Method for recovering lithium from aqueous lithium solution using electrosorption process
The electro-adsorption process with a tailored adsorption electrode enhances lithium recovery from low-grade sources by improving selectivity and efficiency, addressing economic and environmental challenges in existing technologies.
Patent Information
- Application Number
- PCT/KR2025/019275
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2025-11-20
- Publication Date
- 2026-11-12
AI Technical Summary
Existing lithium recovery technologies from low-grade salt lakes are economically unviable due to high energy consumption, environmental burdens, and low lithium extraction efficiency, with limited applicability and selectivity, especially for medium-to-low grade lithium sources.
A method using an electro-adsorption process with an adsorption electrode comprising HxMnyOz adsorbent and conductive carbon material, with specific mass ratios, to selectively adsorb and desorb lithium ions, followed by electroconcentration and conversion to lithium phosphate.
Enhances lithium recovery selectivity and efficiency, achieving concentrations of 3000 ppm or more, with improved economic feasibility and reduced environmental impact.
Smart Images

Figure KR2025019275_12112026_PF_FP_ABST
Abstract
Description
Method for recovering lithium from an aqueous lithium solution using an electro-adsorption process
[0001] The present invention relates to a method for recovering lithium from an aqueous lithium solution using an electric adsorption process.
[0002] Along with the expansion of the electric vehicle and energy storage system markets, the demand for lithium-ion batteries is surging; however, the entire supply of lithium compounds, which are the raw materials for cathode materials, is currently dependent on imports.
[0003] To date, attempts have been made to secure lithium resources by applying extraction technologies to various lithium raw materials, but economically viable production technologies have not yet been secured, with the exception of high-grade minerals and salt lakes.
[0004] More than 70% of the world's lithium compound production comes from lithium salt lakes, and commercially viable lithium salt lakes are limited to South America and China, so the threat of resource weaponization is increasing due to resource protection policies of countries possessing high-quality salt lakes.
[0005] For high-grade lithium salt lakes, there are high barriers to entry for new resource acquisition, and competition is fierce. Medium-to-low grade salt lakes (Li < 500 ppm), which have low lithium concentrations, are scattered globally and easily accessible; however, they are being neglected because the profitability of applying currently developed lithium recovery technologies is low.
[0006] Although various non-evaporative lithium recovery technologies (precipitation, solvent extraction, and adsorption methods) have been proposed to secure lithium resources from low-grade salt lakes, it is judged that they have not achieved economic feasibility because the low lithium content results in high energy consumption during the extraction and concentration processes required for converting lithium compounds, as well as high usage of chemical solvents to remove impurities.
[0007] Recently, active attempts have been made to recover lithium from low-grade salt lakes by applying solvent extraction, precipitation, and adsorption methods, but these efforts remain in the research phase and are subject to restrictions regarding the emission of hazardous substances during the lithium recovery process due to water resource protection policies of countries possessing such lakes.
[0008] Solvent extraction and precipitation methods are constrained by the requirement to remove impurities through a pretreatment process, which results in the disadvantage of generating an excessive amount of sludge. Adsorption methods do not require a pretreatment process for impurity separation, but their low lithium extraction efficiency makes it difficult to expand them into commercial technology.
[0009] Recently, attempts have been made to improve the low lithium selectivity of solvent extraction and precipitation methods by adjusting the pH of salt lake solutions. However, these methods are difficult to apply as lithium recovery technologies due to the disadvantages of increased environmental burden caused by the use of excessive acid / alkali solvents, the incorporation of extractants generated during the process, and hazardous substances contained in unreacted filtrate.
[0010] Electro-adsorption technology is generally classified into ED (Electro dialysis), EDI (Electro deionization), and MCDI (Membrane Capacitive deionization) technologies. The adsorption principle is that when an electric potential is applied, anions in an aqueous solution move to the (+) electrode and cations move to the (-) electrode, and the ions are removed by electrical adsorption to the electrode interface.
[0011] ED and EDI technologies are used as desalination technologies specialized for the production of high-concentration solutions or ultrapure water, but they have the disadvantages of limited applicable solution concentrations, low recovery rates, and high process costs due to high operating potential (>3.5V).
[0012] MCDI technology is used in the field of water treatment for low-concentration solutions and has a low operating potential (<1.5V) and high ion separation / recovery efficiency, but it is limited by concentration limits (2500–3000 ppm, based on NaCl).
[0013] Electro-adsorption technologies developed to date are limited to the separation and desalination of ions in aqueous solutions, and have limitations in terms of selectivity for specific ions and concentration efficiency.
[0014] The object of the present invention is to provide a method for recovering lithium from an aqueous lithium solution using an electric adsorption process.
[0015] The objective of the present invention is achieved by a method for recovering lithium from a lithium aqueous solution using an electric adsorption process, comprising the step of applying a potential to an adsorption electrode and a corresponding electrode to adsorb lithium from the lithium aqueous solution onto the adsorption electrode, wherein the adsorption electrode comprises an adsorbent represented by HxMnyOz, wherein the x / y ratio is 0.4 to 1.2 and the z / y ratio is 1.5 to 3.0.
[0016] The adsorption electrode comprises an adsorption layer including the adsorbent, wherein the adsorption layer comprises the adsorbent and a conductive carbon material, and the mass ratio of the adsorbent to the conductive carbon material may be 60 to 90 to 10 to 40.
[0017] The conductive carbon material may include at least one of activated carbon, graphite, graphene, carbon fiber, carbon nanotube, and carbon black.
[0018] The above adsorption layer further includes a conductive polymer, and the mass ratio of the adsorbent + the conductive carbon material to the conductive polymer may be 85 to 95 to 5 to 15.
[0019] The above conductive polymer may include PvdF.
[0020] The above adsorbent can be obtained by leaching a lithium component from an LMO material.
[0021] The above elution can be performed using a hydrochloric acid, sulfuric acid, or nitric acid solution of 0.1 to 2.0 M at a solid-to-liquid ratio (g / L) of 0.5 to 20.
