Polypropylene-based resin and method for preparing same

A polypropylene-based resin with a balanced ratio of ethylene-propylene copolymers and a multi-stage polymerization process addresses the trade-off between heat resistance and flexibility, enhancing mechanical properties and insulation performance.

WO2026235443A1PCT designated stage Publication Date: 2026-11-12SK INNOVATION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/096454
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-03-27
Filing Date
2026-04-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing polypropylene-based resins face challenges in achieving a balance between heat resistance, mechanical properties, and flexibility, with homopolymers exhibiting insufficient impact strength and flexibility, while copolymers compromise on heat resistance and stiffness.

Method used

A polypropylene-based resin comprising a propylene homopolymer or ethylene-propylene copolymer, a second ethylene-propylene copolymer with varying ethylene content, and an ethylene-propylene rubber copolymer, formulated to achieve a ratio (R) exceeding 0.19 ℃/MPa, balancing melting point and flexural modulus through a multi-stage polymerization process.

Benefits of technology

The resin achieves improved heat resistance, mechanical properties, and uniform insulation, with enhanced durability and flexibility, suitable for electrical and electronic insulation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026096454_12112026_PF_FP_ABST
    Figure KR2026096454_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a polypropylene-based resin and a method for preparing same. The polypropylene-based resin comprises: a propylene homopolymer or first ethylene-propylene copolymer as component (a); a second ethylene-propylene copolymer as component (b); and an ethylene-propylene rubber copolymer as component (c), wherein the content of a structural unit derived from an ethylene monomer in the first ethylene-propylene copolymer may be lower than the content of a structural unit derived from an ethylene monomer in the second ethylene-propylene copolymer, and the polypropylene-based resin has a ratio represented by equation 1 that may be greater than 0.19 °C / MPa. [Equation 1] RP(℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))} Each symbol of equation 1 is as defined in the present specification.
Need to check novelty before this filing date? Find Prior Art

Description

Polypropylene-based resin and method of manufacturing the same

[0001] The present disclosure relates to a polypropylene-based resin and a method for manufacturing the same. Specifically, it relates to an insulating polypropylene-based resin and a method for manufacturing the same.

[0002]

[0003] Among polyolefin resins, polypropylene is widely used in various fields such as wire insulation, automotive parts, and packaging materials due to its excellent mechanical strength, chemical resistance, and processability. These polypropylene-based resins are manufactured through the homopolymerization of propylene or copolymerization with ethylene, and their physical properties may vary depending on the type and content of the comonomer.

[0004] For example, polypropylene homopolymers produced by the homopolymerization of propylene monomers can exhibit stiffness and heat resistance due to their high crystallinity. However, such homopolymers may have limitations in terms of relatively insufficient impact strength and flexibility.

[0005] Meanwhile, polypropylene copolymers produced by copolymerizing propylene monomers and ethylene monomers can have their impact strength and low-temperature properties improved by introducing ethylene monomers. However, such copolymerization can lead to a decrease in heat resistance and stiffness due to a reduction in crystallinity.

[0006] In the case of polypropylene-based resins, there is a continuously being raised need for technology capable of securing balanced properties while improving the trade-off between heat resistance, mechanical properties, and flexibility.

[0007]

[0008] One objective of the present disclosure is to provide a polypropylene-based resin having improved heat resistance and mechanical properties.

[0009] One objective of the present disclosure is to provide a method for manufacturing a polypropylene-based resin having improved heat resistance and mechanical properties.

[0010]

[0011] A polypropylene-based resin according to embodiments of the present disclosure comprises: component (a) a propylene homopolymer or a first ethylene-propylene copolymer; component (b) a second ethylene-propylene copolymer; and component (c) an ethylene-propylene rubber copolymer, and

[0012] The content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and

[0013] The ratio (R) represented by the following Formula 1 for the above polypropylene-based resin P ) may exceed 0.19 ℃ / MPa:

[0014] [Equation 1]

[0015] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))}

[0016] In the above Equation 1, Tm represents the melting temperature (°C) of the polypropylene resin measured by Differential Scanning Calorimetry (DSC), FM represents the flexural modulus (MPa) of the polypropylene resin measured according to the ASTM D790 test method, and XS represents the content (wt%) of the xylene dissolved component of the polypropylene resin measured according to the ASTM D5492 test method.

[0017] In one embodiment, the melting point (Tm) of the polypropylene-based resin may be 150°C to 180°C.

[0018] In one embodiment, the flexural modulus (FM) of the polypropylene-based resin may be 200 MPa to 350 MPa.

[0019] In one embodiment, the content (XS) of the xylene dissolved component of the polypropylene resin may be 35% to 55% by weight.

[0020] In one embodiment, the crystallization temperature (Tc) of the polypropylene-based resin measured by differential scanning calorimetry is 100 ℃ to 140 ℃, and the difference (Tm-Tc) between the melting point and the crystallization temperature may be 30 ℃ to 50 ℃.

[0021] In one embodiment, the first ethylene-propylene copolymer is included as component (a), the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is less than 3.5 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 3.5 weight% or more.

[0022] In one embodiment, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is greater than 0 weight% and less than or equal to 3 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 3.5 weight% to 8 weight%.

[0023] In one embodiment, based on the total weight of the first ethylene-propylene copolymer and the second ethylene-propylene copolymer, the total content of structural units derived from ethylene monomers in each copolymer may be 2% to 7% by weight.

[0024] In one embodiment, the propylene homopolymer is included as component (a), and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 5 weight% or more.

[0025] In one embodiment, the content of component (a) may be 25% to 40% by weight based on the total weight of the polypropylene-based resin.

[0026] In one embodiment, the content of component (b) may be 12% to 25% by weight based on the total weight of the polypropylene-based resin.

[0027] In one embodiment, the content of component (c) may be 40% to 55% by weight based on the total weight of the polypropylene-based resin.

[0028] In one embodiment, the breakdown strength under DC (BDS) of the polypropylene-based resin may be 450 kV / mm to 600 kV / mm.

[0029] In one embodiment, the total content of structural units derived from ethylene monomers in the xylene-insoluble portion of the polypropylene resin may be 6.5% by weight to 10.5% by weight.

[0030] In one embodiment, the melt index of the polypropylene-based resin measured according to the ASTM D1238 test method may be 0.8 dg / min to 2.0 dg / min.

[0031] In one embodiment, the polypropylene-based resin may further include component (d) a third ethylene-propylene copolymer.

[0032] In one embodiment, the polypropylene-based resin may further include an additive comprising at least one selected from the group consisting of an antioxidant, a neutralizing agent, and a nucleating agent.

[0033] In one embodiment, the content of the additive may be 0.2 weight% to 1.0 weight% based on the total weight of the polypropylene-based resin.

[0034] A method for manufacturing a polypropylene-based resin according to embodiments of the present disclosure comprises: introducing a propylene monomer without a comonomer into a first bulk reactor and reacting it, or introducing a first ethylene monomer and a first propylene monomer and reacting them to form component (a) a propylene homopolymer or a first ethylene-propylene copolymer; introducing a second ethylene monomer and a second propylene monomer into a second bulk reactor connected to the first bulk reactor and reacting them to form component (b) a second ethylene-propylene copolymer; introducing a third ethylene monomer and a third propylene monomer into a gaseous reactor connected to the second bulk reactor and reacting them to form component (c) an ethylene-propylene rubber copolymer; and discharging the polypropylene-based resin from the gaseous reactor.

[0035] The component (a) in the first bulk reactor is transferred to the second bulk reactor by a connecting line connecting the first bulk reactor and the second bulk reactor, and

[0036] Components (a) and (b) in the second bulk reactor are transferred to the gaseous reactor by a connecting line connecting the second bulk reactor and the gaseous reactor, and

[0037] The above polypropylene-based resin is,

[0038] Component (a) propylene homopolymer or first ethylene-propylene copolymer;

[0039] Component (b) secondary ethylene-propylene copolymer; and

[0040] Component (c) comprises an ethylene-propylene rubber copolymer, and

[0041] The content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and

[0042] The ratio (R) represented by the following Formula 1 for the above polypropylene-based resin P) may exceed 0.19 ℃ / MPa:

[0043] [Equation 1]

[0044] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))}

[0045] In the above Equation 1, Tm represents the melting temperature (°C) of the polypropylene resin measured by Differential Scanning Calorimetry (DSC), FM represents the flexural modulus (MPa) of the polypropylene resin measured according to the ASTM D790 test method, and XS represents the content (wt%) of the xylene dissolved component of the polypropylene resin measured according to the ASTM D5492 test method.

[0046] In one embodiment, a first ethylene monomer and a first propylene monomer are introduced into a first bulk reactor to form a first ethylene-propylene copolymer as component (a), and the content of the first ethylene monomer introduced into the first bulk reactor is less than 3.5% by weight of the total weight of the first ethylene monomer and the first propylene monomer, and the content of the second ethylene monomer introduced into the second bulk reactor may be 3.5% by weight or more of the total weight of the second ethylene monomer and the second propylene monomer.

