Negative electrode and all-solid-state battery including same

The use of graphite and linear conductive materials in the negative electrode of all-solid-state batteries addresses lithium ion transport issues, maintaining energy density and stability by minimizing solid electrolyte use, enhancing capacity retention and cycle stability.

WO2026235248A1PCT designated stage Publication Date: 2026-11-12LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2025/022394
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-12-11
Filing Date
2025-12-19
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional liquid electrolyte-based lithium-ion batteries face challenges in all-solid-state batteries due to the difficulty of securing lithium ion transport pathways within the anode, complicating the manufacturing process and reducing energy density when solid electrolytes are introduced, and potential side reactions occur.

Method used

A negative electrode for all-solid-state batteries using a cathode active material comprising graphite and a linear conductive material, such as multi-walled carbon nanotubes, with minimal solid electrolyte inclusion to maintain energy density and stability, enhancing conductivity and mechanical strength.

Benefits of technology

The solution provides a negative electrode with improved capacity retention, cycle stability, and high-rate characteristics without significantly introducing solid electrolytes, balancing energy density and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2025022394_12112026_PF_FP_ABST
    Figure KR2025022394_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode for an all-solid-state battery and an all-solid-state battery including same, the negative electrode comprising a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material and a linear conductive material, the negative electrode active material comprises graphite, and the linear conductive material comprises multi-walled carbon nanotubes (MWCNT). According to the present invention, an anode for an all-solid-state battery having an excellent balance among energy density, cycle stability, and high-rate characteristics, and an all-solid-state battery including same, can be provided without substantially incorporating a solid electrolyte into the negative electrode active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode and all-solid-state battery including the same

[0001] The present application claims the benefit of priority based on Korean Patent Application No. 10-2025-0059934 filed May 8, 2025 and Korean Patent Application No. 10-2025-0196508 filed December 11, 2025, and all contents disclosed in the documents of said Korean patent applications are incorporated herein as part of the specification. The present invention relates to a negative electrode and an all-solid-state battery including the same.

[0002] Lithium-ion batteries (LIBs) are widely used in electric vehicles, energy storage devices, and electronic equipment due to their high energy density and long lifespan. In particular, graphite, used as the anode material in LIBs, remains a primary anode material to this day due to its stability and excellent performance.

[0003] Conventional liquid electrolyte-based LIB systems feature the electrolyte effectively penetrating the anode, allowing lithium ions to move smoothly through the interlayer structure of graphite. This structural characteristic is one of the key factors enabling graphite anodes to achieve superior performance.

[0004] However, when using a graphite anode in an all-solid-state battery, there is a problem due to the limitation that, unlike conventional liquid electrolytes, the solid electrolyte has difficulty effectively securing lithium ion transport pathways within the anode.

[0005] To solve the aforementioned problems, a technology involving the mixing of a solid electrolyte with a graphite anode has been considered. However, this method complicates the manufacturing process, and the incorporation of the solid electrolyte into the anode active material layer reduces the proportion of the anode active material, thereby lowering the energy density of the all-solid-state battery. Furthermore, side reactions between the solid electrolyte and the anode active material can occur, potentially leading to an increase in the battery's internal resistance.

[0006] Accordingly, the present invention aims to provide a negative electrode for an all-solid-state battery and an all-solid-state battery including the same, which has an excellent balance between energy density, cycle stability, and high-rate characteristics without substantially introducing a solid electrolyte into the negative electrode active material layer.

[0007] One aspect of the present invention relates to a cathode for an all-solid-state battery comprising a cathode current collector and a cathode active material layer disposed on the cathode current collector, wherein the cathode active material layer comprises a cathode active material and a linear conductive material, wherein the cathode active material comprises graphite and the linear conductive material comprises a multi-walled carbon nanotube (MWCNT).

[0008] In one embodiment, the linear conductive material may further include one or more selected from the group comprising carbon nanofibers (CNF) and vapor-grown carbon fibers (VGCF).

[0009] In one embodiment, the ratio of the length to the average diameter of the linear conductive material may be 500 or more to 5000 or less.

[0010] In one embodiment, the linear conductive material may have a length of 10 μm or more to 50 μm or less.

[0011] In one embodiment, the linear conductive material may have an average diameter of 1 nm or more to 20 nm or less.

[0012] In one embodiment, the linear conductive material has a bulk density of 50 kg / m³ 3 From 170 kg / m² or more 3 It may be less than.

[0013] In one embodiment, the linear conductive material has a specific volume of 1 cm 3 / g or more up to 5 cm 3 It may be less than / g.

[0014] In one embodiment, the linear conductive material has a BET specific surface area of ​​100 m² 2 / g or more to 350 m 2 It may be less than / g.

[0015] In one embodiment, the linear conductive material may have a powder resistivity of 1 mΩ*cm or more to 20 mΩ*cm or less.

[0016] In one embodiment, the linear conductive material is I G / I D It may be 0.8 or more to 1.3 or less.

[0017] In one embodiment, the negative electrode for an all-solid-state battery of the present invention may contain 2 wt% or less of a solid electrolyte relative to the total weight of the negative electrode active material layer.

[0018] In one embodiment, the negative electrode for an all-solid-state battery of the present invention may contain 90 wt% or more of a negative electrode active material relative to the total weight of the negative electrode active material layer.

[0019] In one embodiment, the weight ratio of the negative active material to the linear conductive material may be 15 or more to 65 or less.

[0020] Another aspect of the present invention relates to an all-solid-state battery comprising a positive electrode, a solid electrolyte layer, and a negative electrode for the all-solid-state battery as described above.

[0021] According to the present invention, it is possible to provide a negative electrode for an all-solid-state battery having a capacity retention rate and cycle stability with an excellent balance between energy density, cycle stability, and high-rate characteristics, and an all-solid-state battery including the same, without substantially introducing a solid electrolyte into the negative electrode active material layer.

[0022] Figure 1 is a graph showing the results of evaluating the capacity retention rate of an all-solid-state battery according to the cycle.

[0023] Figure 2 is a graph showing the results of the capacity retention rate evaluation according to the C-rate of an all-solid-state battery.

[0024] Terms and words used in this specification and claims shall not be interpreted as being limited to their ordinary or dictionary meanings, but shall be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0025] Therefore, it should be understood that the configuration of the embodiments described in this specification is merely one of the most preferred embodiments of the present invention and does not represent all of the technical ideas of the present invention, and that various equivalents and modifications that can replace them may exist at the time of filing this application.