[0022] The above adsorbent can be obtained by forming the LMO material by a method of supporting it on the conductive carbon material, and then leaching the lithium component from the LMO material.
[0023] The adsorption electrode further comprises an electrode body coated with the adsorbent, and the adsorption electrode is obtained by coating an adsorbent slurry on the electrode body, and the adsorbent slurry may include the adsorbent, the conductive carbon material, the conductive polymer, and a solvent.
[0024] The above lithium aqueous solution further includes an impurity component, and the impurity component includes at least one of sodium, potassium, magnesium, and calcium, and the adsorption selectivity of the lithium may be 2 to 100 times higher than the selectivity of the sodium component.
[0025] After the above adsorption, the method may further include a step of applying a reverse potential to the adsorption electrode to desorb the lithium ions adsorbed on the adsorbent.
[0026] The above desorption may further include a step of flushing the adsorption electrode with deionized water before applying a reverse potential.
[0027] In the application of power during the adsorption step, the application of the target potential and the application of the process reverse potential are repeated, and the absolute value of the process reverse potential may be smaller than the absolute value of the reverse potential during desorption.
[0028] The method further includes a step of electroconcentrating the lithium extract recovered from the above desorption to increase the lithium concentration, and in the electroconcentration, the process of adsorbing the lithium of the lithium extract onto an adsorption module containing conductive carbon and then desorbing it can be repeated at least twice.
[0029] The lithium concentration in the lithium concentrate obtained by the above electroconcentration is 3000 ppm or more, and may further include a process of recovering lithium phosphate by adding phosphoric acid to the lithium concentrate.
[0030] The method may further include the step of adding a calcium compound to the lithium phosphate filtrate after the recovery of the lithium phosphate to remove at least a portion of the PO4 component of the lithium phosphate filtrate as calcium phosphate.
[0031] The method further includes a step of adding a sulfuric acid solution to the calcium phosphate to form phosphoric acid, and the phosphoric acid can be used in the recovery step of the lithium phosphate.
[0032] According to the present invention, a method for recovering lithium from an aqueous lithium solution using an electric adsorption process is provided.
[0033] FIG. 1 is a flowchart of a lithium recovery method according to one embodiment of the present invention, and
[0034] FIG. 2 is a flowchart illustrating a method for manufacturing an adsorption electrode in a lithium recovery method according to one embodiment of the present invention, and
[0035] FIGS. 3 and 4 are for explaining a method for manufacturing an adsorption electrode in a lithium recovery method according to an embodiment of the present invention, and
[0036] FIG. 5 is a flowchart of the process after lithium desorption in a lithium recovery method according to an embodiment of the present invention, and
[0037] Figure 6 shows the configuration of the adsorption module used in the experimental example, and
[0038] Figure 7 shows the configuration and photograph of the extraction system used in the experimental example, and
[0039] Fig. 8 shows H in Example 1 1.33 Mn 1.67 This shows the ion selectivity of the adsorption electrode with O4 applied, and
[0040] Figure 9 shows the ion selectivity of the adsorption electrode with HMn2O4 applied in Example 1, and
[0041] Figure 10 shows the ion selectivity of an adsorption electrode using HMn2O4 according to adsorption potential control (1.3V, 30 min on / off, 2 days) in Example 2, and
[0042] FIGS. 11a, 11b, and 11c show the ion selectivity of the recovered extract according to desorption conditions in Example 3, and
[0043] FIGS. 12a and 12b show the ion selectivity of the recovered extract according to adsorption conditions in Example 4, and
[0044] FIGS. 13 and 14 show the ion selectivity distribution containing extract according to the adsorption potential control conditions in Example 5, and
[0045] FIGS. 15a, 15b, and 15c show the ion selectivity distributions contained in the extracts applied to the adsorption electrodes prepared according to the HMO / carbon content ratio in Example 6, and
[0046] FIG. 16 is a schematic diagram of the manufacture of an electrode material for improving the conductivity and capacity of the adsorption electrode in Example 7, and
[0047] FIGS. 17a, 17b, 17c, and 17d are SEM images and EDS mappings of the LMO / carbon (P60) composite material prepared by the physical mixing method in Example 7. (a) SEM image, (b) / (c) / (d) EDS mapping, and
[0048] FIGS. 18a, 18b, 18c, and 18d are SEM images and EDS mappings of the LMO / carbon (P60) composite material prepared by the support method in Example 7. (a) SEM image, (b) / (c) / (d) EDS mappings, and
[0049] Figures 19a and 19b show the ion selectivity distributions contained in the extracts applied to the adsorption electrodes prepared according to the HMn2O4 / P60 mixing method in Example 8, and
[0050] FIG. 20 is a configuration diagram of an electric desalination system for concentrating lithium extract in Example 9, and
[0051] Figure 21 shows the change in lithium ion concentration in the adsorption / desorption reaction of the lithium extract with the P60 adsorption electrode applied in Example 9, and
[0052] FIG. 22 shows the change in lithium ion concentration in the secondary adsorption / desorption reaction with the application of the primary lithium concentrate in Example 10, and
[0053] Figure 23 shows the distribution of residual lithium concentration and precipitation efficiency after lithium phosphate precipitation according to the initial lithium ion concentration in Example 11, and
[0054] Figure 24 shows the distribution of residual PO4 concentrations according to the Ca / PO4 molar ratio based on the PO4 content of the lithium phosphate filtrate in Example 12.
[0055] The present invention is a method for selectively separating, concentrating, and recovering lithium ions from an aqueous lithium solution using an electro-adsorption process, and unlike existing technologies, it increases the selectivity and recovery rate of lithium ions.
[0056] The present invention will be described in more detail below with reference to the drawings.
[0057] Unless otherwise noted in the following description, % refers to weight %.
[0058] The attached drawings are merely examples illustrated to further explain the technical concept of the present invention, and therefore the concept of the present invention is not limited to the attached drawings.
