Sheet for preventing thermal runaway of battery, and battery cell assembly comprising same

The battery thermal runaway prevention sheet addresses the inefficiencies of conventional materials by using a fiber-reinforced core with a porous additive and non-combustible coating to delay heat transfer and pressure, ensuring safety and maintaining battery performance during thermal events.

WO2026235481A1PCT designated stage Publication Date: 2026-11-12KCC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/096638
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Conventional battery modules face challenges in efficiently ensuring safety against heat or fire, as materials used to prevent thermal runaway are expensive and lose elasticity with increased input, reducing battery efficiency and failing to adequately compensate for cell swelling.

Method used

A battery thermal runaway prevention sheet comprising a fiber-reinforced core impregnated with a porous additive and a non-combustible film or flame-retardant coating layer, designed to delay heat transfer and withstand high pressures, with a high recovery capability to manage cell swelling and prevent fire spread.

Benefits of technology

The sheet effectively delays heat transfer and pressure buildup during thermal runaway, providing sufficient time for evacuation and maintaining battery performance by securing safety against heat or fire, with high compression/restoration efficiency and minimal impact on battery capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2026096638_12112026_PF_FP_ABST
    Figure KR2026096638_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a sheet for preventing thermal runaway of a battery, and a battery cell assembly comprising same. The sheet for preventing thermal runaway of a battery comprises: a first layer; and a second layer laminated on at least one of the upper portion and the lower portion of the first layer, wherein: the first layer includes a fiber reinforced core material and a porous additive, and is formed by impregnating the fiber reinforced core material with an impregnation solution containing the porous additive; and the second layer includes at least one of a nonflammable film layer and a flame-retardant coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

A sheet for preventing battery thermal runaway and a battery cell assembly including the same

[0001] The present invention relates to a sheet for preventing battery thermal runaway and a battery cell assembly including the same.

[0002] Currently commercialized rechargeable batteries include nickel-cadmium batteries, nickel-hydrogen batteries, nickel-zinc batteries, and lithium-ion batteries. Recently, there has been an increasing demand for high-capacity battery modules applied to electronic devices and automobiles. These high-capacity battery modules are equipped with multiple battery cells.

[0003] In such battery modules, if thermal runaway, fire, or explosion occurs in a portion of multiple battery cells, fragments, flames, and gases of the electrode assembly may be emitted, potentially raising the temperature of adjacent battery cells. Consequently, there is a problem in that thermal runaway or fire may spread to adjacent battery cells, potentially leading to a larger secondary fire or explosion and exacerbating the damage.

[0004] Korean Patent Publication No. 10-2022-0048433 (Patent Document 1) discloses a battery module comprising a plurality of battery cells, a module case, a polymer member, and a filler.

[0005] In the case of conventional battery modules, configurations incorporating specific materials to prevent internal heat or flame propagation are being attempted; however, while a large amount must be added to ensure sufficient heat resistance, there is also the problem that these specific materials are expensive.

[0006] Furthermore, even without considering cost, an issue arises where the material loses elasticity as the input amount increases, making it unable to adequately compensate for cell swelling. This has a negative impact as it reduces battery efficiency.

[0007] Accordingly, conventional battery modules face many difficulties in efficiently ensuring safety against heat or fire.

[0008] [Prior Art Literature]

[0009] (Patent Document 1) KR 10-2022-0048433 A (2022.04.19)

[0010] One objective of the present invention is to provide a battery thermal runaway prevention sheet that can efficiently ensure safety against heat or fire, etc.

[0011] Another objective of the present invention is to provide a battery cell assembly to which a battery thermal runaway prevention sheet is applied, thereby efficiently ensuring safety against heat or fire, etc.

[0012] The present invention provides a battery thermal runaway prevention sheet comprising: a first layer (110); and a second layer (120; 120', 120") laminated on at least one of the upper and lower portions of the first layer (110); wherein the first layer (110) comprises a fiber reinforcing core and a porous additive, formed by impregnating the fiber reinforcing core in an impregnation solution containing the porous additive, and the second layer (120) comprises at least one of a non-combustible film layer and a flame-retardant coating layer.

[0013] The battery thermal runaway prevention sheet according to the present invention reflects the battery operating environment and, when compressed under a high-pressure state caused by cell swelling, can sufficiently delay the transfer of high heat generated during cell thermal runaway to adjacent cells, thereby securing time for vehicle occupants to evacuate from a fire. Specifically, the thermal runaway prevention sheet must have excellent compression / restoration efficiency as it is normally subjected to pressure generated by cell swelling, and is in an environment where it may be exposed to high pressure of 2.0 MPa or higher due to gases generated when thermal runaway occurs in the battery cell. When the internal temperature of a cell rises due to thermal runaway, heat is transferred to nearby cells, and if the temperature of the nearby cells rises, continuous thermal runaway occurs. The thermal runaway prevention sheet according to the present invention can efficiently ensure safety against heat or fire by delaying the time for the explosion cell to rise with high pressure and internal temperature and transfer to the opposite side, thereby securing time for vehicle occupants to safely exit the vehicle.

[0014] In addition, it has a high recovery capability of 90% even in a repeated cell swelling environment, which assists in cell swelling phenomena and enables the battery's performance to be fully realized.

[0015] FIG. 1 schematically shows a vertical cross-sectional view of a battery thermal runaway prevention sheet according to one embodiment of the present invention.

[0016] FIG. 2 schematically shows a vertical cross-sectional view of a sheet for preventing battery thermal runaway according to another embodiment of the present invention.

[0017] FIG. 3 schematically shows a vertical cross-sectional view of a sheet for preventing battery thermal runaway according to another embodiment of the present invention.

