Method to purify contaminated pulp compositions
The solvent extraction method addresses contamination in pulp and pulp compositions by reducing chemical contaminants to low levels, enhancing their suitability for demanding applications.
Patent Information
- Application Number
- PCT/US2026/025965
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
The recycling of pulp and pulp compositions is limited due to contamination, which reduces their value and mechanical properties, and there is a need for methods to remove chemical contaminants to levels suitable for demanding applications like food and medical uses.
A method involving solvent extraction at controlled temperatures and pressures to reduce individual chemical contaminants in pulp and pulp compositions by at least 75% or to the limit of quantification (LOQ), using a solvent-to-pulp ratio less than 100:1 and pressures between 0.5 atm and 1000 atm.
The method effectively reduces chemical contaminants in pulp and pulp compositions to low levels, enabling their use in demanding applications while maintaining mechanical integrity.
Smart Images

Figure IMGF000011_0001_TABLE 
Figure IMGF000028_0001_TABLE 
Figure IMGF000031_0001_TABLE
Abstract
Description
[0001] METHOD TO PURIFY CONTAMINATED PULP COMPOSITIONS
[0002] FIELD OF THE INVENTION
[0003] The present invention generally relates to a method to purify contaminated pulp compositions.
[0004] BACKGROUND OF THE INVENTION
[0005] In the world today, hundreds of millions of tons of pulp are utilized on an annual basis. The pulps are generally produced from renewable resources. However, the utilization of virgin pulp may deplete natural resources and be a negative on energy, water, land use, etc., and increase production of greenhouse gases (GHG), primarily CO2, in the atmosphere.
[0006] Polysaccharides in fiber form are the basis of most pulps and include wood, cotton, rayon, etc. The use of recycled pulp has emerged as one solution to mitigate the issues associated with the end-of-life of virgin polysaccharides. Recovering and re-using pulp diverts waste from landfills and reduces the demand for virgin materials.
[0007] Pulps may be used to produce various forms of paper, cardboards, etc. that also contain other additives such as fillers, binders, pigments, etc. to form a pulp composition. The pulp and / or pulp composition may be reclaimed as one of many forms and recycled into one of many forms including paper, cardboards, etc.
[0008] Today, in the US, the majority of reclaimed materials destined for recycling, including paper, cardboard, etc., are mixed into a single stream which is collected and processed by a material recovery facility (MRF). At the MRF, materials are sorted, washed, and packaged (e.g., in bales) for resale. Pulp-based materials can be sorted into individual materials.
[0009] However, the utilization of reclaimed pulp and reclaimed pulp compositions in recycling is currently limited due to contamination, which renders these less valuable compared to virgin pulp. A key enabler to increase the recycle rates and lowering the CO2 emissions is to reduce the contamination of recycled pulp and recycled pulp compositions to a level allowing broader utilization across more end markets, especially those involving demanding applications. Contamination potentially impacts macroscopic end-use performance such as reduction in mechanical properties such as strength (i.e., tensile, burst, tear, etc.), elongation, absorbency, and impact and increased malodor and non-optimal color.
[0010] While contamination is problematic for all end market applications, demanding applications such as foods, hygiene, medical, etc., have even stricter requirements, especially on certain chemical contaminants or trace chemicals. The relevant chemical contaminants may begrouped into various chemical classes depending on the chemical structure of the contaminants. Non-limiting examples of these chemical classes of contaminants are PF As, heavy metals, pesticides, dioxins, furans, polychlorinated biphenyls (PCBs), phthalates, polycyclic aromatic hydrocarbons (PAHs), organotins, bisphenols, isothiazolins, glyphosphate, alkyl phenols, alkylphenol ethoxylates, aromatic amines, and flame retardants. In addition, the target levels of these contaminants can be extremely low, thus representing trace chemical contaminants. For instance, the target levels may be on the order of parts per million (ppm), parts per billion (ppb), and parts per trillion (pptr), wherein the initial contaminated material may contain levels 1,000 times the targeted levels. Net, a l,000X reduction in chemical contamination is often required.
[0011] While the recycling of pulp and pulp compositions through various cleaning processes is known, there remains a need for recycled pulp and recycled pulp compositions and compositions comprising recycled pulp and recycled pulp compositions, that have minimum numbers and levels of contaminants, especially trace chemical contaminants, and that also have the necessary mechanical integrity of the pulp fibers that allow them to be used in various ways. Beyond recycled pulp and recycled pulp compositions, there is a possibility that certain specific sources of virgin pulp may contain undesirable contamination, especially trace chemical contaminants, and there is a need to remove this contamination prior to production of the final product or package.
[0012] Net, there is an unmet need for a method to remove various forms of contamination, especially chemical contamination, from all forms of pulp and pulp compositions, including reclaimed pulp and reclaimed pulp compositions used for recycling, including blends with virgin pulp and other reclaimed pulp and reclaimed pulp compositions.
[0013] SUMMARY OF THE INVENTION
[0014] Disclosed herein is a method to remove contaminants from a contaminated pulp or contaminated pulp composition to produce a purer pulp or purer pulp composition comprising:
[0015] i. providing a contaminated pulp or contaminated pulp composition comprising an individual contaminant or contaminants, each individual contaminant having a concentration;
[0016] ii. extracting said individual contaminant or contaminants from said contaminated pulp or contaminated pulp composition at a temperature and a pressure, using a solvent, in extraction stages, for a period of time and for a period of time per stage, to produce a purer pulp or pulp composition comprising an individual contaminant or contaminants, each having a concentration;wherein said extraction stages are conducted at a solvent to contaminated pulp or contaminated pulp composition mass ratio; wherein said solvent to contaminated pulp or contaminated pulp composition mass ratio per stage at any time is less than about 100:1; wherein said pressure is between about 0.5 atm and 1,000 atm absolute pressures; wherein said individual contaminants comprise at least one of glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene above LOQ; wherein at least one of the individual contaminants concentration in said purer pulp or pulp composition is reduced compared to each individual contaminants concentration in said contaminated pulp or contaminated pulp composition by at least about 75% or LOQ.
[0017] DETAILED DESCRIPTION OF THE INVENTION
[0018] I. Definitions
[0019] As used herein, the term “pulp” refers to a fibrous composition comprising polysaccharides that include materials originating from but not limited to wood (both hard and soft woods), cotton, rayon, lyocell, trichomes, seed hairs, and bagasse. Wood pulp refers to pulp originating from a wood source.
[0020] As used herein, the term “pulp fiber” refers to the individual fibers that make-up the actual pulp. These fibers may be characterized by a range of geometric parameters including various diameters, lengths, and degree of entanglements and various polysaccharide chemistries.
[0021] As used herein, the term “pulp composition” along with other potential qualifiers refers to the combination of pulp or various pulps, various lignins, ashes, and various functional and nonfunctional additives that create the functional product or package. For example, paper is a pulp composition that potentially includes pulp and other functional and non-functional additives. For example, a recycled pulp composition may be a composition containing at least one recycled pulp but potentially has more than one recycled pulp and may contain virgin pulp along with other additives all at various concentrations.
[0022] As used herein, the term “paper” refers to a pulp composition including pulp or many different pulps and potentially functional and non-functional additives wherein the geometric form is somewhat flat and relatively consistent. The paper may contain additional additives such as but not limited to binders and pigments. Paper may be further processed into other forms such as butnot limited to board, corrugated board, etc. Paper is typically sourced from wood pulp but cotton pulp papers are also known.
[0023] As used herein, the term “Fibrous structure” refers to a structure that comprises one or more fibrous filaments and / or fibers. In one example, a fibrous structure according to the present invention means an orderly arrangement of filaments and / or fibers within a structure in order to perform a function. Non-limiting examples of fibrous structures of the present invention include paper, fabrics (including woven, knitted, and non-woven), and absorbent pads (for example for diapers or feminine hygiene products).
[0024] As used herein, the term “virgin pulp” refers to pulp that has not been used previously to produce a package or product for a targeted end application. For example, virgin wood pulp is pulp that is produced from wood-based sources and has not been used previously in an end application.
[0025] As used herein, the term “non-virgin pulp” refers to pulp that has been used previously to produce a package or product for a targeted end application. For example, non-virgin wood pulp is pulp that is produced from wood-based sources and has not been used previously in an end application.
[0026] As used herein, the term “reclaimed pulp” refers to non-virgin pulp that has been collected for potential use in an end market. For example, reclaimed wood pulp is pulp that was originally virgin wood pulp but has already been used for an intended purpose such as paper in a 1st, 2nd, 3rd, etc. life. The reclaimed pulp may contain recycled pulp from a previous life cycle.
[0027] As used herein, the term “recycled pulp” refers to reclaimed pulp that has been converted into a usable material with established end markets such as packaging. The recycled pulp may be purer than the reclaimed pulp fiber or may be identical except possibly in form. For example, recycled wood pulp is pulp that was reclaimed pulp and then rendered usable in the intended end market. Expanding further, recycled paper is sourced from reclaimed paper that is rendered acceptable for re-use as paper. The difference between recycled and reclaimed pulp is subtle. In cases wherein the reclaimed pulp can be used as-is in an end market, then the terms reclaimed and recycled pulp may be interchangeable.
[0028] As used herein, the terms “pre-consumer reclaimed pulp and pre-consumer reclaimed pulp compositions” follow the ISO 5270 definition, that is, a descriptive term covering material diverted during a manufacturing process. This term excludes re-utilized material, such as rework, regrind or scrap that has been generated in a given process and is capable of being reclaimed within that same process. The term “post-industrial reclaimed pulp and pulp compositions” is sometimes used synonymously with “pre-consumer reclaimed pulp and pulp compositions”. The terms “pre-consumer” reclaimed pulp and “pre-consumer” recycled pulp compositions follow from the aforementioned definitions. For example, pre-consumer recycled pulp compositions are produced from pre-consumer reclaimed pulp compositions that have been rendered acceptable for use in the targeted end market.
[0029] As used herein, “post-consumer reclaimed pulp and pulp compositions” follows the ISO 5270 definition, that is, a descriptive term covering material, generated by the end-users of packages / products, that has fulfilled its intended purpose or can no longer be used (including material returned from within the distribution chain). The term “post-use” is sometimes used synonymously. The terms “post-consumer recycled pulp and post-consumer recycled pulp compositions” follow from the aforementioned definitions. For example, post-consumer recycled pulp compositions are produced from post-consumer reclaimed pulp compositions that have been rendered acceptable for use in a targeted end market.
[0030] As used herein, the term “1stLife” refers to the first market use of a virgin material. “2ndLife” refers to the second use of the pulp or pulp composition in market. “3rd, 4th, etc. Life” refers to the number of times the pulp composition has been used in market past the initial use as a virgin composition.