[0059] In the following description, % represents mass % unless otherwise noted.
[0060] A method for recovering lithium according to an embodiment of the present invention will be described with reference to FIGS. 1 to 5.
[0061] FIG. 1 is a flowchart of a lithium recovery method according to one embodiment of the present invention, FIG. 2 is a flowchart showing a method for manufacturing an adsorption electrode in a lithium recovery method according to one embodiment of the present invention, FIG. 3 and FIG. 4 are for explaining a method for manufacturing an adsorption electrode in a lithium recovery method according to one embodiment of the present invention, and FIG. 5 is a flowchart of a process after lithium desorption in a lithium recovery method according to one embodiment of the present invention.
[0062] First, an adsorption electrode is prepared (S100).
[0063] The electric extraction process used in the present invention is a technology in which metal ions in an aqueous solution passing between electrodes are moved to the (-) electrode and anions to the (+) electrode while an electric potential is applied, and the ions are separated by electric adsorption at the electrode interface. The most important element technology is the development of an adsorption electrode material capable of adsorbing specific metal ions (lithium) at the electrode interface, based on the principle of being able to adsorb or desorb metal ions by changing only the potential of the electrodes.
[0064] The adsorption electrode may have an adsorption layer coated on the electrode body.
[0065] The electrode body may be made of graphite material, but is not limited to this, and may be in the form of a sheet.
[0066] The adsorption layer may include an adsorbent, a conductive carbon material, and a conductive polymer.
[0067] The adsorbent comprises an adsorbent represented by HxMnyOz and may have a spinel structure. Here, the x / y molar ratio may be 0.5 to 1.0 and Z may be 4. Or the x / y ratio may be 0.4 to 1.2 or 0.5 to 1.0 and the z / y ratio may be 1.5 to 3.0 or 1.8 to 2.6. Or x, y, and z may be 1.33, 1.67, and 4, respectively, or 1, 2, and 4.
[0068] The adsorbent can be obtained by leaching lithium from LMO.
[0069] The conductive carbon material may include at least one of activated carbon, graphite, graphene, carbon fiber, carbon nanotube, and carbon black.
[0070] Conductive polymers may include, but are not limited to, PvdF (polyvinylidene fluoride). In addition, NMP (N-methylpyrrolidone), polyacetylene, polyaniline, and polypyrrole may also be used.
[0071] The mass ratio of the adsorbent to the conductive carbon material may be 60 to 90 to 10 to 40 or 75 to 85 to 25 to 35.
[0072] The mass ratio of the adsorbent + conductive carbon material to the conductive polymer may be 85 to 95 to 5 to 15 or 89 to 93 to 7 to 11.
[0073] Adsorbents can be obtained by leaching lithium components from LMO materials.
[0074] Elution can be performed using a hydrochloric acid, sulfuric acid, or nitric acid solution of 0.1 to 2.0 M or 0.1 to 0.5 M at a solid-to-liquid ratio (g / L) of 0.5 to 20 or 0.5 to 2.0. The temperature may be room temperature, and the elution time may be 10 hours to 150 hours.
[0075] The adsorption layer can be manufactured by mixing an adsorbent, a conductive carbon material, a conductive polymer, and a solvent to prepare an adsorbent slurry in a slurry state, and coating the adsorbent slurry onto an electrode body.
[0076] In other embodiments, a conductive carbon material may not be used.
[0077] The solvent may be di-methylactamide, though not limited thereto.
[0078] Coating can be performed using a doctor blade, and the electrode body is coated to a thickness of 200 to 500 μm. After coating, it is dried at 40 to 90°C for 5 to 20 hours.
[0079] The adsorbent can be obtained by forming an LMO material by a method of supporting it on a conductive carbon material, and then leaching out a lithium component from the LMO material, which is explained with reference to FIGS. 2 to 4.
[0080] First, a lithium compound / manganese compound solution is prepared (S110).
[0081] For example, a solution (1M to 3M) is prepared using a water-soluble lithium compound / manganese compound (Li / Mn molar ratio: 0.5 to 1.0).
[0082] Next, the LMO component is formed by supporting it on a conductive carbon material (S120).
[0083] In this step, a conductive carbon material is immersed in a lithium / manganese compound mixed solution (immersion solid / liquid ratio: 10 g / 1 L to 1000 g / 1 L).
[0084] After filtration / drying, heat treatment is performed at 300 to 600°C to form an LMO structure, and the solution preparation or heat treatment is repeated so that the LMO loading amount is in the range of 50 to 90%.
[0085] Lithium is leached from the LMO component to form HMO (S130).
[0086] After the elution reaction is complete, filter / wash and dry.
[0087] Afterwards, a slurry is prepared together with a conductive polymer (S140) and coated onto the electrode body (S150).
[0088] Next, lithium is adsorbed onto the adsorption electrode using an electric adsorption process (S200).
[0089] In this step, a potential is applied to the adsorption electrode and the corresponding electrode to adsorb lithium from the lithium aqueous solution onto the adsorption electrode.
[0090] The lithium aqueous solution may contain at least one of sodium, potassium, magnesium, and calcium as impurity components other than the lithium component.
[0091] The lithium content may be 200 ppm or less, 300 ppm or less, 400 ppm or less, or 10,000 ppm, and the lower limit may be 50 ppm or 100 ppm.
[0092] The sodium content may be 1,000 to 20,000 ppm, the potassium content may be 50 to 1,000 ppm, the magnesium content may be 100 to 5,000 ppm, and the calcium content may be 50 to 1,000 ppm.
[0093] In the adsorption process, the adsorption selectivity of lithium can be 2 to 100 times higher than the selectivity of impurity components. In particular, the adsorption selectivity of lithium can be 2 to 20 times, 2 to 100 times, or 10 to 1,000 times higher than the selectivity of sodium. In addition, the adsorption selectivity of lithium can be 2 to 20 times or 2 to 100 times higher than the selectivity of potassium, magnesium, and calcium, respectively.