[0047] In one embodiment, a propylene monomer is introduced into a first bulk reactor without a comonomer to form a propylene homopolymer as component (a), and the content of the second ethylene monomer introduced into the second bulk reactor may be 5% by weight or more of the total weight of the second ethylene monomer and the second propylene monomer.

[0048] In one embodiment, in the step of forming the component (c) ethylene-propylene rubber copolymer, a third ethylene monomer and a third propylene monomer are introduced into the gas phase reactor and reacted to form the component (c) ethylene-propylene rubber copolymer and the component (d) third ethylene-propylene copolymer, and the polypropylene-based resin may further include the component (d) third ethylene-propylene copolymer.

[0049]

[0050] The polypropylene-based resin according to the embodiments of the present disclosure has improved heat resistance and mechanical properties, and can have more uniform insulation properties.

[0051] According to the method for manufacturing a polypropylene-based resin according to the embodiments of the present disclosure, a polypropylene-based resin having improved heat resistance and mechanical properties and more uniform insulation properties can be manufactured.

[0052]

[0053] The polypropylene-based resin according to the embodiments of the present disclosure can be applied as an electrical and electronic insulating material, such as an insulating layer or a sheathing layer of a wire, for example. In addition, the polypropylene-based resin can be used in various power and communication cable fields, such as as an insulating material for cables, for example, a sheathing material for wires.

[0054]

[0055] FIG. 1 is a schematic process flow diagram of a method for manufacturing a polypropylene-based resin according to one embodiment.

[0056] FIGS. 2a and 2b are schematic diagrams showing the connection sequence of an exemplary reactor applicable to a method for manufacturing a polypropylene-based resin according to one embodiment.

[0057] Figure 3 is a graph showing the change in melting point of polypropylene resins according to the total content (wt%) of ethylene in component (a) and component (b) in each example and comparative example.

[0058] Figure 4 is a graph showing the relationship between the denominator of Equation 1, "FM + {12.5(MPa / wt%) × XS(wt%)}", on the horizontal axis and the numerator, "Tm(°C)", on the vertical axis in each example and comparative example.

[0059]

[0060] Hereinafter, embodiments of the present disclosure are described in detail so that those skilled in the art can easily practice the present invention. However, this is merely illustrative and the present invention is not limited to the illustratively described embodiments.

[0061] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the attached drawings. In this case, the same reference numerals are used for identical components in the drawings, and redundant descriptions of identical components are omitted. The embodiments disclosed in the attached drawings are exemplary and should be understood to include all modifications, equivalents, and substitutions that fall within the spirit and scope of the present invention.

[0062] In addition, the embodiments described below may be understood independently of each other, but are not limited thereto, and embodiments combining at least two of the embodiments described below should also be understood as being included within the technical spirit and scope of the present disclosure.

[0063] Terms used in this specification, such as "is on," "is placed," etc., include not only cases where they are directly placed but also cases where other components are interposed between them.

[0064] Terms such as "first," "second," "below," "lower," "above," and "upper" are used as relative concepts to distinguish different components or locations, and do not specify absolute positions or order.

[0065]

[0066] Polypropylene resin

[0067] A polypropylene-based resin according to embodiments of the present disclosure comprises a component (a) a propylene homopolymer or a first ethylene-propylene copolymer; a component (b) a second ethylene-propylene copolymer; and a component (c) an ethylene-propylene rubber copolymer, wherein the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and a ratio (R) represented by the following Formula 1 for the polypropylene-based resin P ) may exceed 0.19 ℃ / MPa.

[0068] [Equation 1]

[0069] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))}

[0070] In the above Equation 1, Tm represents the melting temperature (°C) of the polypropylene resin measured by Differential Scanning Calorimetry (DSC), FM represents the flexural modulus (MPa) of the polypropylene resin measured according to the ASTM D790 test method, and XS represents the content (wt%) of the xylene dissolved component of the polypropylene resin measured according to the ASTM D5492 test method.

[0071] The ratio (R) represented by the above Equation 1 P ) may be provided as an indicator of durable flexibility. In this specification, "durable flexibility" may mean a flexible characteristic in which damage can be suppressed even under repeated deformation by maintaining a balance between the melting point, which indicates thermal stability, and the flexural modulus, which indicates mechanical stiffness, for a long period of time.

[0072] It is generally known that the flexural modulus and melting point of polypropylene resins have a trade-off relationship.

[0073] The melting point, flexural modulus, and xylene soluble content of the polypropylene-based resin according to the embodiments of the present disclosure are the ratio (R) represented by Formula 1 described above. P By satisfying the relationship where ) exceeds 0.19 ℃ / MPa, the two physical properties of flexural modulus and melting point are harmoniously controlled, so that the polypropylene-based resin can be easily bent, and at the same time, damage caused by repeated bending, twisting, impact, etc. can be suppressed for a long period. Accordingly, both high-temperature stability and flexibility of the insulating material using the polypropylene-based resin can be improved.

[0074] In one embodiment, R P It may be greater than 0.19 ℃ / MPa and less than or equal to 0.25 ℃ / MPa, for example, 0.191 ℃ / MPa to 0.25 ℃ / MPa, 0.193 ℃ / MPa to 0.25 ℃ / MPa, 0.195 ℃ / MPa to 0.25 ℃ / MPa, 0.197 ℃ / MPa to 0.23 ℃ / MPa, or 0.198 ℃ / MPa to 0.20 ℃ / MPa.

[0075] Accordingly, the above-mentioned polypropylene-based resin can more stably secure a balance of physical properties between high-temperature stability and flexibility.

[0076] The melting point of the above polypropylene-based resin can be measured using differential scanning calorimetry (DSC) according to the ASTM D3418 test method. As a non-limiting example, the DSC can be performed using TA Instruments' Q20, Netzsch's DSC 214, or equivalent equipment.

[0077] The above DSC measurement can be performed under a nitrogen atmosphere using an empty aluminum pan as a reference pan and with the sample loaded into the aluminum pan. As a non-limiting example, the amount of the sample may be, for example, about 3 mg to 10 mg. For example, the sample may be analyzed while performing a heating and cooling process at a rate of about 5 ℃ / min to 20 ℃ / min in a temperature range of about -50 ℃ to 200 ℃. For example, the melting point may be determined based on data obtained from a second heating run.

[0078] The flexural modulus of the above polypropylene-based resin can be measured according to the ASTM D790 test method. For example, the above polypropylene-based resin and additives are kneaded using an extruder and prepared in the form of pellets, and the pellets are molded into a specimen through a heating press and cooling press process using press equipment, and then the flexural modulus of the molded material, i.e., the molded product, can be measured.

[0079] The above additive may include, but is not limited to, antioxidants, neutralizing agents and / or nucleating agents. The amount of the above additive may be about 0.1 to 0.8 parts by weight per 100 parts by weight of the total of components (a), (b), and (c).

[0080] As a non-limiting example, the specimen may be manufactured in the form of a rod approximately 125 mm × 12.5 mm × 3.2 mm in size.

[0081] The above flexural modulus can be measured through a three-point bending test using a universal testing machine. Non-limiting examples include Instron®’s 3400 series and 6800 series electromechanical universal testing machines. For example, the three-point bending test can be set so that the ratio of the span length (L) to the specimen thickness is about 14:1 to 20:1, for example, about 16:1. Additionally, the strain rate can be set to about 5 mm / min to 20 mm / min, for example, about 13 mm / min. The test can be performed at a temperature of about 20°C to 30°C and a relative humidity of about 40% to 60% RH.

[0082] In Formula 1 above, XS (wt%) represents the content of xylene soluble fraction measured according to the ASTM D5492 test method. The content of the xylene soluble fraction can be calculated based on the weight of the solid obtained by dissolving the polypropylene-based resin in a xylene solvent, cooling to form a precipitate, separating the supernatant and the precipitate, and then removing the solvent from the supernatant. The xylene soluble fraction (XS) may correspond, for example, to the content of the ethylene-propylene rubber (EPR) component contained in the polypropylene-based resin.

[0083] For example, about 1 g to 10 g of a sample of the above-mentioned polypropylene resin may be prepared and the sample may be dissolved in a xylene solvent. The xylene solvent may be ortho-xylene, meta-xylene, para-xylene, or a mixture thereof, and may be, for example, para-xylene (p-xylene).

[0084] For example, the above polypropylene-based resin sample may be dissolved in a xylene solvent and then heated and refluxed at a temperature of about 120°C to 150°C, for example, about 130°C to 140°C, and subsequently cooled to room temperature to undergo a precipitation process, thereby separating it into a supernatant and a precipitate. The weight of the solid obtained by removing the solvent from the supernatant is W S Let be denoted as and the weight of the initial sample as W T When given that, the xylene dissolved component (XS, wt%) is W S / W T It can be calculated as a percentage.

