Method of preparing sputtered thin-film insulators with poisoning

The sputtering process with targeted gas flow rates ensures high-quality thin-film insulators by oxidizing the target before deposition, enhancing breakdown voltage and reducing failures in OLED and LCD panels.

WO2026235987A1PCT designated stage Publication Date: 2026-11-12AMORPHYX INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/025898
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-29
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Achieving high-quality thin-film insulators with uniform composition and reduced failure events due to low-voltage dielectric breakdown is challenging in OLED and LCD in-plane transfer panels.

Method used

A sputtering process where a metallic target is oxidized by a reactive gas before deposition, with a high flow rate initially to achieve a fully oxidized state, followed by a lower flow rate during deposition to ensure high-quality thin-film insulators are formed.

Benefits of technology

This method results in a substantial reduction in failure events and improves the electrical quality of thin-film insulators, increasing breakdown voltage by four times and reducing leakage currents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026025898_12112026_PF_FP_ABST
    Figure US2026025898_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A sputtering process provides high quality thin-film insulators with improved uniformity of composition. The sputtering process places a metallic target into a fully oxidized state prior to opening a shutter within the sputtering chamber. Upon opening the shutter, oxygen-rich phases with high electrical quality are initially deposited on the substrate as the shutter opens and approaches an intended voltage. This results in deposition of a high-quality thin-film insulator on the substrate, and a substantial reduction in failure events associated with low-voltage dielectric breakdown.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] METHOD OF PREPARING SPUTTERED THIN-FILM INSULATORS WITH POISONING

[0002] BACKGROUND

[0003] Technical Field

[0004] The present disclosure relates to formation of thin-film insulators.

[0005] Description of the Related Art

[0006] Thin-film insulators are central to the operation of organic light emitting diode (OLED) and liquid crystal display (LCD) in-plane transfer (IT) panels, and other applications. The quality of the thin-film insulators can affect the overall performance of such devices. However, it can be difficult to achieve high-quality thin-film insulators.

[0007] All of the subject matter discussed in the Background section is not necessarily prior art and should not be assumed to be prior art merely as a result of its discussion in the Background section. Along these lines, any recognition of problems in the prior art discussed in the Background section or associated with such subject matter should not be treated as prior art unless expressly stated to be prior art. Instead, the discussion of any subject matter in the Background section should be treated as part of the inventor’s approach to the particular problem, which, in and of itself, may also be inventive.

[0008] BRIEF SUMMARY

[0009] Embodiments of the present disclosure provide high quality thin-film insulators with improved uniformity of composition. Embodiments of the present disclosure perform a sputtering process to deposit a thin-film on a substrate. The sputtering process places a metallic target into a fully oxidized state prior to opening a shutter within the sputtering chamber. Upon opening the shutter, oxygen-rich phases with high electrical quality are initially deposited on the substrate as the shutter opensand approaches an intended voltage. This results in deposition of a high-quality thin-film insulator on the substrate, and a substantial reduction in failure events associated with low-voltage dielectric breakdown.

[0010] In one embodiment, while the shutter is closed, a conditioning gas flows into the portion of the deposition chamber in which the target is positioned. The conditioning gas is a reactive gas, such as oxygen, selected to oxidize the target, also known as poisoning the target. The reactive gas has relatively high flow rate selected to ensure that the target reaches a fully-oxidized state prior to opening the shutter. Upon opening the shutter, the sputtering fluid source provides the sputtering fluid into the deposition chamber. Material is dislodged from the target and deposited on the substrate, in oxygen-rich phases. The flow rate of the conditioning gas is reduced upon opening the shutter.

[0011] In one embodiment, a method includes poisoning a target within a sputtering chamber during a startup phase of a sputtering process by flowing a reactive gas into the chamber with a first flow rate while a shutter is closed between the target and a substrate. The method includes initiating a deposition phase of the sputtering process by opening the shutter, flowing the reactive gas into the chamber at a second flow rate lower than the first flow rate during the deposition phase, and depositing a dielectric layer on the substrate during the deposition phase.

[0012] In one embodiment, a method includes biasing a substrate in a reactive sputtering chamber during a sputtering process. The method includes, during a first portion of a startup phase of the sputtering process while a shutter between a target and the substrate is closed, increasing a voltage of the target above a deposition voltage level while a flow rate of a reactive gas into the chamber is approximately zero. The method includes, during a second portion of the startup phase while the shutter is closed, flowing the reactive gas into the chamber and reducing the voltage of the target below the deposition level. The method includes during a deposition phase of the sputtering process after the second portion of the startup phase, opening the shutter, decreasing a flow rate of the reactive gas to a deposition flow rate level, increasing thevoltage of the target to the deposition voltage level, and depositing a dielectric film on the substrate.