[0094] Selectivity is calculated based on the relative concentration of lithium ions to the sum of the concentrations of components contained in the lithium extract recovered after desorption, taking lithium as an example.
[0095] In the application of power during the adsorption stage, the application of the target potential and the application of the process reverse potential may be repeated. For example, this may be performed for 1 to 5 days with ~1.5V, step potential: 0.1 to 0.2V / 5 sec, 5 to 30 min on / ~-1.5V, step potential: -0.1 to -0.2V / 5 sec, 5 to 30 min on. Here, 1.5V is the target potential and -1.5V is the process reverse potential. The absolute values of the target potential and the process reverse potential may be 1.0V to 3.0V.
[0096] The absolute value of the process reverse potential may be smaller than the absolute value of the reverse potential during detachment.
[0097] After adsorption, deionized water is supplied (flushing) to the adsorption electrode to remove the remaining adsorption mother liquid. Subsequently, a reverse potential is applied to desorb lithium ions adsorbed on the adsorbent, thereby obtaining a lithium extract. The absolute value of the process reverse potential may be smaller than the absolute value of the reverse potential during desorption, and the reverse potential may be -1.5V to -3.5V. Specifically, desorption can be carried out for 5 to 24 hours with a reverse potential of -1.5 to -3.5V, a step potential of -0.1 to -0.2V / 5sec, and 5 to 30 min on.
[0098] Post-treatment of the obtained lithium extract is explained with reference to Fig. 5.
[0099] The lithium extract is concentrated electrically (S410).
[0100] In electroconcentration, lithium from the lithium extract is adsorbed onto an adsorption module containing conductive carbon and then desorbed, and this process can be repeated at least twice.
[0101] The concentration of lithium in the lithium concentrate obtained by electroconcentration may be 3,000 ppm or more, 4,000 ppm or more, or 5,000 ppm or more.
[0102] Next, the lithium in the lithium concentrate is converted into lithium phosphate (S420).
[0103] In this process, NaOH and phosphoric acid are added to the lithium concentrate to convert lithium into lithium phosphate, and then the lithium phosphate is recovered.
[0104] Next, the PO4 component is removed from the lithium phosphate filtrate (S430).
[0105] A calcium compound is added to the lithium phosphate filtrate after the recovery of lithium phosphate to remove at least a portion of the PO4 component of the lithium phosphate filtrate as calcium phosphate. Calcium chloride, calcium hydroxide, or calcium oxide may be used as the calcium compound.
[0106] Phosphoric acid is formed from calcium phosphate (S440).
[0107] Phosphoric acid is formed by adding a sulfuric acid solution to calcium phosphate, and the formed phosphoric acid can be used in the lithium phosphate recovery step. The formed phosphoric acid can be concentrated through heating and concentration or the like for use.
[0108] The present invention will be explained in more detail through the following experimental examples.
[0109] Preparation Example 1
[0110] LMO (LiMn2O4 and Li 1.33 Mn 1.67 O4) material was applied as a raw material for adsorption electrodes, and the Li component was deleached from LMO to manufacture the adsorbent powder into an electrode, and the resulting material was used as the electrode material. The elution reaction was carried out at room temperature for 72 hours using a 0.3M HCl solution under conditions where the solid (adsorbent, g) / liquid (HCl, L) ratio was 1. After the elution reaction was completed, the HMO powder was filtered, washed, and dried, and then used as a raw material for manufacturing the electrode material.
[0111] To manufacture the adsorbent powder into an electrode, polyvinylidene fluoride (PvdF), a conductive polymer binder, was used as the binder material, and a graphite sheet was used as the current collector. To prepare the PvdF solution, a 10%-PvdF solution was prepared by dissolving it in DMAc (Di-methylacetamide) solvent, and then a slurry was prepared by uniformly mixing the adsorbent powder with the 9%-PvdF solution using a paste mixer.
[0112] To manufacture the adsorption electrode, a uniformly mixed slurry was cast onto the surface of a graphite current collector to a thickness of approximately 300 μm using an automatic coating machine equipped with a doctor blade. After drying the electrode coated with the adsorbent at 60°C, it was cut to a size of 10 cm x 10 cm to be mounted on an adsorption module, and a hole with an inner diameter of 5 mm was formed in the center of the adsorption electrode to create a flow path for smooth contact with the aqueous solution.
[0113] experimental apparatus
[0114] As shown in Fig. 6, the adsorption module assembly with the adsorption electrode was configured as a unit module by stacking in the order of acrylic plate / +electrode / anion exchange membrane (AEM) / spacer / cation exchange membrane (CEM) / -electrode / acrylic plate. A flow path for flow in and flow out can be formed across the acrylic plate / +electrode / anion exchange membrane (AEM) / spacer.
[0115] At this time, to induce a uniform contact reaction between the adsorption electrode and the aqueous solution, a flow path was formed so that the solution could be supplied to the inside of the adsorption electrode through a hole with an inner diameter of 2 mm at the corner of the adsorption electrode, and an acrylic plate (15 mm T x 160 mm L x 160 mm W) was fabricated so that the solution could be discharged after the reaction through a hole with an inner diameter of 5 mm at the center of the adsorption electrode. Ion exchange membranes (AEM and CEM) were used to prevent loss of ion recovery rate by blocking the movement of detached ions to the opposite electrode during the desorption process in which a reverse potential is applied after the completion of the electro-adsorption reaction.
[0116] The product name of the cation exchange membrane is NEOSEPTA, and the company is ASTOM Corporation of Japan. (4) A spacer is a type of mesh (nylon mesh, urethane mesh, etc.) installed to secure space due to thickness so that fluid can flow into the electrode.
[0117] As shown in Fig. 7, the electric extraction system was configured with (a) a water tank, (b) a metering pump, (c) an adsorption module, (d) a conductivity sensor, (e) a data collection module, (f) a rectifier, and (g) a rectifier control and data collection device, and a lithium-containing solution was supplied into the adsorption module to analyze the conductivity and current / potential behavior according to operating potential.