[0018] FIG. 4 schematically shows a perspective view and a vertical cross-sectional view of a battery thermal runaway prevention sheet according to another embodiment of the present invention.

[0019] Figure 5 is a graph of stress versus strain (percentage (%)) representing the compression curve.

[0020] Various embodiments of the present invention will be described in detail below with reference to the attached drawings.

[0021] The present invention provides, in one aspect, a sheet for preventing battery thermal runaway. The battery thermal runaway prevention sheet according to the present invention is applied to a battery cell assembly to efficiently ensure the safety of the battery cell assembly against heat or fire. For example, in the event of a fire occurring in any one battery cell within the battery cell assembly, the battery thermal runaway prevention sheet according to the present invention can prevent chain ignition to the entire battery cell assembly.

[0022] FIG. 1 schematically shows a vertical cross-sectional view of a battery thermal runaway prevention sheet according to one embodiment of the present invention.

[0023] Referring to FIG. 1, in one embodiment, the battery thermal runaway prevention sheet (100) of the present invention comprises a first layer (110) and a second layer (120; 120', 120").

[0024] The first layer (110) comprises a fiber-reinforcing core and a porous additive, and is formed by impregnating the fiber-reinforcing core in an impregnation solution containing the porous additive. Here, the porous additive comprises at least one of a microporous additive, a mesoporous additive, and a nanoporous additive.

[0025] A second layer (120; 120', 120") is stacked on at least one of the upper and lower parts of the first layer (110). For example, referring to FIG. 1, the second layer (120) may be stacked only on the upper part of the first layer (110), may be stacked only on the lower part of the first layer (110), or may be stacked on both the upper and lower parts of the first layer (110).

[0026] Meanwhile, the second layer (120) includes at least one of a non-combustible film layer and a flame-retardant coating layer. For example, the second layer (120) may include only a non-combustible film layer, only a flame-retardant coating layer, or both a non-combustible film layer and a flame-retardant coating layer.

[0027] FIG. 2 schematically shows a vertical cross-sectional view of a sheet for preventing battery thermal runaway according to another embodiment of the present invention.

[0028] Referring to FIG. 2, in one embodiment, the battery thermal runaway prevention sheet (200) of the present invention further includes a third layer (130; 130', 130") disposed between the first layer (110) and the second layer (120).

[0029] When the battery thermal runaway prevention sheet (200) includes a first layer (110) and a second layer (120') stacked on top of the first layer (110), a third layer (130') is disposed between the first layer (110) and the second layer (120').

[0030] Meanwhile, if the battery thermal runaway prevention sheet (200) includes a first layer (110) and a second layer (120) laminated below the first layer (110), a third layer (130) is placed between the first layer (110) and the second layer (120).

[0031] In addition, when the battery thermal runaway prevention sheet (200) includes both the first layer (110) and the second layer (120', 120") stacked on the upper and lower parts of the first layer (110), the third layer (130', 130") is placed between the first layer (110) and the second layer (120', 120"), respectively.

[0032] Here, the third layer (130) is an adhesive layer that bonds the first layer (110) and the second layer (120).

[0033] FIG. 3 schematically shows a vertical cross-sectional view of a sheet for preventing battery thermal runaway according to another embodiment of the present invention.

[0034] Referring to FIG. 3, in one embodiment, the battery thermal runaway prevention sheet (101) of the present invention further includes a fourth layer (140) in addition to the first layer (110) and second layer (120) described above.

[0035] The fourth layer (140) is laminated to cover at least one of the sides of the first layer (110) and at least one of the sides, top surface, and bottom surface of the second layer (120; 120', 120").

[0036] Specifically, referring to FIG. 3, the fourth layer (140) is laminated to cover at least one of the front, rear, left, and right sides of the first layer (110). Additionally, the fourth layer (140) is laminated to cover at least one of the front, rear, left, and right sides, the top surface, and the bottom surface of the second layer (120; 120', 120").

[0037] The fourth layer (140) serves to prevent at least one of the sides of the first layer (110) and the second layer (120; 120', 120") from being exposed to the outside. Additionally, the fourth layer (140) serves to prevent at least one of the upper and lower surfaces of the second layer (120; 120', 120") from being exposed to the outside.

[0038] FIG. 4 schematically shows a perspective view and a vertical cross-sectional view of a battery thermal runaway prevention sheet according to another embodiment of the present invention. Specifically, FIG. 4(A) schematically shows a perspective view of a battery thermal runaway prevention sheet (201), and FIG. 4(B) schematically shows a vertical cross-sectional view along line L-L' of FIG. 4(A).

[0039] Referring to FIG. 4, in one embodiment, the battery thermal runaway prevention sheet (201) of the present invention further comprises a fourth layer (140) in addition to the aforementioned first layer (110), second layer (120; 120', 120"), and third layer (130; 130', 130").

[0040] The fourth layer (140) is laminated to cover at least one of the sides of the first layer (110), at least one of the sides, top surface, and bottom surface of the second layer (120; 120', 120"), and at least one of the sides of the third layer (130; 130', 130").

[0041] Specifically, referring to FIG. 4, the fourth layer (140) is laminated to cover at least one of the front, rear, left, and right sides of the first layer (110). Additionally, the fourth layer (140) is laminated to cover at least one of the front, rear, left, and right sides, the top surface, and the bottom surface of the second layer (120; 120', 120"). Additionally, the fourth layer (140) is laminated to cover at least one of the front, rear, left, and right sides of the third layer (130; 130', 130").

[0042] The fourth layer (140) serves to prevent at least one of the sides of the first layer (110), the second layer (120; 120', 120"), and the third layer (130; 130', 130") from being exposed to the outside. Additionally, the fourth layer (140) serves to prevent at least one of the upper and lower surfaces of the second layer (120; 120', 120") from being exposed to the outside.