[0031] As used herein, the term “contaminant” refers to any undesirable material contained on, between, or within the pulp fibers or pulp composition. The term “chemical contaminant” refers to any specific chemical or group of chemicals associated with a contaminant. As used herein, the term “contamination” refers to the sum of all contaminants and the term “chemical contamination” refers to the sum of all chemical contaminants. The chemical contaminants may be grouped in classes, which include chemical contaminants that have similar chemical structure. For example, As, Hg, and Cr are non-limiting chemical contaminants in the “heavy metals” classification. Each contaminant may have different chemical attributes, such as solubility and diffusivity in the pulp composition, and target levels depending upon concentration and end use market.
[0032] The term “trace chemical contaminant” or “trace contaminants” refers to a chemical contaminant that is concerning at low levels of detection typically represented by 100s of ppm, ppb, and pptr levels.
[0033] As used herein, the term “surface contaminant” refers to a contaminant that is on the surface of the pulp fiber that resides inside the pulp and is part of the broader pulp composition. Similarly, the term “surface chemical contaminant” refers to the molecular or elemental composition of the surface contaminant. The surface contaminant may be attached to the surface of the pulp fiber either loosely through physical attraction forces, or more strongly through polar or other forces. Ingeneral, a surface contaminant will have less than about 80% of its surface area embedded in the pulp fiber.
[0034] As used herein, the term “bulk contaminant” refers to a contaminant that is in the bulk of the pulp fibers as opposed to resting on the surface or between the pulp fibers. Similarly, the term “bulk chemical contaminant” refers to the molecular or elemental composition of the bulk contaminant. As used herein, a bulk contaminant will have more than about 95% of its surface area embedded in the pulp fiber.
[0035] As used herein, the term “surface contamination” and “surface chemical contamination” refers to the sum of all surface contaminants and all surface chemical contaminants, respectively.
[0036] As used herein, the term “bulk contamination” and “bulk chemical contamination” refers to the sum of all bulk contaminants and all bulk chemical contaminants, respectively.
[0037] As used herein, the term “total contamination” refers to the sum of the surface contamination and bulk contamination and the sum of all the surface chemical contamination and bulk chemical contamination, respectively.
[0038] As used herein, the term “permeable contaminant” refers to a chemical contaminant that is both soluble and diffusible in the pulp fiber.
[0039] As used herein, the term “impermeable contaminant” refers to a chemical contaminant that is either insoluble or non-diffusible or both in the pulp fiber.
[0040] As used herein, the term “permeable contamination” is the sum of all permeable contaminants and the term “impermeable contamination” is the sum of all impermeable contaminants. The sum of all permeable and impermeable contamination is the “chemical contamination” if described in molecular or elemental terms or just simply “the contamination” if described in general terms.
[0041] As used herein, the term “intentional contaminant” refers to a contaminant that is intentionally added by the supply chain for a specific purpose to benefit the producer, retailer, or consumer, but may not be desired in the reclaimed pulp composition. Examples include print, adhesives for labels, pigments (such as TiCh), process additives (such as antioxidant (AO)), etc., that are necessary for marketing, branding, processability, and / or end use performance. As used herein, the term “intentional chemical contaminant” refers to an intentional contaminant described by its chemical composition. As used herein, the term “intentional contamination” refers to the sum of all intentional contaminants and the term “intentional chemical contamination” refers to the intentional contamination described by its chemical composition.As used herein, the term “unintentional contaminant” refers to any contaminant not intentionally added. Examples include dirt and cross-contamination that is not intentionally added by the producer, retailer, or consumer. As used herein, the term “unintentional chemical contaminant” refers to an unintentional contaminant described by its chemical composition. As used herein, the term “unintentional contamination” refers to the sum of all unintentional contaminants and the term “unintentional chemical contamination” refers to the unintentional contamination described by its chemical composition.
[0042] As used herein, the term “degradation point” refers to the temperature at which the pulp begins to substantially degrade. The degradation may be determined through endothermic or exothermic processes.
[0043] As used herein, the term “limit of quantification” or “LOQ” refers to the lower detection limit for a given chemical contaminant as determined by the analytical methods disclosed in section IX. The LOQ is a function of the methods used and may vary from test method to test method. The LOQ used herein is specific to the method listed in section IX.
[0044] As used herein, the term “ppm” refers to mass parts per million, “ppb” refers to mass parts per billion, and “pptr” refers to mass parts per trillion.
[0045] As used herein, the term “contaminated pulp” or “contaminated pulp composition” refers to the pulp or pulp composition that is contaminated and is fed to the method of the current invention.
[0046] As used herein, the term “purer pulp” or “purer pulp composition” refers to the pulp or pulp composition that is reduced in contamination via the method of the current invention.
[0047] As used herein, the “Basis Weight” is the weight per unit area of a sample reported in lbs / 3000 ft2or g / m2and is measured according to the Basis Weight Test Method described herein.
[0048] As used herein, the “Machine Direction” or “MD” means the direction parallel to the flow of The fibrous structure through the fibrous structure making machine and / or sanitary tissue product manufacturing equipment. “Cross Machine Direction” or “CD” as used herein means the direction parallel to the width of the fibrous structure making machine and / or sanitary tissue product manufacturing equipment and perpendicular to the machine direction.
[0049] As used herein, a “Ply” means an individual, integral fibrous structure. “Plies” as used herein means two or more individual, integral fibrous structures disposed in a substantially contiguous, face-to-face relationship with one another, forming a multi-ply fibrous structure and / or multi-ply sanitary tissue product. It is also contemplated that an individual, integral fibrous structure can effectively form a multi-ply fibrous structure, for example, by being folded on itself.II. Contaminated Pulp or Contaminated Pulp Compositions
[0050] The contaminated pulp or pulp compositions of the present invention may comprise virgin pulp, virgin pulp compositions, reclaimed pulp, reclaimed pulp compositions, recycled pulp, recycled pulp compositions, and blends thereof. The reclaimed pulp or reclaimed pulp compositions may contain post-consumer reclaimed pulp or pulp compositions. The reclaimed pulp or pulp compositions may contain pre-consumer reclaimed pulp or pulp compositions. The reclaimed pulp or pulp compositions may contain blends of the aforementioned pulps.
[0051] While use of recycled pulp and recycled pulp compositions are known, the present inventive method removes contamination to a greater extent than the known methods of the prior art. Detailed herein are the types of materials that may have numerous and high levels of contaminants and methods of purifying such materials.
[0052] During pulp’s or pulp’s composition lifecycle (from production through distribution, consumer utilization, and eventual reclaiming) contamination is introduced either intentionally or unintentionally. Non-limiting examples of intentional contamination include surface print, labels, adhesives, barrier plastics like polyethylene or polypropylene or waxes, binders, pigments (such as TiCh), fillers (such as CaCO3), process additives (such as antioxidant (AO), PF As such as FEP), etc. that are necessary for marketing, branding, processability, and / or end use performance. Nonlimiting examples of unintentional contamination are dirt, cross-contamination, certain heavy metals, pesticides, dioxins, furans, PCBs, PFAs such as PFOA, etc. Also, unintentional contamination can be produced from reactions involving intentional contaminants, such as the oxidation of pulp fibers to dioxins, degradation of adhesives or print binders, etc. Further, oxidation of the pulp fiber during reclaiming will produce unintentional contamination. In addition, unintentional contamination may result from interaction with products. For example, packaging materials that contain cleaning mixtures (e.g., limonene, surfactants, etc.,), food (e.g., various organics), etc., will potentially become contaminated with such products. Finally, unintentional contamination can enter the pulp fiber during production, e.g., contamination of a pulp fiber with reaction by-products, unreacted monomers, etc. In embodiments of the present invention, the method reduces the contamination within the virgin pulp or pulp compositions to much lower levels.
[0053] Pre-consumer reclaimed pulps or pulp compositions generally have the lowest level of contamination due to its known composition and controlled history. It may include intentional contamination but because these are known and controlled, it is quite easy to find applicationstolerating such known contaminants. In addition, pre-consumer reclaimed pulp tends to have low amounts of unintentional contamination due to the controlled history preventing external contamination.
[0054] Post-consumer reclaimed pulps or pulp compositions are generally more contaminated than pre-consumer reclaimed pulps or pulp compositions due to extensive cross-contamination from unknown sources resulting in high levels of unintentional contamination.
[0055] Surprisingly, recycled pulp from the present invention may allow the use of reclaimed pulp or pulp compositions from pre-consumer and post-consumer sources as recycled pulp or pulp composition in applications requiring low chemical contamination such as medical and hygiene. In addition, most recycled pulp or pulp composition customers desire purer materials beyond what is available today and the recycled pulp or recycled pulp compositions (and the associated packages and products containing these) of the present invention meets this requirement.
[0056] The reclaimed pulp or pulp compositions may be in many macroscopic forms including but not limited to sheets, boards, rolls, etc.
[0057] The reclaimed pulp or pulp compositions can be a second-life pulp or pulp compositions (has been used only once before it entered the reclaimed pulp stream), third-life pulp or pulp compositions (has been used twice before it entered the reclaimed pulp stream), or higher-life pulp fiber or pulp compositions (has been used many times before it entered the reclaimed pulp stream).
[0058] The reclaimed pulp or pulp compositions may comprise a regrind or edge-trim or in-plant waste pulp fiber or a post-industrial reclaimed pulp or pulp compositions. The reclaimed pulp or pulp compositions may comprise a post-industrial sheet or board.
[0059] The reclaimed pulp or pulp compositions may comprise starch including but not limited to starches from various plants and chemically modified starches. The reclaimed pulp or pulp compositions may comprise polysaccharides, polylactic acid, polyhydroxyalkanoate, or chitin.
[0060] III. Purer Pulp or Purer Pulp Compositions
[0061] Purer pulps or pulp compositions result from the method of the present invention being applied to contaminated pulp or pulp compositions. In some embodiments, the purer pulp or pulp compositions comprise post-consumer recycled pulp or pulp compositions; in other embodiments these comprise post-industrial recycled pulp or pulp compositions and in still other embodiments, the purer materials may be a combination of post-consumer and post-industrial recycled pulp or pulp compositions. The purer pulps may also contain virgin pulp or virgin pulp compositions.The inventive method may be characterized by high levels of contaminant removal including the prevention of homification of the pulp fibers and the maintenance or increase in mechanical properties of the pulp or pulp composition.
