Organic polymer binder for metallurgic and steel manufacturing of cold bonded briquettes
A composite binder of PVA, acrylates copolymer, and sub-bituminous coal extract enhances briquette strength and thermal stability, addressing contamination and environmental issues in steel manufacturing by-products.
Patent Information
- Application Number
- PCT/US2025/028612
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional briquetting methods for steel manufacturing by-products rely on binders that contaminate slag and reduce furnace efficiency, and landfill disposal exacerbates environmental pollution.
A composite binder comprising polyvinyl alcohol (PVA), acrylates copolymer, and sub-bituminous coal extract, optionally with additives like sulfonated lignin and phenolic resin, to enhance adhesion, strength, and thermal stability in cold-pressed metal briquettes.
The binder system improves mechanical strength, thermal stability, and process efficiency, reducing slag formation and environmental impact while maintaining briquette integrity under high-temperature conditions.
Smart Images

Figure US2025028612_12112026_PF_FP_ABST
Abstract
Description
[0001] #2380375 086034-000002
[0002] 1
[0003] ORGANIC POLYMER BINDER FOR METALLURGIC AND STEEL MANUFACTURING OF COLD BONDED BRIQUETTES
[0004] Background
[0005] Due to its exceptional mechanical strength, versatility, and cost-effectiveness, iron alloys— including steel, stainless steel, cast iron, and specialty steels— are the foundation of modern industrial metal applications. The iron and steel industry plays a vital economic role, with steel alone accounting for approximately 93% of the world's annual metal production.
[0006] Approximately 57% of raw steel is produced using blast furnaces, while 43% comes from electric arc furnaces (EAF), which rely on scrap metal recycling. Regardless of the production route, steel manufacturing generates by-products, including slag, dust, fines, and / or sludge. Traditionally, these waste materials are either placed in a landfill or converted into metal briquettes. However, conventional briquetting methods often rely on binders that hinder the reintegration of these briquettes Into steel production. Additionally, landfill disposal exacerbates environmental pollution and presents long-term sustainability challenges.
[0007] To address these issues, there is a need for an advanced binder formulation and briquetting process that eliminates impurities and reduces reliance on problematic binders such as bentonite clay, calcium carbonate (lime), sodium silicate, cement, and molasses. These materials contribute to slag contamination, furnace inefficiencies, and lower-quality briquettes.#2380375 086034-000002
[0008] Summary
[0009] The present disclosure relates to a novel binder formulation for cold-pressed metal briquettes and related methods. Specifically, it pertains to a composite binder that may comprise a polyvinyl alcohol (PVA), an acrylates copolymer, and / or liquid sub-bituminous coal extract, which provides superior adhesion and strength for metallurgical applications. In some embodiments, additional optional components such as sulfonated lignin, phenolic resin, polyacrylamide (PAM), microbiocidal, and / or cellulosic material may be included to enhance specific properties depending on the end-user requirements.
[0010] In one embodiment, a briquette and methods for producing the same are disclosed.
[0011] The present disclosure provides a binder composition comprising polyvinyl alcohol (PVA), liquid or dry acrylates copolymer, and / or liquid sub-bituminous coal extract. Without limiting the invention, a blend of high and low molecular weight PVA is used in preferred embodiments to optimize mechanical strength, binding efficiency, and flexibility in briquettes. A liquid acrylates copolymer (which may be provided in a 40% to 50% by weight solids formulation) at the rate of 0.1%-10% by weight, may enhance particle cohesion and when combined with the PVA may strengthen the binding matrix, enhance downstream metallurgical performance by reducing undesirable deleterious residues and / or promote efficient burn off. The liquid sub-bituminous coal extract (which may be provided at a 0.5%- 15% solids by weight formulation), at a rate of 0.15%–5% by weight of the binder, reacts at high temperatures (for example, from about 65 to about 98 degrees Celsius – about 150°F to about 208°F) with PVA. It may function as both a plasticizer and a binding enhancer, improving adhesion, reducing brittleness, and / or preventing cracking. Its presence may increase the flexibility of the binder system, enhance thermal resistance, and / or contribute to the overall structural integrity of the briquettes under high-temperature conditions.
[0012] In some embodiments, additional optional components such as sulfonated lignin, phenolic resin polyacrylamide (PAM), microbiocidal, engineered cellulosic particulates and / or a#2380375 086034-000002
[0013] 3
[0014] defoamer may be included to enhance specific properties depending on the end-use requirements.
[0015] Formulations disclosed herein may provide a high-performance and adaptable binder system, ensuring optimal mechanical strength (crush strength), thermal stability, and / or process efficiency in cold-pressed metal briquettes. The combination of PVA, acrylates copolymer, and liquid sub-bituminous coal extract may enhance durability, minimize cracking, and / or improve briquette integrity under demanding conditions. Additionally, this binder system is designed for compatibility with various metal fines, offering a versatile solution for different metallurgical applications. Embodiments disclosed herein may also contribute to reduced waste, improved resource efficiency, and / or potential cost savings in production, making it a reliable and sustainable choice for industrial use.
[0016] In some embodiments, the briquette exhibits a Cold Crush Strength (CCS) of approximately 100 psi to about 400 psi. Additionally, when cured, the briquette may have a crush strength in the range of about 600 psi. to about 2,000 psi. While some implementations require an eight-hour to forty-eight cure time.
[0017] In certain embodiments sulfonated lignin (0.5%~10% of the total binder) may be added and it may function as a natural dispersant and lubricant, reducing roll friction during the briquetting process and / or improving material flow. Additionally, it may enhance cohesion, increase water resistance, and / or contribute to thermal stability, helping briquettes maintain their integrity under high temperature.
[0018] As a natural polymer, sulfonated lignin may reduce internal friction between metal fines and binder components, thereby lowering the energy required for pressing. This lubricating effect may enhance the uniformity of the mixture, ensuring a more consistent distribution of binder and improved compaction efficiency. The reduced friction may also minimizes wear on processing equipment, contributing to increased operational lifespan and lower maintenance costs. Furthermore, by enhancing the workability of the mixture, sulfonated lignin may also help prevent premature cracking and ensures a denser, more durable#2380375 086034-000002
[0019] 4
[0020] briquette. This effect is particularly beneficial in cold-pressed metal briquetting, where achieving high compressive strength without excessive brittleness is crucial for handling and transport.