[0118] Example 1
[0119] Adsorption electrode raw materials were prepared using H-Mn-O material, and a slurry was prepared by uniformly mixing it with adsorbent powder at a 9%-PvdF content ratio. The adsorption electrode was manufactured by casting the uniformly mixed slurry onto the surface of a graphite current collector to a thickness of approximately 300 μm using an automatic coating machine equipped with a doctor blade, followed by drying in a 60°C oven for 12 hours. After assembling the adsorption module, the adsorption reaction was carried out by circulating 500 mL of a solution containing Li, Na, K, Mg, and Ca ions, each with a concentration of 100 ppm, at a flow rate of 100 mL / min for approximately 2 days without potential change (off).
[0120] After the adsorption was completed, 100 mL of distilled water was circulated at a flow rate of 100 mL / min to the electrode at which the adsorption was completed, and the lithium ion selectivity of the adsorption electrode was evaluated. The selectivity was calculated based on the relative concentration of lithium ions to the sum of the concentrations of components contained in the lithium extract recovered after desorption.
[0121] As shown in Figures 8 and 9, through the analysis of the ion composition and content contained in the desorption solution from the experimental results, H 1.33 Mn 1.67 O4 showed a lithium selectivity of approximately 41.9%, and HMn2O4 showed a lithium selectivity of approximately 60.3%.
[0122] Example 2
[0123] The adsorption reaction was carried out for 2 days using an adsorption electrode composed of HMn2O4 material, applying a potential of 1.3 V and circulating the adsorption mother liquor at a flow rate of 100 mL / min for 30 minutes, then turning off the potential and maintaining it for 30 minutes to flush out ions saturated on the electrode surface. After the adsorption reaction was completed, a desorption potential of -3.5 V was applied, and 100 mL of distilled water was circulated at a flow rate of 100 mL / min for 1 hour to recover the sample, after which the lithium ion selectivity of the adsorption electrode was evaluated.
[0124] From the experimental results of Figure 10, the composition and content of ions recovered during the electro-adsorption and desorption process were analyzed, and the selectivity of lithium ions was observed to be approximately 56.1%, which was confirmed to be slightly lower compared to the ion exchange method adsorption and electro-desorption efficiency.
[0125] Example 3
[0126] The adsorbent used in Examples 3 to 5 is HMn2O4.
[0127] We intended to investigate the conditions for improving lithium selectivity according to the desorption conditions of the electric adsorption electrode. A mother liquor of 500 mL was prepared using chlorides to contain Li, Na, K, Mg, and Ca ions, each with a concentration of 100 ppm. The mother liquor was circulated into the adsorption module at a flow rate of 100 mL / min. To prevent overcurrent formation during the process of reaching the target potential value (1.3 V), the target potential was reached by maintaining the device at each step potential (0.2 V) for 5 seconds. During the adsorption reaction, the device was operated repeatedly for 3 days in a pattern of maintaining the ON state for 30 minutes at the target potential and then maintaining the OFF state for 30 minutes.
[0128] After the adsorption reaction was completed, 100 mL of distilled water was used as the desorption solution and circulated at a flow rate of 100 mL / min to evaluate the selectivity of lithium ions according to the desorption process control conditions during the recovery process. In order to suppress the incorporation of impurity ions into the recovered solution by removing the solution remaining inside the electrode during the desorption process, after the adsorption reaction was completed, the inside of the electrode was (1) flushed with air to remove the residual solution, (2) washed the residual solution by circulating distilled water, and (3) flushed with distilled water to remove residual impurity ions, and then the ions were recovered by applying a reverse potential of 3.5 V.
[0129] Figures 11a, 11b, and 11c show the distribution of metal ions contained in the recovered lithium solution according to desorption conditions. The highest lithium ion selectivity (Li selectivity: 61%) was observed when residual ions were removed by flushing with distilled water before the desorption reaction. It was observed that the lithium ion selectivity decreased when unadsorbed impurity ions remained inside the electrode. Therefore, potential control conditions for removing residual impurity ions inside the electrode are also considered important to improve lithium ion selectivity.
[0130] Example 4
[0131] In the electro-adsorption reaction process, 1 L of solution with a concentration of 100 ppm of each ion (Li, Na, K, Mg, Ca) was prepared, and the solution was circulated into the adsorption module at a flow rate of 100 mL / min. The adsorption reaction was carried out for 3 days using (1) electro-adsorption (30 min on / off, 1.3 V) and (2) physical adsorption (off). Before the desorption reaction, distilled water was supplied into the adsorption module to flush the interior so that the conductivity of the discharged solution reached the conductivity of distilled water. After washing, the desorption potential (-3.5 V) was applied to analyze the ion selectivity contained in the recovered solution.
[0132] As shown in Figures 12a and 12b, from the results of the ion selectivity analysis of the extraction solution recovered by the same desorption method after electro-adsorption and physical adsorption, a slightly higher lithium ion selectivity was observed in the case of electro-adsorption, and the lithium ion concentration in the recovered solution was approximately 12.9 ppm in the case of the electro-adsorption method, which was higher than that of physical adsorption (5 ppm).
[0133] Example 5
[0134] In the case of the flushing method using distilled water to remove impurity ions remaining at the electrode interface during the recovery process after electroadsorption, it was confirmed that lithium ion selectivity was slightly improved, but it is considered to have the limitation of using an excessive amount of water. In this experiment, a method to improve lithium ion selectivity through adsorption potential control was investigated to separate impurity ions remaining at the electrode interface during the adsorption reaction.