[0026] In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0027] In this specification, when a part is described as “comprising” a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. Thus, for example, a composition comprising compound A may include compounds other than A. However, the term “comprising” also encompasses, as a specific embodiment thereof, “essentially / essentially composed of” and “composed of” in a more restrictive sense; for example, a “composition comprising compound A” may also be (essentially / essentially) composed of compound A.

[0028] In connection with this, terms such as “comprising” or “having,” as described in this specification, are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0029] In this specification, when any layer is described as being located “on” another arbitrary layer, this includes not only cases where any layer is in contact with another arbitrary layer, but also cases where another layer or material exists between the two layers.

[0030] Where in this specification a quantity, concentration, or other value or parameter is given as an enumeration of a range, a preferred range, a preferred upper limit, and a preferred lower limit, it should be understood that any pair of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the range is disclosed separately, specifically discloses all ranges that may be formed. Where a range of numerical values ​​is mentioned in this specification, unless otherwise stated, for example, without limiting terms such as greater than or less than, the range is intended to include its endpoint value and all integers and fractions within that range. The scope of the invention is not intended to be limited to the specific value mentioned when defining the range.

[0031] Among the physical properties mentioned in this specification, if the measured temperature affects the property, the property is measured at room temperature unless specifically otherwise specified. The term "room temperature" refers to a natural temperature that has not been heated or cooled, and may mean, for example, any temperature within the range of about 10°C to 30°C, about 23°C, or about 25°C. Furthermore, unless specifically otherwise specified, the unit of temperature in this specification is °C.

[0032] Among the physical properties mentioned in this specification, if the measured pressure affects the physical property, unless otherwise specifically defined, the physical property is measured at normal pressure, that is, atmospheric pressure (about 1 atmosphere).

[0033] Unless otherwise specifically defined in this specification, content means weight %.

[0034] The first aspect of the present invention relates to a negative electrode for an all-solid-state battery.

[0035] The present invention may relate to a cathode for an all-solid-state battery, for example, comprising a cathode current collector and a cathode active material layer disposed on the cathode current collector, wherein the cathode active material layer comprises a cathode active material and a linear conductive material, and the cathode active material comprises graphite.

[0036] In this specification, the term "graphite cathode" refers to a cathode in which the cathode active material layer comprises at least graphite among the cathode active materials. Unless specifically described otherwise, this does not mean that other cathode active materials other than graphite are included, or that other components (e.g., binder, solid electrolyte, additive, etc.) other than the cathode active material are included in the cathode active material layer.

[0037] In this specification, graphite may refer to any one of natural graphite, artificial graphite, and combinations thereof. In this specification, natural graphite may refer to untreated natural graphite or modified natural graphite, and artificial graphite may refer to artificial graphite produced by heating petroleum coke or pitch coke as raw materials in an electric furnace at 2,500°C or higher. The average particle size (D) of each of the natural graphite and artificial graphite 50 ) may be, for example, 10 μm or more to 25 μm or less, but is not limited thereto. The above average particle size (D 50 ) is measured, for example, using the laser diffraction method, and may refer to the particle diameter at which the cumulative volume in the particle size distribution corresponds to 50% of the total. The BET specific surface area of ​​the natural graphite is, for example, 1.2 m² 2 It can be greater than / g, and 1.3m in another example. 2 / g or more, 1.4m 2 / g or more, 1.5m 2 / g or more or 1.6m 2 / g or more, or 3m 2 / g or less, 2.8 m 2 / g or less, 2.6 m 2 / g or less, 2.4 m 2 / g or less, 2.2 m 2 / g or less, 2.0 m 2 / g or less or 1.8 m 2 It may be less than or equal to / g, but is not limited thereto. The BET specific surface area of ​​the above artificial graphite is, for example, 1 m² 2 It can be less than / g, and 0.9 m in other examples. 2 / g or less or 0.8 m 2 / g or less, or 0.1 m 2 / g or more, 0.2 m 2 / g or more, 0.3 m 2 / g or more, 0.4 m 2 / g or more, 0.5 m 2 / g or more, 0.6 m 2 / g or more or 0.7 m 2 It may be greater than / g but is not limited thereto.

[0038] In this specification, graphite may be, for example, a combination of natural graphite and artificial graphite. The graphite may be, for example, a combination of natural graphite and artificial graphite in a weight ratio of 1:1 to 1:9, and in other examples, may be 1:2 to 1:7 or 1:3 to 1:5, but is not limited thereto. By using a graphite that combines natural graphite and artificial graphite in the above ratios, the present invention can further improve the expression capacity and performance.

[0039] The present invention can provide a cathode with an excellent balance of energy density, cycle stability, and high-rate characteristics without substantially introducing a solid electrolyte by using a linear conductive material having the characteristics described below in combination with other components in the cathode active material layer.

[0040] In this specification, a linear conductive material is a concept distinguished from a point conductive material having a particle shape close to spherical, such as carbon black, acetylene black, or graphite powder, and a linear conductive material may mean a conductive material having a one-dimensional structure in the form of, for example, a line, tube, thread, or fiber. At least one linear conductive material may be intertwined or clustered together to form a bundle or an agglomerate, and the agglomerate may, in some cases, have a shape close to spherical, but is not particularly limited.

[0041] The above-mentioned linear conductive material may include Multi-Walled Carbon Nanotubes (MWCNTs) to further improve the lifespan characteristics and high-rate performance of the all-solid-state battery by ensuring stable contact between active materials even during repeated charge and discharge cycles. By introducing MWCNTs as linear conductive materials into the negative electrode active material layer, high conductivity can be secured with a smaller amount compared to the introduction of point-type conductive materials, which can help improve the energy density of the battery. Additionally, mechanical strength can be enhanced by forming a network structure between the linear conductive materials.

[0042] The above linear conductive material may further include one or more selected from the group including, for example, carbon nanofiber (CNF) and vapor-grown carbon fiber (VGCF).

[0043] Although the above linear conductive material may have the disadvantage of low dispersibility, the inventors have confirmed that by introducing a linear conductive material having the characteristics described below, the occurrence of entanglement due to low dispersibility can be controlled and processability can also be further improved.