[0021] In certain embodiments, a pre-gelatinized starch may be included to enhance green strength, binder cohesion, and / or process stability, making it particularly effective in cold- pressed briquettes where thermal curing is not employed. At an optimized range of 0.05%~ 0.45% of the total binder, pre-gelatinized starch may significantly improve inter-particle adhesion and compaction efficiency without compromising the density or structural integrity of the briquettes. Without being bound by theory, upon hydration, pre-gelatinized starch may rapidly form a viscous gel matrix that binds particles together, increasing the briquette's resistance to breakage and abrasion during handling, transportation, and storage. Additionally, it may improve binder viscosity, preventing migration or segregation during mixing and pressing, thereby ensuring uniform binder distribution and consistent briquette quality.
[0022] A non-limiting example of a suitable pre-gelatinized starch that may be used in embodiments of the present disclosure includes starch derived from corn, potato, tapioca, wheat, rice, waxy maize, and / or high-amylose sources. This composition may be provided as an illustrative example and should not be interpreted as restrictive, as other pre-gelatinized starches with similar properties may also be viable, it also can be tailored for solubility, particle size, and gel strength to meet specific process requirements. Such a formulation may ensure compatibility with PVA and other binder components, creating a cohesive system that supports efficient cold pressing while offering a renewable, biodegradable, and cost-effective alternative to synthetic binders.
[0023] in certain embodiments, a phenolic resin may be included to enhance thermal stability and structural integrity when used in metal recycling where briquettes are subjected to high- temperature stress. At an optimized range of 0.05%-0.45% of the total binder, phenolic resin may significantly improve heat resistance and oxidation stability without making the briquettes excessively rigid or brittle. Without being bound by theory, during combustion.#2380375 086034-000002
[0024] 5
[0025] phenolic resin undergoes thermosetting polymerization, forming a carbonaceous matrix that reinforces the briquette's structure, minimizing deformation and fragmentation under extreme heat. Additionally, its use may reduce volatile organic compound (VOC) emissions and / or prevents excessive mass loss, ensuring that the briquette maintains density and mechanical strength throughout the process. To further enhance its performance in certain embodiments, phenolic resin may be modified with alkaline or acidic catalysts to optimize curing time, adhesion properties, and / or mechanical resilience. Such a formulation may ensure compatibility with PVA and the other components, creating a binder system that withstands high temperatures while minimizing slag formation and / or unwanted furnace deposits.
[0026] In further embodiments, where polyacrylamide (PAM) may be used, it may be included in the range of 0.05%-0.45% and without being bound by theory may act as a binder and / or moisture stabilizer, improving the green strength of briquettes, enhancing flexibility, and / or preventing premature cracking. In certain embodiments, the binder further may comprise Engineered Cellulosic Particulates in an amount ranging from about 0.025% to 0.05%, which, without being bound by theory, may provide fiber reinforcement, reducing microcracks and / or improve tenacity or flexibility under mechanical stress. Additionally, these ingredients may enhance moisture retention, optimize binder distribution, and / or contribute to thermal stability. A further advantage includes the controlled porosity introduced by the particulates, which, without being bound by theory, may improve gas permeability during high-temperature processing, facilitating more efficient combustion or metallurgical reactions.
[0027] A controlled viscosity range (for example, a PVA having a viscosity between about 1400 to about 3000 cps at room temperature, between about 1400 to about 2000 cps at room temperature, and / or between about 2000-about 3000 cps at room temperature) may help to ensure the right balance between binding efficiency and processability, preventing excessive brittleness and / or weakness in briquettes. In certain embodiments, binder formulation may utilize a unique blend of high and low molecular weight polyvinyl alcohols (PVA). Without being bound by theory, high molecular weight PVA may enhance mechanical#2380375 086034-000002
[0028] 6
[0029] strength, cohesion, and / or durability. While, without being bound by theory, low molecular weight PVA may improve solubility, penetration, and / or overall binder distribution within the briquette matrix. This combination of PVA may be used to optimize adhesion, flexibility, and / or water retention, ensuring superior performance under mechanical stress and thermal exposure.
[0030] In some embodiments, PVA may be further modified to improve its solubility and / or reaction kinetics, enabling a more efficient binding process that results in higher compressive strength. Additionally, the liquid sub-bituminous coal extract may be treated with sodium hydroxide to enhance its solubility and reactivity with PVA, contributing to thermal stability, adhesion properties, and / or oxidation resistance, thereby preventing premature degradation in high-temperature environments.
[0031] In some embodiments, the binder mixture further includes a microbicidal agent in an amount of about 0.1% to about 5.0% of the binder mixture. Additionally, it may further include a defoamer or anti-foam agent, such as glycols and polyols, in an amount of about 0.001% to about 0.1% of the total binder. Examples of suitable defoamers include propylene glycol (PG), butylene glycol (BG), ethylene oxide-propylene oxide (EO / PO) block copolymers, and 2-ethylhexanol, which provide effective foam control while maintaining good compatibility with polyvinyl alcohol (PVA) and fully evaporating at elevated temperatures, thereby minimizing residual contamination in the final product.
[0032] The invention offers improved thermal stability by combining PVA, liquid acrylates copolymer, liquid sub-bituminous coal extract, phenolic resin and / or sulfonated lignin, preventing thermal degradation. Without being bound by theory, the superior binding strength provided by the PVA blend and liquid acrylates copolymer ensures high compressive strength. Increased green strength may be achieved through the inclusion of Engineered Cellulosic Particulates and / or PAM, which provide structural integrity before the curing phase. Such formulations may also serve as an eco-friendly alternative, reducing reliance on petroleum-based resins while maintaining high-performance characteristics.#2380375 086034-000002
[0033] These and other advantages and features of the invention are set forth in the claims annexed hereto and form an integral part of this disclosure. However, for a better understanding of the invention and the advantages and objectives achieved by its use, reference should be made to the drawings and the accompanying descriptive material, which illustrate example embodiments of the invention. This summary is provided solely to introduce a selection of concepts further described below In the detailed description and is not intended to identify key or essential features of the claimed subject matter, nor to limit its scope.