[0085] In the above Equation 1, approximately 12.5 MPa / wt% is a conversion factor (k), which means a factor for converting the xylene dissolved content unit (wt%) into a mechanical property unit (MPa) by considering the effect of the xylene dissolved content (XS, wt%) on the mechanical properties of the resin.

[0086] In the above Equation 1, XS (wt%) can be converted into a mechanical contribution to consider the effect of the xylene dissolved component on the mechanical properties of the resin, and for this purpose, it can be converted by multiplying the content of the xylene dissolved component (XS, wt%) by the conversion factor (k).

[0087] The above conversion factor (k) may refer to a coefficient derived empirically to reflect, for example, the trend of change in flexural modulus due to an increase in xylene dissolved content.

[0088] In the above Equation 1, the denominator FM + {12.5(MPa / wt%) × XS(wt%)} can be used as an indicator representing the flexural modulus of the matrix excluding the ethylene-propylene rubber copolymer, which is component (c), from the above polypropylene-based resin.

[0089] For example, the copolymer may be a random copolymer.

[0090] The above polypropylene-based resin may have improved heat resistance and mechanical properties by including components (a) to (c) together.

[0091] In addition, the above polypropylene-based resin is not manufactured by feeding components (a) to (c) into an extruder at once and melt-mixing them, but can be manufactured through a process in which the polymerization and mixing of each component proceed together using a device, for example, in which a two-stage bulk reactor and a gas-phase reactor are connected in series. Accordingly, component (b) acts as a compatibilizer between component (a) and component (c), so that the above polypropylene-based resin can have a uniform phase despite being a three-component resin. Accordingly, the above polypropylene-based resin can have uniform and stable insulation properties.

[0092] In one embodiment, the melting point (Tm) of the polypropylene-based resin may be 150 ℃ to 180 ℃, and may be, for example, 154 ℃ to 170 ℃, 157 ℃ to 170 ℃, or 160 ℃ to 170 ℃.

[0093] In one embodiment, the flexural modulus (FM) of the polypropylene-based resin may be 200 MPa to 350 MPa, 210 MPa to 350 MPa, 250 MPa to 350 MPa, 300 MPa to 350 MPa, or 315 MPa to 340 MPa. Accordingly, the polypropylene-based resin may have high mechanical properties along with improved heat resistance.

[0094] In one embodiment, the content (XS) of the xylene dissolved component of the polypropylene resin may be 35% to 55% by weight, for example, 35% to 55% by weight, or 35% to 45% by weight.

[0095] In one embodiment, the crystallization temperature (Tc) of the polypropylene-based resin measured by differential scanning calorimetry may be 100 ℃ to 140 ℃, and may be, for example, 120 ℃ to 135 ℃, 124 ℃ to 135 ℃, or 126 ℃ to 135 ℃.

[0096] In one embodiment, the difference (Tm-Tc) between the melting point and the crystallization temperature may be 30°C to 50°C. For example, the difference (Tm-Tc) between the crystallization temperatures may be 32°C to 45°C or 35°C to 40°C.

[0097] Accordingly, it is possible to secure sufficient flexibility required for wire sheathing while maintaining high thermal stability.

[0098] The crystallization temperature obtained by the above differential scanning calorimetry analysis can be measured, for example, according to the ASTM D3418 test method.

[0099] The first ethylene-propylene copolymer is a copolymer of the first ethylene monomer and the first propylene monomer, and the second ethylene-propylene copolymer may be a copolymer of the second ethylene monomer and the second propylene monomer.

[0100] In one embodiment, the polypropylene-based resin may include a first ethylene-propylene copolymer as component (a).

[0101] Accordingly, when the above-mentioned polypropylene-based resin comprises a first ethylene-propylene copolymer as component (a), the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer may be less than 3.5 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 3.5 weight% or more. Accordingly, the heat resistance and mechanical properties of the above-mentioned polypropylene-based resin can be improved together. For example, if the content of each structural unit derived from ethylene monomers described above falls outside the above range, R PIt may not be easy to control it to more than 0.19 ℃ / MPa.

[0102] For example, the first ethylene-propylene copolymer is a copolymer of the first ethylene monomer and the first propylene monomer, and the second ethylene-propylene copolymer may be a copolymer of the second ethylene monomer and the second propylene monomer.

[0103] In this specification, the content of a structural unit derived from a specific monomer among each copolymer may refer to the content of said monomer among the total monomers forming said copolymer, unless specifically stated otherwise. However, said content may vary within an acceptable margin of error depending on structural changes that occur during the process of polymerizing monomers to form a bonded structure.

[0104] Accordingly, the content of the first ethylene monomer in the total weight of the first ethylene monomer and the first propylene monomer may be less than 3.5 weight%, and the content of the second ethylene monomer in the total weight of the second ethylene monomer and the second propylene monomer may be 3.5 weight% or more. The content of the first propylene monomer may be the value obtained by subtracting the content of the first ethylene monomer from the total weight of 100 weight%. The content of the second propylene monomer may be the value obtained by subtracting the content of the second ethylene monomer from 100 weight%.

[0105] In one embodiment, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer may be greater than 0 wt% and less than or equal to 3 wt%, for example, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2.4 wt%, or 0.1 wt% or more and less than 2.4 wt%.

[0106] In one embodiment, the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 3.5 wt% to 8 wt%, and for example, 3.6 wt% to 8 wt%, 4 wt% to 8 wt%, 4 wt% to 7.5 wt%, 5 wt% to 7.5 wt%, 5 wt% to 7.0 wt%, or 5 wt% to 6.5 wt%.

[0107] In one embodiment, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is greater than 0 weight% and less than or equal to 3.0 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 3.5 weight% to 8 weight%.

[0108] In one embodiment, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is 0.1% to 2.4% by weight, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 4% to 8% by weight.

[0109] In one embodiment, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is 0.1 weight% or more and less than 2.4 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer may be 5 weight% to 7.5 weight%.

[0110] In the case where the content of structural units derived from the first ethylene monomer is 2.5 weight% or more and is equal to the content of structural units derived from the second ethylene monomer, R P It may be 0.19 ℃ / MPa or less. In this case, a decrease in the melting point may occur, which may reduce thermal stability.

[0111] When the content of structural units derived from the second ethylene monomer is less than 2.0 weight% and is the same as the content of structural units derived from the first ethylene monomer, RP It may be 0.19 ℃ / MPa or less. In this case, an excessive increase in flexural modulus may result, which may reduce flexibility.

[0112] When the content of structural units derived from the first and second ethylene monomers is about 3.5 weight%, the flexural modulus is lowered, but a decrease in melting point and other factors may also occur, which may reduce thermal stability.

[0113] In this way, when the content of each structural unit derived from the first ethylene monomer and the second ethylene monomer is the same, both characteristics of high thermal stability and flexibility required for wire sheathing cannot be satisfied, and at least one characteristic cannot be secured.

[0114] In one embodiment, based on the total weight of the first ethylene-propylene copolymer and the second ethylene-propylene copolymer, the total content of structural units derived from ethylene monomers in each copolymer may be 2% to 7% by weight.

[0115] For example, based on the total weight of the first ethylene monomer, the first propylene monomer, the second ethylene monomer, and the second propylene monomer, the total content of the first ethylene monomer and the second ethylene monomer may be 2% to 7% by weight.

[0116] In one embodiment, based on the total weight of the first ethylene-propylene copolymer and the second ethylene-propylene copolymer, the total content of structural units derived from ethylene monomers in each copolymer may be 2.3% to 5% by weight, 2.3% to 4% by weight, or 2.3% to 3% by weight.

[0117] In one embodiment, the polypropylene-based resin may further include component (d) a third ethylene-propylene copolymer.

[0118] For example, the ethylene-propylene rubber copolymer of component (c) may be a rubber copolymer of the 3A ethylene monomer and the 3A propylene monomer. The 3rd ethylene-propylene copolymer of component (d) may be a copolymer of the 3B ethylene monomer and the 3B propylene monomer.

[0119] In one embodiment, the content of structural units derived from ethylene monomers in the third ethylene-propylene copolymer may be 20% to 40% by weight, or 25% to 35% by weight. Accordingly, the flexural modulus of the polypropylene-based resin can be more easily controlled to the above-described range.

[0120] In one embodiment, based on the total weight of the ethylene-propylene rubber copolymer of component (c) and the third ethylene-propylene copolymer of component (d), the content of structural units derived from ethylene monomers may be 25% to 45% by weight, and for example, 30% to 45% by weight, 35% to 45% by weight, or 35% to 42% by weight.

[0121] In one embodiment, the polypropylene-based resin may include the propylene homopolymer as a component (a).

[0122] In this way, when the polypropylene-based resin comprises the propylene homopolymer as component (a), the content of structural units derived from the ethylene monomer in the second ethylene-propylene copolymer may be 5 weight% or more, and may be, for example, 5 weight% to 10 weight% or 6 weight% to 7.5 weight%.