[0013] In one embodiment, a system includes one or more computer memories storing software instructions and one or more processors configured to execute the software instructions to perform a sputtering process. The sputtering process includes poisoning a target within a sputtering chamber during a startup phase of the sputtering process by flowing a reactive gas into the chamber with a first flow rate while a shutter is closed between the target and a substrate. The process includes initiating a deposition phase of the sputtering process by opening the shutter, flowing the reactive gas into the chamber at a second flow rate lower than the first flow rate during the deposition phase, and depositing a dielectric layer on the substrate during the deposition phase.

[0014] BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWINGS

[0015] The detailed description is described with reference to the accompanying figures. The sizes and relative positions of elements in the figures are not necessarily drawn to scale. For example, the shapes of various elements and angles are not drawn to scale and some of these elements are enlarged and positioned to improve figure legibility. As is understood by one of skill in the art, the shape of a particular element may be modified (e.g., rounded, thinned, elongated, etc.) to suit a particular application.

[0016] Figure 1 A is a simplified illustration of a sputtering system, in accordance with one embodiment.

[0017] Figure IB is a simplified illustration of the sputtering system of Figure 1 A in a startup phase of a sputtering process, in accordance with one embodiment.

[0018] Figure 1C is a simplified illustration of the sputtering system of Figure 1 A in a deposition phase of the sputtering process, in accordance with one embodiment.

[0019] Figure 2 is a timing diagram of a sputtering process, in accordance with one embodiment.

[0020] Figure 3 is a graph illustrating target voltage and a reactive gas flow rate, in accordance with one embodiment.Figure 4 is a graph illustrating target voltage and a reactive gas flow rate, in accordance with one embodiment.

[0021] Figure 5 is a Weibull plot of breakdown fields and cumulative failure percentages for a sputtering process, in accordance with one embodiment.

[0022] Figure 6 is a cross-sectional view of a thin-film transistor including a thin-film insulator, in accordance with one embodiment.

[0023] Figure 7 is a flow diagram of a method for performing a sputtering process, in accordance with one embodiment.

[0024] Figure 8 is a flow diagram of a method for performing a sputtering process, in accordance with one embodiment.

[0025] DETAILED DESCRIPTION

[0026] In the following description, certain specific details are set forth in order to provide a thorough understanding of various disclosed embodiments. However, one skilled in the relevant art will recognize that embodiments may be practiced without one or more of these specific details, or with other methods, components, materials, etc. In other instances, well-known systems, components, and circuitry associated with integrated circuits have not been shown or described in detail, to avoid unnecessarily obscuring descriptions of the embodiments.

[0027] Unless the context requires otherwise, throughout the specification and claims which follow, the word “comprise” and variations thereof, such as, “comprises” and “comprising” are to be construed in an open, inclusive sense, that is as “including, but not limited to.” Further, the terms “first,” “second,” and similar indicators of sequence are to be construed as interchangeable unless the context clearly dictates otherwise.

[0028] Reference throughout this specification to “one embodiment” or “an embodiment” means that a particular feature, structure or characteristic described in connection with the embodiment is included in at least one embodiment. Thus, the appearances of the phrases “in one embodiment” or “in an embodiment” in various places throughout this specification are not necessarily all referring to the sameembodiment. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0029] As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” include plural referents unless the content clearly dictates otherwise. It should also be noted that the term “or” is generally employed in its broadest sense, that is as meaning “and / or” unless the content clearly dictates otherwise.

[0030] Figure 1A is a simplified illustration of a reactive sputtering system 100, in accordance with one embodiment. As will be set forth in more detail below, the components of the sputtering system 100 cooperate to perform sputtering processes that result in the deposition of high quality thin-film insulators. In one embodiment, the sputtering system is a pulsed-DC sputtering system.

[0031] In one embodiment, the sputtering system 100 corresponds to a sputtering tool. For simplicity in illustrating principles of the present disclosure, Figure 1 A illustrates various components of the sputtering system 100 as simple blocks. In practice, the sputtering system 100 can have various compositions, arrangements, structures, and configurations without departing from the scope of the present disclosure.

[0032] In one embodiment, the sputtering system 100 includes a sputtering chamber 101. The sputtering chamber 101 may also be termed a deposition chamber. Deposition of thin-film insulators occurs within the sputtering chamber 101. Various other types of thin films may also be deposited with the sputtering chamber 101.

