfate pentahydrate (250 g / L), sulfuric acid (100 g / L), and a bath temperature of 40°C was used, and the current density was 10 A / dm².2 Electrical charge 120 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0075] Next, an aqueous solution containing 39 g / L cobalt sulfate heptahydrate, 24 g / L disodium molybdate dihydrate, and 45 g / L trisodium citrate dihydrate, with a pH of 5.6 and a bath temperature of 30°C, was used, and the current density was 7 A / dm². 2 Electrical charge 14 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0076] Next, an aqueous solution containing 12.5 g / L of sodium dichromate dihydrate, 2.5 g / L of zinc ions, pH 12, and a bath temperature of 30°C was used, and the current density was 4 A / dm². 2 Electrical charge 6 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0077] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0078] <Example 6> Rolled copper foil with a nominal thickness of 18 μm was used as the copper foil. The copper foil was immersed in a hydrocarbon-based organic solvent for 60 seconds to remove the rolling oil before each treatment was performed.
[0079] First, an aqueous solution containing 35 g / L of copper sulfate pentahydrate and 100 g / L of pentasodium diethylenetriaminepentaacetate, with a pH of 4.8 and a bath temperature of 30°C, was used to measure the current density at 5 A / dm². 2 Electrical charge 30 C / dm 2 The process was carried out using [method / technology]. A copper plate was used as the anode.
[0080] Next, an aqueous solution containing 39 g / L cobalt sulfate heptahydrate, 24 g / L disodium molybdate dihydrate, and 45 g / L trisodium citrate dihydrate, with a pH of 5.6 and a bath temperature of 30°C, was used, and the current density was 7 A / dm². 2 Electrical charge 14 C / dm 2 The process was carried out using [method / technology]. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0081] Next, an aqueous solution of sodium dichromate dihydrate at 10 g / L, pH 4.2, and bath temperature 30°C was used, and the current density was 0.5 A / dm². 2 Electrical charge 1 C / dm 2 The process was carried out using [method / technology]. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0082] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0083] <Comparative Example 1> An aqueous solution containing 280 g / L of copper sulfate pentahydrate, 100 g / L of sulfuric acid, 2 mg / L of gelatin, and 20 mg / L of chloride ions was used, with a bath temperature of 40°C, and the current density was 50 A / dm². 2 Then, a titanium plate was treated as the cathode to obtain an untreated electrolytic copper foil with a nominal thickness of 18 μm. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode. The treatment was the same as in Example 5, except that the copper foil used was different.
[0084] <Comparative Example 2> The same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each treatment was performed.
[0085] First, an aqueous solution containing 45 g / L of copper sulfate pentahydrate, 90 g / L of sulfuric acid, 15 mg / L of tungsten ions, 500 mg / L of titanium ions, and 5 mg / L of chloride ions, with a bath temperature of 40°C, was used to obtain a current density of 10 A / dm². 2 Electricity level 65 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0086] Next, an aqueous solution of copper sulfate pentahydrate (250 g / L), sulfuric acid (100 g / L), and a bath temperature of 40°C was used, and the current density was 10 A / dm². 2 Electrical charge 300 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0087] Next, an aqueous solution containing 39 g / L cobalt sulfate heptahydrate, 24 g / L disodium molybdate dihydrate, and 45 g / L trisodium citrate dihydrate, with a pH of 5.6 and a bath temperature of 30°C, was used, and the current density was 7 A / dm². 2 Electrical charge 14 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0088] Next, an aqueous solution containing 12.5 g / L of sodium dichromate dihydrate, 2.5 g / L of zinc ions, pH 12, and a bath temperature of 30°C was used, and the current density was 4 A / dm². 2 Electrical charge 6 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0089] Finally, the copper foil was treated by immersing it in an aqueous solution of 5 mL / L γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0090] <Comparative Example 3> As the copper foil, the same untreated electrolytic copper foil as in Example 1 was used. The untreated electrolytic copper foil was immersed in dilute sulfuric acid to remove the oxide film before each treatment was performed.
[0091] First, an aqueous solution containing 100 g / L of copper sulfate pentahydrate, 100 g / L of sulfuric acid, 0.15 g / L of indium sulfate nonahydrate, and 5 g / L of starch hydrolysate (molecular weight 100-10000) was used at a bath temperature of 40°C, with a current density of 25 A / dm². 2 Electricity level 70 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0092] Next, an aqueous solution containing 39 g / L cobalt sulfate heptahydrate, 24 g / L disodium molybdate dihydrate, and 45 g / L trisodium citrate dihydrate, with a pH of 5.6 and a bath temperature of 30°C, was used, and the current density was 7 A / dm². 2 Electrical charge 14 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0093] Next, an aqueous solution of sodium dichromate dihydrate at 10 g / L, pH 4.2, and bath temperature 30°C was used, and the current density was 0.5 A / dm². 2 Electrical charge 1 C / dm 2 The deposited surface of the copper foil was treated as the cathode. An insoluble electrode made of platinum group oxide-coated titanium was used as the anode.