[0062] Furthermore, the pulp or pulp compositions may be incorporated into various consumer products and package materials that require low levels of chemical contamination. For example, these purer pulps or pulp compositions may be used in sanitary tissue products and inventive packages with low numbers and low levels of contaminants while still exhibiting consumer-expected tactile feel and overall high performance.
[0063] IV. Contaminants and Contamination
[0064] The chemical contaminants in the contaminated pulp or contaminated pulp composition may be numerous and fall into various chemical classes. These chemical classes may be benign while others may be more problematic. The chemical contaminants of importance herein include but are not limited to pesticides, aldehydes, allergic fragrances, izioalines, alkylphenol ethoxylates, alkylphenols, bisphenols, dioxins, dioxin-like, furans, PCBs, organotins, metals, phthalates, polyaromatic hydrocarbons (PAHs), and PF As (including but not limited to polymeric PF As). The concentration of these chemical contaminants are typically in the ppm, ppb, and pptr type of levels. The analytical methods used to measure these contaminants have lower sensitivity limits. These limits are referred to as Limit of Quantification (LOQ). The LOQ may not be stagnant with time as analytical techniques are improved.
[0065] Using the analytical methods disclosed in section IX Methods, the LOQs of the various contaminants may differ by orders of magnitude. For example, the current LOQ of a typical pesticide may be about 10 ppb; the current LOQ of typical alkylphenol ethoxylate may be about 50 ppb; the current LOQ of a typical alkylphenol may be about 5 ppb; the current LOQ of bisphenol-A may be about 5 ppb; the current LOQ of typical dioxin may be about 0.2 pptr; the current LOQ of a typical furan may be about 0.2 pptr; the current LOQ of a typical PCB may be about 5 pptr; the current LOQ of a typical heavy metal may be about 100 ppb; the current LOQ of a typical organotin may be about 300 pptr; the current LOQ of typical phthalate may be about 50 ppb; the current LOQ of a typical PAH may be about 1 ppb.
[0066] Several wood pulp-based papers (a pulp composition) including two containing only virgin pulp and one containing post-consumer reclaimed pulp, were broadly classified for chemical contamination using the analytical methods disclosed in section IX Methods, as shown in TABLE 1. Note: To simplify the presentation of chemical contamination results, the concentration data isdisplayed in terms of multiples of LOQ instead of absolute weight fraction involving ppm, ppb, or pptr description. The current LOQ for the method used is shown in TABLE 1. For example, if the contaminant concentration is 10 ppm and the LOQ is 1 ppm, then the concentration would be 10 X LOQ or just 10 displayed in the data tables.
[0067] TABLE 1
[0068] Chemical Contamination of Wood Pulp Based Papers
[0069] Reclaimed Post- Virgin
[0070] Consumer
[0071] #1 #2 #1
[0072] LOQ xLOQ xLOQ xLOQ
[0073] Pesticides
[0074] Diethyltoluamide (DEET) 10 ppb <1 <1 28.0 Glyphosate 10 ppb <1 <1 12.0 Alkylphenol ethoxylates
[0075] iso-Nonylphenolmonoethoxylate 50 ppb <1 <1 4.0
[0076] iso-Nonylphenoldiethoxylate 50 ppb <1 <1 6.2
[0077] iso-Nonylphenoltriethoxylate 50 ppb <1 <1 7.0
[0078] iso-Nonylphenoltetraethoxylate 50 ppb <1 <1 3.4
[0079] Bisphenols
[0080] Bisphenol A 5 ppb <1 <1 32.0
[0081] Dioxins and dioxinlike and PCB
[0082] 1,2,3,4,6,7,8-HpCDD 0.2 pptr <1 <1 145.5
[0083] OCDD 0.2 pptr <1 <1 1355.0
[0084] OCDF 0.2 pptr <1 <1 43.8
[0085] PCB 81 0.05 pptr <1 <1 87.8
[0086] PCB 105 5 pptr <1 <1 73.2
[0087] PCB 118 10 pptr <1 <1 68.9 Phthalates
[0088] Di-2-ethylhexyl phthalate 50 ppb <1 <1 134.0 Diisononyl phthalate 50 ppb <1 <1 100.0
[0089] PAHs
[0090] Fluoranthene 1 ppb <1 <1 17.0
[0091]
[0092] Phenanthrene I ppb 1.7 <1 13.0
[0093] As shown in the previous table, chemical contaminants of the types previously mentioned were generally not found in the papers sourced from virgin pulp compositions, which is likely representative of the broader virgin papers available today. However, high levels of the relevant chemical contaminants were found in the paper from reclaimed post-consumer pulp, again likely indicative of the broader reclaimed paper sources available today. For example, up to -1000 X LOQ was determined for OCDD and -100 X LOQ for the phthalates.In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least one chemical contaminant and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0094] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least two chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0095] In embodiments of the present invention, said chemical contaminants in said contaminated pulp or contaminated pulp composition include at least three chemical contaminants and such is selected from the group comprising pesticides, alkyl phenols, alkylphenol ethoxylates, bisphenols, dioxins, furans, PCBs, phthalates, PAHs, PF As, or mixtures thereof.
[0096] In embodiments of the present invention, the pesticides comprise one or more of piperonyl butoxide, BAC, DEET, glyphosphate, and DDAC. In another embodiment of the present invention, the alkylphenol ethoxylates comprise one or more of iso-Nonylphenolmonoethoxylate, iso-Nonylphenoldiethoxylate, iso-Nonylphenoltriethoxylate, and iso-Nonylphenoltetraethoxylate. In yet another embodiment of the present invention, the alkyl phenols comprise one or more of iso-Nonylphenol, 4-tert-butylphenol, and 4-tert-Pentylphenol. In even yet another embodiment of the present invention, the bisphenols comprise bisphenol-A. In even yet another embodiment of the present invention, the dioxins comprise one or more of 1,2, 3,6,7, 8-HxCDD, 1.2.3.4.6.7.8-HpCDD, and OCDD. In even yet another embodiment of the present invention, the furans comprise OCDF. In even yet another embodiment of the present invention, the PCBs comprise one or more of PCB 77, PCB 81, PCB 126, PCB 105, PCB 114, PCB 118, PCB 123, PCB 156, and PCB 167. In event yet another embodiment of the present invention, the phthalates comprise one or more of di-2-propylheptyl phthalate, disobutyl phthalate, dibutyl phthalate, di- 1 -ethylhexyl phthalate, and diisononyl phthalate. In even yet another embodiment of the present invention, the PAHs comprise one or more of acenaphthene, acenaphthylene, anthracene, benzo[a]anthracene, benzo[b]fluoroanthene, benzo[e]pyrene, benzo[g.h.i]perylene, chrysene, cyclopenta[c.d]pyrene, flyoroanthene, fluorene, naphthalene, phenanthrene, and pyrene. In even yet another embodiment of the present invention, the organotins comprise one or more of monobutylin, dibutyltin, and dioctylin. In even yet another embodiment of the present invention, the PF As comprise one or more of Perfluorooctanoic acid and Perfluorooctane sulfonic acid.In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise glyphosphate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenolmonoethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoldiethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltriethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise iso-Nonylphenoltetraethoxylate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise Bisphenol A. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDD. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise OCDF. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 81. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 105. In embodiments of the present invention, the contaminants in contaminated pulp or contaminated pulp composition may comprise PCB 118. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-2-ethylhexyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise di-isononyl phthalate. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise fluoranthene. In embodiments of the present invention, the contaminants in the contaminated pulp or contaminated pulp composition may comprise phenanthrene.
[0097] In general, the efficacy of the cleaning method of the present invention to remove a specific chemical contaminant is determined by the removal efficiency, defined as the difference in concentration of the chemical contaminant in the contaminated pulp or contaminated pulp composition and the concentration of the chemical contaminant in the purer pulp or purer pulp composition divided by the concentration of the chemical contaminant in contaminated pulp or contaminated pulp composition. However, the removal efficiency is somewhat insufficient due to the inability to determine any actual concentrations below the LOQ. For example, if a cleaning process reduces the contamination from 2 X LOQ to less than the LOQ, then the true removalefficiency could range anywhere between 50% and 100%, which is a significant difference. Thus, the removal efficiency is only completely accurate when the contaminated pulp or contaminated pulp composition and the purer pulp or purer pulp composition concentration are both above LOQ. For simplicity, if the purer pulp or purer pulp composition has a chemical contaminant concentration below LOQ, then removal efficiency is calculated by assuming the chemical contaminant concentration of the purer pulp or purer pulp composition is at the LOQ and the removal efficiency is considered a minimum value and designated with >. For the above example, the removal efficiency would be calculated as 100(2 X LOQ - 1 X LOQ) / (2 X LOQ) = 100(2- 1) / 2 = 50%. Thus, the removal efficiency would be listed as > 50%. In certain cases, the purer pulp or purer pulp composition will have a higher level of a certain chemical contaminant than the initial contaminated pulp or contaminated pulp composition which contradicts the meaning of purer. This anomaly may be due to 1) measurement error or measurement variability, 2) contaminant hot spots and cold spots in the contaminated pulp or pulp composition, 3) external contamination during sampling, and 4) the purification process adds that specific contaminant. If this anomaly occurs consistently for a given chemical species for a given cleaning process, then such is more likely attributable to the purification process and should be more closely examined, but such was not generally the case for the cleaning processes of the present invention. Net, such isolated measurement anomalies were considered measurement error and not considered meaningful to the invention. In such cases, the removal efficiency is set to 0%.
[0098] In one embodiment, the removal efficiency of the DEET contaminant is > 70% wherein said DEET concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the DEET contaminant is > 85% wherein said DEET concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per billion.
[0099] In one embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 50% wherein said glyphosphate concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per billion. In another embodiment of the present invention, the removal efficiency of the glyphosphate contaminant is > 90% wherein said glyphosphate concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per billion.
[0100] In one embodiment of the present invention, the removal efficiency of the isononylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate contaminant are all > 50% wherein said iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and isononylphenoltetraethoxylate concentration in the contaminated pulp or contaminated pulp composition is at least 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate contaminant are all > 70% wherein said iso-nonylphenolmonoethoxylate, iso-nonylphenoldiethoxylate, iso-nonylphenoltriethoxylate, and iso-nonylphenoltetraethoxylate concentration in the contaminated pulp or contaminated pulp composition is at least 50 parts per billion.
[0101] In one embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 50% wherein said Bisphenol-A concentration in the contaminated pulp or contaminated pulp composition is at least 5 parts per billion. In another embodiment of the present invention, the removal efficiency of the Bisphenol-A contaminant is > 95% wherein said Bisphenol-A concentration in the contaminated pulp or contaminated pulp composition is at least 5 parts per billion.