[0043] Meanwhile, as described above, the first layer (110) comprises a fiber-reinforcing core and a porous additive. Here, the first layer (110) is formed by impregnating the fiber-reinforcing core with an impregnation solution containing a porous additive. Meanwhile, the porous additive comprises at least one of a microporous additive, a mesoporous additive, and a nanoporous additive.

[0044] The first layer (110) acts as an insulating layer that delays heat transfer in the event of a fire in the battery cell assembly. The first layer (110) also has elasticity and compressive strain capable of withstanding the pressure when swelling occurs in the battery cell.

[0045] The fiber-reinforced core material of the present invention includes, for example, discrete fibers, woven materials, nonwoven materials, batts, batting, webs, mats, felts, or combinations thereof, but is not limited thereto.

[0046] Specifically, the fiber-reinforcing core of the present invention comprises one or more selected from polyester, polyacrylonitrile (PAN), oxidized polyacrylonitrile, decarbonized heat-treated PAN, carbon, silica, polyaramid, polycarbonate, polyolefin, rayon, nylon, glass fiber (glass wool), high-density polyolefin, ceramic, acrylic, fluoropolymer, polyurethane, polyamide, and polyimide, but is not limited thereto. The fiber-reinforcing core of the present invention may be polyacrylonitrile (PAN), oxidized polyacrylonitrile, decarbonized heat-treated PAN, or glass fiber.

[0047] The fiber-reinforced core of the present invention contains 30 to 100 weight percent of oxidized polyacrylonitrile fiber (OPF) based on the total weight of the fiber-reinforced core. Here, the fiber-reinforced core may have voids inside.

[0048] The fiber-reinforced core material may be, for example, a porous nonwoven fabric containing oxidized polyacrylonitrile fibers (OPF) and having internal pores. Here, OPF is a fiber containing oxidized polyacrylonitrile (Oxi-PAN) and is one of the porous inorganic fiber core materials.

[0049] The fiber-reinforced core of the present invention may have a thermal conductivity of, for example, 0.1 W / m·K or less. If the thermal conductivity of the fiber-reinforced core exceeds 0.1 W / m·K, heat from a thermal runaway cell may be transferred to an adjacent cell within tens of seconds. Consequently, as the adjacent cell reaches the thermal runaway temperature within a short period of time, there is a problem in that it is difficult to secure sufficient time for a person to exit the vehicle.

[0050] The fiber-reinforced core of the present invention may have a thickness of 10 mm or less, 6 mm or less, or 0.1 to 4 mm. If the thickness of the fiber-reinforced core is 0.1 mm or less, it may be difficult to achieve sufficient thermal insulation, and if the thickness exceeds 10 mm, although the thermal insulation effect is excellent, it takes up an excessive amount of internal space in the battery, which causes a problem of reduced capacity of the battery itself.

[0051] Meanwhile, the fiber-reinforced core material may have a density of 80 to 250 kg / m³ or 85 to 230 kg / m³. If the fiber-reinforced core material satisfies the above density range, the impregnation liquid described below and the particles contained therein can fill the voids with the impregnation liquid and the particles contained therein being appropriately distributed on the surface of the fiber-reinforced core material.

[0052] The impregnation solution of the present invention contains a porous additive comprising at least one of a microporous additive, a mesoporous additive, and a nanoporous additive. The porous additive is attached in a distributed state to the surface of the yarn of the fiber reinforcing core and serves to fill the voids.

[0053] In the present invention, a fiber-reinforced core is impregnated with an impregnation solution containing a porous additive so that the porous additive can fill the pores of the fiber-reinforced core to a predetermined level. By doing so, the thermal conductivity of the fiber-reinforced core can be controlled to a predetermined level to obtain a desired heat transfer delay effect.

[0054] The impregnation solution contains a solvent and silica in a weight ratio of 100 parts by weight of solvent to 3 to 20 parts by weight of porous additive.

[0055] The solvent is water, preferably distilled water or deionized water. The solvent may also be mixed with organic solvents, such as alcohols, for the purpose of improving the compatibility and storage stability of the additive.

[0056] The porous additive has a particle size of 1 to 100 nm and a specific surface area of ​​50 to 1,000 m²2 / g, the pore size may be several nm to several tens of μm. The porous additive comprises, for example, one or more selected from hollow microglass spheres, silica, cenospheres, and aerogel particles, for example but not limited to.

[0057] For example, silica may be inorganic silica. Inorganic silica may include one or more selected from, for example, fumed silica, precipitated silica, silica-based aerogel, silica glass, and silicon ester. Preferably, silica may be fumed silica or precipitated silica.

[0058] Fumed silica is produced by hydrolyzing tetrachlorosilane with a high-temperature flame of over 1000°C; it has a low powder density of approximately 0.05 g / mL and very high silica purity. Fumed silica has a large inter-particle space, which minimizes heat transfer by gases, and due to its low thermal conductivity, heat transfer by itself is also minimal. Furthermore, fumed silica is stable even at high temperatures and possesses flame retardancy, resulting in excellent heat retardation effects.

[0059] The porous additive is included in the impregnation solution in an amount of 3 to 20 parts by weight, or 5 to 15 parts by weight, based on 100 parts by weight of the solvent. If the content of the porous additive falls outside the above range, the thermal retardation effect may be reduced.

[0060] The impregnation solution may further include one or more of a silane compound, an organic resin, and a silica sol. Based on 100 parts by weight of solvent, one or more of 0.1 to 15 parts by weight of a silane compound, 0.01 to 10 parts by weight of an organic resin, and more than 0 to 15 parts by weight of a silica sol may be included in the impregnation solution.