[0033] The sputtering chamber 101 includes a target support 102. The target mount 102 is configured to hold a target 104 during sputtering processes. The sputtering chamber includes a substrate support 106 configured to hold a substrate 108.

[0034] The target 104 includes a target material. The target material is the material that will be utilized to form a thin film on the exposed surface of the substrate 108 during a sputtering process, as will be set forth in more detail below. In one embodiment, the target 108 includes a metal. The sputtering process deposits a thin-film insulator corresponding to an oxide of the metal of the target 108. In one example, the target 104 includes aluminum. The sputtering process deposits aluminum oxide asthe thin-film insulator on the substrate 108. Other target materials and other types of thin-films can be utilized without departing from the scope of the present disclosure. In one embodiment, the target includes titanium, hafnium, tantalum, silicon, yttrium, or other suitable materials.

[0035] In the example of Figure 1 A, the target 104 is held above the substrate 108 such that the bottom surface of the target 104 faces the top surface of the substrate 108. However, in other examples, the positions of the target support 102 and the substrate support 106 may be reversed such that the upward facing surface of the target 104 faces the downward facing surface of the substrate 108. Various other configurations and orientations of targets and substrates can be utilized without departing from the scope of the present disclosure.

[0036] A substrate support 106 is positioned within the thin-film deposition chamber 102. The substrate support 106 supports the substrate 108 during thin-film deposition processes. At the beginning of a thin-film deposition process, a substrate 108 may be transferred into the thin-film deposition chamber 102 and positioned on the substrate support 106. After a thin-film deposition process is performed on the substrate 108, the substrate 108 can be transferred out of the thin-film deposition chamber 102. The substrate 108 can include an insulator substrate, a wafer, or another type of substrate.

[0037] In some embodiments, the target support 102 and the substrate support 106 correspond to, or may include electrodes. Voltages may be applied between the target support 102 and the substrate support 106 during the sputtering process. These voltages can include DC voltages, AC voltages, or combinations of DC offsets and AC voltages.

[0038] In some embodiments, the substrate support 106 includes a heater. The heater can heat the substrate 108 during thin-film deposition processes. Heating of the substrate 108 during thin-film deposition processes can help promote redistribution or settling of deposition materials on the surface of the substrate 108 to help ensure even thicknesses of the deposition material on the substrate 108.In some embodiments, the sputtering system 100 includes a power source 110. The power source 110 is coupled to the target support 102 and the substrate support 106. The power source 110 is configured to apply a voltage between the target support 102 and the substrate support 106. In some embodiments, this corresponds to applying a voltage to the target 104.

[0039] In one embodiment, the sputtering chamber 101 includes a shutter 109. The shutter 109 is illustrated by a dashed line in Figure 1 A. The shutter 109 can be opened or closed. When the shutter 109 is closed, the shutter 109 corresponds to a physical barrier between the target 104 and the substrate 108. When the shutter 109 is closed, the shutter 109 prevents sputtering of material from the target 104 onto the substrate 108. When the shutter 109 is open, material can be sputtered from the target 104 onto the substrate 108. As will be set forth in more detail below, the shutter 109 is closed during a startup phase of a sputtering process and is open during a deposition phase of the sputtering process. In some embodiments, a voltage is applied to the shutter 109 when the shutter 109 is closed. In some embodiments, the shutter 109 is grounded when the shutter 109 is closed.

[0040] In one embodiment, the sputtering system 100 includes a conditioning gas source 116. The conditioning gas source 116 is configured to supply a conditioning gas into the sputtering chamber 101. The conditioning gas is selected to react with the target 104 in order to condition the target 104 so that sputtering the target will result in deposition of a high-quality thin film. In one embodiment, the conditioning gas includes oxygen. In one embodiment, the conditioning gas includes nitrogen.

[0041] In one embodiment, a valve 118 is coupled between the conditioning gas source 116 and a fluid inlet 120. The valve 118 controls supply of the conditioning gas 116 into the sputtering chamber 101. The valve 118 can stop flow of the conditioning gas, enable flow of the conditioning gas, and adjust the flow rate of the conditioning gas.

[0042] The fluid inlet 120 is positioned such that when the shutter 109 is closed, the conditioning gas can be provided onto the target 104. In the example configuration of Figure 1 A, the shutter 109 separates an upper portion of the sputtering chamber 101from a lower portion of the sputtering chamber 101. The target 104 is supported in the upper portion of the sputtering chamber 101. The substrate 108 is positioned in the lower portion of the sputtering chamber 101. The fluid inlet 120 opens into the upper portion of the sputtering chamber 101. Other configurations can be utilized without departing from the scope of the present disclosure.