[0044] For example, the ratio of length to average diameter of the above linear conductive material may be 500 or more to 5000 or less. In other examples, the ratio of length to average diameter of the above linear conductive material may be 600 or more, 700 or more, 800 or more, 900 or more, 1000 or more, 1100 or more, 1200 or more, or 1300 or more, or 4900 or less, 4800 or less, 4700 or less, 4600 or less, 4500 or less, 4400 or less, 4300 or less, 4200 or less, 4100 or less, 4000 or less, 3900 or less, 3800 or less, 3700 or less, 3600 or less, 3500 or less, 3400 or less, or 3300 or less.

[0045] The linear conductive material may, for example, have a length of 10 μm or more and 50 μm or less. In other examples, the linear conductive material may have a length of 11 μm or more, 12 μm or more, 13 μm or more, 14 μm or more, 15 μm or more, 16 μm or more, or 17 μm or more, or 49 μm or less, 48 ​​μm or less, 47 μm or less, 46 μm or less, 45 μm or less, 44 μm or less, 43 μm or less, or 42 μm or less, but is not limited thereto. The length of the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0046] The above linear conductive material may, for example, have an average diameter of 1 nm or more to 20 nm or less. In other examples, the above linear conductive material may have an average diameter of 2 nm or more, 3 nm or more, 4 nm or more, 5 nm or more, 6 nm or more, 7 nm or more, 8 nm or more, 9 nm or more, or 10 nm or more, or 19 nm or less, 18 nm or less, 17 nm or less, or 16 nm or less, but is not limited thereto. The average diameter of the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0047] The above linear conductive material has, for example, a bulk density of 50 kg / m³3 From 170 kg / m² or more 3 It may be less than or equal to. In another example, the above linear conductive material has a bulk density of 60 kg / m³. 3 Above, 70 kg / m² 3 Above, 80 kg / m² 3 Above, 90 kg / m² 3 110 kg / m³ or more 3 or greater than 160 kg / m² 3 Below, 150 kg / m² 3 Below, 140 kg / m² 3 Below, 130 kg / m² 3 120 kg / m³ or less or less than 120 kg / m³ 3 It may be less than, but is not limited to. The bulk density of the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0048] The above linear conductive material has, for example, a specific volume of 1 cm 3 / g or more up to 5 cm 3 It may be less than / g. In another example, the above linear conductive material has a specific volume of 1.5 cm³ 3 / g or more, 2.0 cm 3 / g or more or 2.5 cm 3 / g or more, or 4.5 cm 3 / g or less, 4.0 cm 3 / g or less, 3.5 cm 3 / g or less or 3.0 cm 3 It may be less than or equal to / g, but is not limited thereto. The specific volume of the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0049] The above linear conductive material has, for example, a BET specific surface area of ​​100 m² 2 / g or more to 350 m 2 It may be less than / g. In another example, the above linear conductive material has a BET specific surface area of ​​150 m². 2 / g or more, 180 m 2 / g or more or 200 m 2 / g or more, or 300 m 2 / g or less, 280 m 2 / g or less, 250 m 2 / g or less or 220 m 2 It may be less than or equal to / g, but is not limited thereto. The BET specific surface area of ​​the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0050] The above linear conductive material may, for example, have a powder resistivity of 1 mΩ*cm or more to 20 mΩ*cm or less. In other examples, the above linear conductive material may have a powder resistivity of 3 mΩ*cm or more, 5 mΩ*cm or more, 7 mΩ*cm or more, or 9 mΩ*cm or more, or 18 mΩ*cm or less, 16 mΩ*cm or less, 14 mΩ*cm or less, 12 mΩ*cm or less, or 10 mΩ*cm or less, but is not limited thereto. The powder resistivity of the linear conductive material may be measured, for example, in the manner according to the evaluation example described below.

[0051] The above linear conductive material is, for example, I G / I D α may be 0.8 or more to 1.3 or less. In another example, the above linear conductive material is I G / I D α may be 0.85 or higher, 0.9 or higher, 0.95 or higher, 1.0 or higher, or 1.05 or higher, or 1.25 or lower, 1.2 or lower, or 1.15 or lower, but is not limited thereto. I of the linear conductive material G / I D It may be measured in the manner according to the evaluation example described below, for example.

[0052] The present invention, by combining the above-described configurations, can control the weight of the components included in the negative electrode active material layer as described below, and accordingly, can provide a battery having excellent ion conductivity and energy density without substantially introducing a solid electrolyte into the negative electrode active material layer.

[0053] In this specification, the meaning of "substantially not introducing a solid electrolyte into the negative electrode active material layer" may mean, for example, that a solid electrolyte is not intentionally introduced into the negative electrode active material layer. However, this does not mean that the possibility is excluded that the solid electrolyte of the solid electrolyte layer may be included in the surface and / or interior of the negative electrode active material layer due to the negative electrode active material layer being in contact with the solid electrolyte layer.

[0054] The cathode of the present invention may, for example, contain 2 wt% or less of a solid electrolyte relative to the total weight of the cathode active material layer. In another example, the cathode of the present invention may contain 1.5 wt% or less, 1 wt% or less, 0.5 wt% or less, 0.4 wt% or less, 0.3 wt% or less, 0.2 wt% or less, or 0.1 wt% or less of the solid electrolyte relative to the total weight of the cathode active material layer, and preferably, the cathode active material layer may not contain a solid electrolyte.

[0055] The negative active material may comprise, for example, 90 wt% or more relative to the total weight of the negative active material layer. In other examples, the negative active material relative to the total weight of the negative active material layer may comprise 90.5 wt% or more, 91 wt% or more, 91.5 wt% or more, 92 wt% or more, 92.5 wt% or more, 93 wt% or more, 93.5 wt% or more, or 94 wt% or more, or 99 wt% or less, 98 wt% or less, 97 wt% or less, 96 wt% or less, or 95 wt% or less. By enabling the negative active material layer to comprise the negative active material as described above through a combination of such configurations, the present invention can further improve the energy density of the battery.

[0056] The above-described negative electrode active material layer may be characterized by including, for example, a linear conductive material in an amount of 1 wt% or more to 5 wt% or less. In another example, the above-described negative electrode active material layer may include a linear conductive material in an amount of 1.5 wt% or more or 2 wt% or more, or 4.5 wt% or less, 4 wt% or less, 3.5 wt% or less, or 3 wt% or less.