[0094] Finally, the copper foil was treated by immersing it in an aqueous solution of γ-aminopropyltriethoxysilane at a bath temperature of 30°C for 15 seconds, and then allowed to air dry.
[0095] (Surface Ratio Conductivity) Using a Fabry-Perot resonator FP-CND-BB (manufactured by EM Lab Co., Ltd.) for conductivity measurement, the surface conductivity of the surface in contact with the insulating resin substrate was measured in the frequency range of 23 GHz to 67 GHz, and the obtained value was calculated as 5.8 × 10⁻⁶. 7 The surface specific conductivity was determined by dividing by S / m (the conductivity of international standard soft copper).
[0096] The surface conductivity showed a decreasing trend with increasing frequency. Table 1 shows the surface conductivity at 67 GHz.
[0097] (SI characteristics) MEGTRON7 (manufactured by Panasonic Corporation) was used as the insulating resin substrate.
[0098] The surface-treated copper foils from the examples and comparative examples were bonded to both sides of an insulating resin substrate using a vacuum hot press machine KVHC-II (manufactured by Kitagawa Seiki Co., Ltd.) to create a double-sided copper-clad laminate.
[0099] The bonding conditions were under atmospheric conditions, at a temperature of 200°C and a surface pressure of 4 MPa for 80 minutes.
[0100] Using each of the fabricated double-sided copper-clad laminates, microstrip line substrates were formed so that the design characteristic impedance was 50Ω and the circuit lengths were 10 inches and 2 inches.
[0101] Using the fabricated microstrip line substrate, insertion loss was measured in the frequency range of 10 MHz to 67 GHz with a vector network analyzer N5227B (manufactured by Keysight Technologies, Inc.).
[0102] Using the 2-inch measurement results, the 10-inch measurement results were de-embedded using the software Automatic Fixture Removal (AFR / Keysight Technologies, Inc.) to extract the insertion loss for 8 inches, which was then converted to dB / inch.
[0103] For insertion loss at 67 GHz, a value of -1.5 dB / inch (-3 dB / 2 inch) or higher was evaluated as "good," and a value of less than -1.5 dB / inch was evaluated as "poor."
[0104] (Measured Characteristic Impedance) For the results of the de-embedded 8-inch section, the measured characteristic impedance of the circuit portion was determined using the software Enhanced Time Domain Analysis with TDR (manufactured by Keysight Technologies, Inc.), and the standard deviation was calculated.
[0105] The results are shown in [Table 1].
[0106]
[0107] A comparison of the examples and comparative examples demonstrated that if the surface conductivity is low, the SI characteristics (insertion loss) cannot be maintained well.
[0108] Furthermore, even with high surface conductivity, if the standard deviation of the measured characteristic impedance was large, the SI characteristics tended to deteriorate due to increased reflection caused by impedance mismatch. In particular, when the surface conductivity fell below 0.5, the SI characteristics deteriorated sharply.
[0109] The surface-treated copper foil according to the present invention has a surface specific conductivity of 0.5 or higher near the interface with the insulating resin substrate, and a standard deviation of the measured characteristic impedance of 0.3 or lower. Therefore, it can maintain good SI characteristics even in high-frequency signal transmission, making it suitable for use in printed circuit boards for high-frequency signal transmission. Accordingly, the present invention has high industrial applicability.
[0110] 10 Surface-treated copper foil 20 Copper foil 30 Surface treatment 31 Roughening treatment 32 Dissimilar metal plating treatment 33 Chemical conversion treatment
Claims
1. Surface-treated copper foil in which at least one surface is surface-treated, wherein the surface conductivity of the surface-treated copper foil surface, represented by the following (Equation 1), is 0.5 or more, and the standard deviation of the measured characteristic impedance of the circuit formed with the surface-treated copper foil is 0.3 or less. (Equation 1) Surface conductivity of the surface-treated copper foil surface / 5.8 × 10 7 2. The surface-treated copper foil according to claim 1, wherein the surface conductivity is the surface conductivity at a frequency of 67 GHz or less.
3. A copper-clad laminate using the surface-treated copper foil according to claim 1 or claim 2.
4. A printed circuit board using surface-treated copper foil according to claim 1 or 2.
5. A printed circuit board using the copper-clad laminate described in claim 3.