[0123] Accordingly, heat resistance and mechanical properties can be improved while sufficiently securing electrical properties as an insulating coating material.

[0124] In one embodiment, the total content of structural units derived from ethylene monomers in the xylene-insoluble portion of the polypropylene resin may be 6.5% by weight to 10.5% by weight.

[0125] Accordingly, internal ductility is imparted while maintaining the crystallinity of the polypropylene-based resin, thereby improving the balance between the flexural modulus and the melting point.

[0126] The above xylene-insoluble component may refer to a solid obtained by dissolving the above polypropylene-based resin in a xylene solvent, cooling to form a precipitate, separating the supernatant and the precipitate, and then vacuum drying the precipitate. The above xylene-insoluble component may, for example, include first and second ethylene-propylene copolymer components contained in the above polypropylene-based resin. Additionally, the above xylene-insoluble component may, for example, include first to third ethylene-propylene copolymer components contained in the above polypropylene-based resin.

[0127] In one embodiment, the content of component (a) may be 25% to 40% by weight based on the total weight of the polypropylene-based resin.

[0128] In one embodiment, the content of component (b) may be 12% to 25% by weight based on the total weight of the polypropylene-based resin.

[0129] In one embodiment, the content of component (c) may be 40% to 55% by weight based on the total weight of the polypropylene-based resin.

[0130] According to one embodiment, when the polypropylene-based resin further comprises component (d) a third ethylene-propylene copolymer, the total content of component (c) and component (d) based on the total weight of the polypropylene-based resin may be 40% to 55% by weight.

[0131] In one embodiment, the weight ratio of component (c), an ethylene-propylene rubber copolymer, and component (d), a third ethylene-propylene copolymer, may be 10:1 to 15:1.

[0132] In one embodiment, the breakdown strength under DC (BDS) of the polypropylene-based resin may be 450 kV / mm to 600 kV / mm, for example, 450 kV / mm to 550 kV / mm, 470 kV / mm to 550 kV / mm, or 475 kV / mm to 550 kV / mm. The breakdown strength under DC may be measured at room temperature, for example, according to the ASTM D149 test method, by simply replacing the AC power source with DC. The breakdown strength under DC may be measured at room temperature using, for example, a Phenix 6TC4100-10 instrument (using a sphere-to-sphere electrode). Accordingly, the risk of breakdown in a high-temperature environment may be prevented or reduced.

[0133] In one embodiment, the melt index of the polypropylene-based resin measured according to the ASTM D1238 test method may be 0.8 dg / min to 2.0 dg / min, and for example, 1.0 dg / min to 1.3 dg / min. Accordingly, dimensional stability of the wire and cable can be ensured even after long-term use in a high-temperature environment.

[0134] The above melt index can be measured using, for example, a Melt Flow Indexer, a Melt Flow Tester, etc.

[0135] In one embodiment, the propylene-based resin may further include an additive comprising an antioxidant, a neutralizing agent, and / or a nucleating agent.

[0136] In one embodiment, the additive may include an antioxidant and a nucleating agent.

[0137] The antioxidant may include phenolic antioxidants and / or phosphite-based antioxidants. As a non-limiting example, the antioxidant may include one or more of the following: pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate) (Irganox® 1010), tris(2,4-di-tert-butylphenyl)phosphite (Irgafos® 168), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (Irganox® 1330), 2,2'-thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox® 1035) manufactured by BASF. The above antioxidants may include, for example, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate) and tris(2,4-di-tert-butylphenyl)phosphite.

[0138] As a non-limiting example, the neutralizing agent may include metal stearates, and may include one or more types, such as calcium stearate (SC-110) manufactured by Songwon Industry, zinc stearate, magnesium stearate, etc. Accordingly, the residue of the catalyst, i.e., the Ziegler-Natta catalyst, can be deactivated.

[0139] As a non-limiting example, the nucleating agent may include one or more types of organic phosphate-based metal salt nucleating agents (e.g., aluminum hydroxybis[2,2'-methylene-bis(4,6,-di-tert-butylphenyl)phosphate], sorbitol-based nucleating agents (e.g., dimethyldibenzylidene sorbitol (DMDBS), Millad® 3988), organic acid salt-based nucleating agents (e.g., adipose-based, benzoate-based). Accordingly, it can help in the formation of a more uniform crystal phase. The nucleating agent may include, for example, a sorbitol-based nucleating agent.

[0140] In one embodiment, the content of the additive may be 0.2 weight% to 1.0 weight% based on the total weight of the polypropylene-based resin.

[0141]

[0142] Method for manufacturing polypropylene-based resin

[0143] FIG. 1 is a schematic process flow diagram of a method for manufacturing a polypropylene-based resin according to one embodiment. FIG. 2a and FIG. 2b are schematic diagrams showing the connection sequence of each reactor applicable to the method for manufacturing a polypropylene-based resin according to one embodiment.

[0144] A method for manufacturing a polypropylene-based resin according to embodiments of the present disclosure may comprise: introducing a propylene monomer without a comonomer into a first bulk reactor and reacting it, or introducing a first ethylene monomer and a first propylene monomer and reacting them to form component (a) a propylene homopolymer or a first ethylene-propylene copolymer (step S10); introducing a second ethylene monomer and a second propylene monomer into a second bulk reactor connected to the first bulk reactor and reacting them to form component (b) a second ethylene-propylene copolymer (step S20); introducing a third ethylene monomer and a third propylene monomer into a gaseous reactor connected to the second bulk reactor and reacting them to form component (c) an ethylene-propylene rubber copolymer (step S30), and discharging the polypropylene-based resin from the gaseous reactor (step S40). Each reaction of the monomers described above may be a polymerization reaction, for example, a random polymerization reaction.

[0145] The polypropylene-based resin described above can be manufactured by the above manufacturing method. Refer to the above description regarding the polypropylene-based resin.

[0146] Component (a) in the first bulk reactor is transferred to the second bulk reactor by a connecting line connecting the first bulk reactor and the second bulk reactor, and components (a) and (b) in the second bulk reactor can be transferred to the gaseous reactor by a connecting line connecting the second bulk reactor and the gaseous reactor. Accordingly, component (a) can also be present in the second bulk reactor while the second ethylene monomer and the second propylene monomer are reacting in the second bulk reactor. Components (a) and (b) can also be present in the gaseous reactor while the third ethylene monomer and the third propylene monomer are reacting in the gaseous reactor.

[0147] The polypropylene-based resin discharged from the above-mentioned gas-phase reactor may include component (a), component (b) and component (c).

[0148] The above polypropylene resin is not manufactured by simultaneously feeding each of the previously prepared components (a) to (c) into an extruder and melt-mixing them. The above polypropylene resin can be manufactured by using a device in which a two-stage bulk reactor and a gas-phase reactor are connected in series, for example, so that mixing proceeds together during the polymerization process of each component. In this process, component (b) acts as a compatibilizer between component (a) and component (c), so that the above polypropylene resin can have a more uniform phase. Accordingly, the above polypropylene resin can have more uniform insulation properties and improved heat resistance and mechanical properties.

[0149] Accordingly, the polypropylene-based resin comprises component (a) a propylene homopolymer or a first ethylene-propylene copolymer; component (b) a second ethylene-propylene copolymer; and component (c) an ethylene-propylene rubber copolymer, wherein the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and the ratio (R) represented by the following Formula 1 for the polypropylene-based resin P ) may exceed 0.19 ℃ / MPa.

[0150] [Equation 1]

[0151] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))}

[0152] Refer to the above-mentioned content regarding Equation 1.

[0153] As a non-limiting example, the first and second bulk reactors may be loop reactors, and the gas reactor may be a fluidized bed reactor.

[0154] As a non-limiting example, referring to FIG. 2a, the first bulk reactor and the gaseous reactor may be connected by a first connecting line (41, 42), and a second connecting line (43) branching from the first connecting line may be connected to the second bulk reactor. In this case, the first bulk reactor and the second bulk reactor are connected by the front end (41) of the first connecting line and the second connecting line (43), and the second bulk reactor and the gaseous reactor may be connected by the second connecting line (43) and the rear end (42) of the first connecting line.

[0155] For example, a component (a) in the first bulk reactor can be moved to the second bulk reactor by the front end (41) of the first connecting line and the second connecting line (43) connecting the first bulk reactor and the second bulk reactor.

[0156] For example, components (a) and (b) in the second bulk reactor can be moved to the gas reactor by the second connecting line (43) connecting the second bulk reactor and the gas reactor and the rear end (42) of the first connecting line.

[0157] The second connecting line (43) can be used in different flow directions depending on the operating conditions. For example, the flow of component (a) in the first bulk reactor moving to the second bulk reactor and the flow of component (a) and component (b) in the second bulk reactor moving to the gaseous reactor may be in opposite directions to each other, and these flows may occur sequentially with a time difference depending on the process operating conditions.