[0102] In one embodiment of the present invention, the removal efficiency of the 1, 2, 3, 4, 6,7,8-HpCDD contaminant is > 50% wherein said 1,2,3,4,6,7,8-HpCDD concentration in the contaminated pulp or contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the 1,2,3,4,6,7,8-HpCDD contaminant is > 85% wherein said 1,2,3,4,6,7,8-HpCDD concentration in the contaminated pulp or contaminated pulp composition is at least 0.2 parts per trillion.
[0103] In one embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 50% wherein said OCDD concentration in the contaminated pulp or contaminated pulp composition is at least 0.2 parts per trillion. In another embodiment of the present invention, the removal efficiency of the OCDD contaminant is > 85% wherein said OCDD concentration in the contaminated pulp or contaminated pulp composition is at least 0.2 parts per trillion.
[0104] In one embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 50% wherein said PCB 81 concentration in the contaminated pulp or contaminated pulp composition is at least 0.05 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 81 contaminant is > 85% wherein said PCB 81 concentration in the contaminated pulp or contaminated pulp composition is at least 0.05 parts per trillion.
[0105] In one embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 50% wherein said PCB 105 concentration in the contaminated pulp orcontaminated pulp composition is at least 5 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 105 contaminant is > 85% wherein said PCB 105 concentration in the contaminated pulp or contaminated pulp composition is at least 5 parts per trillion.
[0106] In one embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 50% wherein said PCB 118 concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per trillion. In another embodiment of the present invention, the removal efficiency of the PCB 118 contaminant is > 85% wherein said PCB 118 concentration in the contaminated pulp or contaminated pulp composition is at least 10 parts per trillion.
[0107] In embodiments of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 50% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp or contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-2-ethylhexyl phthalate contaminant is > 85% wherein said Di-2-ethylhexyl phthalate concentration in the contaminated pulp or contaminated pulp composition is at least about 50 parts per billion.
[0108] In embodiments of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 50% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp or contaminated pulp composition is at least about 50 parts per billion. In another embodiment of the present invention, the removal efficiency of the Di-isononyl phthalate contaminant is > 85% wherein said Di-isononyl phthalate contaminant concentration in the contaminated pulp or contaminated pulp composition is at least about 50 parts per billion.
[0109] In embodiments of the present invention, the removal efficiency of the fluoranthene contaminant is > 50% wherein said fluoranthene concentration in the contaminated pulp or contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the fluoranthene contaminant is > 85% wherein said fluoranthene concentration in the contaminated pulp or contaminated pulp composition is at least about 1 parts per billion.
[0110] In embodiments of the present invention, the removal efficiency of the phenanthrene contaminant is > 50% wherein said phenanthrene concentration in the contaminated pulp or contaminated pulp composition is at least about 1 parts per billion. In another embodiment of the present invention, the removal efficiency of the phenanthrene contaminant is > 85% wherein saidphenanthrene concentration in the contaminated pulp or contaminated pulp composition is at least about 1 parts per billion.
[0111] In embodiments of the present invention, the removal efficiency of the Perfluorooctanoic acid contaminant is > 50% wherein said Perfluorooctanoic acid concentration in the contaminated pulp or contaminated pulp composition is at least LOQ. In embodiments of the present invention, the removal efficiency of the Perfluorooctane sulfonic acid contaminant is > 50% wherein said Perfluorooctane sulfonic acid concentration in the contaminated pulp or contaminated pulp composition is at least LOQ.
[0112] In general, bulk contamination will not be appreciably removed by simple aqueous surface washing approaches of the prior art. Permeable bulk contamination can be removed by diffusion mechanisms through gradients in chemical potential, whereas bulk impermeable contamination is essentially trapped by the bulk pulp fiber, and methods to free the trapped contaminant dissolution or disintegration of the pulp fiber.
[0113] IV. Pulp Surface Purification Methods
[0114] Surface purification methods reduce surface contamination. This contamination may exist on the surface of the pulp fibers or in-between fibers. One example of a surface purification method may include, but is not limited to, surface washing with a surface washing fluid that is typically water based. The contaminated pulp or contaminated pulp composition will generally be in the form of board, loose or compacted fibers, loose or compacted flexible packages, loose or compacted rigids, loose or compacted non-wovens, etc. which will be difficult to surface wash due to excessive overall size. Hence, prior to surface washing, a granulation or shredding step is preferred. The surface washing will typically include mechanical agitation to loosen surface dirt and other contaminants to allow physical removal and transfer to the washing fluid wherein the dirt or other contaminants may or may not solubilize.
[0115] Surface washing technologies are available extensively on the market for pulp and pulp compositions. However, surface washing technologies involving water-based washing media are typically not effective at removing chemical contamination from pulp or pulp compositions especially those from reclaimed sources because such contamination may not be present on the surface but present in the bulk of the pulp or pulp composition.
[0116] V. Bulk Purification
[0117] In general, bulk contamination will not be appreciably reduced by simple aqueous surface washing discussed previously.One example of a bulk purification process may include, but is not limited to, extraction, which may be a preferred bulk purification method for removing permeable contaminants. Extraction involves the use of a purification solvent to remove bulk permeable contaminants through creation of a chemical potential gradient between the surface of the contaminated pulp fiber or the surface of the contaminated pulp composition and the solvent. The rate of permeable chemical contaminant removal will depend upon the diffusivity and solubility of the contaminant in the pulp fiber under the conditions created in the process. The time required to remove permeable contaminants through diffusion mechanisms can be quite long and not conducive to economically viable processes at commercial scale. Methods to resolve these time scale limitations include 1). increased diffusivity through elevated temperature and / or pulp fiber relaxation through solvent swelling, 2). decrease of diffusion path length through increased surface area to volume ratio of the reclaimed pulp fiber exposed to the solvent, 3) increased convective transport of the contaminant through the pulp fiber / solvent interface by: increased solubility of the contaminant in the solvent, increased partitioning of the contaminant within the solvent relative to the pulp fiber; increased convection around the pulp fiber / solvent interface, and increased solvent sink relative to pulp fiber sink. The solubility of the bulk purification solvent in the pulp fiber can be increased by operating the extraction at high pressures especially at, near, or above the critical pressure. Bulk purification methods may also serve as surface purification methods and vice versa. For example, solvent extraction may be effective at bulk purification due to effective diffusion from the bulk but such solvent may also remove surface contamination consistent with surface purification.
[0118] It is important for the extraction method to be scalable to large volumes at low cost. Hence, the time required for extraction should be low to allow for such scalability. In embodiments of the present invention, the total time for extraction is less than about 6 hours, preferably less than about 4 hours, more preferably less than about 2 hours, and even more preferably less than about 1 hour. If the extraction is completed in stages, then the time per stage may be less than this range but the overall time will still fall within these times.
[0119] Extractions may take place above, near, at, or below the degradation or primary melting point (whichever is lower) of the pulp or pulp composition. Extractions generally occur in a two-phase system involving a solvent-rich phase and a pulp fiber-rich phase. Leaching extractions are a subset of extractions typically involving a liquid state for the solvent-rich phase and a solid state for the pulp fiber-rich phase. Liquid-liquid extractions are a subset of extractions typically involving two liquid states. In an embodiment of the present invention, the extraction is leaching.In leaching processes, the contaminated pulp fiber may be contacted with excessive solvent during every stage and every time of the process. Such leaching processes are called flooded leaching processes. In flooded leaching processes, the mass of leaching solvent to mass of contaminated pulp or contaminated pulp composition exposed to the solvent at every point in time and in every stage of the process is preferably equal to or greater than about 5:1. In certain flooded leaching processes, the solvent is rapidly stirred such that the contaminated pulp or contaminated pulp composition is suspended in the solvent even when the density of the pulp is greater than the solvent. Such flooded leaching processes 1) ensure complete contact between the surface of the reclaimed pulp fiber and the leaching solvent and 2) lower the mass transfer resistance within the solvent boundary layer around the contaminated pulp fiber surface due to the convective motion. Beyond stirring, similar reduced boundary layer may be achieved in flooded leaching processes by allowing the contaminated pulp to settle through the solvent by density gradient. Examples of flooded leaching processes include stirred tanks of the continuous, semi -continuous, and batch types. Additional examples of flooded leaching processes include settling tanks wherein the contaminated pulp is allowed to settle out or through the solvent that is filled inside a tank or other vessel.
[0120] In leaching processes, the solvent may be contacted with excessive contaminated pulp or contaminated pulp composition during every stage and every time of the process. Such leaching processes are called packed leaching processes. In packed leaching processes of the current invention, the mass of leaching solvent to mass of contaminated pulp exposed to the solvent at every point in time and in every stage of the process is preferably equal to or less than about 5:1. In certain packed leaching processes, the solvent is flowed through a packed column or bed of pulp. Such packed leaching processes provide efficient means for removing contaminated solvent and ensuring optimal concentration gradient. Examples of packed leaching include but are not limited due flow through packed beds, percolation extractors, screw-based extractors, Hildebrandt extractors, etc.
[0121] In some embodiments, a purification process may include an extraction that comprises flooded leaching. In embodiments of the present invention, the extraction may comprise packed leaching. In embodiments of the present invention, the extraction comprises a combination of flooded and packed leaching.
[0122] For leaching processes of the current invention, it may be beneficial to select a leaching solvent and operating temperature and pressure such that the leaching solvent is at its boiling point during the extraction. Such designs allow the solvent to be continuously refluxed, which mayenable locally high concentration gradients as the refluxed solvent contacts the reclaimed pulp fiber. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the bulk purification is above atmospheric. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the bulk purification is about atmospheric. In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the bulk purification is below atmospheric (i.e., under vacuum). In embodiments of the present invention, the bulk extraction is either packed or flooded leaching or combinations of both, and the pressure of the leaching is about atmospheric, and the leaching solvent is at or near the normal boiling point. For wood-based pulp or pulp compositions, preferred leaching solvents for flooded leaching have boiling points in the 2°C to 90°C range. Nonlimiting examples of such solvents are THF, di-ethyl ether, hexanes, acetone, ethanol, methanol, propanol, iso-propanol, MEK, and ethyl acetate or blends thereof. The leaching solvents may contain minor amounts of water (< ~50 wt% water) that are intentionally added or are added or inherently as part of the contaminated pulp or pulp composition to any of the aforementioned solvents. In embodiments of the present invention, said leaching solvent may have a normal boiling point between 20°C and 90°C. In embodiments of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the leaching temperature is at or near the boiling point. In another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the purification temperature is at or near the boiling point and the pressure is at or near atmospheric. The pressure may also be between about 0 atm (vacuum conditions) and higher. In yet another embodiment of the present invention, the leaching solvent has a normal boiling point between 20°C and 90°C and the pressure is above atmospheric but below 1,000 atm. The leaching solvent may also have a boiling point above the leaching temperature. In even yet another embodiment of the present invention, the leaching solvent has a normal boiling point above the leaching temperature. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is acetone; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is ethyl acetate; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm. In another embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent is hexanes; said temperature of saidleaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 0.5 atm and about 1,000 atm.