[0034] Numerous variations and modifications will be apparent to those skilled in the art from the following description. Accordingly, the invention is not limited to the specific embodiments disclosed herein.23803 / 5 086034-000002
[0035] 8
[0036] Brief Description of Figures
[0037] Figure 1 illustrates an operational flowchart for producing an Organic Polymer Binder, which includes PVA, sub-bituminous coal extract, and acrylates copolymer, as implemented in the core of the invention.
[0038] Figure 2 illustrates an operational flowchart for producing a briquette in accordance with some embodiments of the invention.
[0039] Figure 3 is a digital image of a briquette produced by the method described herein including additives such as sulfonated lignin, phenolic resin, polyacrylamide, microbicidal agent and cellulosic material.#2380375 086034-000002
[0040] 9
[0041] Detailed Description of the Invention
[0042] For the purposes of promoting an understanding of the principles of the invention, reference will now be made to certain embodiments and specific language will be used to describe the same. It will nevertheless be understood that no limitation of the scope of the invention is thereby intended, such alterations and further modifications, and such further applications of the principles of the invention as described herein being contemplated as would normally occur to one skilled in the art to which the invention relates. Additionally, in the detailed description below, numerous alternatives are given for various features. It will be understood that each such disclosed alternative, or combinations of such alternatives, can be combined with the more generalized features discussed in the Summary above, or set forth in the embodiments described below to provide additional disclosed embodiments herein.
[0043] Maintaining the mineral chemistry of steel waste without altering its composition an important consideration for producing high-quality briquettes suitable for reuse. Moreover, improving alloy and iron content recoveries while minimizing impurities in steel waste processing is a key objective of the present disclosure, which helps to ensure a more efficient, cost-effective, and sustainable approach to steel waste stream recycling,
[0044] An organic polymer binder is disclosed for producing briquettes from ferrous and / or ferro¬ alloy steel by-products and waste streams generated during metal manufacturing. These by¬ products include, but are not limited to, fines, dust, baghouse dust, sludge, spent shot, laser dust, mill scale, titanium fines, ferro silica, ferro molybdenum, nickel, and / or chrome.
[0045] Binders may be formulated to yield briquettes with a final binder content ranging from about 1.75% to less than about 10%. In contrast, conventional briquetting processes typically produce briquettes with binder contents of approximately 10% to 20%, with conventional binders usually comprising materials such as molasses, cement, lime, sodium bentonite clay, and / or other deleterious substances that contribute to increased slag generation during steel production.#2380375 086034-000002
[0046] 10
[0047] Organic polymer binders described herein offer the potential to improve the mineral chemistry and provide a higher value return to the steelmaking process by eliminating the additional slag and undesirable substances commonly associated with conventional binder formulations. Typically, these harmful materials accumulate in the slag layer during steelmaking, whereas the upper layer is referred to as the "slag" portion and the lower layer—often containing pure iron~~is referred to as the "tap" layer.
[0048] The present disclosure provides a binder composition comprising polyvinyl alcohol (PVA), liquid or dry acrylates copolymer, and / or liquid sub-bituminous coal extract. Without limiting the invention, a blend of high and low molecular weight PVA is used in preferred embodiments to optimize mechanical strength, binding efficiency, and flexibility in briquettes. A liquid acrylates copolymer (which may be provided in a 40% to 50% by weight solids formulation) at the rate of 0.1%-10% by weight, may enhance particle cohesion and when combined with the PVA may strengthen the binding matrix, enhance downstream metallurgical performance by reducing undesirable deleterious residues and / or promote efficient burn off. The liquid sub-bituminous coal extract (which may be provided at a 0.5%-15% solids by weight formulation), at a rate of 0.15%-5% by weight of the binder, reacts at high temperatures (for example, from about 65 to about 98 degrees Celsius - about 150°F to about 208°F) with PVA. It may function as both a plasticizer and a binding enhancer, improving adhesion, reducing brittleness, and / or preventing cracking. Its presence may increase the flexibility of the binder system, enhance thermal resistance, and / or contribute to the overall structural integrity of the briquettes under high-temperature conditions.
[0049] In some embodiments, additional optional components such as sulfonated lignin, phenolic resin polyacrylamide (PAM), microbiocidal, engineered cellulosic particulates and / or a defoamer may be included to enhance specific properties depending on the end-use requirements.
[0050] Formulations disclosed herein may provide a high-performance and adaptable binder system, ensuring optimal mechanical strength (crush strength), thermal stability, and / or process efficiency in cold-pressed metal briquettes. The combination of PVA, acrylates#2380375 086034-000002
[0051] 11
[0052] copolymer, and liquid sub-bituminous coal extract may enhance durability, minimize cracking, and / or improve briquette integrity under demanding conditions. Additionally, this binder system is designed for compatibility with various metal fines, offering a versatile solution for different metallurgical applications. Embodiments disclosed herein may also contribute to reduced waste, improved resource efficiency, and / or potential cost savings in production, making it a reliable and sustainable choice for industrial use.
[0053] In some embodiments, the briquette exhibits a Cold Crush Strength (CCS) of approximately 100 psi to about 400 psi. Additionally, when cured, the briquette may have a crush strength in the range of about 600 psi. to about 2,000 psi. While some implementations require an eight-hour to forty-eight cure time.
[0054] In certain embodiments sulfonated lignin (0.5%–10% of the total binder) may be added and it may function as a natural dispersant and lubricant, reducing roll friction during the briquetting process and / or improving material flow. Additionally, it may enhance cohesion, increase water resistance, and / or contribute to thermal stability, helping briquettes maintain their integrity under high temperature.
[0055] As a natural polymer, sulfonated lignin may reduce internal friction between metal fines and binder components, thereby lowering the energy required for pressing. This lubricating effect may enhance the uniformity of the mixture, ensuring a more consistent distribution of binder and improved compaction efficiency. The reduced friction may also minimizes wear on processing equipment, contributing to increased operational lifespan and lower- maintenance costs. Furthermore, by enhancing the workability of the mixture, sulfonated lignin may also help prevent premature cracking and ensures a denser, more durable briquette. This effect is particularly beneficial in cold-pressed metal briquetting, where achieving high compressive strength without excessive brittleness is crucial for handling and transport.