[0057] The weight ratio of the negative active material to the linear conductive material may be, for example, 15 or more to 65 or less. In other examples, the weight ratio of the negative active material to the linear conductive material may be 20 or more, 25 or more, or 30 or more, or 60 or less, 55 or less, 50 or less, 45 or less, 40 or less, or 35 or less.

[0058] The above cathode active material layer may further include, for example, a binder.

[0059] Examples of the above binders include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol (PVA), polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone (PVP), polytetrafluoroethylene (PTFE), polyethylene (PE), polypropylene (PP), butadiene rubber (BR), ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.

[0060] For example, the binder may be included in an amount of less than 3 wt% with respect to the negative electrode active material layer. In other examples, the binder may be included in an amount of less than 2.8 wt% or less than 2.6 wt% with respect to the negative electrode active material layer, or in an amount of 1 wt% or more, 1.5 wt% or more, or 2 wt% or more.

[0061] The ratio of the thickness of the cathode active material layer to the above-mentioned cathode current collector may be, for example, 10 or less. In this specification, thickness may mean, for example, average thickness, and average thickness may mean the value obtained by averaging the thickness of any 5 to 10 points on the measurement target. In this specification, thickness may mean the thickness after isotropic pressing unless specifically described otherwise. In other examples, the ratio of the thickness of the cathode active material layer to the above-mentioned cathode current collector may be 9.5 or less, 9 or less, 8.5 or less, 8 or less, or 7.5 or less, or 3 or more, 4 or more, 5 or more, 6 or more, or 7 or more.

[0062] The thickness of the above-mentioned cathode current collector may be, for example, 0.1 μm or more to 100 μm or less. In another example, the thickness of the above-mentioned cathode current collector may be 5 μm or more to 20 μm or less.

[0063] The thickness of the above-mentioned cathode active material layer may be, for example, 3 μm or more to 100 μm or less. In other examples, the thickness of the above-mentioned cathode active material layer may be 10 μm or more, 20 μm or more, 30 μm or more, 40 μm or more, 50 μm or more, 60 μm or more, or 70 μm or more, or 95 μm or less, 90 μm or less, 85 μm or less, 80 μm or less, or 75 μm or less.

[0064] The above-described negative electrode active material may be characterized by optionally further including silicon or transition metal oxide, for example. By combining graphite with the above-described composition as the negative electrode active material, the stability of the SEI layer (solid electrolyte interface layer) is improved, and excellent conductivity can be achieved, while also possessing high capacity and high-speed charge / discharge characteristics.

[0065] The silicon may be, for example, any one of solid silicon, silicon alloy, silicon oxide, silicon / carbon composite, and combinations thereof. The silicon / carbon composite is, for example, carbon being SiO₂ x (0≤x<2) By heat treatment in a state combined with particles, the carbon material becomes SiO x (0≤x<2) Form coated on the particle surface or SiO x (0≤x<2) The particles may have a form in which carbon is dispersed in an atomic state inside, but are not limited thereto. The average particle size (D of the above silicon) 50 ) is, for example, 5 μm or more to 20 μm or less and the maximum particle size (D max ) may be 30 µm or more to 40 µm or less, and the tap density is 0.1 g / cm³ 3 0 to 5 g / cm² 3 It may be less than or equal to, but is not limited thereto. The above average particle size (D 50 ) and maximum particle size (D max ) may be measured using, for example, the laser diffraction method.

[0066] The above transition metal oxide may be, for example, any one of iron oxide (Fe2O8, Fe3O4), cobalt oxide (Co3O4), manganese oxide (MnO2, Mn3O4), nickel oxide (NiO), copper oxide (CuO, Cu2O), vanadium oxide (V2O5), molybdenum oxide (MoO3), titanium oxide (TiO2), and combinations thereof.

[0067] The above-mentioned cathode active material layer may additionally include, for example, additives. The additives may be, for example, fillers, coating agents, dispersants, thickeners, ion conductivity aids, etc., but are not limited thereto, and any known material generally used for cathodes may be used without limitation.

[0068] The above-mentioned cathode current collector may have one or more shapes selected from, for example, thin, plate, mesh, punched metal, and foam. The above-mentioned cathode current collector may be, for example, a metal foil or a metal mesh, or a carbon sheet. As for the metal constituting the cathode current collector, at least one selected from copper, nickel, chromium, gold, platinum, silver, aluminum, iron, titanium, zinc, cobalt, vanadium, magnesium, lead, germanium, indium, tin, zirconium, and stainless steel may be exemplified. The above-mentioned cathode current collector may include at least one metal selected from copper, nickel, and stainless steel in order to ensure reduction resistance. The cathode current collector may, for example, have a carbon coating layer on its surface. The cathode current collector may also be, for example, a metal foil or a substrate on which the above-mentioned metal is plated or deposited.

[0069] A second aspect of the present invention relates to an all-solid-state battery.

[0070] The details regarding the first aspect of the present invention may be applied in the same way to the details regarding the second aspect unless specifically described otherwise.

[0071] The present invention may be characterized by including, for example, an anode, a solid electrolyte layer, and the aforementioned cathode.

[0072] The all-solid-state battery of the present invention may, for example, have a capacity retention rate of 80% or more at 1C. In other examples, the all-solid-state battery of the present invention may have a capacity retention rate of 82% or more, 84% or more, 86% or more, or 88% or more at 1C, and the upper limit is not specifically limited. The capacity retention rate of the all-solid-state battery at 1C may be measured, for example, in the manner according to the evaluation example described below.

[0073] The all-solid-state battery of the present invention may, for example, have a ratio of the discharge capacity in 90 cycles to the discharge capacity in 1 cycle of 80% or more. In other examples, the all-solid-state battery of the present invention may have a ratio of the discharge capacity in 90 cycles to the discharge capacity in 1 cycle of 81% or more, 82% or more, 83% or more, 84% or more, 85% or more, or 86% or more, and the upper limit is not particularly limited. The ratio of the discharge capacity in 90 cycles to the discharge capacity in 1 cycle of the all-solid-state battery may be measured, for example, in the manner according to the evaluation example described below.

[0074] The above anode may include, for example, an anode current collector and an anode active material layer located on at least one surface of the anode current collector.