[0043] A sputtering gas source 122 supplies a fluid into the thin-film deposition chamber 102. In some embodiments, the sputtering gas includes an inert gas, such as argon, or another inert gas. During operation, the power source 110 applies a voltage between the target support 102 and the substrate support 106. The applied voltage causes ionization of the atoms of the fluid. When the atoms of the sputtering gas source become ionized, the atoms are drawn toward the target 104 via electrostatic force. For example, the target support 102 may receive a negative voltage that causes positively charged ions to be drawn toward the target 104. When the positively charged ions impact the target 104, the positively charged ions cause some of the material of the target 104 to be ejected from the target 104 and to travel toward the substrate 108. The ejected target material accumulates on the substrate, thereby forming a thin film of the target material on the substrate 108.

[0044] In one embodiment, a valve 124 is coupled between the sputtering gas source 122 and a fluid inlet 122. The valve 124 controls supply of the sputtering gas into the sputtering chamber 101. The valve 124 can stop flow of the sputtering gas, enable flow of the sputtering gas, and adjust the flow rate of the sputtering gas. In one embodiment, the fluid inlet 122 supplies the sputtering gas into the lower portion of the sputtering chamber 101, though other configurations can be utilized without departing from the scope of the present disclosure.

[0045] The sputtering system 101 includes an exhaust outlet 126. The exhaust outlet 126 carries exhaust fluids, byproducts, and access conditioning gas and sputtering gas from that the sputtering chamber 101. Though not shown, the sputtering system 101 can include one or more pumps and other control valves to control flow of exhaust fluids and byproducts from the sputtering chamber 101.The sputtering system 100 includes a control system 128. The control system 128 controls the function of the various components of the sputtering system 100. For example, the control system 128 executes the sputtering process including controlling the power source 110 to apply selected voltages, controlling the valves 118 and 124 to control flow of the conditioning and sputtering gasses, and controlling any other functions.

[0046] In some embodiments, the control system 128 includes one or more processors and one or more memories. The one or more memories store instructions which, when executed by the one or more processors, cause the sputtering system 100 to execute a sputtering process. Further details regarding the sputtering process are set forth below.

[0047] Figure IB is an illustration of the sputtering system 100 of Figure 1A during a startup phase of a sputtering process, in accordance with some embodiments. During the startup phase, the shutter 109 is closed. The closing of the shutter 209 is indicated by the solid line that had previously been dashed in Figure 1 A. A voltage is applied to the target 104 via the power source 110.

[0048] After a selected duration of time, the conditioning gas source 116 begins to supply the conditioning gas 134 into the sputtering chamber 101 with a first flow rate. In one embodiment, the first flow rate is a relatively high flow rate. One effect of the high flow rate of the conditioning gas is that a larger portion (or an entirety) of the target 104 reacts with the conditioning gas, thereby changing the composition of the target 104 prior to opening of the shutter 109.

[0049] As set forth previously, in one example, the target 104 is aluminum and the conditioning gas 134 is oxygen. The high flow rate of oxygen ensures that the target 104 reaches a fully-oxidized state prior to shutter 109 opening. As will be set forth in more detail below, the highly oxidized state of the target 104 results in deposition of a high-quality film of AI2O3 on the substrate 108.

[0050] Though not shown, in one embodiment the process includes a precleaning phase prior to changing a composition (poisoning) the target 104.Figure 1C illustrates the sputtering system 100 of Figure 1A during a deposition phase of the sputtering process, in accordance with some embodiments. In Figure 1C, the shutter 109 has been opened. The valve 124 is opened and the sputtering gas source 122 provides the sputtering gas 136 into the sputtering chamber 101. As was described previously, the sputtering gas 136 becomes ionized and is driven toward the target 108. The impact of the ionized sputtering gas 136 with the target 104 causes material 138 from the target 104 to become dislodged or to otherwise break away from the target 104. The material 138 is driven onto the substrate 108. The accumulation of the material 138 from the target 104 on the substrate 108 results in deposition of a thin-film insulator.

[0051] Returning to the example in which the target is aluminum and the conditioning gas 134 is oxygen, a high-quality film of aluminum oxide (AI2O3) is deposited on the substrate 108. When the shutter opens the voltage of the target (target voltage), gradually increases towards the desired value for the process (process voltage). This avoids the deposition of AlOx species onto the substrate which are much poorer in terms of electrical quality (higher leakage current, lower breakdown field). Accordingly, a high-quality film of AI2O3 is deposited.