[0158] In addition, in another embodiment, the second connecting lines may be composed of a plurality, for example, two, to each handle flow in opposite directions. In this case, each connecting line may be formed independently to be suitable for unidirectional flow, and for the sake of brevity of the drawing, a configuration having two second connecting lines is not illustrated.

[0159] Additionally, in another embodiment, referring to FIG. 2b, the first bulk reactor and the second bulk reactor are connected by a third connecting line (44), and a component (a) in the first bulk reactor can be moved to the second bulk reactor by the third connecting line (44). The second bulk reactor and the gas reactor are connected by a fourth connecting line (45), and components (a) and (b) in the second bulk reactor can be moved to the gas reactor by the fourth connecting line (45).

[0160] The aforementioned connection line may be a connecting means such as a conduit, pipe, or tube, and is not particularly limited.

[0161] As a non-limiting example, in the above manufacturing method, Spheripol is used in a first bulk reactor and a second bulk reactor. ® Bulk reactors used in the process, for example, loop reactors, can be used.

[0162] As a non-limiting example, in the above manufacturing method, a gas-phase reactor used in the Spheripol® process may be used as the gas-phase reactor.

[0163] In the first and second bulk reactors and the gas phase reactor, for example, a Ziegler-Natta catalyst or an equivalent olefin polymerization catalyst may be installed or introduced.

[0164] In one embodiment, a first ethylene monomer and a first propylene monomer can be introduced into a first bulk reactor to form a first ethylene-propylene copolymer as component (a).

[0165] When forming a first ethylene-propylene copolymer as component (a), the content of the first ethylene monomer introduced into the first bulk reactor may be less than 3.5% by weight of the total weight of the first ethylene monomer and the first propylene monomer, and the content of the second ethylene monomer introduced into the second bulk reactor may be 3.5% by weight or more of the total weight of the second ethylene monomer and the second propylene monomer. The amount of the first propylene monomer introduced may be the value obtained by subtracting the amount of the first ethylene monomer introduced from the total weight of 100% by weight. The amount of the second propylene monomer introduced may be the value obtained by subtracting the amount of the second ethylene monomer introduced from 100% by weight.

[0166] By controlling the input amounts of the first and second ethylene monomers differently to less than 3.5 weight% and 3.5 weight% or more, respectively, based on the total weight of the first ethylene monomer and the first propylene monomer introduced into the first bulk reactor, the heat resistance and mechanical properties of the polypropylene-based resin can be improved together.

[0167] For the respective contents of the first ethylene monomer and the first propylene monomer introduced into the first bulk reactor, refer to the above-described contents regarding the polypropylene-based resin.

[0168] For the respective contents of the second ethylene monomer and the second propylene monomer introduced into the second bulk reactor, refer to the above-described contents regarding the polypropylene-based resin.

[0169] Refer to the above description regarding the third ethylene monomer and the third propylene monomer in the above gas-phase reactor, and the above polypropylene-based resin.

[0170] In one embodiment, the content of the first ethylene monomer introduced into the first bulk reactor may be greater than 0 wt% and less than or equal to 3.0 wt%, for example, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2.4 wt%, or greater than or equal to 0.1 wt% and less than 2.4 wt%.

[0171] In one embodiment, the content of the second ethylene monomer introduced into the second bulk reactor may be 3.5 wt% to 8 wt%, and for example, 3.6 wt% to 8 wt%, 4 wt% to 8 wt%, 4 wt% to 7.5 wt%, 5 wt% to 7.5 wt%, 5 wt% to 7.0 wt%, or 5 wt% to 6.5 wt%.

[0172] In one embodiment, the input amount of the first ethylene monomer is greater than 0 weight% and less than or equal to 3.0 weight%, and the input amount of the second ethylene monomer may be 3.5 weight% to 8 weight%.

[0173] In one embodiment, the input amount of the first ethylene monomer may be 0.1% to 2.4% by weight, and the input amount of the second ethylene monomer may be 4% to 8% by weight.

[0174] In one embodiment, the input amount of the first ethylene monomer is 0.1 weight% or more and less than 2.4 weight%, and the input amount of the second ethylene monomer may be 5 weight% to 7.5 weight%.

[0175] In one embodiment, based on the total weight obtained by adding the weights of the first ethylene monomer and the first propylene monomer introduced into the first bulk reactor and the weights of the second ethylene monomer and the second propylene monomer introduced into the second bulk reactor, the total content obtained by adding the contents of the first ethylene monomer and the second ethylene monomer, i.e., the total amount of the first and second ethylene monomers introduced, may be 2% to 7% by weight. Accordingly, heat resistance and mechanical properties can be improved while sufficiently securing the physical properties required as an insulating coating material.

[0176] In one embodiment, a third ethylene monomer and a third propylene monomer are introduced into the gas phase reactor and reacted to form component (c) an ethylene-propylene rubber copolymer and component (d) a third ethylene-propylene copolymer.

[0177] Among the third ethylene monomer and the third propylene monomer, the monomers forming component (c) the ethylene-propylene rubber copolymer may be referred to as the third-A ethylene monomer and the third-A propylene monomer.

[0178] Among the third ethylene monomer and the third propylene monomer, the monomers forming component (d) the third ethylene-propylene copolymer may be referred to as the third B ethylene monomer and the third B propylene monomer.

[0179] The third ethylene monomer may consist of the third-A ethylene monomer and the third-B ethylene monomer.

[0180] The third propylene monomer may consist of the third-a propylene monomer and the third-b propylene monomer.

[0181] In one embodiment, based on the total weight of the sum of the weights of the 3A ethylene monomer and the 3A propylene monomer, the amount of the 3A ethylene monomer added may be, for example, 20% to 40% by weight, or 30% to 35% by weight.

[0182] In one embodiment, a propylene monomer is introduced into a first bulk reactor without a comonomer to form a propylene homopolymer as component (a).

[0183] In this way, when the propylene homopolymer is formed as component (a), the amount of the second ethylene monomer introduced into the second bulk reactor may be 5% by weight or more based on the total weight of the second ethylene monomer and the second propylene monomer.

[0184] In one embodiment, the amount of the second ethylene monomer introduced into the second bulk reactor may be, for example, 5% to 10% by weight or 6% to 7.5% by weight.

[0185] Accordingly, heat resistance and mechanical properties can be improved while sufficiently securing the physical properties required as an insulating coating material.

[0186] In one embodiment, the content of component (a) may be 25% to 40% by weight based on the total weight of the polypropylene-based resin discharged from the gas-phase reactor.

[0187] In one embodiment, the content of component (b) may be 12% to 25% by weight based on the total weight of the polypropylene-based resin discharged from the gas-phase reactor.

[0188] In one embodiment, the total content of component (c) and component (d) may be 40% to 55% by weight based on the total weight of the polypropylene-based resin discharged from the gas phase reactor.

[0189] In one embodiment, the weight ratio of the ethylene-propylene rubber copolymer, which is component (c) formed, and the third ethylene-propylene copolymer, which is component (d), may be 10:1 to 15:1.

[0190] As a non-limiting example, the content of each component (a) to (c) or component (a) to (d) included in the polypropylene resin can be controlled to the above-described range by controlling the content of ethylene monomer and / or propylene monomer introduced into the first bulk reactor, the second bulk reactor and the gas phase reactor, respectively.

[0191] In one embodiment, during the polymerization reaction of the propylene monomer or the polymerization reaction of the first ethylene monomer and the first propylene monomer in the first bulk reactor, the temperature inside the first bulk reactor may be controlled to 55°C to 70°C, or 55°C to 62.5°C.

[0192] In one embodiment, the polymerization reaction time in the first bulk reactor may be 45 minutes to 60 minutes.

[0193] In one embodiment, during the polymerization reaction of the second ethylene monomer and the second propylene monomer in the second bulk reactor, the temperature inside the second bulk reactor can be controlled to 55°C to 70°C, or 55°C to 62.5°C.

[0194] In one embodiment, the polymerization reaction time in the second bulk reactor may be 15 minutes to 35 minutes.

[0195] In one embodiment, during the polymerization reaction of the third ethylene monomer and the third propylene monomer in the gas phase reactor, the temperature inside the gas phase reactor may be controlled to 70°C to 85°C or 70°C to 80°C.

[0196] In one embodiment, the polymerization reaction time in the gas-phase reactor may be 30 minutes to 60 minutes.

[0197] In one embodiment, the manufacturing method may further include the step of extruding the polypropylene-based resin or a composition containing it discharged from the gas phase reactor to form pellets.

[0198] The extrusion of the above polypropylene-based resin or a composition containing the same can be performed by an extruder. As a non-limiting example, the extruder may include a strand die, etc.

[0199] In one embodiment, the composition comprising the polypropylene-based resin may include the polypropylene-based resin and an additive, and the above description regarding the additive is referenced.

[0200] In one embodiment, a composition comprising the polypropylene-based resin and additives can be fed into an extruder.