[0056] In certain embodiments, a pre-gelatinized starch may be included to enhance green strength, binder cohesion, and / or process stability, making it particularly effective in cold-#2380375 086034-000002
[0057] 12
[0058] pressed briquettes where thermal curing is not employed. At an optimized range of 0.05%- 0.45% of the total binder, pre-gelatinized starch may significantly improve inter-particle adhesion and compaction efficiency without compromising the density or structural integrity of the briquettes. Without being bound by theory, upon hydration, pre-gelatinized starch may rapidly form a viscous gel matrix that binds particles together, increasing the briquette's resistance to breakage and abrasion during handling, transportation, and storage. Additionally, it may improve binder viscosity, preventing migration or segregation during mixing and pressing, thereby ensuring uniform binder distribution and consistent briquette quality.
[0059] A non-limiting example of a suitable pre-gelatinized starch that may be used in embodiments of the present disclosure includes starch derived from corn, potato, tapioca, wheat, rice, waxy maize, and / or high-amylose sources. This composition may be provided as an illustrative example and should not be interpreted as restrictive, as other pre-gelatinized starches with similar properties may also be viable, it also can be tailored for solubility, particle size, and gel strength to meet specific process requirements. Such a formulation may ensure compatibility with PVA and other binder components, creating a cohesive system that supports efficient cold pressing while offering a renewable, biodegradable, and cost-effective alternative to synthetic binders.
[0060] In certain embodiments, a phenolic resin may be included to enhance thermal stability and structural integrity when used in metal recycling where briquettes are subjected to high- temperature stress. At an optimized range of 0.05%–0.45% of the total binder, phenolic resin may significantly improve heat resistance and oxidation stability without making the briquettes excessively rigid or brittle. Without being bound by theory, during combustion, phenolic resin undergoes thermosetting polymerization, forming a carbonaceous matrix that reinforces the briquette's structure, minimizing deformation and fragmentation under extreme heat. Additionally, its use may reduce volatile organic compound (VOC) emissions and / or prevents excessive mass loss, ensuring that the briquette maintains density and mechanical strength throughout the process. To further enhance its performance in certain embodiments, phenolic resin may be modified with alkaline or acidic catalysts to optimize#2380375 086034-000002
[0061] 13
[0062] curing time, adhesion properties, and / or mechanical resilience. Such a formulation may ensure compatibility with PVA and the other components, creating a binder system that withstands high temperatures while minimizing slag formation and / or unwanted furnace deposits.
[0063] In further embodiments, where polyacrylamide (PAM) may be used, it may be included in the range of 0.05%–0.45% and without being bound by theory may act as a binder and / or moisture stabilizer, improving the green strength of briquettes, enhancing flexibility, and / or preventing premature cracking. In certain embodiments, the binder further may comprise Engineered Cellulosic Particulates in an amount ranging from about 0.025% to 0.05%, which, without being bound by theory, may provide fiber reinforcement, reducing microcracks and / or improve tenacity or flexibility under mechanical stress. Additionally, these ingredients may enhance moisture retention, optimize binder distribution, and / or contribute to thermal stability. A further advantage includes the controlled porosity introduced by the particulates, which, without being bound by theory, may improve gas permeability during high-temperature processing, facilitating more efficient combustion or metallurgical reactions.
[0064] A controlled viscosity range (for example, a PVA having a viscosity between about 1400 to about 3000 cps at room temperature, between about 1400 to about 2000 cps at room temperature, and / or between about 2000-about 3000 cps at room temperature) may help to ensure the right balance between binding efficiency and processability, preventing excessive brittleness and / or weakness in briquettes. In certain embodiments, binder formulation may utilize a unique blend of high and low molecular weight polyvinyl alcohols (PVA). Without being bound by theory, high molecular weight PVA may enhance mechanical strength, cohesion, and / or durability. While, without being bound by theory, low molecular weight PVA may improve solubility, penetration, and / or overall binder distribution within the briquette matrix. This combination of PVA may be used to optimize adhesion, flexibility, and / or water retention, ensuring superior performance under mechanical stress and thermal exposure.#2380375 086034-000002
[0065] 14
[0066] In some embodiments, PVA may be further modified to improve its solubility and / or reaction kinetics, enabling a more efficient binding process that results in higher compressive strength. Additionally, the liquid sub-bituminous coal extract may be treated with sodium hydroxide to enhance its solubility and reactivity with PVA, contributing to thermal stability, adhesion properties, and / or oxidation resistance, thereby preventing premature degradation in high-temperature environments.
[0067] In some embodiments, the binder mixture further includes a microbicidal agent in an amount of about 0.1% to about 5.0% of the binder mixture. Additionally, it may further include a defoamer or anti-foam agent, such as glycols and polyols, in an amount of about 0.001% to about 0.1% of the total binder. Examples of suitable defoamers include propylene glycol (PG), butylene glycol (BG), ethylene oxide-propylene oxide (EO / PO) block copolymers, and 2-ethylhexanol, which provide effective foam control while maintaining good compatibility with polyvinyl alcohol (PVA) and fully evaporating at elevated temperatures, thereby minimizing residual contamination in the final product.
[0068] The invention offers improved thermal stability by combining PVA, liquid acrylates copolymer, liquid sub-bituminous coal extract, phenolic resin and / or sulfonated lignin, preventing thermal degradation. Without being bound by theory, the superior binding strength provided by the PVA blend and liquid acrylates copolymer ensures high compressive strength. Increased green strength may be achieved through the inclusion of Engineered Cellulosic Particulates and / or PAM, which provide structural integrity before the curing phase. Such formulations may also serve as an eco-friendly alternative, reducing reliance on petroleum-based resins while maintaining high-performance characteristics.
[0069] The agglomeration process employing an organic polymer binder, along with any dry additives, can produce briquettes with adequate green strength— defined as a cold crush strength (CCS) ranging from about 100 psi. to 400 psi. The term "green" or cold crush strength (CCS) refers to the load-bearing capacity of the briquette in its unfired or partially cured state, such as when it is discharged from the roller press. Additionally, this agglomeration process may yield briquettes with sufficient cured crush strength.#2380375 086034-000002
[0070] 15
[0071] Furthermore, organic polymer binders described herein may result in a briquette that may be stored in unconditioned spaces and / or outside and / or may be abie to withstand the elements. Organic polymer binders described herein, and associated agglomeration processes herein may utilize minimal energy and may not require any induration to cure the briquette. Curing time for briquettes described here may be about eight (8) hours to about forty-eight (48) hours for the briquette to be fully cured. However, the briquettes described herein may be handled e.g., but without limitation, by a front-end loader) and / or stacked in a storage container after about one to two hour of cure time.