[0052] Figure 2 is a graph illustrating parameters of a sputtering process, in accordance with one embodiment. The sputtering process of Figure 2 is one example of the sputtering process described in relation to Figures 1 A-1C. In Figure 2, the target 104 includes aluminum and the conditioning gas 134 includes molecular oxygen (O2). However, other materials can be utilized without departing from the scope of the present disclosure. Figure 2 illustrates target voltage, conditioning gas pressure, and chamber pressure versus time during a deposition process.

[0053] Figure 2 illustrates a startup phase of a deposition process, in accordance with one embodiment. The startup phase includes the portion of the deposition cycle during which the shutter is closed. In one example, at time 0 s, the pressure within the sputtering chamber is increased to about 50 mTorr. After about 40 seconds, the voltage of the target begins to increase from 0 V to about 370 V, beyond a process voltage of 350 V corresponding to a voltage at which deposition will primarily take place. Shortlyafter the initial application of voltage to the target, the pressure drops to about 2 mTorr. Other values of voltage and pressure can be utilized without departing from the scope of the present disclosure.

[0054] At about 250 seconds, the flow of the conditioning gas O2 is initiated while the shutter is closed. In some embodiments, the flow rate of the conditioning gas is about 400 seem. This corresponds to a first flow rate value and, as will be shown, is higher than the flow rate of the conditioning gas during the deposition phase.

[0055] When the O2 begins to flow into the sputtering chamber, the aluminum target 104 begins to react with the O2. This reaction causes the target 104 to oxidize, becoming AI2O3. The flow of the O2 during the startup phase causes the target voltage to initially increase and then to drop to a level of about 290 V, below the deposition voltage.

[0056] At about 375 seconds, the shutter 109 opens. This corresponds to the end of the startup phase and the beginning of the deposition phase of the sputtering process. At the opening of the shutter 109, the flow rate of the conditioning gas is also significantly decreased to a second flow rate. The second flow rate corresponds to a deposition value. In other words, the second flow rate is the flow rate that is utilized while the thin-film is accumulating on the substrate 108. In one embodiment, the second flow rate is about 3 seem, though other values can be utilized without departing from the scope of the present disclosure. Accordingly, the first flow rate is several times higher than the second flow rate. In one embodiment, the first flow rate is at least three times higher than the second flow rate.

[0057] In one embodiment, the opening of the shutter and the decrease in flow rate results in an increase of the target voltage to the deposition voltage. As set forth previously, in one embodiment, the deposition voltage is about 350 V, though other voltages can be utilized without departing from the scope of the present disclosure.

[0058] In one embodiment, the sputtering system 100 operates in a constant power mode during the deposition process. Power is a product of voltage and current. Changes in the conditioning gas flow rate result in changes in current. Because the system is operating in a constant power mode, changes in current result in changes inthe voltage. Accordingly, changing the flow rate of the conditioning gas results in changes in the voltage of the target 104. These relationships are described in further detail below.

[0059] Figures 3 and 4 and their descriptions are utilized to assist in an understanding of principles of the present disclosure. Figure 3 is a graph illustrating target voltage vs oxygen flow rate during O2 addition and O2 extraction with an open shutter, in accordance with one embodiment. The flow rate has a range between 0 seem and 10 seem. O2 addition corresponds to a state in which the conditioning gas is flowing into the deposition chamber. O2 extraction corresponds to a state in which the conditioning gas is flowing out of the deposition chamber. As can be seen, there is some hysteresis in the target voltage based on in-flow and out-flow of O2. Most notably within a range between about 2 seem and 6 seem, the process voltage is higher for a given flow rate in the extraction state than for the addition state. The hysteresis is a result of the target having a metastable oxidization state.

[0060] In Figure 3, there is an initial curve between about 0 seem and 2 seem in which there is little hysteresis. There is also a portion between 6 seem and 10 seem where there is relatively little hysteresis. Thin-films deposited in the initial curve region tend to have higher concentration of metal, resulting in higher conductivity and lower breakdown voltages. Films deposited in the higher flow rate regime have higher oxygen content, resulting in lower conductivity and higher breakdown voltages. A single film deposited with portions in both of these conditions would have non-uniform composition.

[0061] As set forth previously, in one embodiment the sputtering system 100 is operated in a constant power mode. Power is a product of voltage and current.