[0075] The above positive active material layer may optionally include, for example, a binder, a conductive material, a solid electrolyte and / or additives together with the positive active material.

[0076] The above-mentioned positive electrode active material reversibly absorbs and desorbs lithium ions. The above-mentioned positive electrode active material may be, for example, lithium transition metal oxides such as lithium cobalt oxide (LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese oxide (NCM), lithium manganate, and lithium iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, iron oxide, or vanadium oxide, but is not limited thereto; any material used as a positive electrode active material in the relevant technical field may be used. The above-mentioned positive electrode active material may be used individually or in a mixture of two or more types.

[0077] The above lithium transition metal oxide is, for example, Li a A 1-b B b D2 (wherein 0.90≤a≤1, and 0≤b≤0.5); Li a Ni 1-b-c Co b B c O 2-α F2(wherein 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0 <α<2); Li a Ni 1-b-c Mn b B c D α (In the above formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0≤α≤2); Li a Ni 1-b-c Co b B c D α (In the above formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2); Li a E 1-b B b O 2-c D c(In the above formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05); LiE 2-b B b O 4-c D c (In the above formula, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b B c O 2-α F α (In the above formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a CoG b O2(wherein the above formula, 0.90≤a≤1, 0.001≤b≤0.1); Li a MnG b O2(wherein the above formula, 0.90≤a≤1, 0.001≤b≤0.1); Li a Mn2GbO4 (wherein the above formula, 0.90≤a≤1, 0.001≤b≤0.1); Li a Ni 1-b-c Mn b B c O 2-α F α (In the above formula, 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2(wherein 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni b E c G d O2(wherein 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c Mn d GeO2 (wherein the above formula, 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0 ≤d≤0.5, 0.001≤e≤0.1); Li a NiG bO2 (wherein the above equation, 0.90≤a≤1, 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3- f) J2(PO4)3(0≤f≤2); Li (3-f) Fe2(PO4)3(0≤f≤2); it may be a compound represented by any one of the chemical formulas of LiFePO4. In such a compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; and J may be V, Cr, Mn, Co, Ni, Cu, or a combination thereof. As a positive electrode active material, a compound having a coating layer added to the surface of such a compound may be used, or a mixture of the compound described above and the compound having a coating layer added may be used. A coating layer added to the surface of such compounds may contain, for example, a lithium ion conductive oxide. The lithium ion conductive oxide is, for example, LiNbO3, Li4Ti5O 12 Examples include Li3PO4, but are not limited thereto. The compounds forming this coating layer may be amorphous or crystalline. Methods for forming the coating layer may include, for example, spray coating or immersion methods, but can be selected without limitation as long as they do not adversely affect the physical properties of the cathode active material.

[0078] When the above-mentioned positive active material is a ternary lithium transition metal oxide such as NCA or NCM and contains nickel (Ni), it may be possible to increase the capacity density of the all-solid-state battery and reduce the metal leaching of the positive active material in the charged state, and accordingly, the cycle characteristics of the all-solid-state battery in the charged state may be improved.

[0079] The shape of the above-mentioned positive active material may be a particle shape, for example, a sphere, an elliptical sphere, etc. The particle size of the positive active material is not particularly limited and must be within a range applicable to the positive active material of a conventional all-solid-state secondary battery. The content of the positive active material of the positive is also not particularly limited and must be within a range applicable to the positive of a conventional all-solid-state secondary battery.

[0080] Regarding the binder included in the positive active material layer, for example, the details concerning the binder included in the negative active material layer described above may be applied in the same way, and the binder included in the negative active material layer and the binder included in the positive active material layer may each be the same or different from each other.

[0081] The conductive material included in the above-mentioned positive active material layer can be used to improve the conductivity of the positive electrode, and can be used without special restrictions as long as it is conductive without causing chemical changes. Examples include carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskies such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be included.

[0082] The solid electrolyte included in the above-mentioned positive electrode active material layer may include, for example, sulfide-based solid electrolytes, oxide-based solid electrolytes, polymer-based solid electrolytes, and / or halide-based solid electrolytes, but is not limited thereto.

[0083] The above sulfide-based solid electrolyte contains sulfur atoms (S), has ionic conductivity of metals belonging to Group 1 or Group 2 of the periodic table, and may have electronic insulation properties. The above sulfide-based solid electrolyte preferably contains at least Li, S, and P as elements and has lithium ion conductivity, but may include other elements other than Li, S, and P depending on the purpose or case. As the above-mentioned sulfide-based solid electrolyte, for example, Li2S-P2S5, Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2OP2S5, Li2S-LiBr-P2S5, Li2SLi2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, Li2SGa2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2SSiS2, Li2S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2SSiS2-Li3PO4, or Li 10 GeP2S 12The above may include the above. The above sulfide-based solid electrolyte may include an azirodite-based solid electrolyte comprising one or more selected from Li6PS5F, Li6PS5Cl, Li6PS5Br, Li6PS5I, or Li6PS5X (where X is two or more selected from F, Cl, Br, and I). Alternatively, the above sulfide-based solid electrolyte may include an amorphous sulfide glass manufactured using Li2S, P2S5, etc. as a raw material, or may include a glass ceramic obtained by heat treating the sulfide glass, but is not limited thereto.

[0084] The above oxide-based solid electrolyte is, for example, LiPON, Li 3x La(2 / 3-x)(1 / 3-2x)TiO3(0.04 <x<0.16), Li 1+x Al x Ti 2-x (PO4)3(0 <x<2), Li 1+x Al x Ge 2-x (PO4)3(0 <x<2), Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr, Ti)O3, Pb 1-x La x Zr 1-y Ti y O3(0≤x<1, 0≤y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3, HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3(0 <x<2, 0<y<3), Li x Al y Ti z (PO4)3(0 <x<2, 0<y<1, 0<z<3), Li 1+x+y(Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1 0≤y≤1), Li x La y TiO3(0 <x<2, 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M is Te, Nb, or Zr, 1≤x≤10), Li7La3Zr2O 12 , Li 3+x La3Zr 2-a M a O 12 (M is Ga, W, Nb, Ta, or Al, 0 <a<2, 1≤x≤10) 또는 이들의 조합을 포함할 수 있다. 또한 산화물계 고체 전해질은 Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M-doped LLZO, M=Ga, W, Nb, Ta, or Al, 0 <a<2, 1≤x≤10) 중에서 선택된 가넷계(Garnet-type) 고체 전해질, 또는 리튬-알루미늄-티타늄 인산염계(LATP, Li 1+x Al x Ti 2-x (PO4)3), lithium-aluminum-germanium phosphate system (LAGP, Li 1.5 Al 0.5 Ge 1.5 It may include a NASICON-based solid electrolyte selected from (PO4)3-based, lithium-silicon-titanium phosphate-based (LSTP, LiSiO2TiO2(PO4)3), or a combination thereof, but is not limited thereto.