[0201] The extruder above can mix and extrude the composition while heating and melting it, and thereby form pellets.

[0202] The content of the above additive may be 0.2% to 1.0% by weight based on the total weight of the composition.

[0203] In one embodiment, the manufacturing method may further include the step of forming a press-formed sheet by high-temperature molding the pellet. The press forming may be performed, for example, using a hot press, and the hot press may be a hydraulic press such as a Wabash. For example, after the pellet is fed into a metal mold, a sheet may be formed by performing a hot press at a temperature of about 200°C to 240°C and a pressure of about 5 ton to 20 ton. Subsequently, the press-formed sheet may be manufactured by performing a cooling press at a temperature of about 20°C to 50°C using a cooling press.

[0204] In one embodiment, the thickness of the press-formed sheet may be 0.001 mm to 5.0 mm.

[0205] In another embodiment, the method for manufacturing the polypropylene-based resin may include the step of extruding the polypropylene-based resin discharged from the gas phase reactor to form an extruded sheet.

[0206] For example, the polypropylene-based resin and the additive can be fed into a twin-screw extruder to melt and sheet. As a non-limiting example, the extruder may include a T-die, a sheet die, etc.

[0207]

[0208] In the following, embodiments of the present disclosure are further described with reference to specific experimental examples. The embodiments and comparative examples described in the experimental examples are merely illustrative for explaining the present disclosure, and the technical scope of the present disclosure is defined by the appended claims and is not limited by the experimental examples.

[0209]

[0210] Examples and Comparative Examples

[0211]

[0212] Examples 1 to 6 and Comparative Examples 1 to 9

[0213] A polypropylene-based resin was prepared by applying Spheripol® process conditions using a Ziegler-Natta catalyst. Specifically, as shown in FIG. 2b, the polypropylene-based resin was prepared using a reactor in which a first bulk reactor, a second bulk reactor, and a gas reactor were connected in series. Component (a) was prepared in the first bulk reactor, component (b) was prepared in the second bulk reactor, and components (c) and (d) were prepared in the gas reactor. Component (a) was produced in the first bulk reactor and then sequentially transferred to the second bulk reactor and the gas reactor, and component (b) was produced in the second bulk reactor and then transferred to the gas reactor.

[0214] The reaction temperature and reaction time in each reactor were as follows.

[0215] No. 1 Bulk Reactor: 62.5 ℃ and 60 min

[0216] No. 2 Bulk Reactor: 62.5 ℃ and 35 min

[0217] Gas phase reactor: 77 ℃ and 40 min

[0218] The polypropylene resins according to each of the examples and comparative examples were prepared in substantially the same way, except that the composition of the polypropylene resin was controlled as described in Tables 1 and 2 below by controlling the content of ethylene monomer and / or propylene monomer fed into the first bulk reactor, the second bulk reactor, and the gas phase reactor, respectively.

[0219] In Table 1 above, homopolymer means homopolymer of propylene, copolymer means ethylene-propylene copolymer, and EPR means ethylene-propylene rubber copolymer.

[0220] Specifically, in Table 1 above, the content of each component (a) to component (d) represents a weight % (wt%) based on the total weight of the polypropylene-based resin. The total content of each component (a) to component (d) is about 100 wt%.

[0221] In Table 2 above, the ethylene content (wt%) represents the content of structural units derived from ethylene monomers based on the weight of the copolymer of each component. Additionally, the total ethylene content (wt%) in component (a) + component (b) refers to the total content of structural units derived from ethylene monomers based on the total weight of component (a) and component (b). Additionally, the total ethylene content (wt%) in component (c) + component (d) refers to the total content of structural units derived from ethylene monomers based on the total weight of component (c) and component (d).

[0222]

[0223] Ingredient (a) Ingredient (b) Ingredient (c) + Ingredient (d) Type Content (wt%) Type Content (wt%) Type Content (wt%) Example 1 No. 1 Mother Polymer 35.6 Copolymer 19.2 EPR + Copolymer 45.2 Example 2 No. 2 Mother Polymer 36.4 Copolymer 19.6 EPR + Copolymer 44.0 Example 3 No. 36.8 Copolymer 19.8 EPR + Copolymer 43.4 Example 4 No. 4 Copolymer 35.7 Copolymer 19.2 EPR + Copolymer 45.1 Example 5 No. 5 Mother Polymer 32.9 Copolymer 17.7 EPR + Copolymer 49.5 Example 6 No. 6 Mother Polymer 29.6 Copolymer 16.0 EPR + Copolymer 54.4 Comparative Example No. 1 Mother Polymer 36.5 Mother Polymer 19.6 EPR + Copolymer 43.9 Comparative Example 2 Copolymer 36.7 Copolymer 19.7 EPR + Copolymer 43.6 Comparative Example 3 Copolymer 35.6 Copolymer 19.2 EPR + Copolymer 45.3 Comparative Example 4 Copolymer 36.8 Copolymer 19.8 EPR + Copolymer 43.4 Comparative Example 5 Copolymer 36.5 Copolymer 19.6 EPR + Copolymer 43.9 Comparative Example 6 Copolymer 35.2 Copolymer 18.9 EPR + Copolymer 45.9 Comparative Example 7 Copolymer 36.7 Copolymer 19.7 EPR + Copolymer 43.6 Comparative Example 8 Copolymer 32.5 Copolymer 17.5 EPR + Copolymer 50.1 Comparative Example 9 Copolymer 29.9 Copolymer 16.1 EPR + Copolymer 53.9

[0224]

[0225] Content of ethylene in component (a) (wt%) Content of ethylene in component (b) (wt%) Total content of ethylene in component (a) + component (b) (wt%) Total content of ethylene in component (c) + component (d) (wt%) Example 1-7.9 2.8 38.0 Example 2-6.5 2.3 38.3 Example 31.16 12.9 40.5 Example 40.8 5.5 2.4 39.2 Example 5-7.8 2.7 38.7 Example 6-7.9 2.8 38.0 Comparative Example 1---37.5 Comparative Example 22.9 2.9 2.9 38.2 Comparative Example 33.13 13.1 38.6 Comparative Example 41.11 11 38.8 Comparative Example 51.91.91.937.8 Comparative Example 63.63.63.638.0 Comparative Example 72.52.52.539.4 Comparative Example 82.72.72.738.0 Comparative Example 93.13.13.138.9

[0226]

[0227] Experimental Example

[0228] The physical properties of the polypropylene-based resins prepared according to the above examples and comparative examples were evaluated in the following manner.

[0229]

[0230] Experimental Example 1: Contents of each component (a) to (d)

[0231] The content of components (a) to (d) in the polypropylene-based resins according to the examples and comparative examples was calculated based on the polymerization heat in each reactor and the total amount of the final resin produced.

[0232] First, the amount of heat removed from each reactor during the reaction in the first and second bulk reactors was measured. The amount of heat removed from each reactor was calculated based on the flow rate of the cooling medium, the specific heat of the cooling medium, the inlet and outlet temperatures of the cooling medium, and / or the reaction time.

[0233] The amount of component (a) produced was calculated from the total heat removed in the first bulk reactor, and the amount of component (b) produced was calculated from the total heat removed in the second bulk reactor.

[0234] Finally, after measuring the total amount of polypropylene-based resin discharged and recovered from the gas phase reactor, the total amount of components (c) and (d) produced was calculated by subtracting the amount of component (a) and component (b) produced above.

[0235] If necessary, the weight ratio of component (c) and component (d) can be calculated through xylene-soluble component analysis or nuclear magnetic resonance (NMR) analysis, etc.

[0236]

[0237] Experimental Example 2: Content of each ethylene monomer

[0238] (1) Flakes of components (a) to (d) taken from the first bulk reactor, the second bulk reactor, and the gas phase reactor, respectively, were prepared into film specimens according to the method below.

[0239] Each flake was placed into a 0.5T mold in a heating press (Wabash) set to 230 ℃, and formed by pressing while heating at a pressure of 15 ton for 5 minutes. Subsequently, a film specimen with a thickness of 500 μm was prepared by cooling and pressing in a cooling press under conditions of 30 ℃ and 100 bar for 2 minutes.

[0240] The ethylene content of film specimens prepared by press forming was measured using FT-IR analysis. The integrated area of ​​the ethylene-derived methylene rocking band was 770–700 cm⁻¹. -1 It was calculated in the area. The reference region is 4500-4000 cm. -1 It was set as the sum of the integral areas of the overtone and combination bands of the range.

[0241]

[0242] The normalized value R was calculated as follows.

[0243] Normalized value R = A(770-700) / A(4500-4000)

[0244] Here, A(770-700) is 770-700 cm -1 It is the integral area of ​​the region, and A(4500-4000) is 4500-4000 cm² -1 It is the integral area of ​​the region.

[0245] The ethylene content is the above normalized value R 13 It was calculated by substituting into a calibration equation based on standard samples confirmed by C-NMR.