[0061] In the present invention, the silane compound reacts with the hydroxyl groups of the fiber reinforcing core to further bind the fiber reinforcing core and serves to attach the porous additive to the surface of the fiber reinforcing core yarn.

[0062] Silane compounds may include alkoxysilanes with two or more functions, such as trifunctional or tetrafunctional alkoxysilanes, or silicone resins in which the number of oxygen atoms bonded to each silicon atom is 1 to 4.

[0063] Silane compounds have the chemical formula (R a SiO 3 / 2 ) a (R b 2SiO 2 / 2 ) b (R c 3SiO 1 / 2 ) c It may include a branched-chain organopolysiloxane having an average unit of . Here, R a , R b , and R c Each is a group of monovalent hydrocarbons that are identical or different and substituted or unsubstituted, where a is a positive number, b is 0 or a positive number, and c is 0 or a positive number.

[0064] Specifically, the silane compounds are tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetraisopropoxysilane, tetra-n-butoxysilane, tetraisobutoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, isobutyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, It may be one or more selected from the group consisting of N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, dimethyldimethoxysilane, vinylmethyldimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-isocyanatopropyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, phenyltriethoxysilane, and phenyltrimethoxysilane.

[0065] A silane compound is included in the impregnation solution in an amount of 0.1 to 15 parts by weight, or 0.1 to 10 parts by weight, based on 100 parts by weight of the solvent. If the content of the silane compound is below the above range, it is difficult to secure physical properties such as strength and water resistance of the manufactured product, and if it exceeds the above range, the stability of the impregnation solution is reduced and the strength of the manufactured product may be lowered.

[0066] In the present invention, the organic resin acts as an elastic resin against battery cell swelling. The organic resin may include, for example, an acrylic resin.

[0067] The organic resin is included in the impregnation solution in an amount of 0.01 to 10 parts by weight, or 0.1 to 5 parts by weight, or 0.1 to 3 parts by weight, based on 100 parts by weight of the solvent. If the content of the organic resin is below the above range, the elastic effect is reduced, and if it exceeds the above range, the thermal retardation effect may be reduced.

[0068] In the present invention, the silica sol serves to further bind the fiber reinforcing core together with a silane compound and to attach a porous additive to the surface of the yarn of the fiber reinforcing core.

[0069] Silica sol may be included in the impregnation solution in an amount of more than 0 to 15 parts by weight, or 0.1 to 10 parts by weight, based on 100 parts by weight of the solvent. If the content of silica sol falls outside the above range, the strength of the manufactured product may decrease.

[0070] As described above, the second layer (120; 120', 120") includes at least one of a non-combustible film layer and a flame-retardant coating layer. The second layer (120; 120', 120") serves to improve the appearance characteristics of the battery thermal runaway prevention sheet, supplement impact resistance, enhance durability, minimize the reduction in thermal insulation, and block dust. When the second layer (120; 120', 120") includes both a non-combustible film layer and a flame-retardant coating layer, the second layer (120; 120', 120") may include a hot melt web between the non-combustible film layer and the flame-retardant coating layer.

[0071] The non-combustible film layer is a film layer having non-combustible performance and may include, for example, an organic film layer, an inorganic film layer, or an organic-inorganic mixed film layer, without limitation.

[0072] The organic film layer may include one or more selected from, for example, aramid film, polycarbonate film, polyimide film, polyethylene terephthalate film, cycloolefin polymer film, unoriented polypropylene film, and nylon film.

[0073] The inorganic film layer may include one or more types selected from, for example, inorganic fiber films (e.g., glass wool, glass fiber), MICA films, ceramic films, and asbestos films.

[0074] An organic-inorganic mixed film layer can be manufactured by mixing a material constituting an organic film layer with a material constituting an inorganic film layer. An organic-inorganic mixed film layer can be manufactured by impregnating or coating an inorganic film layer with a flame-retardant or non-flammable organic resin. Specifically, an organic-inorganic mixed film layer can be manufactured by impregnating or coating, for example, glass wool, MICA film, ceramic film, or asbestos film with a resin having silicone as the main component.

[0075] The flame-retardant coating layer may be a coating layer comprising at least one of silicone, silicate, and a flame retardant. Since the heat resistance temperature of inorganic materials is superior to that of organic materials at high temperatures, the flame-retardant coating layer of the present invention may serve to supplement the durability of the battery thermal runaway prevention sheet. In the case of the flame-retardant coating layer of the second layer (120), the viscosity may be 10,000 to 30,000 cPs.

[0076] Silicon is a thermosetting synthetic resin produced by the polymerization of organic derivatives, and through thermal curing, it is formed into a polymer that can secure mechanical properties.

[0077] One or more silicates may be used by mixing sodium silicate, calcium silicate, titanosilicate, aluminosilicate, lithium silicate, and tetraorthosilicate. Since silicates are stable at room temperature and have low viscosity, they are suitable for controlling the viscosity of the composition and, when mixed, play a role in improving impact resistance after film formation.

[0078] The flame retardant includes at least one of phosphorus-based flame retardants and inorganic flame retardants.