[0072] Referring now to Figure 1, one embodiment of a method (100) of preparing a liquid binder for use in the agglomeration process of briquettes is described in the flow chart of this figure. At Block 102, the process of Fig. 1 begins with the preparation of the PVA solution. At Block 103, polyvinyl alcohol (PVOH) in powder or granule form is added slowly to hot water maintained at a temperature between 150“F to 208°F (65°C to 98°C). The PVOH content is maintained between 18% to 30% solids, using a blend of different molecular weight PVOH resins to enhance both viscosity and binding efficiency. At Block 104, the binder solution is mixed thoroughly to achieve the desired viscosity of 1400-3000 cps of the binder solution, with the mixing process lasting between one to twenty-four (1 to 24) hours. During this phase, an acrylates copolymer (0.5% to 10%) is added while maintaining the temperature between 150°F and 208°F (65°C to 98°C) and agitating for 10 to 45 minutes. Once this step is completed, optional additives may be introduced (105), such as sulfonated lignin (0.5%-10%) to improve cohesion, water resistance, and / or lubrication, polyacrylamide (PAM) (0.05%~0.45%) to enhance green strength, microbicidal agents (0.1%~5%) for microbial control, and defoamers to prevent excessive foam formation. At block 106, once the PVA solution is properly mixed, it is transferred to another tank for further processing. At block 107, sub-bituminous coal extract is introduced into the solution in amounts ranging from 0.15% to 5%. The mixture is maintained at a temperature of 100" F to 185°F (38°C to 85°C) and stirred at a slow agitation speed of about 20 to about 50 rpm for 0.5 to 6 hours, ensuring proper blending and reaction. At block 109, the reaction is maintained above around 180°F (80C) to promote polymerization between the PVA and coal extract, forming a#2380375 086034-000002
[0073] 16
[0074] high-performance liquid binder. Following this step, the mixture undergoes a cooling phase where it is brought down to ambient temperature before further processing. At block 110, the cooled binder solution is filtered using a 50 to 100 mesh screen, ensuring the removal of any undissolved particles and achieving a homogeneous final solution. At block 111, the solution undergoes quality control testing to verify its solids content (targeting about 18% to about 30%) and viscosity (targeting about 1400 to about 3000 cps). Additional tests may be conducted based on specific process requirements. At Block 112, once the binder meets all quality control standards, it is packaged and stored under controlled conditions to prevent degradation, ensuring it remains stable and effective for its intended use in the briquetting process. At block 113, the process is completed, and the binder is now ready for further application.
[0075] Referring now to Figure 2, this figure is a block flow diagram that illustrates one embodiment of a method for briquette production. This exemplary process for the formation of a briquette utilizing the liquid binder solution described herein is also provided and the operational flowchart 200 for this process Is illustrated in Figure 2. In block 202, the starting material, which may be filings, chips, clippings, shot dust, shot fines, bag house dust, sludge, spent shot, laser dust, mill scale, titanium fines, ferro molybdenum, nickel, chrome, and / or other appropriate material is sized to about 6 mm or less particle size. At block 204, the starting material (regardless of form) is screened to remove any oversized material. At block 206, the material is loaded into a mixer (for example a high shear mixer) and mixed at 1 rpm to 100 rpm. At block 208, a plurality of Engineered Cellulosic Particulates may be introduced into the batch at a rate ranging from approximately 0.005% to about 5.0% of the total batch weight. The precise amount may vary based on the desired mechanical properties of the final briquette and / or its compatibility with other binder components.
[0076] The incorporation of Engineered Cellulosic Particulates may serve as a fiber connector, enhancing the tensile strength of the briquettes and reinforcing their structural integrity. Without being bound by theory, the fibrous nature of the cellulose chips may help to create an internal support network, distributing stress more evenly and reducing the risk of#2380375 086034-000002
[0077] 17
[0078] cracking or fragmentation. Such reinforcement effect can be particularly beneficial during handling, transportation, and / or storage, as well as when the briquettes are subjected to compressive forces or thermal stresses. Additionally, without being bound by theory the presence of Engineered Cellulosic Particulates may improve the binder distribution within the briquette matrix, contributing to enhanced green strength before curing. This improvement may lead to more uniform compaction and better overall performance in the furnace. The selection of cellulose chips as an additive is specifically aimed at optimizing the balance between mechanical durability, binder efficiency, and processing conditions, ensuring a robust and reliable final product.
[0079] At block 210, a resin dust powder may be added to the mixture at a rate of about 0.01 to about 10.0% of batch weight. A non-limiting example of a suitable resin dust powder may be a powdered phenolic Novolac resin combined with hexamethylenetetramine (hexa) as a curing agent. This composition is provided as an illustrative example and should not be interpreted as restrictive, as other resin systems with similar properties may also be viable. The inclusion of a phenolic resin can be particularly advantageous for applications where higher thermal stability is required, as it contributes to an elevated melt temperature when the briquettes are introduced into the furnace. Such a characteristic may enhance the mechanical integrity of the briquettes under high-temperature conditions, reducing premature degradation or deformation during the initial heating stages. Additionally, the phenolic resin may impart a water-resistant barrier to the briquettes, which can be particularly beneficial in environments with high humidity or exposure to moisture. This water resistance could facilitate outdoor storage and transportation, mitigating the risk of material degradation due to moisture absorption. Moreover, by improving the briquette's durability under unconditioned storage conditions, the phenolic resin may enhance logistical flexibility, allowing for extended storage periods without significant loss of structural integrity. Other resin-based powders with comparable thermal and hydrophobic properties may also be considered, depending on specific process requirements and end¬ use conditions as would be contemplated by one of ordinary skill in the art.#2380375 086034-000002
[0080] 18
[0081] At block 212, a pre-gelatinized starch powder may be added to the mixture at a rate of about 0.01 to about 10.0% of batch weight. A non-limiting example of a suitable pre¬ gelatinized starch may include starch derived from corn, potato, tapioca, wheat, rice, waxy maize, and / or other high-amylose source. This composition is provided as an illustrative example and should not be interpreted as restrictive, as other pre-gelatinized starches with similar properties may also be utilized. Pre-gelatinized starch may act as a cold-activated binder that hydrates rapidly, enhancing Inter-particle adhesion and green strength in cold- pressed briquettes. Without being bound by theory, a pre-gelatinized starch may increase binder viscosity, ensuring uniform distribution and consistent compaction. A starch may also reduce friction during pressing, improving efficiency and equipment lifespan. The biodegradable, renewable nature of starch may make it an eco-friendly, cost-effective alternative to synthetic binders, contributing to both performance and sustainability.