[0085] The above oxide-based solid electrolyte may be crystalline, amorphous, glassy, ​​or glass-ceramic, and may have various crystalline states depending on the manufacturing method and composition.

[0086] The above-mentioned polymer-based solid electrolyte is not particularly limited to any polymer material that is an ion-conducting material and is commonly used as a solid electrolyte material for all-solid-state batteries. The above-mentioned polymer-based solid electrolyte may include, for example, polyether-based polymers, polycarbonate-based polymers, acrylate-based polymers, polysiloxane-based polymers, phosphazene-based polymers, polyethylene oxide (PEO), polyethylene derivatives, alkylene oxide derivatives, phosphate ester polymers, polyaisation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, or polymers containing ionic dissociators. Alternatively, the above-mentioned polymer-based solid electrolyte may include, as a polymer resin, a branched copolymer, a comb-like polymer, and a cross-linked polymer resin, etc., in which an amorphous polymer such as polymethyl methacrylate (PMMA), polycarbonate, polysiloxane, and / or phosphazene is copolymerized as a comonomer to a polyethylene oxide (PEO) main chain.

[0087] The above-mentioned halide-based solid electrolyte may, for example, contain a halogen element as the main component of anion. Containing a halogen element as the main component of anion may mean that the proportion (molar ratio) of the halogen element is the highest among all anions constituting the halide-based solid electrolyte. The ratio of the halogen (X) element to all anions constituting the above-mentioned halide-based solid electrolyte may, for example, be 50 mol% or more, 70 mol% or more, 90 mol% or more, or 100 mol%. The halogen element may be one or more types. The above-mentioned halide-based solid electrolyte may, for example, not contain a sulfur element (S element). The above-mentioned halide-based solid electrolyte may, for example, contain a Li element, an M element (M is a metal other than Li), and an X element. X may, for example, be F, Cl, Br, I, or a combination thereof. The above halide-based solid electrolyte may include, for example, Br or Cl as X. The above halide-based solid electrolyte may include, for example, a metal element such as Sc, Y, B, Al, Ga, or In as M. The composition of the above halide-based solid electrolyte is, for example, Li 6-3a M a Br b Cl c (M is a metal other than Li, and 0 <a<2, 0≤b≤6, 0≤c≤6, b+c=6)일 수 있다. 상기 할라이드계 고체 전해질은 예를 들어 Li3YBr6, Li3YCl6, 또는 Li3YBr2C l4 It could be the back.

[0088] More specifically, the solid electrolyte may include a sulfide-based solid electrolyte in terms of achieving high energy density and stability. Specifically, the solid electrolyte may include an azirodite-based sulfide solid electrolyte, but is not limited thereto.

[0089] Regarding the additives included in the positive electrode active material layer, for example, the details concerning the additives included in the negative electrode active material layer described above may be applied in the same way, and the additives included in the negative electrode active material layer and the additives included in the positive electrode active material layer may each be the same or different from one another.

[0090] The thickness of the above positive active material layer may be, for example, 50 μm or more to 200 μm or less, more specifically 70 μm or more to 150 μm or less, and more specifically 80 μm or more to 110 μm or less, but is not limited thereto.

[0091] The anode current collector may have one or more shapes selected from, for example, thin, plate, mesh, punched metal, and foam. The anode current collector may be composed of, for example, a metal foil or a metal mesh, and may be a metal foil for ease of handling, but is not limited thereto. Examples of metals constituting the anode current collector include at least one selected from copper, nickel, chromium, gold, platinum, silver, aluminum, iron, titanium, zinc, cobalt, vanadium, magnesium, lead, germanium, indium, tin, zirconium, and stainless steel. The anode current collector may include aluminum for the purpose of ensuring oxidation resistance. The anode current collector may have a carbon coating layer on its surface, for example. The anode current collector may also be, for example, a metal foil or a substrate on which the metal is plated or deposited. The thickness of the positive current collector may be, for example, 0.1 μm or more or 1 μm or more, 1 mm or less or 100 μm or less, but is not limited thereto.

[0092] For example, the same provisions regarding the solid electrolyte included in the above-described solid electrolyte included in the anode active material layer may apply to the solid electrolyte included in the above-described solid electrolyte layer, and the solid electrolyte included in the above-described solid electrolyte layer and the solid electrolyte included in the anode active material layer may be the same or different from each other. However, the average particle size of the solid electrolyte included in the anode active material layer may be smaller than the average particle size of the solid electrolyte included in the solid electrolyte layer.

[0093] The thickness of the solid electrolyte layer may be, for example, 30 μm or more to 100 μm or less. In other examples, the thickness of the solid electrolyte layer may be 35 μm or more to 80 μm or less, 40 μm or more to 70 μm or less, or 45 μm or more to 60 μm or less, but is not limited thereto.

[0094] In the following, the present invention is described in detail with reference to examples to specifically explain the disclosure of the present invention as described above and the intended functions and effects of the present invention. However, the examples may be modified in various different forms, and the scope of this specification is not to be interpreted as being limited only to these examples. It is emphasized that the examples are provided to represent the present invention and to explain it more specifically to those skilled in the art.

[0095] Example.

[0096] (cathode)

[0097] A slurry for the negative electrode active material layer was prepared by mixing graphite, a conductive material, and a binder with NMP (N-methyl-2-pyrrolidone) in a weight ratio of 94.5:3:2.5 based on dry weight. In this case, a mixture of artificial graphite and natural graphite in a weight ratio of 8:2 was used as the graphite, and the conductive material had a length of 17 μm to 42 μm, an average diameter of 13 nm, and a bulk density of 115 kg / m³. 3 and the specific volume is 2.7 cm 3 It is / g, and the BET specific surface area is 212 m² 2 / g, the powder resistivity is 9.8 mΩ*cm, and I G / I D Multiwall Carbon Nanotube (MWCNT) with a value of 1.1 was used, and PVDF was used as the binder.