[0123] Leaching solvents with a normal boiling point below the leaching temperature are also preferred due to the elevated leaching pressures. In embodiments of the present invention, the leaching solvent has a normal boiling point below the leaching temperature. In another embodiment of the present invention, the leaching solvent comprises di-methyl ether (DME). In an embodiment of the present invention, wherein said bulk purification is leaching; wherein said leaching solvent comprises DME; said temperature of said leaching is between about 20°C and about 120°C; and said pressure of said leaching is between about 2 atm and about 1,000 atm.
[0124] Preferred leaching solvents include solvents that have higher affinity for the chemical contaminants than for the reclaimed pulp fiber. Solvents with high affinity for the chemical contaminants include but are not limited to diethyl ether, MEK, ethyl acetate, THF, acetone, methylene chloride, iso-propanol, propanol, ethanol, and methanol. Other oxygenated and polar hydrocarbon solvents likely have similar desired affinity. Solvents lacking such characteristics can still be used, but higher solvent to pulp fiber ratios may be required. It is preferred that the solvent should not significantly dissolve the pulp fiber at the temperature and pressure of the process (< ~5wt% may be dissolved). The solvent may slightly swell the pulp fiber but not enough to cause agglomeration or coalescence. The solvents may contain water for various functional or nonfunctional reasons (below ~50wt%).
[0125] In embodiments of the present invention, said leaching solvent is selected from the group comprising hydrocarbons. In another embodiment of the present invention, said leaching solvent is selected from the group comprising aliphatic hydrocarbons. In even another embodiment of the present invention, said leaching solvent is selected from the group comprising aromatic hydrocarbons. In even yet another embodiment of the present invention, said leaching solvent is selected from the group comprising alkanes.
[0126] In embodiments of the present invention, said leaching solvent is selected from the group comprising methane, ethane, propane, normal butane, isobutane, normal pentane, isopentane, neopentane, hexanes (normal hexane, isohexane, neohexane, heptanes), octanes, or mixtures thereof.
[0127] The temperature may be changed during the course of the extraction process but is generally consistent within a given stage of a unit operation. The pressure may be changed to vary solubility of the solvent in the reclaimed pulp fiber or to increase solubility of the chemical contaminant within the solvent.A leaching extraction process may take place in stages and be combined with additional leaching extraction processes of other types not discussed in this application. The same is true for liquid-liquid extraction processes. In addition, liquid-liquid process may be combined with leaching process in various stages to form a given purification process. In embodiments of the present invention, the number of stages is one or more than one. In another embodiment of the present invention, the number of liquid-liquid stages is more than one. In yet another embodiment of the present invention, the number of leaching stages is more than one. In still yet another embodiment of the present invention, the number of liquid-liquid stages is one or more and the number of leaching stages is one or more. A single stirred tank reactor will achieve a certain removal efficiency. The efficiency can be improved by having multiple stirred tank reactors in series wherein the reclaimed pulp fiber from the 1ststage is predominately separated from the 1ststage purification solvent and this 1ststage pulp fiber is used in the 2ndstage with fresh purification solvent. This is repeated for each additional stage. This method improves the removal efficiency at the expense of additional reactors and complexity but maintains the overall time, throughput, and solvent utilization. Practically speaking, the number of reactor stages can be anywhere from 1 to ~ 10 for stirred tank systems. If a larger number of stages are needed, then a continuous counter-current method may be used.
[0128] While not wishing to be bound by theory, the theoretical maximum contaminant removal capacity for a leaching process is based upon the thermodynamic equilibrium / partitioning of the chemical contaminants between the contaminated pulp or pulp composition and leaching solvent at the temperature and pressure of the process. Thermodynamic equilibrium may not be achieved due to kinetic limitations in the leaching process. This is true for the complete leaching process and is also true for each leaching stage. A higher leaching solvent to contaminated pulp or pulp composition mass ratio will drive both thermodynamics and kinetics in favor of purification at the expense of greater solvent consumption and greater extraction process size, which equals greater cost. Thus, a balance must be found between these important design and operational variables for the targeted chemical contaminant removal efficiency. In addition, the contaminated solvent from any stage may be used “as-is” as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.
[0129] Another important kinetic driver is surface area to volume ratio of the contaminated pulp or contaminated pulp composition exposed to the leaching solvent. In general, the time required to extract a chemical contaminant from a contaminated pulp or contaminated pulp composition isa strong function of the diffusion pathlength within the pulp fiber. The diffusion pathlength is indirectly proportional to the surface area to volume ratio of the geometrical form of the contaminated pulp or contaminated pulp composition and the ability to access the surface area with leaching solvent. Hence, a higher surface area to volume ratio will produce a reduced diffusion pathlength and faster diffusion kinetics. For leaching processes, a high surface area to volume ratio is a critical parameter for quick and efficient contaminant removal both surface and bulk.
[0130] A known means for increasing the effective mass transfer through a given surface area to volume ratio and given set of conditions at the contaminated pulp or contaminated pulp composition solvent interface is through applying energy to the reclaimed pulp fiber such as but not limited to vibrational in the form of ultrasonic energy and / or microwave.
[0131] Following the bulk purification involving extraction, the pulp or pulp composition may be devolatilized to produce a purer pulp or purer pulp composition. The contaminated solvent may contain a small amount of dissolved pulp fiber, the extracted contaminants, and the pure leaching solvent. There are many ways to recover the purer pulp or purer pulp composition and bulk purification solvent independent of the extracted contaminants.
[0132] In general, a small amount of pulp fiber may dissolve into the leaching solvent regardless of process type or solvent. In particular, low molecular weight waxes, lignin, sugars, and, sugar oligomers are particularly prone to solubilization into the extracting solvent. These may become problematic in distillation-based recovery of the purified solvent due to deposition of these on process equipment. Methods are known to reduce this tendency. One such method is to lower the temperature of the contaminated solvent to below the cloud point to precipitate the extracts followed by filtration.
[0133] Distillation and / or flash evaporation of the contaminated bulk purification solvent may be used to regenerate the solvent for re-use in the various extraction operations. However, distillation may not be economically feasible on-going considering the high solvent volume utilized in the present invention. In addition, because the chemical contaminants of interest in this invention are extremely low in concentration, the concentration of these chemical contaminants in the contaminated solvent may be correspondingly low or even lower. Thus, a preferred method to purify the contaminated solvent is through direct removal of the contaminants without volatilizing the bulk solvent phase. Such methods include precipitation, ion exchange, adsorption / absorption methods, etc. Non-limiting examples include passing the contaminated solvent through a bed of activated carbon or alumina. This method can be used alone or in combination with distillation to achieve the right level of purification at the right energy consumption. In addition, thecontaminated solvent from any stage may be used “as-is” as the solvent for another stage. Contaminated solvent at any point in the process may be renewed through known methods of distillation, filtration, ion-exchange, etc., or combinations.
[0134] The purer pulp or purer pulp composition may contain small amounts of the solvent in either physically adsorbed or bulk absorbed form. The concentration of the solvent in the purer pulp or purer pulp composition may be reduced by devolatilization techniques. In an embodiment of the present invention, said purer pulp or purer pulp composition is devolatilized to a content of <1 wt% solvent. In an embodiment of the present invention, said purer pulp or purer pulp composition is devolatilized to a content of < about 50 ppm solvent.
[0135] Multi-staged stirred tank flooded extractors operating at the boiling point of a polar organic leaching solvent provide improvements in chemical contaminant removal over existing methods. For example (as shown in Examples 2 and 3), a flooded leaching process of the present invention provided targeted contaminant removal efficiencies greater than about 50%.
[0136] In embodiments of the present invention, the leaching solvent comprises ethyl acetate. In yet another embodiment of the present invention, the leaching solvent is ethyl acetate and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate and may also comprise water.
[0137] In embodiments of the present invention, the leaching solvent is acetone. In yet another embodiment of the present invention, the leaching solvent comprises acetone and the process pressure is about atmospheric pressure. In another embodiment of the present invention, said bulk purification comprises flooded leaching in a stirred tank conducted at about 56.1 °C and about atmospheric pressure with a leaching solvent comprising acetone. In yet another embodiment of the present invention, the leaching solvent comprises acetone and water.
[0138] In another embodiment of the present invention (Inventive Example 1), a purification of a contaminated pulp composition involving reclaimed cellulosic paperboard to produce a purer pulp composition comprises flooded leaching in a stirred tank involving 4 stages conducted at about 77.1 °C and about atmospheric pressure with a leaching solvent comprising ethyl acetate; wherein the ethyl acetate to contaminated pulp composition mass ratio is ~ 10:1 per stage for a leaching time of ~ 30 minutes per stage for a total ethyl acetate to contaminated pulp composition mass ratio of about 40:1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET and glyphosphate, are 74.6% and > 91.7%, the alkylphenolethoxylates,isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, and isononylphenoltetraethoxylate are > 75.0%, > 83.9%, > 85.7%, and > 70.6%, the bisphenol A is > 96.9%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, are 68.0% and 75.4%, the OCDF is 82.5%, the PCBs, PCB 81, PCB 105 and PCB 118, are 87.5%, 85.8%, and 87.0%, the phthalates, Di-2-ethylhexylphthalate and diisononylphthalate, are 93.4% and 84.4%, and the PAHs, fluoranthene and phenanthrene, are >94.1% and 86.9% wherein the initial concentration of these contaminants in the contaminated pulp composition are above the listed LOQs.
[0139] In another embodiment of the present invention (Inventive Example 2), a purification of a contaminated pulp composition involving a reclaimed pulp composition involving reclaimed cellulosic paperboard to produce a purer pulp composition comprises flooded leaching in a stirred tank involving 4 stages conducted at about 52°C and about atmospheric pressure with a leaching solvent comprising acetone; wherein the acetone to contaminated pulp composition mass ratio is ~ 10:1 per stage for a leaching time of - 30 minutes per stage for a total acetone to contaminated pulp composition ratio of about 40:1 and a total leaching time of about 120 minutes; wherein the % removal of the pesticides, DEET and glyphosphate, are 85.7% and > 91.7%, the alkylphenolethoxylates, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, and isononylphenoltetraethoxylate are > 75.0%, > 83.9%, > 85.7%, and > 70.6%, the bisphenol A is > 96.9%, the dioxins, 1,2, 3, 4, 6, 7, 8 -HpCDD and OCDD, are 89.1% and 89.8%, the OCDF is 85.6%, the PCBs, PCB 81, PCB 105 and PCB 118, are > 96.7%, 94.8%, and 95.1%, the phthalates, Di-2-ethylhexylphthalate and diisononylphthalate, are 94.9% and 12.0% wherein the initial concentration of these contaminants in the contaminated pulp composition are above the listed LOQs.