[0082] At block 214, the liquid binder solution— primarily composed of PVA (polyvinyl alcohol), liquid copolymer acrylate, and liquid sub-bituminous coal extract— ay be used with or without optional additives, such as sulfonated lignin, PAM, and / or other functional enhancers, depending on the desired formulation —and may be introduced at a rate ranging from approximately 1.75%i to less than 10%> of the total batch weight. The exact proportion may be adjusted based on the required binding strength, processing conditions, and material compatibility. Once added, the materials may be continuously mixed in a continuous mixer for a duration ranging from approximately 30 seconds to 10 hours, depending on factors such as binder viscosity, particle size distribution, and / or the degree of homogeneity required for optimal briquette formation. Without being bound by theory, in the formulation of this embodiment, PVA serves as the primary polymer binder, ensuring adhesion between the feed materials and providing the necessary green strength for handling and compaction. And, further, without being bound by theory liquid copolymer acrylates and liquid sub-bituminous coal extract may contribute to the structural integrity of the briquettes while potentially enhancing carbon content, which may be beneficial in metallurgical applications.#2380375 086034-000002
[0083] 19
[0084] This carefully balanced combination of PVA, liquid copolymer acrylates, and sub-bituminous coal extract ensures strong initial binding, durability during handling and / or storage, and / or enhanced performance in industrial applications, particularly in processes requiring consistent mechanical and thermal stability. Additionally, the formulation is designed for improved burnout efficiency, minimizing residual binder content during combustion, which may reduce impurities in the furnace, enhances metal purity, and / or decreases slag formation, optimizing overall furnace performance.
[0085] The batch material may then be at block 216 screw-fed into a rol! compactor or briquette press machine to form briquettes (see digital image of a briquette at Figure 3).
[0086] Briquettes may take various suitable forms; however, the primary and standard shape used in this process is a flattened cylindrical briquette with an oval cross-section. These briquettes are designed for sizes ranging from a minimum cross-section with a perimeter ranging from 2 inches to a maximum of 5 inches, with a length between 2 inches and 5 inches and height from 0.8 inch to 2 inches.
[0087] While other shapes—such as cuboid, spherical, cyli ndrical, rectangular prism, pyramid, rectangular tetrahedral, cone, and triangular prism-may be possible, the flattened cylindrical shape remains the primary design due to its optimized handling, stacking efficiency, and / or ability to meet mechanical performance requirements in industrial applications.
[0088] At block 218, the briquettes, regardless of their shape, optionally may be discharged from the roll compactor onto an infrared conveyor belt where the temperature increases to about 150°F for a period of about two to about five minutes. At block 220 the briquettes may then be transported to a storage area for curing. As noted previously, the curing time briquettes produced as described herein may be up to about eight (8) hours or up to about twenty-four (24) hours for complete curing and / or for being ready for transport; however, the briquettes may be handled, for example with a front-end loader, after only about one (1) hour of curing time, which may allow the briquettes to be stacked in a storage facility.#2380375 086034-000002
[0089] 20
[0090] Once cured and in their final form, the briquettes typically contain only about 0.05% to 10.0% binder. During the high-temperature process, the majority of the binder is burned off, which is crucial to prevent unwanted residues from contaminating the final steel product. Any remaining residue could introduce impurities, affect metal purity, or alter the steel's mechanical properties. Additionally, excess residue can accumulate in the furnace, leading to slag formation, increased maintenance requirements, and reduced operational efficiency. Ensuring the binder burns cleanly minimizes these risks, optimizing both steel quality and furnace performance. The briquette resulting from the process described herein may have a green strength of about 100 psi to about 400 psi, a Cold Crush Strength (CCS) and / or an adequate cured crush strength of about 600 psi to about 2,000 psi. At block 222, the briquettes, regardless of shape may be transported over a screen (for example, a 1 / 4- inch, 3 / 8-inch, 5 / 8 inch, and / or other dimension screen) in order to remove any remaining flashing, fines, or dust from the briquette. At block 224, the final briquettes are ready. At block 226, quality control analyses, such as crush strength, shape, and / or size measurements, are conducted. Finally, at block 228, the process is completed, and the briquettes may be stored or transported.
[0091] Figure 3 is a digital image showing an exemplary briquette 300 produced utilizing a liquid binder and method described herein. As mentioned previously herein, the briquette may be any shape or size. The shape and size of the resulting briquette may be determined by the machinery and / or mold utilized during the formation of the briquettes.
[0092] Table 1 below summarizes testing conducted on briquettes produced according to a method described herein. As shown in the table, various samples of briquettes with varying cure times and CCS measurements were tested. It is clear from the table that a longer cure time may result in a larger CCS measurement.
[0093] Table 1. Properties of briquete samples.
[0094] Briquette Cure Time CCS Measurement
[0095] Sample 1 1 minute 100 psi
[0096] Sample 2 30 minutes 150 psi#2380375 086034-000002
[0097] 21
[0098] Sample 3 60 minutes 300 psi
[0099] Sample 4 12 hours 500 psi
[0100] Sample 5 24 hours 1000+ psi
[0101] Binders, including those binders described herein, may be burned off during the steel production process, for example at temperatures ranging between about 800°C to about 3,500°C. For example, as a part of the steel making process the briquettes are placed in a blast furnace or electric arc furnace; when heat is applied, the briquette melts and the binder residue burns off in the form of vapor exhaust.