[0135] In the electro-adsorption reaction process, 1 L of solution with a concentration of 100 ppm of each ion (Li, Na, K, Mg, Ca) was prepared and the solution was circulated into the adsorption module at a flow rate of 100 mL / min. As shown in Fig. 13, the adsorption reaction was carried out for 3 days by repeating the operation in a pattern of (1) reaching the target potential (1.1 V) and maintaining it for 3 minutes, then maintaining it in the off state for 5 minutes, and as shown in Fig. 14, the adsorption reaction was carried out for 3 days in a pattern of (2) reaching the target potential (1.1 V) and maintaining it for 3 minutes, then reaching the potential to -1.1 V and maintaining it in the off state for 5 minutes. The lithium selectivity according to the system operating conditions was evaluated.
[0136] We intended to analyze the separation efficiency of impurity ions remaining at the electrode interface due to the application of reverse potential during the adsorption reaction, and separated the extract by applying the same desorption conditions (-3.5V).
[0137] C. Analysis of lithium ion selectivity in the extract according to adsorption potential control confirmed that when a reverse potential is applied during the separation process of unadsorbed ions, the lithium ion selectivity improves to approximately 81%.
[0138] Example 6
[0139] We intended to evaluate lithium ion selectivity by applying an electroadsorption process to a solution containing high concentrations of various ions other than lithium ions. For the adsorption mother liquor, a low-grade salt lake mother liquor was prepared by adding LiCl to filtered seawater to achieve a lithium ion concentration of approximately 200 ppm.
[0140] The composition of the salt lake simulant solution is as shown in Table 1 below.
[0141]
[0142]
[0143] H as an adsorption electrode material 1.33 Mn 1.67 O4 was applied and uniformly mixed with flake graphite according to weight ratio. An adsorption electrode was prepared by mixing this with a PvdF solution to achieve a powder:PvdF weight ratio of 8:2 and casting the resulting slurry. Under adsorption conditions, 200 mL of the simulated solution was circulated into the adsorption module at a flow rate of 100 mL / min. The applied adsorption potential was set to 1.3 V, maintained for 3 minutes, then switched off and maintained for another 3 minutes; this pattern was repeated to conduct the adsorption reaction for 3 days. After the reaction was completed, distilled water was supplied into the adsorption module to remove residual impurity ions at the electrode interface. Subsequently, distilled water was circulated, and an inverse potential of 3.5 V was applied to separate the extract.
[0144] From the experimental results shown in Figs. 15a, 15b, and 15c, it was observed that the lithium ion selectivity decreased as the carbon content increased. This is attributed to the fact that as the carbon content increased, the adsorption capacity of the electrode material increased, and +2 valence metal ions and Na ions present at high concentrations penetrated into the electrode interface and interior, preventing the smooth removal of residual impurity ions using distilled water. When an electrode with an HMO / carbon content ratio of 90% / 10% was applied, the lithium ion selectivity value in the lithium extract was confirmed to be approximately 61%.
[0145] Example 7
[0146] The separation efficiency of metal ions in aqueous solutions using electro-extraction technology varies depending on the conductivity and capacity of the electrode material; therefore, we aimed to examine the design of electrode materials to improve the separation speed and capacity of metal ions. Although lithium-selective adsorbent materials (LMOs) were introduced as electrode materials for the selective extraction of lithium ions from aqueous solutions containing various metal ions, they are subject to limitations due to a decrease in conductivity during the manufacturing process of carbon / adsorbent composite materials compared to carbon materials.
[0147] To address the problem of reduced conductivity depending on the particle size and amount of adsorbent incorporated during the physical mixing process of carbon and adsorbent, a method was examined to secure conductivity and capacity by forming adsorbent components on the surface of the carbon material.
[0148] A method was attempted to introduce an adsorbent component to the surface of a carbon material by using a water-soluble reactant (Li-acetate / Mn-acetate) to prepare a Li / Mn-acetate solution by mixing and dissolving it in distilled water under conditions where the Li / Mn molar ratio is 0.5, then supporting the carbon material (P60) and separating / drying it, followed by heat treatment.
[0149] FIG. 16 is a schematic diagram of the manufacture of an electrode material for improving the conductivity and capacity of an adsorption electrode.
[0150] SEM imaging and EDS mapping analysis were performed on the product prepared according to physical mixing and impregnation of the carbon surface so that the LMO:C content ratio was approximately 4:6 during the manufacturing process of the LMO / carbon (P60) composite material.
[0151] The method for forming an LMO structure on a carbon surface involved immersion in a 1M Li / Mn acetate solution (Li / Mn molar ratio: 0.5) for about 1 hour, followed by separation / drying and heat treatment at 500 degrees.
[0152] As shown in Figs. 17a, 17b, 17c, 17d, 18a, 18b, 18c, and 18d, for composite materials prepared by physical mixing, the EDS mapping results confirmed that the mixing uniformity of the carbon material and LMO components was low and the particles were locally concentrated, whereas for composite materials prepared by supporting LMO components on the surface of the carbon material, a fine LMO structure was uniformly formed on the surface of the carbon material and the mixing uniformity of each component was observed to be high.
[0153] Example 8
[0154] To evaluate the lithium extraction efficiency using an LMO / carbon (P60) composite material prepared by the impregnation method, HMn2O4 was applied as the adsorption electrode material. The P60 carbon material was prepared by impregnating it in a 1M Li / Mn acetate (Li / Mn molar ratio: 0.5) solution, followed by filtration, drying, and heat treatment, so that the LMO / P60 content ratio was approximately 7:3. Before application as an electrode material, the LMO / P60 and hydrochloric acid solution were mixed and stirred using a 0.3M hydrochloric acid solution under conditions where the solid (g) / liquid (L) ratio was 1. After the elution reaction, the mixture was prepared into a slurry with an HMO / P60 and PvdF content (g) ratio of 92:8, and this was cast onto the surface of a graphite current collector to a thickness of approximately 300 μm using an automatic coating machine equipped with a doctor blade. For comparative evaluation of the loading / physical mixing method, each powder was mixed to have the same LMO / P60 content ratio (approx. 7:3), and an electrode was manufactured after preparing a slurry and casting using the same method.