[0079] Phosphorus-based flame retardants comprise one or more selected from the group consisting of ammonium polyphosphate (APP), triphenyl phosphate (TPP), tricresyl phosphate (TCP), triethyl phosphate (TEP), isopropyl phenyl diphenyl phosphate, red phousphours (CG-P), tris(2-chloroethyl)phosphate (TCEP), phosphorus oxide, tetraphenyl resorcinol bis(diphenylphosphate) (TR), and resorcinol diphosphate (RDP). The phosphorus-based flame retardants of the present invention are polymers that form carbonaceous char upon thermal decomposition. The formation of char reduces combustible fuel and extinguishes the fire by creating a thick barrier on the surface of burning molecules to block heat. This process occurs during the condensation phase, and phosphorus is an important flame retardant in this phase. Phosphorus undergoes thermal decomposition to produce phosphoric acid, which acts as a dehydration catalyst in combustible materials, thereby increasing the amount of char. Although the mechanism of char formation is very complex, phosphorus compounds are highly effective flame retardants for polymers that contain oxygen atoms within their structures and form char during combustion, such as Polycarbonate (PC) or Polyphenylene Oxide (PPO). In particular, phosphorus-based flame retardants are eco-friendly materials that do not generate dioxins, which are carcinogens.

[0080] Inorganic flame retardants may be one or more selected from the group consisting of aluminum hydroxide (Al(OH)3), magnesium hydroxide (Mg(OH)2), calcium carbonate (CaCO3), magnesium carbonate (MgHCO3), zinc borate, and silica. Inorganic flame retardants may be included for a synergistic effect with phosphorus-based flame retardants. For example, zinc borate and aluminum hydroxide may be more effective in removing smoke.

[0081] The third layer (130; 130', 130") is attached to the upper or lower surface of the first layer (110) and serves to flatten the surface by compensating for any irregularities that may be formed on the first layer (110). Meanwhile, the third layer (130; 130', 130") is an adhesive layer that bonds the first layer (110) and the second layer (120) as described above.

[0082] In one embodiment, the third layer (130; 130', 130") is an adhesive layer comprising at least one of a hot melt web and a PSA film. The hot melt web is an adhesive that exhibits adhesiveness when heat is applied and is in the form of a sheet, such as a nonwoven fabric. The PSA (Pressure Sensitive Adhesive) film is an adhesive in the form of a film that exhibits adhesiveness by applying pressure without applying heat.

[0083] The hot melt web may be formed from a material comprising, for example, one or more selected from the group consisting of polyamide, polyester, polyurethane, polyolefin, ethylene vinyl acetate (EVA), silicone, acrylic, and butadiene.

[0084] The PSA film may be formed from a material including, for example, a silicone-based or acrylic-based material for pressure-sensitive adhesives (PSA). In the present invention, the third layer (130; 130', 130") may be a co-polyester-based hot melt web, such as a PES hot melt web.

[0085] Hot melt webs include, for example, JCC’s PA-2080, PA2120, PA6106, PA 6300, PES 3110, PES 3111, PES3115D, PES 3140, PES 3160, PES W90, PES W125, OES 165, PES-125FR, PA W106, PA W120, TPU W50, PA W106, PA W120, TPU W50, TPU W105, EVA W80; Tomis’ T6308W, Y4019W, H2001W; KETAEBO’s PA, PES, EVA, TPU webs; WithTech’s PA, Copolyanide, polyamide webs; or protechnic’s webs.

[0086] The following describes how to attach the first layer (110), the second layer (120), and the third layer (130).

[0087] As an example, a release film is attached to one side of the third layer (130), and then the opposite side is laminated onto the surface of the first layer (110) and laminated to attach the third layer (130) to the first layer (110). Afterward, the release film attached to the third layer (130) is removed, and the second layer (120) is laminated onto it and laminated to attach the second layer (120) to the third layer (130).

[0088] As another example, the first layer (110) is laminated on one side of the third layer (130) and the second layer (120) is laminated on the other side of the third layer (130), so that the first layer (110), the third layer (130), and the second layer (120) are laminated simultaneously to attach these layers.

[0089] In one embodiment, the fourth layer (140) is formed of a material including silicon.

[0090] The fourth layer (140) improves the appearance characteristics of the battery thermal runaway prevention sheet, improves the water resistance and chemical resistance of the first layer (110) and the second layer (120; 120', 120"), and serves to block dust.

[0091] A method for stacking the first layer (110), the second layer (120; 120', 120"), the third layer (130; 130', 130"), and the fourth layer (140) is described below in a schematic manner. The method of stacking these layers is one example and is not limited thereto.

[0092] As an example, a release film is attached to one side of the third layer (130), and then the opposite side is laminated onto the surface of the first layer (110) and laminated to attach the third layer (130) to the first layer (110). Afterward, the release film attached to the third layer (130) is removed, and the second layer (120) is laminated onto it and then laminated to attach the second layer (120) to the third layer (130). After cutting the sheet in which the first layer (110), the third layer (130), and the second layer (120) are sequentially laminated into an appropriate size, a coating liquid containing silicone is applied to the left and right cut surfaces or the top and bottom surfaces to form the fourth layer (140).

[0093] As another example, a first layer (110) is laminated on one side of the third layer (130) and a second layer (120) is laminated on the other side of the third layer (130), and then the first layer (110), the third layer (130), and the second layer (120) are laminated simultaneously to attach these layers. After cutting the sheet in which the first layer (110), the third layer (130), and the second layer (120) are sequentially laminated into an appropriate size, a coating liquid containing silicone is applied to the left and right cut surfaces or the top and bottom surfaces to form a fourth layer (140).

[0094] As another example, to improve the finish, a flame-retardant coating layer containing organic material may be applied to the left and right cut surfaces of a sheet in which the first layer (110), the third layer (130), and the second layer (120) are sequentially laminated, and then a coating liquid containing silicone may be applied to form a fourth layer. The flame-retardant coating layer included in the fourth layer (140) may be the same as or different from the flame-retardant coating layer of the second layer (120), and the viscosity may be 1,000 to 7,000 cPs.

[0095] The battery thermal runaway prevention sheet according to the present invention has impact resistance such that it is not penetrated when a 1 kg, 1 inch steel ball is dropped from a height of less than 10 to 20 cm.