[0062] Accordingly, a drop in voltage, as seen in Figure 3, will result from a corresponding increase in current. The increase in current is based on secondary electron emission yield during the sputtering process. The drop in voltage indicates formation of the oxide in the target.

[0063] Figure 4 is a graph illustrating target voltage vs oxygen flow rate during O2 addition and O2 extraction with a closed shutter, in accordance with oneembodiment. As can be seen, the voltage is higher in Figure 4 beyond the 3 seem flow rate than for the same flow rate in Figure 3 with the shutter open. The steady high voltage below about 6 seem is an indication that there is a lack of oxidization of the target in that range. This would correspond to deposition of a thin film with higher concentration of metal and lower breakdown voltages.

[0064] Beneficially, the process described in relation to Figures 1 A-2 ensures a very high degree of oxidization before the shutter opens by utilizing the high flow rate. The process then changes to a low flow rate as soon as deposition begins. The result is a high quality thin-film insulator with low conductivity, high uniformity of composition, high breakdown voltages, and low leakage currents.

[0065] Figure 5 illustrates a failure rates vs breakdown field of thin-film insulators for a process in which flow rate is uniform before and after shutter opening, and for a process in which flow rate is higher before shutter opening than after, in accordance with one embodiment. In other words, the high flow rate curve corresponds to the process described in relation to Figures 1 A-2, in which a high flow rate of the conditioning gas is utilized while the shutter is closed, followed by a drop in the flow rate after the shutter opens.

[0066] The data shown at left compares the two processes in terms of dielectric breakdown. The left axis is a special function of the cumulative failure (CF) referred to as a Weibull plot. The right y-axis is the cumulative failure percentage.

[0067] The use of a Weibull plot accentuates two main components of the distribution: the head and tail. The head of the distribution is the most vertical part at higher breakdown field. This part is associated with the intrinsic field strength (e.g., breakdown field of AI2O3). The tail of the distribution is associated with defective regions and is called extrinsic (e.g., Al Ox).

[0068] As can be seen, the process of Figure 2 has no tail. The result is that the breakdown field is increased from < 0.1 V / nm to > 0.4 V / nm. This 4X increase in breakdown field means that the improved thin-film insulator can withstand a 4X larger applied voltage before reducing yield. This is a substantial improvement.Thin-films formed in accordance with the uniform flow-rate process have been shown to be linked to a significant reduction in the yield of MIM and MIS capacitors, due to a reduction in breakdown voltage. The reduction in breakdown voltage is related to the deposition of oxygen-deficient suboxides during the early stages of reactive sputtering of aluminum oxide, a phenomenon which is generally applicable to other gate insulators which would also be deposited via reactive sputtering (e.g., silicon dioxide, hafnium dioxide, zirconium dioxide, etc.).

[0069] As set forth in relation to Figures 1 A-2 and 5, the process utilizing the higher reactive gas flow rate is required to reach an oxygen-rich state of the target and avoid deposition of electrically-poor AlOx suboxides.

[0070] The result is a 4X increase in the maximum voltage which could be safely applied across any capacitor encompassing the reactively-sputtered gate insulator.

[0071] A higher applied voltage leads to a lower resistance of all switching thin-film transistors in their ON states, and a corresponding increase in refresh rate obtainable in an LCD or OLED IT panels.

[0072] In one embodiment, the target is conditioned to a state that is fully reacted with the reactive gas. This is obtained by inserting an additional step in the conditioning sequence referred to as poisoning. Poisoning the target corresponds to setting a high reactive gas flow rate to react the surface to completion. Once the shutter is opened, the reactive gas flow is reduced to the desired value corresponding to the process voltage and process gas flow. The degree of oxidation on the target surface approaches the desired value from an oxygen-rich state, avoiding the deposition of oxygen-deficient suboxides with poor insulator quality.

[0073] Figure 6 is a cross-sectional view of a thin-film transistor 140, in accordance with one embodiment. The thin-film transistor includes a thin-film insulator 146 formed in accordance with the process described in relation to Figures 1A-2 and 5.