[0246]

[0247] (2) The ethylene content in the xylene-insoluble portion of the manufactured polypropylene resin was measured as follows. The ethylene content may be a value corresponding to the total content of structural units derived from ethylene monomers based on the total weight of the copolymers included in components (a), (b), and (d).

[0248] 2 g of a polypropylene-based resin sample was added to p-xylene (purity about 99%) to prepare a 1 w / v% solution, and the total volume of the solution was made to be 200 mL.

[0249] The prepared solution was refluxed at approximately 135 °C for 1 hour, transferred to a 500 mL Erlenmeyer flask, and left to stand at room temperature for 30 minutes while stirring. Subsequently, the precipitate in the solution settled at the bottom of the flask, separating into a supernatant and a precipitate. The supernatant was separated by decanting to obtain the precipitate.

[0250] The solvent was removed from the above precipitate in a vacuum oven at 60°C to obtain a solid, and the solid was placed into a 0.5T mold in a heating press equipment (Wabash) set at 230°C and molded by pressing while heating at a pressure of 15 ton for 5 minutes. Subsequently, a film specimen with a thickness of 500 μm was prepared by cooling and pressing in a cooling press under conditions of 30°C and 100 bar for 2 minutes.

[0251] Afterwards, the ethylene content of the above film specimen was calculated in the same way as in (1) of Experimental Example 2.

[0252]

[0253] Experimental Example 3: Melting Point and Crystallization Temperature

[0254] 10 mg of a polypropylene-based resin sample was placed in an aluminum pan, and differential scanning calorimetry (DSC) was performed using a TA Instruments DSC instrument (Q20) with an empty aluminum pan as the reference pan.

[0255] The analysis was performed in a nitrogen atmosphere, and the process of heating the sample to 200 ℃ at a rate of 10 ℃ / min and then cooling it to -50 ℃ at a rate of 10 ℃ was repeated twice.

[0256] The highest temperature of the endothermic peak was evaluated as the melting point from the data obtained during the second heating run.

[0257] The crystallization temperature was evaluated from the data obtained during the first cooling run.

[0258]

[0259] Figure 3 illustrates the change in the melting point of a polypropylene-based resin according to the total content (wt%) of ethylene in component (a) and component (b). Referring to Figure 3, the polypropylene-based resin according to the example showed a higher melting point compared to the comparative example in the range where the total content (wt%) of ethylene in component (a) and component (b) was substantially the same.

[0260]

[0261] Experimental Example 4: Content of Xylene Dissolved Content

[0262] The content of xylene soluble fraction was measured according to the ASTM D5492 test method.

[0263] 2 g of a polypropylene-based resin sample was added to p-xylene (purity about 99%) to prepare a 1 w / v% solution, and the total volume of the solution was made to be 200 mL.

[0264] The prepared solution was refluxed at approximately 135°C for 1 hour, then transferred to a 500 mL Erlenmeyer flask and left to stand at room temperature for 30 minutes while stirring. Subsequently, the precipitate in the solution settled at the bottom of the flask and separated into a supernatant and a precipitate.

[0265] The above supernatant was separated by a decanting method. The weight of the solid obtained by naturally evaporating the solvent from the separated supernatant at room temperature (W S ) was measured. The weight of the above solid was measured using a precision electronic balance (precision 0.1 mg).

[0266] The weight (W) of the above solid S ) is the weight of the initial sample (W T The percentage of the value divided by 2 g was calculated as xylene soluble content (XS, wt%).

[0267]

[0268] Experimental Example 5: Flexural Modulus

[0269] 100 parts by weight of polypropylene resin, 0.05 parts by weight of calcium stearate (SC-110), 0.1 parts by weight of Irganox 1010, 0.2 parts by weight of Irgafos 168, and 0.2 parts by weight of Millad® 3988 were mixed and then melt-kneaded using an extruder to produce pellets.

[0270] The manufactured pellets were placed into a 2T mold equipped in a heating press (Wabash) set to 230 ℃, and molded by heating and pressing at a pressure of 15 ton for 5 minutes. Subsequently, a polypropylene-based resin specimen in the shape of a rectangular bar measuring 125 mm x 12.5 mm x 3.2 mm was prepared by cooling and pressing in a cooling press under conditions of 30 ℃ and 100 bar for 2 minutes.

[0271] A three-point bending test was performed using a universal testing machine (Instron® 3400) according to the ASTM D790 test method. The flexural modulus was calculated using the initial slope (N / mm) of the load-deformation curve.

[0272] Span length (L) ratio: 16:1

[0273] Deformation rate: 13 mm / min

[0274] Temperature and Humidity: Room temperature and 50% RH

[0275]

[0276] Experimental Example 6: Ratio (R) expressed by Equation 1 P )

[0277] By substituting the melting point, xylene soluble content, and flexural modulus evaluated in Experimental Examples 3 to 5 above into the following Formula 1, the ratio (R P ) calculated.

[0278] [Equation 1]

[0279] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))}

[0280]

[0281] The relationship between them is shown in Figure 4, with the denominator of Equation 1, FM + (12.5(MPa / wt%) Х XS(wt%)), on the horizontal axis and the numerator, Tm(°C), on the vertical axis. In addition, R calculated from the above relationship P In terms of (℃ / MPa) values, the polypropylene resin according to the examples showed a value greater than 0.19 ℃ / MPa, and the polypropylene resin according to the comparative examples showed a value less than or equal to 0.19 ℃ / MPa.

[0282] The above "FM + (12.5(MPa / wt%) Х XS(wt%))" can be used as an indicator representing the flexural modulus of the matrix excluding the ethylene-propylene rubber copolymer, which is component (c), in the above polypropylene-based resin.

[0283] Referring to FIG. 4, the polypropylene-based resin according to the examples exhibits a high melting point (Tm) relative to the flexural modulus of the matrix. On the other hand, the polypropylene-based resin according to the comparative examples shows a significantly lower melting point (Tm) compared to the examples.

[0284] That is, assuming that it contains substantially the same amount of component (c), the polypropylene resin according to the examples can secure a higher melting point (Tm) under substantially the same flexural modulus conditions compared to the comparative examples.

[0285]

[0286] Experimental Example 7: Melt Index

[0287] A 5g sample of polypropylene-based resin was fed into an MI-4 Melt Flow Indexer (GOETTFERT) to measure the melt index. The measurement conditions were as follows.

[0288] Measured temperature: 230℃

[0289] Load: 2.16kg (Weighted load method)

[0290] Measurement time: Measurement of the mass of resin that flowed for 10 minutes

[0291]

[0292] Experimental Example 8: Dielectric Breakdown Strength

[0293] 100 parts by weight of polypropylene resin, 0.05 parts by weight of calcium stearate (SC-110), 0.1 parts by weight of Irganox 1010, 0.2 parts by weight of Irgafos 168, and 0.2 parts by weight of Millad® 3988 were mixed and then melt-kneaded using an extruder to produce pellets.

[0294] The manufactured pellets were placed into a 0.1T mold equipped in a heating press (Wabash) set to 230 ℃, and molded by heating and pressing at a pressure of 15 ton for 5 minutes. Subsequently, a sheet-shaped polypropylene resin specimen with a thickness of approximately 130 μm was prepared by cooling and pressing in a cooling press under conditions of 30 ℃ and 100 bar for 2 minutes.

[0295]

[0296] In accordance with ASTM D149, the dielectric breakdown strength of the above specimen was measured at room temperature using a DC high-voltage generator (Phenix 6TC4100-10, using spherical electrodes) while maintaining a constant electrode spacing. At this time, a spherical brass electrode with a diameter of 25 mm was used, and the electrode and specimen were tested while immersed in insulating oil.

[0297] The voltage was increased at a rate of 1 kV / s, and the dielectric breakdown strength was calculated based on the dielectric breakdown voltage for the specimen thickness.

[0298]

[0299] The results of Experimental Examples 3 to 8 are shown in Tables 3 and 4 below.