[0096] The battery thermal runaway prevention sheet according to the present invention has folding characteristics that do not result in appearance defects, cracks, or debris after being folded 180 degrees.

[0097] The battery thermal runaway prevention sheet according to the present invention has flame-retardant properties that prevent fire from occurring during thermal insulation testing.

[0098] The battery thermal runaway prevention sheet according to the present invention has appearance characteristics free from appearance defects such as color mismatch, leveling, stains, and crumbs.

[0099] The battery thermal runaway prevention sheet according to the present invention has a thermal conductivity of 0.040 W / mK or less at room temperature.

[0100] The battery thermal runaway prevention sheet according to the present invention has a compression force deflection (CFD) of 0 to 15 percentage points at a pressure of 1.0 to 2.0 MPa, where the compression force deflection (CFD) is calculated by the following mathematical formula 1.

[0101] [Mathematical Formula 1]

[0102] | High Temperature (600℃ or higher) Compression Ratio - Room Temperature (25℃) Compression Ratio |

[0103] Here, the battery thermal runaway prevention sheet (100) of the present invention has a room temperature compression ratio of 40 to 75% at 25°C and a high temperature compression ratio of 40 to 85% at 600°C or higher (e.g., 600 to 1,200°C, or 600 to 800°C).

[0104] Accordingly, the battery thermal runaway prevention sheet (100) of the present invention, as shown in FIG. 5, has a small compressive strain (CFD) value, so it maintains its shape or thickness at room temperature even when exposed to high temperatures of 600°C or higher and high pressures of 1.0 MPa or higher, and is effective for thermal retardation.

[0105] Figure 5 is a graph of stress versus strain (percentage (%)) representing the compression curve.

[0106] In the present invention, the compression ratio of the battery thermal runaway prevention sheet (100) is measured according to the ISO3386 standard and calculated by [Equation 2] below.

[0107] [Mathematical Formula 2]

[0108]

[0109] The battery thermal runaway prevention sheet according to the present invention has an dielectric breakdown voltage of 2.0 KV / mm or higher. The battery thermal runaway prevention sheet according to the present invention has water repellency (water resistance) such that after being placed in a constant temperature and humidity chamber at 50°C and 95% humidity for 24 hours, the moisture content is within 5%.

[0110] In another aspect, the present invention provides a battery cell assembly to which a battery thermal runaway prevention sheet according to the present invention is applied.

[0111] Specifically, the battery cell assembly of the present invention comprises a plurality of battery cells, each wrapped by a battery thermal runaway prevention sheet according to the present invention. Due to this configuration, the battery cell assembly of the present invention can prevent chain ignition to all of the plurality of battery cells when a flame occurs in at least one battery cell.

[0112] [Example]

[0113] 1. Preparation of Floors 1 through 4

[0114] 1.1 1st Floor

[0115] Commercially available OPF (oxidized polyacrylonitrile fiber, purchased from TFJ) was used as the fiber reinforcement core.

[0116] An impregnation solution was prepared using the ingredients listed in Table 1. Specifically, the ingredients listed in Table 1 were placed in a reaction vessel and mixed to prepare the impregnation solution.

[0117]

[0118] - MTMS: Methyltrimethoxysilane

[0119] The fiber-reinforced core material was cut into pieces measuring 300 mm (width) x 300 mm (length) x 4 mm (height), immersed in a bath containing an impregnation solution for 5 seconds, and then cured by drying in a 150°C oven for 60 minutes.

[0120] 1.2 Second floor

[0121] Non-combustible film layer: An inorganic fiber (glass fiber) with a thickness of 100 μm was impregnated for about 1 minute in a solution mixed with 300 g of silicone resin, 700 g of xylene, and 1 g of carbon black, pressed, and then dried for use.

[0122] Flame retardant coating layer: A flame retardant coating solution was prepared by mixing 300g of EVA (Ethylene Vinyl Acetate), 300g of calcium carbonate, 200g of ammonium phosphate (APP), and 200g of ultrapure water for dilution, and stirring for about 1 hour (viscosity: 15,000 cPs).

[0123] 1.3 Third floor

[0124] 3rd layer: Hot melt web (PA W106) purchased from JCC, 20g / m² 2 used.

[0125] 1.4 4th Floor

[0126] ① Flame-retardant coating

[0127] 300g of EVA (Ethylene Vinyl Acetate), 300g of calcium carbonate, 200g of ammonium phosphate (APP), and 500g of ultrapure water for dilution were mixed and stirred for about 1 hour. The mixture was then applied using a 50-100㎛ applicator, dried, and used. (Viscosity: 3,000 cPs)

[0128] ② 500 g of silicone-coated methylphenylsilicone resin (P80X, Evonik), 300 g of MEK, and 200 g of toluene were mixed and used.

[0129] 2. Manufacturing of sheets for preventing battery thermal runaway

[0130] 2.1 Examples 1 to 10

[0131] Battery thermal runaway prevention sheets of Examples 1 to 10 were manufactured using the prepared first to fourth layers as shown in Table 2.

[0132] Example 1: A non-combustible film layer (second layer) of 100 μm was placed on the first layer and then laminated to produce a battery thermal runaway prevention sheet with a thickness of 3.4 T (mm).

[0133] Example 2: A flame-retardant coating solution was applied to the first layer to a thickness of 70 μm and dried to form a flame-retardant coating layer (second layer), and then a battery thermal runaway prevention sheet with a thickness of 3.4 T was manufactured.

[0134] Example 3: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 1, except that after forming a non-combustible film layer in Example 1, a flame-retardant coating layer was formed on the non-combustible film layer.