[0155] For the adsorption mother liquor, LiCl was added to filtered seawater to prepare a low-grade salt lake mother liquor (Li 107 ppm, Na 9853 ppm, K 317 ppm, Mg 1115 ppm, Ca 341 ppm) with a lithium ion concentration of approximately 100 ppm. Under adsorption conditions, 200 mL of the solution was circulated into the adsorption module at a flow rate of 100 mL / min. The applied adsorption potential was set to 1.3 V, maintained for 5 minutes, then turned off and maintained for another 5 minutes, repeating this pattern to carry out the adsorption reaction for one day. After the reaction was completed, distilled water was supplied into the adsorption module to remove impurity ions remaining at the electrode interface, and then distilled water was circulated to apply a reverse potential of 3.5 V to separate the extract.
[0156] As shown in FIGS. 19a and 19b, when the adsorption electrodes prepared by different HMO / carbon mixing methods were applied, the results of the ion selectivity analysis of the recovered extract showed that the electrode prepared by the loading method had a higher lithium ion selectivity (72%) than the electrode prepared by the physical mixing method (60%).
[0157] Example 9
[0158] An adsorption module consisting of 200 P60 adsorption electrodes was applied to prepare a high-concentration lithium solution from the lithium extract recovered by applying a lithium-selective electric extraction system. The HMO adsorption electrode was used without separate pretreatment for the application of the electroconcentration process of the recovered lithium extract. Figure 20 shows the configuration diagram of the electric desalination system for concentrating the lithium extract in Example 9.
[0159] The composition and content of the lithium extract are as shown in Table 2.
[0160] Table 2
[0161]
[0162] Using an HMO adsorption electrode, 50 L of the recovered lithium extract mother solution was circulated into the adsorption module at a flow rate of 13 L / min to reach an adsorption potential of 1.3 V, and the adsorption reaction was carried out for 10 minutes. After the adsorption reaction was completed, air was blown into the electrode to remove the residual solution and discharge it into the adsorption mother solution storage tank. Then, 4 L of distilled water was circulated into the adsorption module as the desorption solution to reach a desorption potential of -1.3 V, and the desorption reaction was carried out for 10 minutes. Before starting the second adsorption reaction, air was blown into the electrode to remove the remaining desorption solution inside the electrode and discharge it into the desorption solution storage tank.
[0163] As shown in Figure 21, the concentration of lithium ions contained in the residual liquid after three cycles was observed to be about 1 ppm, and the concentration of lithium ions contained in the solution recovered after desorption was about 401 ppm, and the lithium ion recovery rate was confirmed to be about 97%.
[0164] Example 10
[0165] Separation and concentration experiments were conducted using the same electrode configuration and operating method to prepare a concentrate, using a solution with a lithium concentration of approximately 401 ppm recovered from the lithium extract through a primary electro-desalination process as a raw material. As shown in Figure 22, in the case of the adsorption reaction, a lithium recovery rate of approximately 90.4% and a residual lithium ion concentration of 39.5 ppm were observed after 5 repetitions. Regarding the lithium ions contained in the solution recovered after desorption, a lithium concentration of approximately 2,277 ppm was observed after 2 repetitions and approximately 3,579 ppm after 5 repetitions. The deionized water generated in the electro-lithium concentration process can be recycled as process water.
[0166] 50 L of lithium extract was used as the raw material (target for electroadsorption) and 4 L of deionized water as the recovery solution (desorption solution) to produce 4 L of lithium concentrate with a concentration of approximately 401 ppm (recovery rate 97%). During the process of producing the lithium concentrate, deionized water with a lithium ion concentration of 1 ppm or less (0.3 ppm or less for Na, K, Mg, and Ca concentrations, respectively) was produced as a byproduct, and the deionized water is at a level where it can be recycled as washing water and desorption solution in the electroadsorption process.
[0167] Due to the use of a limited amount of raw material, the maximum concentration reached during the first concentration reaction is limited by the adsorbent / desorbent ratio, but as the adsorbent / desorbent ratio increases, the maximum concentration reached can increase.
[0168] In this experiment, primary concentrated water was used as a secondary concentrated water raw material to produce a concentrated solution with a lithium ion concentration of 2000 ppm or higher.
[0169] Example 11
[0170] We intended to evaluate the efficiency of lithium phosphate production from the lithium concentrate recovered through an electric lithium concentration process, and analyzed the lithium phosphate recovery rate according to the lithium ion concentration in the reaction between a lithium chloride solution and a caustic soda / phosphoric acid solution. Under reaction conditions, caustic soda (NaOH) and phosphoric acid (H3PO4) solutions were added to the lithium chloride solution such that the molar ratios of Li / PO4 and Na / PO4 were each 3, and the reaction was carried out at room temperature for 8 hours while maintaining a stirring speed of 300 RPM.
[0171] From the experimental results of Figure 23, it was observed that the recovery rate of the lithium phosphate precipitation reaction was very low at about 8% under the condition where the initial concentration of lithium ions was 250 ppm, and that the recovery rate of the lithium phosphate precipitation reaction also increased to about 90% when the initial concentration of lithium ions was increased to about 3000 ppm.
[0172] Example 12
[0173] When PO4 components remain in the filtrate after the production of lithium phosphate from the lithium concentrate recovered through an electric lithium concentration process, losses occur due to the formation of lithium phosphate during the concentration of unrecovered lithium components. To suppress this, the efficiency of PO4 removal using Ca(OH)2 was evaluated to eliminate the PO4 components remaining as impurities.
[0174] Sodium hydroxide (NaOH) and phosphoric acid (H3PO4) solutions were added to a lithium chloride solution with a lithium ion concentration of about 2000 ppm so that the molar ratios of Li / PO4 and Na / PO4 were each 3, and the reaction was carried out at room temperature for 8 hours while maintaining a stirring speed of 300 RPM, after which the lithium phosphate powder was separated from the filtrate.