[0098] The above slurry for the negative electrode active material layer was uniformly applied onto a 10㎛ thick copper foil using a blade coater, and vacuum dried at 120℃ for 10 minutes to obtain a negative electrode with a negative electrode active material layer having a thickness of 143㎛ (before isotropic pressurization). At this time, the loading amount of the negative electrode active material layer was approximately 4.43 mAh / cm² 2 It was.

[0099] (anode)

[0100] LiNi as the positive active material 0.8 Co 0.15 Mn 0.05 O2 (NCM), an azirodite-based (Li6PS5Cl) sulfide solid electrolyte, carbon nanofiber (CNF) as a conductive material, and polytetrafluoroethylene (Teflon binder) as a binder were prepared. The above materials were mixed in a weight ratio of positive active material : solid electrolyte : conductive material : binder = 83.7 : 14.9 : 0.2 : 1.2 based on dry weight, and then formed into a large sheet to produce a positive electrode sheet. Subsequently, the positive electrode sheet was compressed onto a 12 µm thick aluminum foil to produce a positive electrode. The loading amount of the positive active material layer (positive electrode sheet) was 4.1 mAh / cm². 2 It was.

[0101] (Solid electrolyte layer)

[0102] As a solid electrolyte layer, a solid electrolyte layer with a thickness of 10 μm was used, comprising an azirodite-based (Li6PS5Cl) sulfide solid electrolyte and a binder.

[0103] (Solid-state battery)

[0104] The positive electrode, solid electrolyte layer, and negative electrode were laminated and sealed in a pouch under vacuum. Here, parts of the positive and negative current collectors were extended outward from the pouch to maintain the battery's vacuum. These extensions served as the positive and negative terminals.

[0105] Next, an all-solid-state battery was manufactured by applying a hydrostatic pressure (WIP) treatment at 500 MPa for 30 minutes to the above pouch. After the hydrostatic pressure treatment, the thickness of the negative electrode active material layer was 72.7 μm (after isotropic pressure), the thickness of the solid electrolyte layer was 50 μm, and the thickness of the positive electrode active material layer was 95 μm. The N / P ratio of the manufactured all-solid-state battery was 1.08.

[0106] Comparative Example 1.

[0107] An all-solid-state battery was manufactured in the same manner as in the example, except that a slurry for the negative electrode active material layer was prepared by mixing graphite and a binder with NMP (N-methyl-2-pyrrolidone) in a weight ratio of 97.5:2.5 based on dry weight without a conductive material.

[0108] Comparative Example 2.

[0109] An all-solid-state battery was manufactured in the same manner as in the example, except that a point-type conductive material (carbon black) was used instead of MWCNT (Multiwall Carbon Nanotube) having the same characteristics as in the example as the conductive material.

[0110] Comparative Example 3.

[0111] A solid-state battery was manufactured in the same manner as in the example, except that when manufacturing the cathode, graphite, a conductive material, and a binder were mixed with NMP (N-methyl-2-pyrrolidone) in a weight ratio of 96.0:1.5:2.5 based on dry weight to prepare a slurry for the cathode active material layer, and SWCNT (Singlewall Carbon NanoTube) was used instead of MWCNT (Multiwall Carbon NanoTube) as the conductive material.

[0112] Evaluation Example 1. Energy Density Evaluation

[0113] The results of calculating the volume energy density for the all-solid-state batteries manufactured in the above examples are as shown in Table 1 below.

[0114] The volumetric energy density (Wh / L) of the battery is measured according to Equation 1 below.

[0115] [Equation 1]

[0116] Volumetric energy density = (Q Х V ave ) / Battery volume (L)

[0117] In Equation 1 above, Q is the discharge capacity (Ah) of the battery, and V ave This is the nominal voltage, which corresponds to the average operating voltage during battery discharge.

[0118] Charge and discharge were performed in a cell with an arbitrary discharge capacity within the range of 3 V to 4.25 V, and the measured nominal voltage (V ave The volume energy density was calculated by substituting ) into Equation 1.

[0119] Classification Energy Density (Wh / L) Example 486

[0120] Evaluation Example 2. Evaluation of capacity retention rate according to cycle

[0121] For the above Examples and Comparative Examples 1 to 3, the capacity retention rate according to the cycle was measured at the following operating voltage range and operating temperature of 60°C. The specific charge / discharge conditions are as follows.

[0122] (Charging / Discharging Conditions)

[0123] Charging: 0.33 C 4.2V CC / CV, 0.1C cut-off

[0124] Discharge: 0.33C, 3.0V, CC

[0125] Under the above conditions, a total of 90 charge-discharge cycles were repeated, and the capacity retention rate was defined as the relative ratio (%) of the discharge capacity after one cycle to the discharge capacity after one cycle based on the discharge capacity of each cycle. As a result, as shown in Figure 1, it was confirmed that the Example and Comparative Example 1 had excellent lifespan characteristics, whereas Comparative Example 2 showed a significantly reduced capacity retention rate after 50 cycles, and Comparative Example 3 showed a significantly reduced capacity retention rate after 10 cycles.

[0126] Evaluation Example 3. Evaluation of Capacity Retention Rate According to C-Rate (Charging / Discharging Speed)

[0127] For the above Examples and Comparative Examples 1 to 3, the capacity retention rate according to the C-rate was measured at the following operating voltage range and operating temperature of 60°C. The specific charge and discharge conditions are as follows.

[0128] (Charging / Discharging Conditions)

[0129] Charging: 0.33 C 4.2V CC / CV method, 0.1C cut-off

[0130] Discharge: CC method at 0.1C, 0.33C, 0.5C, 1C, 0.1C, and 0.33C up to 3.0V

[0131] Under the conditions described above, the discharge capacity was measured while varying the discharge C-rate in steps. The ratio (%) of the discharge capacity at each C-rate to the discharge capacity at 0.1 C-rate was defined as the capacity retention rate according to the C-rate, and the results are shown in FIG. 2. As shown in FIG. 2, it was confirmed that in the case of the example, there was little performance degradation even at high rates, whereas Comparative Examples 1 to 3 showed rapid performance degradation as the C-rate increased.