[0102] While several embodiments have been described and illustrated herein, those of ordinary skill in the art will readily envision a variety of other means and / or structures for performing the function and / or obtaining the results and / or one or more of the advantages described herein, and each of such variations and / or modifications is deemed to be within the scope of the embodiments described herein. More generally, those skilled in the art will readily appreciate that all parameters, dimensions, materials, and configurations described herein are meant to be exemplary and that the actual parameters, dimensions, materials, and / or configurations will depend upon the specific application or applications for which the teachings is / are used. Those skilled in the art will recognize or be able to ascertain using no more than routine experimentation, many equivalents to the specific embodiments described herein. It is, therefore, to be understood that the foregoing embodiments are presented by way of example only and that, within the scope of the appended claims and equivalents thereto, embodiments may be practiced otherwise than as specifically described and claimed. Embodiments of the present disclosure are directed to each individual feature, system, article, material, and / or method described herein. In addition, any combination of two or more such features, systems, articles, materials, and / or methods, if such features, systems, articles, materials, and / or methods are not mutually inconsistent, is included within the scope of the present disclosure.#2380375 086034-000002
[0103] All definitions, as defined and used herein, should be understood to control over dictionary definitions, definitions in documents incorporated by reference, and / or ordinary meanings of the defined terms.
[0104] The indefinite articles “a” and "an," as used herein in the specification and in the claims, unless clearly indicated to the contrary, should be understood to mean "at least one."
[0105] The phrase "and / or" as used herein in the specification and in the claims, should be understood to mean "either or both" of the elements so conjoined, i.e., elements that are conjunctively present in some cases and disjunctively present in other cases. Multiple elements listed with "and / or" should be construed in the same fashion, i.e., "one or more" of the elements so conjoined. Other elements may optionally be present other than the elements specifically identified by the "and / or" clause, whether related or unrelated to those elements specifically identified. Thus, as a non-limiting example, a reference to " A and / or B", when used in conjunction with open-ended language such as "comprising" can refer, in one embodiment, to A only (optionally including elements other than B); in another embodiment, to B only (optionally including elements other than A); in yet another embodiment, to both A and B (optionally including other elements); etc.
[0106] As used herein in the specification and in the claims, "or" should be understood to have the same meaning as "and / or" as defined above. For example, when separating items in a list, "or" or "and / or" shall be interpreted as being inclusive, i.e., the inclusion of at least one, but also including more than one of a number or list of elements, and, optionally, additional unlisted items. Only terms clearly indicated to the contrary, such as "only one of" or "exactly one of," or, when used in the claims, "consisting of," will refer to the inclusion of exactly one element of a number or list of elements. In general, the term "or" as used herein shall only be interpreted as indicating exclusive alternatives (i.e. "one or the other but not both") when preceded by terms of exclusivity, such as "either" "one of," "only one of," or "exactly one of." " Consisting essentially of," when used in the claims, shall have its ordinary meaning as used in the field of patent law.#2380375 086034-000002
[0107] As used herein, the term "about," when referring to a vaiue or to an amount of mass, weight, time, volume, concentration or percentage is meant to encompass variations of in some embodiments ±20%, in some embodiments ±10%, in some embodiments ±5%, in some embodiments ±1%, in some embodiments ±0.5%, and in some embodiments ±0.1% from the specified amount, as such variations are appropriate to perform the disclosed method.
[0108] As used herein, ranges can be expressed as from "about" one particular value, and / or to "about" another particular value. It is also understood that there are several values disclosed herein, and that each value is also herein disclosed as "about" that particular value in addition to the value itself. For example, if the value "10" is disclosed, then "about 10" is also disclosed. It is also understood that each unit between two particular units are also disclosed. For example, if 10 and 15 are disclosed, then 11, 12, 13, and 14 are also disclosed.
[0109] As used herein in the specification and in the claims, the phrase "at least one," in reference to a list of one or more elements, should be understood to mean at least one element selected from any one or more of the elements in the list of elements, but not necessarily including at least one of each and every element specifically listed within the list of elements and not excluding any combinations of elements in the list of elements. This definition also allows that elements may optionally be present other than the elements specifically identified within the list of elements to which the phrase "at least one" refers, whether related or unrelated to those elements specifically identified. Thus, as a non¬ limiting example, "at least one of A and B" {or, equivalently, "at least one of A or B," or, equivalently "at least one of A and / or B") can refer, in one embodiment, to at least one, optionally including more than one, A, with no B present (and optionally including elements other than B); in another embodiment, to at least one, optionally including more than one, B, with no A present (and optionally including elements other than A); in yet another embodiment, to at least one, optionally including more than one, A, and at least one, optionally including more than one, B (and optionally including other elements); etc.#2380375 086034-000002
[0110] 24
[0111] It should also be understood that, unless clearly indicated to the contrary, in any methods claimed herein that include more than one step or act, the order of the steps or acts of the method is not necessarily limited to the order in which the steps or acts of the method are recited.
[0112] In the claims, as well as in the specification above, all transitional phrases such as "comprising," "including," "carrying," "having," "containing," "involving," "holding," "composed of," and the like are to be understood to be open-ended, i.e., to mean including but not limited to. Only the transitional phrases "consisting of" and "consisting essentially of" shall be closed or semi-closed transitional phrases, respectively, as set forth in the United States Patent Office Manual of Patent Examining Procedures, Section 2111.03.
[0113] It Is to be understood that the embodiments are not limited in its application to the details of construction and the arrangement of components set forth in the description or illustrated in the drawings. The invention is capable of other embodiments and of being practiced or of being carried out in various ways. Unless limited otherwise, the terms "connected,'' "coupled," "in communication with," and "mounted," and variations thereof herein are used broadly and encompass direct and indirect connections, couplings, and mountings. In addition, the terms "connected" and "coupled" and variations thereof are not restricted to physical or mechanical connections or couplings.
[0114] The foregoing description of several embodiments of the invention has been presented for purposes of illustration. It is not intended to be exhaustive or to limit the invention to the precise steps and / or forms disclosed, and obviously many modifications and variations are possible in light of the above teaching.#2380375 086034-000002
[0115] 25
[0116] Embodiments
[0117] The following provides an enumerated listing of some of the embodiments disclosed herein. It will be understood that this listing is non-limiting, and that individual features or combinations of features (e.g. 2, 3 or 4 features) as described in the Detailed Description above can be incorporated with the below-listed Embodiments to provide additional disclosed embodiments herein.