[0135] Example 4: A third layer with the release liner removed was placed on the first layer, and a second layer (non-combustible film layer) was placed on the third layer and then heat-laminated to manufacture a battery thermal runaway prevention sheet with a thickness of 3.4T.

[0136] Example 5: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 4, except that a flame-retardant coating layer with a thickness of 70 μm was coated and dried instead of the second layer (non-combustible film layer) in Example 4.

[0137] Example 6: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 4, except that a flame-retardant coating layer was formed on the non-combustible film layer after forming the non-combustible film layer in Example 4.

[0138] Example 7: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 4, except that a fourth layer with a thickness of 10 μm was formed on the side of the battery thermal runaway prevention sheet manufactured in Example 4 by spraying.

[0139] Example 8: A battery thermal runaway prevention sheet was manufactured in the same manner as in Example 5, except that a fourth layer was formed on the side of the battery thermal runaway prevention sheet manufactured in Example 5 by spraying to a thickness of 10 μm.

[0140] Example 9: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 6, except that a fourth layer with a thickness of 10 μm was formed on the side of the battery thermal runaway prevention sheet manufactured in Example 6 by spraying.

[0141] Example 10: A battery thermal runaway prevention sheet with a thickness of 3.4T was manufactured in the same manner as in Example 1, except that layer 1) of 1.4 with a thickness of 10 μm and layer 2) of 1.4 with a thickness of 10 μm were sequentially coated on the front and sides of the sheet formed in Example 1.

[0142] 2.2 Comparative Example 1

[0143] For Comparative Example 1, a battery thermal runaway prevention sheet manufactured with only the first layer was used.

[0144]

[0145] [Performance Evaluation]

[0146] The performance of the battery thermal runaway prevention sheet manufactured in the experimental example was evaluated as follows.

[0147] (1) △CFD (Compressive strain)

[0148] The compression ratio of the manufactured battery thermal runaway prevention sheet was measured according to Equation 1. The evaluation criterion was calculated as the difference (% points) between the room temperature compression ratio and the high temperature compression ratio of 600°C or higher under 1.5 MPa conditions. A smaller difference was evaluated as superior.

[0149] (2) Dust

[0150] When using Ichiban CT 405 tape, it was evaluated as excellent (○) if it could be reattached after 5 removals, average (△) if it could be reattached after 3 removals, and poor (×) if it was difficult to reattach even after 1 removal.

[0151] (3) Appearance

[0152] If there are no pinholes or lifting in the 50mm x 50mm space, it is evaluated as excellent (○), if there is one, it is average (△), and if there are two or more, it is poor (×).

[0153] (4) Integration (adhesion)

[0154] The manufactured battery thermal runaway prevention sheet was folded so that the opposite sides touched with the center as the center, and the presence or absence of delamination or lifting was checked at the folded area.

[0155] It was evaluated as Excellent (○) if there was no lifting on the opposite side, Average (△) if a fold mark remained, and Poor (×) if lifting, i.e., peeling, occurred after folding.

[0156] (5) Non-combustible

[0157] The manufactured battery thermal runaway prevention sheet was exposed to a flame at a distance of 15 cm to observe flame transition. It was evaluated as excellent (○) if the flame was extinguished within 6 seconds, average (△) if it was extinguished within 10 seconds, and poor (×) if the flame persisted for more than 10 seconds.

[0158] (6) Impact resistance

[0159] The impact resistance height of the test specimen is measured by dropping a weight (1 kg) from a height to be measured onto a manufactured battery thermal runaway prevention sheet. If the sheet is not penetrated at 20 cm or more, it is evaluated as excellent (○); if it is not penetrated at 10 cm or more but less than 20 cm, it is evaluated as average (△); and if it is penetrated at less than 10 cm, it is evaluated as poor (×).

[0160] (7) Bending properties

[0161] The manufactured battery thermal runaway prevention sheet was folded so that the opposite sides touched the center, and the presence of cracks and external defects in the folded area was checked. It was evaluated as Excellent (○) if no creases remained, Average (△) if creases remained, and Poor (×) if there were any cracked areas.

[0162] (8) Water resistance

[0163] A battery thermal runaway prevention sheet measuring 15 cm x 15 cm was prepared and placed in an oven at approximately 110°C for about 2 hours. Afterward, the specimens were placed in a 50°C, 95% humidity chamber for 96 hours. Subsequently, each specimen was packaged in a polyethylene bag (PE bag). When the specimen temperature returned to room temperature, the weight was measured, and the weight of the polyethylene bag was subtracted to calculate the weight gain of the specimen. It was evaluated as excellent (○) if within 5%, average (△) if between 6% and 8%, and poor (×) if 8% or more.

[0164] The evaluation results are presented in the table below.

[0165]

[0166] Compared to the comparative example, Examples 1-10 showed superior evaluation results in dust evaluation, appearance evaluation, impact resistance evaluation, etc. compared to Comparative Example 1.

[0167] Various embodiments of the present invention are described below. The following embodiments may be combined with one another unless an obvious technical conflict arises.

[0168] Example 1. A battery thermal runaway prevention sheet comprising: a first layer (110); and a second layer (120; 120', 120") laminated on at least one of the upper and lower portions of the first layer (110); wherein the first layer (110) comprises a fiber reinforcing core and a porous additive, formed by impregnating the fiber reinforcing core in an impregnation solution containing the porous additive, and the second layer (120) comprises at least one of a non-combustible film layer and a flame-retardant coating layer.

[0169] Example 2. A battery thermal runaway prevention sheet according to Example 1, further comprising a third layer (130; 130', 130") disposed between the first layer (110) and the second layer (120), wherein the third layer (130) is an adhesive layer that bonds the first layer (110) and the second layer (120).