[0175] The lithium ion concentration in the filtrate was analyzed to be approximately 330 ppm and the PO4 ion concentration to be approximately 1500 ppm. The Ca / PO4 molar ratio based on the PO4 ion concentration was adjusted to a range of 1.5 to 4, and after adding Ca(OH)2, the reaction was carried out by stirring at 300 RPM for 24 hours at room temperature.
[0176] From the experimental results in Figure 24, it was observed that under conditions where the Ca / PO4 molar ratio was 3 or higher, more than 99% of the PO4 component was removed, and no Ca component remained.
[0177] No loss of content was observed in the remaining lithium components, and it was confirmed that the remaining lithium solution could be concentrated to over 2000 ppm through the electroconcentration process described in Examples 9 and 10 and recycled as a raw material for the production of lithium phosphate.
[0178] Example 13
[0179] In the separation process of the PO4 component contained in the filtrate after the production of lithium phosphate, the PO4 component was precipitated and separated using Ca(OH)2, and a conversion method to recover the phosphoric acid component from the precipitate was examined. The compound converted through the reaction of Ca and the PO4 component was identified as calcium phosphate, an insoluble phosphate, and to recover the phosphoric acid component from it, the phosphoric acid component was separated from calcium phosphate using sulfuric acid as shown in the following formula.
[0180]
[0181] Calcium phosphate powder and 2M sulfuric acid solution were mixed under conditions where the solid (g) / liquid (L) ratio was 200, and the reaction was carried out by stirring at 300 RPM for 12 hours at room temperature. After separating and analyzing the filtrate, it was confirmed that the PO4 content was approximately 99,000 ppm and the residual SO4 content was approximately 9,000 ppm.
[0182] After concentrating the recovered solution at 80°C for 10 hours, the PO4 content of the prepared solution was confirmed to be approximately 930,000 ppm. This was used as a raw material for producing lithium phosphate from a lithium chloride solution with a lithium ion concentration of approximately 2,000 ppm. By quantitatively adding the solution such that the Li / PO4 and Na / PO4 molar ratios were each 3, a reaction was performed at room temperature for 24 hours, and a lithium phosphate recovery rate of approximately 85% was confirmed.
Claims
1. A method for recovering lithium from an aqueous lithium solution using an electro-adsorption process, The method includes the step of applying a potential to an adsorption electrode and a corresponding electrode to adsorb lithium from a lithium aqueous solution onto the adsorption electrode. The above adsorption electrode includes an adsorbent represented by HxMnyOz, and Here, a method in which the x / y ratio is 0.4 to 1.2 and the z / y ratio is 1.5 to 3.
0.
2. In Paragraph 1, The above-mentioned adsorption electrode is, It includes an adsorption layer containing the above-mentioned adsorbent, and The above adsorption layer comprises the above adsorbent and the conductive carbon material, and A method in which the mass ratio of the adsorbent to the conductive carbon material is 60 to 90 to 10 to 40.
3. In Paragraph 2, A method in which the conductive carbon material comprises at least one of activated carbon, graphite, graphene, carbon fiber, carbon nanotube, and carbon black.
4. In Paragraph 2, The above adsorption layer further comprises a conductive polymer, and A method in which the mass ratio of the adsorbent + the conductive carbon material to the conductive polymer is 85 to 95 to 5 to 15.
5. In Paragraph 4, The above conductive polymer is a method comprising PvdF.
6. In Paragraph 2, The above adsorbent is obtained by a method of leaching a lithium component from an LMO material.
7. In Paragraph 6, The above elution is performed using a hydrochloric acid, sulfuric acid, or nitric acid solution of 0.1 to 2.0 M at a solid-to-liquid ratio (g / L) of 0.5 to 20.
8. In Paragraph 6, The above adsorbent is obtained by forming the LMO material by a method of supporting it on the conductive carbon material, and then leaching the lithium component from the LMO material.
9. In Paragraph 4, The above-mentioned adsorption electrode is, It further includes an electrode body coated with the above-mentioned adsorbent, The above-mentioned adsorption electrode is, It is obtained by coating an adsorbent slurry onto the above electrode body, and A method comprising the adsorbent slurry comprising the adsorbent, the conductive carbon material, the conductive polymer, and a solvent.
10. In Paragraph 4, The above lithium aqueous solution further contains impurity components, and The above impurity component includes at least one of sodium, potassium, magnesium, and calcium, and A method in which the adsorption selectivity of the lithium above is 2 to 100 times higher than the selectivity of the sodium component above.
11. In Paragraph 10, A method further comprising the step of applying a reverse potential to the adsorption electrode after the above adsorption to desorb lithium ions adsorbed on the adsorbent.
12. In Paragraph 11, A method further comprising the step of flushing the adsorption electrode with deionized water before applying a reverse potential in the above desorption.
13. In Paragraph 11, A method in which the application of power during the adsorption step involves the repeated application of a target potential and a process reverse potential, wherein the absolute value of the process reverse potential is smaller than the absolute value of the reverse potential during desorption.
14. In Paragraph 11, The method further includes a step of electroconcentrating the lithium extract recovered from the above desorption to increase the lithium concentration, A method of repeating the process of adsorbing and desorbing lithium from the lithium extract solution onto an adsorption module containing conductive carbon at least twice in the above electroconcentration.
15. In Paragraph 14, The lithium concentration in the lithium concentrate obtained by the above electroconcentration is 3000 ppm or higher, and A method further comprising the process of recovering lithium phosphate by adding phosphoric acid to a lithium concentrate.
16. In Paragraph 15, A method further comprising the step of adding a calcium compound to the lithium phosphate filtrate after the recovery of the lithium phosphate, thereby removing at least a portion of the PO4 component of the lithium phosphate filtrate as calcium phosphate.
17. In Paragraph 16, A method further comprising the step of adding a sulfuric acid solution to the calcium phosphate to form phosphoric acid, wherein the phosphoric acid is used in the step of recovering lithium phosphate.