[0140] Following the flooded leaching, the purer pulp or pulp composition may be physically wetted with the residual solvent and potentially contain a small amount of absorbed solvent. As discussed earlier, there are many ways to recover the purer recycled pulp or pulp composition and bulk purification solvent independent of the extracted contaminants. The purer recycled pulp or pulp composition can be dried and devolatilized by many known commercial means. One method is through cyclonic drying. Another method is through melt extrusion with a devolatilization section. In embodiments of the present invention, the purer recycled pulp or pulp composition is processed to reduce the leaching solvent to below about lwt% in the reclaimed pulp or pulp composition and more preferably less than about 50 ppm. The contaminated solvent can be cleaned with known methods of distillation, ion exchange, filtration, etc. The resulting devolatilizedreclaimed pulp or pulp composition may be used as it or may be further processed into other forms including pellets via various processes.
[0141] VI. EXAMPLES
[0142] In general, the established methods for purifying contaminated pulp or pulp compositions including water washing are currently not able to sufficiently remove chemical contaminants. Net, there is an unmet need for a cleaning technology that is capable of more completely removing chemical contamination sufficient for highly contaminated sources and for any market desiring purer recycled pulp materials. In addition, there is an unmet need for recycled compositions that do not have, or have very low levels of, chemical contamination.
[0143] COMPARATIVE EXAMPLE - Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purer Water-Washed Post-Consumer Recycled Pulp Composition
[0144] 2,500 grams of de-ionized water was added to a 5L stirred round bottom flask. In addition, ImL of Triton X=100 surfactant was added to the water. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the water to ~80C) in about 5 minutes. After reaching ~80C, the heat input was lowered to maintain a constant temperature of ~80C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Paper was cut into 1 cm X 1 cm squares and represented the contaminated pulp composition. The -250 grams of the cut Reclaimed Post-Consumer Paper was added to the round bottom flask which contained the hot water / surfactant solution. The washing was continued for -30 minutes. The stirring was terminated, and the heat was removed. The water solution was decanted from the mixture of solids and liquids. This completed washing step #1. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a second washing step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve -80C. The time to reach 80C after the addition of the fresh-water solution to the paperboard was -5 minutes. The 2nd washing continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #2. An additional 2,500 grams of preheated water / Triton X-100 solution was added to the paperboard in the 5L round bottom. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve 80C. The time to reach -80C after the additionof fresh-water solution was -5 minutes. This washing step continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. This completed washing step #3. An additional 1,000 grams of preheated fresh water / Triton X-100 solution was added to the paperboard in the 5L round bottom to complete a fourth washing step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to achieve ~80C in the water solution. The time to reach ~80C after the addition of fresh-water solution was -5 minutes. The 4th washing continued for a total of ~30 minutes. The stirring was stopped, and the heat removed. The water solution was decanted off. The paperboard contained a small amount of contaminated water solution within the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual water solution via gravity. The paperboard was then completely dried of contaminated water solution at room temperature overnight to produce the purer pulp composition. The washing solution to contaminated pulp composition ratio per stage was -10:1 for four stages giving a total washing solution to contaminated pulp composition ratio of -40: 1. The washing time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The contaminated pulp composition represented by Reclaimed Post-Consumer Pulp and the resulting purer pulp composition represented by the Recycled Post-Consumer Pulp discussed above was analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table 2. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was > 96.4%, 44.2%, 35.0%, 35.5%, 40.0%, 17.6%, 72.5%, 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 0.0%, 14.9%, and 10.0% respectively, which was indicative of generally poor contaminant removal especially for the dioxins, pcbs, and phthalates.
[0145] The pulp before and after the purification was characterized for water retention value. The water wash resulted in a 10.4% reduction of water-retention value which may be indicative of increased homification.
[0146] The pulp before and after the purification were processed into handsheets following Tappi T205 and then evaluated for tensile properties and chemical composition. The tensile strength for the handsheets after purification was reduced by about 11% possibly due to increased homification.The washing process removed about 6.5% ash but didn’t significantly remove lignin from the pulp fibers.
[0147] TABLE 2
[0148] Purification Method Using Traditional Water Washing of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Water-Washed Post-Consumer Recycled Pulp Composition
[0149] Reclaimed Post-Consumer Pulp Composition Before After
[0150] % Removed Purification Purification
[0151] LOQ xLOQ xLOQ
[0152] Pesticides
[0153] Diethyltoluamide (DEET) 10 ppb 28.0 <1 > 96.4% Glyphosate 10 ppb 12.0 6.7 44.2% Alkylphenol ethoxylates
[0154] iso-Nonylphenotmonoethoxylate 50 ppb 4.0 2.6 35.0% iso-Nonylphenoldiethoxylate 50 ppb 6.2 4.0 35,5% iso-Nonylphenoltriethoxylate 50 ppb 7.0 4.2 40.0% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 2.8 17.6% Bisphenols
[0155] BisphenolA 5 ppb 32.0 8.8 72.5% Dioxins and dioxinlike and PCB
[0156] 1,2,3.4,6,7,8-HpCDD 0.2 pptr 145.5 163.0 0.0%
[0157] OCDD 0.2 pptr 1355.0 1445.0 0.0%
[0158] OCDF 0.2 pptr 43.8 47.7 0.0%
[0159] PCB 81 0.05 pptr 87.8 92.8 0.0%
[0160] PCB 105 5 pptr 73.2 87.2 0.0%
[0161] PCB 118 10 pptr 68.9 83.2 0.0% Phthalates
[0162] Di-2-ethylhexyl phthalate 50 ppb 134.0 114.0 14.9% Diisononyl phthalate 50 ppb 100.0 90.0 10.0% Polycyclic aromatic hydrocarbons {PAH)
[0163] Fluoranthene I ppb 17.0 dot n.a.
[0164] Phenanthrene 1 ppb 13.0 dnt rua.
[0165] % Increase Water Retention Value (g / g) 1.25 + / - 0.1 1.12 + / -0.01 -10.4%
[0166] FQA Fines Level (%) 9.4+ / - 0.0 10.1+ / - 0.2 7.4% Handsheet Tensile Strength (kN / m) 1.8+ / - 0.1 1.6 + / -0.1 -11.1% Handsheet Zero Span Tensile Strength ( kg-f ) 8.41 + / - 0.32 8.20 + / - 0.34 -2.5%
[0167] Compositional information wt% % Removed Ash(%) 6.2 5.8 6.5%
[0168] Klason Lignin {%) 14.2 + / -0.1 14.3+ / - 0.3 -0.7%
[0169] Acid soluble Lignin f%) 0.9 + / -0.0 0.9 + / -0.1 0.0%
[0170] % Lignin Level 15.2 + / - 0.1 15.2+ / - 0.3 0.0%
[0171]
[0172] INVENTIVE EXAMPLE 1 -Ethyl Acetate Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purer Post-Consumer Recycled Pulp Composition 2,500 grams of ethyl acetate was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanicalstirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the ethyl acetate to boiling (-77.1 C) in about 5 minutes. After reaching the boiling point of ethyl acetate, the heat input was lowered to achieve a consistent reflux rate of -10 ml / min at the boiling point of -77.1C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares. The -250 grams of the cut Reclaimed Post-Consumer Pulp Composition in paperboard form was added to the round bottom flask which contained the boiling ethyl acetate. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The ethyl acetate was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. An additional 2,500 grams of preheated fresh ethyl acetate at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the ethyl acetate at -10 mL / min. The time to reach reflux after the addition of fresh ethyl acetate to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The ethyl acetate was decanted off. The paperboard contained a small amount of contaminated solvent residual within the porosity of the paperboard. This wet paperboard was placed in a filter funnel with 60 mesh grating to further remove residual ethyl acetate via gravity. The paperboard was then completely dried of contaminated solvent at room temperature over-night to produce the Purer Pulp Composition or specifically Recycled Post-Consumer Pulp Composition. The leaching solvent to contaminated pulp composition ratio per stage was -10:1 for four stages giving a total solvent to contaminated pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The pulp composition beforeand after purification were analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table #3. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene, the % removal was 74.6%, >91.7%, >93.5%, >83.9%, >85.7%, >70.6%, >96.9%, 68.0%, 75.4%, 82.5%, 87.5%, 85.8%, 87.0%, 93.4%, 84.4%, >94.1%, and 86.9%, respectively, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0173] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 4.8% increase in the water-retention value which may be indicative of decreased hornification, which is opposite the trend observed with traditional water washing.