[0074] The thin-film transistor 140 includes a gate electrode 144 positioned on a substrate 102. In one embodiment, the substrate 102 includes a substantiallynonconductive material. The substrate can be glass, a polymer, plastic, or other materials. In some embodiments, the substrate is glass, a polymer, plastic, or other material. In other embodiments, the substrate is a rubber. As used herein, “rubber” includes polymers of isoprene as well as forms of polyisoprene. In some such embodiments, the substrate is a plastic. Any suitable plastic may be used. In some embodiments, the plastic is a polyimide, an arylamide, acrylamide, polybenzimidazole (PBI), polyetherimide, polyetherketoneketone (PEKK), polyether ether ketone (PEEK), polyamide, polyimide, polyamide-imides, polystyrene (PS), polyphenylene oxide (PPO), polyphthalamide (PPA), polyvinyl alcohol (PVA), acrylonitrile butadiene styrene (ABS), polycarbonate (PC), thermoset, PBI-PEEK, urea, epoxies, polyurethanes, or any combination thereof. In some embodiments, the plastic is a polyethylene. In particular embodiments, the plastic is a high-density polyethylene.

[0075] In one embodiment, the gate electrode 144 includes a conductive material such as titanium aluminum. In one embodiment, the gate electrode includes TiAh. The thickness of the TiAh is between 80 nm and 100 nm, though other thicknesses can be used without departing from the scope of the present disclosure. The TiAh can have an amorphous structure.

[0076] In one embodiment, the thin-film transistor includes a gate insulator 146 corresponding to a thin-film insulator formed by the process described in relation to forgoing Figures. In one embodiment, the gate insulator 146 includes hafnium oxide. The gate insulator 146 can include AI2O3, though other materials can be utilized without departing from the scope of the present disclosure. The gate insulator 146 can have a thickness between 10 nm and 20 nm, though other thicknesses can be utilized without departing from the scope of the present disclosure.

[0077] The thin-film transistor 140 includes a source electrode 146 and drain electrode 148 on the thin-film insulator 146. The source electrode 146 and the drain electrode 148 can include a metal such as copper, aluminum, titanium, tungsten, or other suitable metals.

[0078] In one embodiment, the thin-film transistor 140 includes a semiconductor layer 150. The semiconductor layer 150 can include one or more ofIGZO (compositions of In, Ga, Zn, and O), low temperature poly crystalline silicon (LTPS), amorphous silicon, or other suitable semiconducting materials. In an example in which the gate insulator 146 includes AI2O3 between 10 nm and 20 nm in thickness, the semiconductor material 150 can include IGZO between 30 nm and 50 nm in thickness, formed with a PVD process. In an example in which the gate insulator 146 includes AI2O3 between 5 nm and 15 nm in thickness and the gate electrode 144 includes molybdenum, the semiconductor material 150 can include LTPS between 40 nm and 60 nm in thickness, formed with a PECVD process followed by an ELA process. In an example in which the gate insulator 146 includes AI2O3 between 3 nm and 8 nm in thickness, the semiconductor material 150 can include amorphous silicon between 40 nm and 60 nm in thickness, formed with a PECVD process. In an example in which the gate insulator 146 includes AI2O3 between 5 nm and 15 nm in thickness and the gate electrode 144 includes titanium, the semiconductor material 150 can include IGZO between 15 nm and 25 nm in thickness, formed with a PVD process followed by an ELA process.

[0079] In one embodiment, the thin-film transistor 140 includes a passivation layer 152 on the semiconductor layer 150. The passivation layer 152 can include a dielectric material with a thickness between 50 nm and 500 nm. The passivation layer 152 can include one or more of silicon dioxide, silicon nitride, or other dielectric materials.

[0080] Figure 7 is a flow diagram of a method 700 for forming a thin-film insulator, in accordance with one embodiment. The method 700 can utilize processes, systems, and components described in relation to foregoing figures. At 702, the method 700 includes reactive sputter depositing of electrically insulating films onto a substrate from an elemental target in an atmosphere including a reactive gas. At 704, the method 700 includes poisoning the target, for a predetermined time, during a pre-sputtering sequence and immediately preceding the depositing. At 706, the method 700 includes simultaneously reducing a flow rate of the reactive gas, to a predetermined level, while starting the depositing, such that, a Weibull plot of a cumulative failure F of breakdown voltage (data obtained from capacitor test structures) is linear, and data — expressed inWeibull form — includes a two-parameter fit, with parameters (3 and 17 defined as follows,

[0081] ln(— ln(l - F)) = P ln(V) - pin (p)

[0082] the difference in parameters extracted from Weibull plots for top-injection versus bottom-injection being statistically insignificant.

[0083] Figure 8 is a flow diagram of a method 800 for forming a thin-film insulator, in accordance with one embodiment. The method 800 can utilize processes, systems, and components described in relation to foregoing figures. At 802, the method 800 includes poisoning a target within a sputtering chamber during a startup phase of a sputtering process by flowing a reactive gas into the chamber with a first flow rate while a shutter is closed between the target and a substrate. At 804, the method 800 includes initiating a deposition phase of the sputtering process by opening the shutter at 806, the method 800 includes flowing the reactive gas into the chamber at a second flow rate lower than the first flow rate during the deposition phase. At 808, the method 800 includes depositing a dielectric layer on the substrate during the deposition phase.