[0132] Evaluation Example 4. Measurement of the length of a linear conductive material

[0133] To measure the length of the linear conductive material, the sample was dispersed in ethanol, and then ultrasonically dispersed using a probe sonicator for about 15 minutes. The prepared dispersion was applied onto a glass substrate by drop casting and air-dried at room temperature. The dried sample was observed using a scanning electron microscope (SEM), with the acceleration voltage set to 10 kV and the magnification set to 30,000x. A total of 20 SEM images were acquired, and the lengths of 20 individual CNTs per image were measured using Image J software. The total of 400 measured length data points were averaged to define the length of the linear conductive material.

[0134] Evaluation Example 5. Measurement of the average diameter of a linear conductive material

[0135] The average diameter of the linear conductive material was measured in the same manner as in Evaluation Example 1, except that the observation magnification was set to 100,000 times.

[0136] Evaluation Example 6. Measurement of bulk density of linear conductive material

[0137] After placing sufficiently dried linear conductive material powder into an antistatic cylinder, the volume was measured after tapping it vertically about 300 times, and the mass of the sample was measured, and the mass of the sample / volume after tapping was defined as the bulk density of the linear conductive material.

[0138] Evaluation Example 7. Measurement of specific volume of linear conductive material

[0139] After spinning a linear conductive material to produce a filament of approximately 5 cm, the filament samples were separated into multiple strands and dried in a vacuum oven at 60°C for 2 hours to remove residual moisture. The mass m of the filament in air was measured using an ultra-precision microbalance (resolution 0.01 mg). air Measure the apparent mass m in toluene. LAfter measuring, the specific volume was calculated using the following Equations 2 and 3. At this time, the mass was measured using a high ionizer at room temperature under 45 ± 5% RH conditions. This measurement was repeated at least 5 times, and the average value was taken as the specific volume of the linear conductive material.

[0140] [Equation 2]

[0141] V = (m air - m L ) / ρ L

[0142] In Equation 2, V is the volume of the filament, and m air is the mass of the filament in air, and m L is the apparent mass of the filament, and ρ L is the density of toluene at room temperature.

[0143] [Equation 3]

[0144] ν = V / m air

[0145] In Equation 3, ν is the specific volume of the filament.

[0146] Evaluation Example 8. Measurement of BET specific surface area of ​​linear conductive material

[0147] The BET specific surface area of ​​the linear conductive material was measured according to ASTM D6556-18.

[0148] Evaluation Example 9. Measurement of powder resistivity of linear conductive material

[0149] The linear conductive material powder was dried in an 80°C oven for 2 hours to remove residual moisture and organic matter, and then stabilized for at least 1 hour at room temperature and a relative humidity of 45% ±5%. Subsequently, approximately 100 mg of the powder was loaded into a tungsten carbide die and compressed at a pressure of 10 tonf for 1 minute to produce a pellet with a diameter φ=13 mm and a thickness L≈1 mm. After separating the compressed pellet from the die, the diameter and thickness were precisely measured using digital calipers. Next, silver paste was evenly applied to both sides of the pellet to form electrodes, and the electrical resistance R was measured using a current source / voltmeter (based on a Kirchhoff circuit), after which the powder resistivity was calculated using Equation 4 below.

[0150] [Equation 4]

[0151] ρ=R×L / A

[0152] In Equation 4, ρ is the resistivity of the powder, R is the electrical resistance, A is the area through which the current flows, and L is the length in the direction of current flow.

[0153] The average value was measured at least 5 times under the same conditions and taken as the powder resistivity of the linear conductive material.

[0154] Evaluation Example 10. Measurement of Raman properties of a linear conductive material

[0155] Linear conductive material powder was evenly distributed on a slide, and the Raman spectrum was measured under conditions of a wavelength of 633 nm and an output of 1 mW or less. D band (~1350 cm⁻¹) -1 ) and G band (~1580 cm -1 The location was checked, and fitting was performed using the Lorentzian function.

Claims

1. A cathode comprising a cathode current collector and a cathode active material layer disposed on the cathode current collector, wherein the cathode active material layer comprises a cathode active material and a linear conductive material, wherein the cathode active material comprises graphite and the linear conductive material comprises MWCNT (Multi-Walled Carbon Nanotube). A cathode for an all-solid-state battery.

2. The negative electrode for an all-solid-state battery according to claim 1, wherein the linear conductive material further comprises one or more selected from the group comprising carbon nanofibers (CNF) and vapor-grown carbon fibers (VGCF).

3. A negative electrode for an all-solid-state battery according to claim 1, wherein the ratio of the length to the average diameter of the linear conductive material is 500 or more to 5000 or less.

4. The negative electrode for an all-solid-state battery according to claim 1, wherein the linear conductive material has a length of 10 μm or more to 50 μm or less.

5. The negative electrode for an all-solid-state battery according to claim 1, wherein the linear conductive material has an average diameter of 1 nm or more to 20 nm or less.

6. In claim 1, the linear conductive material has a bulk density of 50 kg / m³ 3 From 170 kg / m² or more 3 Lee Ha-in, negative electrode for all-solid-state battery.

7. In claim 1, the linear conductive material has a specific volume of 1 cm 3 / g or more up to 5 cm 3 Negative electrode for all-solid-state batteries with a g or less.

8. In claim 1, the linear conductive material has a BET specific surface area of ​​100 m² 2 / g or more to 350 m 2 Negative electrode for all-solid-state batteries with a g or less.

9. The negative electrode for an all-solid-state battery according to claim 1, wherein the linear conductive material has a powder resistivity of 1 mΩ*cm or more to 20 mΩ*cm or less.

10. In claim 1, the linear conductive material is I G / I D A negative electrode for an all-solid-state battery, having a value of 0.8 or more and 1.3 or less.

11. A negative electrode for an all-solid-state battery according to claim 1, comprising 2 wt% or less of a solid electrolyte relative to the total weight of the negative electrode active material layer.

12. In Paragraph 1, A negative electrode for an all-solid-state battery comprising 90 wt% or more of a negative electrode active material relative to the total weight of the negative electrode active material layer.

13. In Paragraph 1, A negative electrode for an all-solid-state battery, wherein the weight ratio of the negative active material to the linear conductive material is 15 or more to 65 or less.

14. An all-solid-state battery comprising a positive electrode, a solid electrolyte layer, and a negative electrode for an all-solid-state battery according to claim 1.