[0170] Example 3. A battery thermal runaway prevention sheet according to Example 1, further comprising a fourth layer (140) laminated to cover at least one of the sides of the first layer (110) and at least one of the sides, top surface, and bottom surface of the second layer (120; 120', 120").

[0171] Example 4. A battery thermal runaway prevention sheet according to Example 2, further comprising a fourth layer (140) laminated to cover at least one of the sides of the first layer (110), at least one of the sides, top surface, and bottom surface of the second layer (120; 120', 120"), and at least one of the sides of the third layer (130; 130', 130").

[0172] Example 5. A sheet for preventing battery thermal runaway, wherein the porous additive in Example 1 comprises one or more selected from hollow microglass spheres, silica, cenospheres, and aerogel particles.

[0173] Example 6. The non-combustible film layer of Example 1 comprises an organic film layer, an inorganic film layer, or an organic-inorganic mixed film layer; the organic film layer comprises one or more selected from aramid film, polycarbonate film, polyimide film, polyethylene terephthalate film, cycloolefin polymer film, unoriented polypropylene film, and nylon film; the inorganic film layer comprises one or more selected from inorganic fiber film, MICA film, ceramic film, and asbestos film; and the organic-inorganic mixed film layer is manufactured by impregnating or coating the inorganic film layer with a flame-retardant or non-combustible organic resin, thereby forming a sheet for preventing thermal runaway in a battery.

[0174] Example 7. A sheet for preventing battery thermal runaway, wherein the flame-retardant coating layer of Example 1 comprises at least one of silicone, silicate, and a flame retardant.

[0175] Example 8. A battery thermal runaway prevention sheet in Example 2, wherein the third layer (130; 130', 130") is an adhesive layer comprising at least one of a hot melt web and a PSA film.

[0176] Example 9. In Example 3 or Example 4, the fourth layer (140) is formed of a material including silicon, a battery thermal runaway prevention sheet.

[0177] Example 10. In any one of Examples 1 to 9, the battery thermal runaway prevention sheet has a Compression Force Deflection (CFD) of 0 to 15 percentage points at a pressure of 1.0 to 2.0 MPa, wherein the Compression Force Deflection (CFD) is calculated by the following Equation 1:

[0178] [Mathematical Formula 1]

[0179] | High Temperature (600℃ or higher) Compression Ratio - Room Temperature (25℃) Compression Ratio |

[0180] Example 11. A battery cell assembly comprising a plurality of battery cells, each wrapped by a battery thermal runaway prevention sheet according to any one of Examples 1 to 10, characterized in that it prevents chain ignition to all of the plurality of battery cells when a flame occurs in at least one battery cell.

Claims

1. First layer (110); and A second layer (120; 120', 120") stacked on at least one of the upper and lower parts of the first layer (110); Includes, The first layer (110) comprises a fiber reinforcing core and a porous additive, and is formed by impregnating the fiber reinforcing core in an impregnation solution containing the porous additive. The second layer (120) is a battery thermal runaway prevention sheet comprising at least one of a non-combustible film layer and a flame-retardant coating layer.

2. In Claim 1, It further includes a third layer (130; 130', 130") disposed between the first layer (110) and the second layer (120), The third layer (130) is an adhesive layer that bonds the first layer (110) and the second layer (120), a battery thermal runaway prevention sheet.

3. In Claim 1, A battery thermal runaway prevention sheet further comprising a fourth layer (140) laminated to cover at least one of the sides of a first layer (110) and at least one of the sides, top surface, and bottom surface of a second layer (120; 120', 120").

4. In Claim 2, A battery thermal runaway prevention sheet further comprising a fourth layer (140) laminated to cover at least one of the sides of a first layer (110), at least one of the sides, top surface, and bottom surface of a second layer (120; 120', 120"), and at least one of the sides of a third layer (130; 130', 130").

5. In Claim 1, A sheet for preventing battery thermal runaway, comprising one or more porous additives selected from hollow microglass spheres, silica, cenospheres, and aerogel particles.

6. In Claim 1, The non-combustible film layer includes an organic film layer, an inorganic film layer, or an organic-inorganic mixed film layer, and The organic film layer comprises one or more selected from aramid film, polycarbonate film, polyimide film, polyethylene terephthalate film, cycloolefin polymer film, unoriented polypropylene film, and nylon film, and The inorganic film layer comprises one or more types selected from inorganic fiber films, MICA films, ceramic films, and asbestos films, and A battery thermal runaway prevention sheet, wherein the organic-inorganic mixed film layer is manufactured by impregnating or coating an inorganic film layer with a flame-retardant or non-flammable organic resin.

7. In Claim 1, A sheet for preventing thermal runaway in a battery, wherein the flame-retardant coating layer comprises at least one of silicone, silicate, and a flame retardant.

8. In Claim 2, A battery thermal runaway prevention sheet, wherein the third layer (130; 130', 130") is an adhesive layer comprising at least one of a hot melt web and a PSA film.

9. In claim 3 or claim 4, The fourth layer (140) is a battery thermal runaway prevention sheet formed from a material including silicon.

10. In any one of claims 1 to 8, The battery thermal runaway prevention sheet has a Compression Force Deflection (CFD) of 0 to 15 percentage points at a pressure of 1.0 to 2.0 MPa, and Here, the compressive strain (CFD) is a battery thermal runaway prevention sheet calculated by the following Equation 1: [Mathematical Formula 1] | High Temperature (600℃ or higher) Compression Ratio - Room Temperature (25℃) Compression Ratio | 11. A plurality of battery cells, each wrapped by a battery thermal runaway prevention sheet according to any one of claims 1 to 8, comprising A battery cell assembly characterized by preventing chain ignition to multiple battery cells when a flame occurs in at least one battery cell.