[0300]

[0301] Ratio (R P, °C / MPa) Melting point (Tm, °C) Xylene dissolved content XS (wt%) Flexural modulus (MPa) Example 1 0.199 163.64 0.7315 Example 2 0.198 164.53 9.7334 Example 3 0.193 157.13 8.9327 Example 4 0.191 159.14 0.8322 Example 5 0.195 163.94 5.0276 Example 6 0.195 163.55 0.1213 Comparative Example 10.169 166.04 0.4475 Comparative Example 20. 186151.439.1325 Comparative Example 30.181150.640.7322 Comparative Example 40.182161.939.5394 Comparative Example 50.183156.239.7358 Comparative Example 60.177146.541.1313 Comparative Example 70.187153.239.2328 Comparative Example 80.183152.845.6265 Comparative Example 90.182151.249.7208

[0302]

[0303] Content of ethylene monomer in xylene-insoluble fraction (wt%) Crystallization temperature (Tc, °C) Tm-Tc ( °C) Melt index (dg / min) Dielectric breakdown strength (DC, kV / mm) Example 1 7.6 1 27.1 36.5 1.1 522 Example 2 7.1 1 26.7 37.8 1.1 487 Example 3 7.4 1 24.5 32.6 1.2 474 Example 4 7.3 1 25.9 33.2 1.3 483 Example 5 8.1 1 26.7 37.2 1.0 467 Example 6 8.6 1 26.1 37.4 0.9 455 Comparative Example 1 5.9 1 28.9 37.1 1.4 474 Comparative Example 2 7.41 22.129.31.2478 Comparative Example 37.7121.529.11.1486 Comparative Example 46.4125.636.31.1483 Comparative Example 56.9124.232.01.0485 Comparative Example 68.1121.525.01.1487 Comparative Example 77.2122.930.31.3490 Comparative Example 88.2120.532.30.9458 Comparative Example 98.4121.329.91.1450

[0304]

[0305] The ratio of Formula 1 (R) to the polypropylene-based resin according to the examples PAll values ​​were controlled to be greater than 0.19 ℃ / MPa, thereby improving the balance between the melting point and the flexural modulus. Accordingly, the polypropylene-based resin according to the examples can exhibit excellent flexibility while also exhibiting characteristics that allow damage caused by repeated bending, twisting, and impact to be suppressed for a long period of time.

[0306] However, the ratio of Formula 1 (R) to the polypropylene-based resin according to Comparative Examples 2, 3 and 5 to 9 P All were evaluated to be 0.19 ℃ / MPa or lower, with a melting point lower than 157 ℃. In this case, when applied as a wire sheathing material, there is a possibility that heat resistance will decrease in a high-temperature environment and thermal deformation may occur.

[0307] In the case of Comparative Examples 1 and 4, the flexural modulus was too high at 475 MPa and 394 MPa, respectively. In this case, the rigidity of the resin may increase excessively, which could lead to a decrease in flexibility, and there is a possibility that the flexural flexibility may decrease or cracks may occur when applied as a wire sheathing material. Furthermore, in the case of Comparative Example 4, although the flexural modulus was higher than that of Examples 1 and 2, the melting point was found to be lower, indicating that increased rigidity and heat resistance properties could not be secured simultaneously.

Claims

1. Component (a) propylene homopolymer or primary ethylene-propylene copolymer; Component (b) secondary ethylene-propylene copolymer; and Component (c) comprises an ethylene-propylene rubber copolymer, and The content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and The ratio (R) represented by the following Formula 1 for the above polypropylene-based resin P Polypropylene-based resin with a ℃ / MPa greater than 0.19 ℃: [Equation 1] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))} In the above Equation 1, Tm represents the melting temperature (°C) of the polypropylene resin measured by Differential Scanning Calorimetry (DSC), FM represents the flexural modulus (MPa) of the polypropylene resin measured according to the ASTM D790 test method, and XS represents the content (wt%) of the xylene dissolved component of the polypropylene resin measured according to the ASTM D5492 test method.

2. The polypropylene resin according to claim 1, wherein the melting point (Tm) of the polypropylene resin is 150 ℃ to 180 ℃.

3. The polypropylene resin according to claim 1, wherein the flexural modulus (FM) of the polypropylene resin is 200 MPa to 350 MPa.

4. A polypropylene resin according to claim 1, wherein the content (XS) of the xylene dissolved portion of the polypropylene resin is 35% to 55% by weight.

5. The polypropylene-based resin according to claim 1, wherein the crystallization temperature (Tc) of the polypropylene-based resin measured by differential scanning calorimetry is 100 ℃ to 140 ℃, and the difference (Tm-Tc) between the melting point and the crystallization temperature is 30 ℃ to 50 ℃.

6. A polypropylene-based resin according to claim 1, wherein component (a) comprises a first ethylene-propylene copolymer, the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is less than 3.5 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer is 3.5 weight% or more.

7. A polypropylene-based resin according to claim 6, wherein the content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is greater than 0 weight% and less than or equal to 3 weight%, and the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer is 3.5 weight% to 8 weight%.

8. A polypropylene-based resin according to claim 1, wherein, based on the total weight of the first ethylene-propylene copolymer and the second ethylene-propylene copolymer, the total content of structural units derived from ethylene monomers in each copolymer is 2% to 7% by weight.

9. In claim 1, the propylene homopolymer is included as component (a), and A polypropylene-based resin having a content of structural units derived from ethylene monomers in a second ethylene-propylene copolymer of 5 weight% or more.

10. A polypropylene resin according to claim 1, wherein the content of component (a) is 25% to 40% by weight based on the total weight of the polypropylene resin.

11. A polypropylene resin according to claim 1, wherein the content of component (b) is 12% to 25% by weight based on the total weight of the polypropylene resin.

12. A polypropylene resin according to claim 1, wherein the content of component (c) is 40% to 55% by weight based on the total weight of the polypropylene resin.

13. The polypropylene-based resin according to claim 1, wherein the breakdown strength under DC (BDS) of the polypropylene-based resin is 450 kV / mm to 600 kV / mm.

14. A polypropylene resin according to claim 1, wherein the total content of structural units derived from ethylene monomers in the xylene-insoluble portion of the polypropylene resin is 6.5% by weight to 10.5% by weight.

15. The polypropylene-based resin according to claim 1, further comprising component (d) a third ethylene-propylene copolymer.

16. The invention of claim 1 further comprises an additive comprising at least one selected from the group consisting of antioxidants, neutralizing agents, and nucleating agents, and A polypropylene resin having a content of the above additive of 0.2% to 1.0% by weight based on the total weight of the polypropylene resin.

17. A step of introducing a propylene monomer into a first bulk reactor without a comonomer and reacting it, or introducing a first ethylene monomer and a first propylene monomer and reacting them to form component (a) a propylene homopolymer or a first ethylene-propylene copolymer; A step of introducing a second ethylene monomer and a second propylene monomer into a second bulk reactor connected to a first bulk reactor and reacting them to form component (b) a second ethylene-propylene copolymer; A step of introducing a third ethylene monomer and a third propylene monomer into a gas phase reactor connected to a second bulk reactor and reacting them to form component (c) ethylene-propylene rubber copolymer; and The method includes a step of discharging a polypropylene-based resin from the above-mentioned gas-phase reactor, and The component (a) in the first bulk reactor is transferred to the second bulk reactor by a connecting line connecting the first bulk reactor and the second bulk reactor, and Components (a) and (b) in the second bulk reactor are transferred to the gaseous reactor by a connecting line connecting the second bulk reactor and the gaseous reactor, and The above polypropylene-based resin is, Component (a) propylene homopolymer or first ethylene-propylene copolymer; Component (b) secondary ethylene-propylene copolymer; and Component (c) comprises an ethylene-propylene rubber copolymer, and The content of structural units derived from ethylene monomers in the first ethylene-propylene copolymer is smaller than the content of structural units derived from ethylene monomers in the second ethylene-propylene copolymer, and The ratio (R) represented by the following Formula 1 for the above polypropylene-based resin P Method for manufacturing a polypropylene-based resin in which ) is greater than 0.19 ℃: [Equation 1] R P (℃ / MPa) = Tm(℃) / {FM + (12.5(MPa / wt%) × XS(wt%))} In the above Equation 1, Tm represents the melting temperature (°C) of the polypropylene resin measured by Differential Scanning Calorimetry (DSC), FM represents the flexural modulus (MPa) of the polypropylene resin measured according to the ASTM D790 test method, and XS represents the content (wt%) of the xylene dissolved component of the polypropylene resin measured according to the ASTM D5492 test method.

18. In paragraph 17, a first ethylene monomer and a first propylene monomer are introduced into a first bulk reactor to form a first ethylene-propylene copolymer as component (a), and A method for manufacturing a polypropylene-based resin, wherein the content of the first ethylene monomer introduced into the first bulk reactor is less than 3.5 weight% of the total weight of the first ethylene monomer and the first propylene monomer, and the content of the second ethylene monomer introduced into the second bulk reactor is 3.5 weight% or more of the total weight of the second ethylene monomer and the second propylene monomer.

19. In paragraph 17, a propylene monomer is introduced into the first bulk reactor without a comonomer to form a propylene homopolymer as component (a), and A method for manufacturing a polypropylene-based resin, wherein the content of the second ethylene monomer introduced into the second bulk reactor is 5% by weight or more of the total weight of the second ethylene monomer and the second propylene monomer.

20. In the step of forming the above component (c) ethylene-propylene rubber copolymer, the third ethylene monomer and the third propylene monomer are introduced into the gas phase reactor and reacted to form the component (c) ethylene-propylene rubber copolymer and the component (d) third ethylene-propylene copolymer, and A method for manufacturing a polypropylene-based resin, wherein the above polypropylene-based resin further comprises component (d) a third ethylene-propylene copolymer.