[0118] 1. A binder composition for forming cold-pressed metal briquettes comprising:
[0119] A polyvinyl alcohol polymer, a liquid acrylate copolymer and a liquid sub- bituminous coal extract;
[0120] and wherein said liquid acrylates copolymer comprises 0.5% to 10% by mass of the binder composition; and
[0121] wherein the liquid sub-bituminous coal extract comprises 0.15%~5% of the binder composition,
[0122] 2. The binder of embodiment I, wherein the binder further comprises phenolic resin in an amount ranging from 0.05% to 0.45% by mass of the binder composition.
[0123] 3. The binder of embodiment 1, wherein the binder further comprises pre-gelatinized starch.
[0124] 4. The binder of embodiment 3, wherein said pre -gelatinized starch is a corn starch, a potato starch, a tapioca starch, a wheat starch, a rice starch, a waxy maize starch, or a high-amylose starch.
[0125] 5. The binder of embodiment 3, wherein the quantity of said pre -gelatinized starch comprises 0.05% to 0.45% by mass of the binder.
[0126] 6. The binder of embodiment 1, wherein the binder further comprises sulfonated lignin in an amount ranging from 0.5% to 10% by mass of the binder.
[0127] 7. The binder of embodiment 1, wherein the binder further comprises polyacrylamide in an amount ranging from 0.05% to 0.45% by mass.*2380375 086034-000002
[0128] 26
[0129] 8. The binder of embodiment 1, wherein the binder further comprises engineered cellulosic particulates in an amount ranging from 0.025% to 0.05% by mass.
[0130] 9. The binder of embodiment 1, wherein the binder further comprises a microbicidal agent in an amount ranging from 0.1% to 5.0% by mass.
[0131] 10. The binder of embodiment 1, wherein the binder further comprises a defoamer selected from glycols, polyols, or ethyl hexanol in an amount ranging from 0.001% to 0.1% by mass.
[0132] 11. A method for producing a cold-pressed metal briquette comprising admixing mixing metal fines with the binder composition of claim 1 and pressing the mixture into a briquette shape under applied pressure.
[0133] 12. The method of embodiment 11, wherein the binder content in the briquette ranges from 1.75% to less than 10% by mass of the total briquette weight.
[0134] 13. The method of embodiment 11, wherein the binder is reacted at high temperatures prior to mixing to enhance adhesion and thermal stability.
[0135] 14. A cold-pressed metal briquette produced using the binder composition of embodiment I, wherein the briquette exhibits improved compressive strength, oxidation resistance, and thermal stability for metallurgical applications.
[0136] 15. The method of embodiment 11, wherein the cold-pressed metal briquette comprises an agglomerated metal.
[0137] 16. The method of embodiment 15, wherein the cold-pressed metal briquette comprises a flattened cylindrical shape with an oval cross-section.
[0138] 17. The method of embodiment 15, wherein said cold-pressed metal briquette further comprises a cross-section with a with a perimeter ranging from 2 inches to a maximum of 5 inches.#2380375 086034-000002
[0139] 18. The method of embodiment 17, wherein said cold-pressed metal briquette comprises a length along the major axis of between 2 inches and 5 inches.
Claims
#2380375 086034-00000228Claims1. A binder composition for forming cold-pressed metal briquettes comprising:A polyvinyl alcohol polymer, a liquid acrylate copolymer and a liquid sub- bituminous coal extract;and wherein said liquid acrylates copolymer comprises 0.5% to 10% by mass of the binder composition; andwherein the liquid sub-bituminous coal extract comprises 0.15%~5% of the binder composition.
2. The binder of claim I, wherein the binder further comprises phenolic resin in an amount ranging from 0.05% to 0.45% by mass of the binder composition.
3. The binder of claim I, wherein the binder further comprises pre-gelatinized starch.
4. The binder of claim 3, wherein said pre-gelatinized starch is a corn starch, a potato starch, a tapioca starch, a wheat starch, a rice starch, a waxy maize starch, or a high-amylose starch.
5. The binder of claim 3, wherein the quantity of said pre -gelatinized starch comprises 0.05% to 0.45% by mass of the binder.
6. The binder of claim 1, wherein the binder further comprises sulfonated lignin in an amount ranging from 0.5% to 10% by mass of the binder.
7. The binder of claim 1, wherein the binder further comprises polyacrylamide in an amount ranging from 0.05% to 0.45% by mass.
8. The binder of claim 1, wherein the binder further comprises engineered cellulosic particulates in an amount ranging from 0.025% to 0.05% by mass.
9. The binder of claim 1, wherein the binder further comprises a microbicidal agent in an amount ranging from 0.1 ‘l-fr to 5.0% by mass.#2380375 086034-0000022910. The binder of claim 1, wherein the binder further comprises a defoamer selected from glycols, polyols, or ethyl hexanol in an amount ranging from 0.001 to 0.1% by mass.
11. A method for producing a cold-pressed metal briquette comprising admixing mixing metal fines with the binder composition of claim I and pressing the mixture into a briquette shape under applied pressure.
12. The method of claim 11, wherein the binder content in the briquette ranges from 1.75% to less than 10% by mass of the total briquette weight.
13. The method of claim 11, wherein the binder is reacted at high temperatures prior to mixing to enhance adhesion and thermal stability.
14. A cold-pressed metal briquette produced using the binder composition of claim I, wherein the briquette exhibits improved compressive strength, oxidation resistance, and thermal stability for metallurgical applications.
15. The method of claim 11, wherein the cold-pressed metal briquette comprises an agglomerated metal.
16. The method of claim 15, wherein the cold-pressed metal briquette comprises a flattened cylindrical shape with an oval cross- section.
17. The method of claim 15, wherein said cold-pressed metal briquette further comprises a cross-section with a with a perimeter ranging from 2 inches to a maximum of 5 inches.
18. The method of claim 17, wherein said cold-pressed metal briquette comprises a length along the major axis of between 2 inches and 5 inches,