[0174] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in an 11% reduction in tensile strength despite the decreased hornification. The solvent leaching process didn’t remove significant ash but did significantly remove lignin at 10% removal from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 3
[0175] Purification of Reclaimed Post-Consumer Fiber #1 to Produce Post-Consumer Recycled Fiber using Stirred Tank Reactor Flooded Leaching with Ethyl Acetate at Boiling Point
[0176] Reclaimed Post-Consumer Pulp Composition Before After
[0177] % Removed Purification Purification
[0178] LOQ xLOQ xLOQ
[0179] Pesticides
[0180] Diethyltoluamide (DEET) 10 ppb 28.0 7.1 74.6% Glyphosate lO ppb 12.0 <1 > 91.7% Alkylphenol ethoxylates
[0181] iso-Nonylphenolmonoethoxylate 50 ppb 4.0 <1 > 75.0% iso-Nonylphenoldiethoxylate 50 ppb 6.2 <1 > 83.9% iso-Nonylphenoltriethoxylate 50 ppb 7.0 <1 > 85.7% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 <1 > 70.6% Bisphenols
[0182] Bisphenol A 5 ppb 32.0 <1 > 96.9% Dioxins and dioxinlike and PCB
[0183] 1,2,3,4,6,7,8-HpCDD 0.2 ppTf 145.5 46.5 68.0%
[0184] OCDD 0.2 ppTf 1355.0 333.0 75.4%
[0185] OCDF 0.2 ppTr 43.8 7.7 82.5%
[0186] PCB 81 0.05 ppTr 131.0 16.4 87.5%
[0187] PCB 105 5 ppTr 73.2 10.4 85.8%
[0188] PCB 118 10 ppTr 68.9 9.0 87.0% Phthalates
[0189] Di-2-ethythexyl phthalate 50 ppb 134.0 8.8 93.4%
[0190] Di iso nonyl phthalate 50 ppb 100.0 15.6 84.4% Polycyclic aromatic hydrocarbons (PAH)
[0191] Fluoranthene I ppb 17.0 <1 > 94.1% Phenanthrene 1 ppb 13.0 1.7 86.9%
[0192] % increase Water Retention Value (g / g) 1.25 + / -0.1 1.31+ / - 0.19 4.8%
[0193] FQA Fines Level (%) 9.4+ / - 0.0 9.6+ / - 0.2 2.1% Handsheet Tensile Strength (kN / m) 1.8 + / - 0.1 1.6+ / - 0.1 -11.1% Handsheet Zero Span Tensile Strength (kg-f) 8.41 + / - 0.32 8.16+ / - 0.40 -3.1%
[0194] Compositional Information Wt% % Removed Ash(%) 6.2 6.8 -9.7%
[0195] Klason Lignin {%) 14.2+ / - 0.1 12.8+ / - 0.1 9.9%
[0196] Acid soluble Lignin (%) 0.9 + / - 0.0 0.9+ / - 0.0 0.0%
[0197] % Lignin Level 15.2+ / - 0.1 13.7 + / - 0.1 9.9%
[0198]
[0199] INVENTIVE EXAMPLE 2 -Acetone Leaching of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purer Post-Consumer Recycled Pulp Composition
[0200] 2,500 grams of acetone was added to a 5L stirred round bottom flask. The flask was outfitted with a mechanical stirrer, one reflux condenser, and one heat jacket. The mechanical stirring was set to 400 rpm. The heating jacket was controlled by a variable voltage transformer. The heat was applied to rapidly bring the acetone to boiling (~52C) in about 5 minutes. After reaching the boiling point of acetone, the heat input was lowered to achieve a consistent reflux rateof -10 ml / min at the boiling point of ~52C. Contaminated pulp composition in the form of Reclaimed Post-Consumer Pulp Composition in paperboard form was cut into 1 cm X 1 cm squares and represented the contaminated pulp composition. The -250 grams of the cut recycled Reclaimed Post-Consumer Fiber #1 was added to the round bottom flask which contained the boiling acetone. The extraction was continued for -30 minutes. The stirring was terminated, and the heat was removed. The acetone was decanted from the mixture of solids and liquids. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a second extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 2nd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a third extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 3rd extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. An additional 2,500 grams of preheated fresh acetone at or near the boiling point was added to the paperboard in the 5L round bottom to complete a fourth extraction step. Stirring was started at 400 to 500 rpm while heating was applied sufficient to reflux the acetone at -10 mL / min. The time to reach reflux after the addition of fresh acetone to the paperboard was -5 minutes. The 4th extraction continued for a total of -30 minutes. The stirring was stopped, and the heat removed. The acetone was decanted off. The paperboard contained a small amount of contaminated solvent residual within the porosity of the paperboard. This wet paperboard was placed in a filter flask w / o vacuum to further remove residual acetone. The paperboard was then completely dried of contaminated solvent at room temperature over-night to produce the Purer Pulp Composition or specifically Recycled Post-Consumer Pulp. The leaching solvent to contaminated pulp composition ratio per stage was -10:1 for four stages giving a total solvent to contaminated pulp composition ratio of -40:1. The leaching time per stage was approximately -35 minutes per stage for a total time of -140 minutes. The Pulp Composition before and after purification were analyzed for the classes of chemical contaminants typically present in recycled materials by GALAB Laboratories GmbH (Am Schleusengraben 7, 21029 Hamburg, Germany) using the methods disclosed in section IX Methods, as shown in Table #4. For the contaminants DEET, glyphosphate, isononylphenolmonoethoxylate,isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, and diisononylphthalate, the % removal was 85.7%, > 91.7%, > 75.0%, > 83.9%, > 85.7%, > 70.6%, > 96.9%, 89.1%, 89.8%, 85.6%, > 96.7%, 94.8%, 95.1%, 94.9%, and 12.0%, which was indicative of outstanding removal across a broad spectrum of chemical species and classifications.
[0201] The Pulp Composition before and after the purification was characterized for water retention value. The solvent leaching resulted in a 3.2% increase in the water-retention value which may be indicative of decreased hornification, which is opposite the trend observed with traditional water washing.
[0202] The Pulp Composition before and after the purification were processed into handsheets following Tappi T205 to produce a recycled paperboard and then evaluated for tensile properties and chemical composition. The solvent leaching resulted in a 17% increase in tensile strength possibly due to the decreased hornification. The solvent leaching process didn’t remove significant ash but did significantly remove lignin at -15% reduction from the pulp fibers, which is indicative of some lignin extraction possibly due to favorable partitioning between the solvent and the cellulose-based paper fibers.TABLE 4
[0203] Purification of Method Using Current Invention involving Acetone Leaching of Reclaimed Post-Consumer of Reclaimed Post-Consumer Pulp Composition in Paperboard Form to Produce a Purer Post-Consumer Recycled Pulp Composition
[0204] Reclaimed Post-Consumer Pulp Composition
[0205] Before After
[0206] % Removed Purification Purification
[0207] LOQ xLOQ xLOQ
[0208] Pesticides
[0209] Diethyltoluamide (DEET) 10 ppb 28.0 4.0 85.7% Glyphosate 10 ppb 12.0 <1 >91.7% Alkylphenol ethoxylates
[0210] iso-Nonylphenolmonoethoxylate 50 ppb 4.0 <1 > 75.0% iso-Nonylphenoldiethoxylate 50 ppb 6.2 <1 > 83.9% iso-Nonylphenoltriethoxylate 50 ppb 7.0 <1 > 85.7% iso-Nonylphenoltetraethoxylate 50 ppb 3.4 <1 > 70.6% Bisphenols
[0211] BisphenolA 50 ppb 32.0 <1 > 96.9% Dioxins and dioxlntike and PCB
[0212] 1,2,3,4,6.7,8-HpCDD 0.2 ppTr 145.5 15.8 89.1% OCDD 0.2 ppTr 1355.0 138.0 89.8% OCDF 0.2ppTr 43.8 6.3 85.6% PCB 81 0.05 ppTr 30.0 <1 > 96.7% PCB 105 5 ppTr 73.2 3.8 948% PCB 118 10 ppTr 68.9 3.4 95.1% Phthalates
[0213] Di-2-ethylhexyl phthalate 50 ppb 134.0 6.8 94.9% Diisononyl phthalate 50 ppb 100.0 88.0 12.0% Polycyclic aromatic hydrocarbons (PAH)
[0214] Fluoranthene I ppb 17.0 dnt n.a. Phenanthrene I ppb 13.0 dnt n.a.
[0215] % increase Water Retention Value (g / g) 1.25+ / - 0.1 1.29+ / - 0.15 3.2%
[0216] FQA Fines Level (%) 9.4+ / - 0.0 9.5+ / - 0.1 1.1% Handsheet Tensile Strength (kN / m) 1.8 +7-0.1 2.1+ / - 0.1 16.7% Handsheet Zero Span Tensile Strength (kg-f ) 8.41+ / - 0.32 9.31 +7-0.44 10.7% Compositional information % Removed Ash(%) 6.2 6.1 1.6%
[0217] Klason Lignin (%) 14.2+ / - 0.1 12.0+ / - 0.1 15.5%
[0218] Acid soluble Lignin (%) 0.9 + / - 0.0 1.0 +7- 0.0 -11.1%
[0219] % Lignin Level 15.2 + / - 0.1 12.9+ / - 0.1 15.1%
[0220]
[0221] VII. TEST METHODS
[0222] 1. TRACE CHEMICALS TEST METHOD
[0223] The content on a mass per mass basis of trace chemicals present in any pulp or pulp composition is determined using methods containing sample extraction and instrumental analysis approaches known of those of skill in the art and understood to be capable of extracting and detecting essentially all of a particular trace chemical in these materials. Suitable overall method specifics vary based on the particular trace chemical being quantified, though a common overall method structure is generally followed. A suitable method generally begins with increasing thesurface area of a representative recycled pulp, tissue comprising recycle pulp, or packaging material comprising recycle pulp sample by cutting, shredding, and / or milling into small particles. An extraction step is then performed using a solvent capable of dissolving or diffusing into the sample and in which the trace chemical is readily soluble. The extraction process conditions (e.g., time and temperature) are optimized to maximize trace chemical recovery and common approaches include but are not limited to Soxhlet extraction, accelerated solvent extraction, and / or ultrasonic extraction. Internal standards (usually stable-isotope-labeled versions of the trace chemicals if mass spectrometry-based detection approaches are used) are added during the extraction step to account for potential losses during extraction and subsequent processing steps. After extraction is complete, the extraction solvent is isolated and worked up for instrumental analysis. Depending on the solvent used for extraction, the required quantitation limit, and the specific instrumental approach used, generation of a specimen suitable for instrumental analysis may require multiple cleanup and / or concentration steps including but not limited to centrifugation / filtration, liquid / liquid extraction, and / or column chromatography. The trace chemical in the worked-up specimen is then quantified using instrumental methods (e.g., GC-MS, GC-MS / MS, GC-HRMS, LC-MS / MS, etc.) known to those of skill in the art and specifically adapted to the trace chemical of interest. Suitable instrumental approaches may be developed de novo or may be based on standard, known methods for particular trace chemicals (e.g., US EPA Method 1613 in the case of dioxins and furans or US EPA 1668 for PCBs). Based on a combination of raw instrumental quantitative results, extraction solvent workup steps, original extraction volume, and starting specimen mass, the mass content of a trace chemical per mass of starting specimen material is calculated and is reported as the level of the trace chemical in the material tested. Given the generally low levels of trace chemicals present, common units used in reported levels of trace chemicals are pg / kg and ng / kg (equivalent to the ppb and ppt levels, respectively).
[0224] One of skill in the art will recognize that trace chemicals are often present at very low “trace” levels, meaning that under some circumstances, environmental and / or laboratory background levels of these same trace chemicals may give rise to false positive detects or falsely elevated results if appropriate precautions are not taken. While one of skill in the art recognizes that a suite of measures may be needed to minimize such false results, one obligatory measure is to include a true “blank” beginning with solvent carried in parallel through the extraction step, extraction solvent workup, and instrumental analysis.