[0084] These and other changes can be made to the embodiments in light of the above-detailed description. In general, in the following claims, the terms used should not be construed to limit the claims to the specific embodiments disclosed in the specification and the claims, but should be construed to include all possible embodiments along with the full scope of equivalents to which such claims are entitled. Accordingly, the claims are not limited by the disclosure.

Claims

CLAIMS1. A method, comprising:poisoning a target within a sputtering chamber during a startup phase of a sputtering process by flowing a reactive gas into the chamber with a first flow rate while a shutter is closed between the target and a substrate;initiating a deposition phase of the sputtering process by opening the shutter;flowing the reactive gas into the chamber at a second flow rate lower than the first flow rate during the deposition phase; anddepositing a dielectric layer on the substrate during the deposition phase.

2. The method of claim 1, further comprising decreasing a voltage of the target by initiating the flow of the reactive gas at the first flow rate during the startup phase.

3. The method of claim 2, further comprising increasing the voltage of the target by reducing the flow of the reactive gas to the second flow rate during the deposition phase.

4. The method of claim 3, wherein the voltage is higher prior to initiating the flow of the reactive gas at the first flow rate during the startup phase than during the deposition phase.

5. The method of claim 1, wherein the reactive gas includes oxygen.

6. The method of claim 5, wherein the target is aluminum.

7. The method of claim 1, wherein the reactive sputtering chamber is a pulsed DC sputtering chamber.

8. The method of claim 1, further comprising forming a thin-film transistor on the substrate, wherein the dielectric layer is part of the thin-film transistor.

9. The method of claim 1, further comprising forming a tunneling device on the substrate, wherein the dielectric layer is part of the tunneling device.

10. The method of claim 1, further comprising performing a precleaning process prior to poisoning the target.

11. A method, comprising:applying a bias to a substrate in a reactive sputtering chamber during a sputtering process;during a first portion of a startup phase of the sputtering process while a shutter between a target and the substrate is closed, increasing a voltage of a target above a deposition voltage level while a flow rate of a reactive gas into the chamber is approximately zero;during a second portion of the startup phase while the shutter is closed:flowing the reactive gas into the chamber; andreducing the voltage of the target below the deposition level; during a deposition phase of the sputtering process after the second portion of the startup phase:opening the shutter;decreasing a flow rate of the reactive gas to a deposition flow rate level;increasing the voltage of the target to the deposition voltage level; anddepositing a dielectric film on the substrate.

12. The method of claim 11, wherein the reactive gas includes oxygen.

13. The method of claim 12, wherein the target is aluminum.

14. The method of claim 11, wherein the reactive sputtering chamber is a pulsed DC sputtering chamber.

15. The method of claim 11, further comprising forming a thin-film transistor on the substrate, wherein the dielectric layer is part of the thin-film transistor.

16. The method of claim 11, further comprising forming a tunneling device on the substrate, wherein the dielectric layer is part of the tunneling device.

17. The method of claim 11, maintaining a pressure within the chamber at a constant level during the second portion of the startup phase and the deposition phase.

18. The method of claim 11, further comprising opening the shutter and decreasing the flow rate of the reactive gas substantially simultaneously at a beginning of the deposition phase.

19. The method of claim 11, wherein the second portion of the startup phase includes poisoning the target.

20. A system, comprising:one or more computer memories storing software instructions;one or more processors configured to execute the software instructions to perform a sputtering process, the sputtering process including:poisoning a target within a sputtering chamber during a startup phase of the sputtering process by flowing a reactive gas into the chamber with a first flow rate while a shutter is closed between the target and a substrate;initiating a deposition phase of the sputtering process by opening the shutter;flowing the reactive gas into the chamber at a second flow rate lower than the first flow rate during the deposition phase; anddepositing a dielectric layer on the substrate during the deposition phase.

21. The system of claim 20, wherein the process includes decreasing a voltage applied to the target upon initiating the flow of the reactive gas at the first flow rate during the startup phase.

22. The system of claim 21, wherein the process includes increasing the voltage applied to the target upon reducing the flow of the reactive gas to the second flow rate during the deposition phase.

23. The system of claim 22, wherein the voltage is higher prior to initiating the flow of the reactive gas at the first flow rate during the startup phase than during the deposition phase.