[0225] Using the suitable overall methodology outlined above, one of skill in the art may quantify a range of trace chemicals potentially present in a recycled pulp, tissue comprising recycle pulp, orpackaging material comprising recycle pulp sample of interest. For example, just to describe a few of the trace chemicals listed herein, the level of isononylphenol (CAS RN 11066-49-2) may be determined and reported as mass of trace chemical per mass of material in units of pg / kg. Similarly, the level of PCB 118 (CAS RN 31508-00-6) may be determined and reported in units of ng / kg, the level of OCDD (CAS RN 3268-87-9), a dioxin, may be determined and reported in units of ng / kg, the level of bisphenol A (CAS RN 80-05-7), also known as BP A, may be determined and reported in units of pg / kg, and the level of diisononyl phthalate (CAN RN 28553-12-0), also known as DINP, may be determined and reported in units of pg / kg.
[0226] 2. WATER RETENTION VALUE TEST METHOD
[0227] The water retention value of pulp was measured according to Tappi UM 256.
[0228] 3. % FINES LEVEL (FIBER QUALITY ANALYSIS TEST METHOD)
[0229] The pulp morphology including fiber length, width, coarseness, fines was characterized optically according Tappi T271 om-23 using a Fiber Quality Analyzer (FQA-360).
[0230] 4. HANDSHEET TENSILE PROPERTIES TEST METHOD
[0231] Hand sheet was made according to Tappi T205 for paper mechanical properties test. The tensile properties of hand sheet were measured according to Tappi T494.
[0232] 5. HANDSHEET ZERO SPAN TENSILE TEST METHOD
[0233] The Zero-span breaking strength of pulp was measured according to Tappi T231.
[0234] 6. % LIGNIN LEVEL TEST METHOD
[0235] The % lignin level in pulp was determined according to the standard protocol provided by the National Renewable Energy Laboratory. (J. Agric. Food Chem. 2010, 58, 16, 9043-9053).
[0236] 7. WATER CONTENT TEST METHOD
[0237] The water (moisture) content present in a fibrous structure is measured using the following Water Content Test Method.
[0238] A fibrous structure or portion thereof (“sample”) is placed in a conditioned room at a temperature of 73°F ± 4°F (about 23°C ± 2.2°C) and a relative humidity of 50% ± 10% for at least 24 hours prior to testing. The weight of the sample is recorded when no further weight change is detected for at least a 5 minute period. Record this weight as the “equilibrium weight” of thesample. Next, place the sample in a drying oven for 24 hours at 70°C with a relative humidity of about 4% to dry the sample. After the 24 hours of drying, immediately weigh the sample. Record this weight as the “dry weight” of the sample. The water (moisture) content of the sample is calculated as follows:
[0239] % Water (moisture) in sample = 100% x (Equilibrium weight of sample - Dry weight of sample)
[0240] Dry weight of sample
[0241] The % Water (moisture) in sample for 3 replicates is averaged to give the reported % Water (moisture) in sample.
[0242] VIII. COMBINATIONS
[0243] A. A method to remove contaminants from a contaminated pulp or contaminated pulp composition to produce a purer pulp or purer pulp composition comprising:
[0244] i. providing a contaminated pulp or contaminated pulp composition comprising an individual contaminant or contaminants, each individual contaminant having a concentration;
[0245] ii. extracting said individual contaminant or contaminants from said contaminated pulp or contaminated pulp composition at a temperature and a pressure, using a solvent, in extraction stages, for a period of time and for a period of time per stage, to produce a purer pulp or pulp composition comprising an individual contaminant or contaminants, each having a concentration;
[0246] wherein said extraction stages are conducted at a solvent to contaminated pulp or contaminated pulp composition mass ratio; wherein said solvent to contaminated pulp or contaminated pulp composition mass ratio per stage at any time is less than about 100:1; wherein said pressure is between about 0.5 atm and 1,000 atm absolute pressures; wherein said individual contaminants comprise at least one of glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2-ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene above LOQ; wherein at least one of the individual contaminants concentration in said purer pulp or pulp composition is reduced compared to each individual contaminants concentration in said contaminated pulp or contaminated pulp composition by at least about 75% or LOQ.
[0247] B. The method of paragraph A, wherein said number of extraction stages is between about 1 and about 50.C. The method of paragraph A or B, wherein said contaminated pulp or contaminated pulp composition is a reclaimed post-consumer pulp or reclaimed post-consumer pulp composition.
[0248] D. The method of any one of paragraphs A-C, wherein said reclaimed post-consumer pulp or reclaimed post-consumer pulp composition is a reclaimed post-consumer paper.
[0249] E. The method of any one of paragraphs A-D, wherein said period of time represented by the sum of times for the individual extraction stages is less than about 360 minutes.
[0250] F. The method of any one of paragraphs A-E, wherein said solvent is purified after said extraction and re-used in the extraction process by a solvent purification process or processes.
[0251] G. The method of any one of paragraphs A-F, wherein said solvent comprises one or more organic solvents or a mixture of organic solvents and less than about 50 wt% water.
[0252] H. The method of any one of paragraphs A-G, wherein said solvent comprises at least one of an oxygenated solvent or mixtures thereof.
[0253] I. The method of any one of paragraphs A-H, wherein said solvent comprises at least one of dimethyl ether (DME), diethyl ether, MEK, ethyl acetate, THF, acetone, propanol, isopropanol, ethanol, methanol, or mixtures thereof.
[0254] J. The method of any one of paragraphs A-I, wherein said solvent comprises methylene chloride or mixtures of methylene chloride and other organic solvents.
[0255] K. The method of any one of paragraphs A- J, wherein said solvent comprises at least one of methane, ethane, propane, normal butane, isobutane, normal pentane, isopentane, neopentane, hexanes (normal hexane, isohexane, and neohexene), heptanes, octanes, or mixtures thereof.L. The method of any one of paragraphs A-K, wherein said pressure is about atmospheric.
[0256] M. The method of any one of paragraphs A-L, wherein said temperature is about the normal boiling point of the said solvent.
[0257] N. The method of any one of paragraphs A-M, wherein said temperature is between about 20°C and 90°C.
[0258] O. The method of any one of paragraphs A-N, wherein the Water-Retention- Value (WRV) of said purer pulp or purer pulp composition is at least 2% greater than the WRV of the contaminated pulp or contaminated pulp composition.
[0259] P. The method of any one of paragraphs A-O, wherein the tensile strength of paper produced from said purer pulp or purer pulp composition is at least 10% greater than the tensile strength of paper produced from said contaminated pulp or contaminated pulp composition and wherein the said solvent is acetone or blends of acetone and water.
[0260] Q. The method of any one of paragraphs A-P, wherein the Water-Retention- Value (WRV) of said purer pulp or purer pulp composition is at least 2% greater than the WRV of the contaminated pulp or contaminated pulp composition; and wherein the tensile strength of paper produced from said purer pulp or purer pulp composition is at least 10% greater than the tensile strength of paper produced from said contaminated pulp or contaminated pulp composition.
[0261] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as “40 mm” is intended to mean “about 40 mm.”
[0262] Every document cited herein, including any cross referenced or related patent or application and any patent application or patent to which this application claims priority or benefit thereof, is hereby incorporated herein by reference in its entirety unless expressly excluded or otherwise limited. The citation of any document is not an admission that it is prior art with respect to any invention disclosed or claimed herein or that it alone, or in any combination with any otherreference or references, teaches, suggests or discloses any such invention. Further, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.
[0263] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.
Claims
CLAIMSWhat is claimed is:
1. A method to remove contaminants from a contaminated pulp or contaminated pulp composition to produce a purer pulp or purer pulp composition comprising:i. providing a contaminated pulp or contaminated pulp composition comprising an individual contaminant or contaminants, each individual contaminant having a concentration;ii. extracting said individual contaminant or contaminants from said contaminated pulp or contaminated pulp composition at a temperature and a pressure, using a solvent, in extraction stages, for a period of time and for a period of time per stage, to produce a purer pulp or pulp composition comprising an individual contaminant or contaminants, each having a concentration;wherein said extraction stages are conducted at a solvent to contaminated pulp or contaminated pulp composition mass ratio; wherein said solvent to contaminated pulp or contaminated pulp composition mass ratio per stage at any time is less than 100: 1; wherein said pressure is between 0.5 atm and 1,000 atm absolute pressures; wherein said individual contaminants comprise at least one of glyphosphate, isononylphenolmonoethoxylate, isononylphenoldiethoxylate, isononylphenoltriethoxylate, isononylphenoltetraethoxylate, bisphenol A, 1,2,3,4,6,7,8-HpCDD, OCDD, OCDF, PCB 81, PCB 105, PCB 118, di2- ehtylhexylphthalate, diisononylphthalate, fluoranthene, and phenanthrene above LOQ; wherein at least one of the individual contaminants concentration in said purer pulp or pulp composition is reduced compared to each individual contaminants concentration in said contaminated pulp or contaminated pulp composition by at least 75% or LOQ.2 The method of Claim 1, wherein said number of extraction stages is between 1 and 50.3 The method of Claim 1 , wherein said contaminated pulp or contaminated pulp composition is a reclaimed post-consumer pulp or reclaimed post-consumer pulp composition.4 The method of Claim 3, wherein said reclaimed post-consumer pulp or reclaimed postconsumer pulp composition is a reclaimed post-consumer paper.
5. The method of Claim 1, wherein said period of time represented by the sum of times for the individual extraction stages is less than 360 minutes.
6. The method of Claim 1, wherein said solvent is purified after said extraction and re-used in the extraction process by a solvent purification process or processes.7 The method of Claim 1, wherein said solvent comprises one or more organic solvents or a mixture of organic solvents and less than 50 wt% water.8 The method of Claim 6, wherein said solvent comprises at least one of an oxygenated solvent or mixtures thereof.9 The method of Claim 7, wherein said solvent comprises at least one of dimethyl ether (DME), diethyl ether, MEK, ethyl acetate, THF, acetone, propanol, iso-propanol, ethanol, methanol, or mixtures thereof.10 The method of Claim 8, wherein said solvent comprises methylene chloride or mixtures of methylene chloride and other organic solvents.11 The method of Claim 6, wherein said solvent comprises at least one of methane, ethane, propane, normal butane, isobutane, normal pentane, isopentane, neopentane, hexanes (normal hexane, isohexane, and neohexene), heptanes, octanes, or mixtures thereof.12 The method of Claim 1, wherein said pressure is atmospheric.13 The method of Claim 1, wherein said temperature is the normal boiling point of the said solvent.14 The method of Claim 1, wherein said temperature is between 20°C and 90°C.15 The method of Claim 1, wherein the Water Retention Value (WRV) of said purer pulp or purer pulp composition is at least 2% greater than the WRV of the contaminated pulp or contaminated pulp composition.