Selective solubilization of gangue from molybdenum concentrate using biosolvents

The use of organic and inorganic acids in biosolvents selectively removes impurities from molybdenum concentrates, enhancing purity and improving ore quality for sustainable mining practices.

WO2026236498A1PCT designated stage Publication Date: 2026-11-12ALLONNIA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/US2026/027113
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2026-05-07
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The decline in ore grades and increasing demand for high-grade ores necessitate more efficient and sustainable methods for extracting impurities from molybdenum concentrates to improve ore quality and meet production targets.

Method used

A method using an extraction composition comprising organic and inorganic acids, optionally derived from biosolvents, to selectively solubilize impurities such as Al, Si, Cu, F, Pb, As, Mg, Ca, Zn, and Fe from molybdenum concentrates, followed by separation and recycling of the extraction composition.

Benefits of technology

This approach enhances the purity of molybdenum concentrates by selectively removing impurities, improving the ore's value and enabling more efficient downstream processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2026027113_12112026_PF_FP_ABST
    Figure US2026027113_12112026_PF_FP_ABST
Patent Text Reader

Abstract

A mixture includes a molybdenum concentrate and an extraction composition. The extraction solution includes an aqueous solution that includes a first organic acid, an optional additional organic acid, and optionally an inorganic acid. The extraction composition is configured to selectively solubilize one or more impurity components from the molybdenum concentrate. A method for extracting a metal from molybdenum concentrate. The method includes selectively solubilizing one or more impurity components including one or more minerals, one or more salts, or any combination thereof from molybdenum concentrate into an extraction composition. The extraction composition includes an aqueous solution of an organic acid selected from the group consisting of citric acid, oxalic acid, formic acid, lactic acid, acetic acid, malic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic, and combinations thereof.
Need to check novelty before this filing date? Find Prior Art

Description

PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1SELECTIVE SOLUBILIZATION OF GANGUE FROM MOLYBDENUM CONCENTRATE USING BIOSOLVENTS BACKGROUND

[0001] In the mining industry, there has been a general decline in ore grades over time.Decreasing ore quality requires more efficient operation or additional capital expenditure to meet production targets. This also presents an additional issue as further development of electrification technologies, such as battery economy and urbanization fuels, drives demand for relatively higher-grade ores of nickel, lithium, copper, rare earth metals, among others. Accordingly, there exists a need for methods for more sustainable mining practices to ensure production of high-grade ore.SUMMARY

[0002] This summary is provided to introduce a selection of concepts that are further described below in the detailed description. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.

[0003] In one aspect, embodiments herein relate to a mixture including a molybdenum concentrate, and an extraction composition. The extraction composition includes an aqueous solution that includes a first organic acid, an optional additional organic acid, and optionally an inorganic acid. The extraction composition is configured to selectively solubilize one or more impurity components from the molybdenum concentrate. The one or more impurity components comprise one or more of an atom, a mineral, a salt of Pb, Mg, Al, Si, F, Fe, Ca, As, Zn, or any combination thereof.

[0004] In another aspect, embodiments herein relate to a method for extracting a metal from molybdenum concentrate that includes selectively solubilizing one or more impurity components including one or more minerals, one or more salts, or any combination thereof from the molybdenum concentrate into an extraction composition. The extraction composition comprises an aqueous solution of an organic acid, an optional additional organic acid, and an optional inorganic acid.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1

[0005] In another aspect, embodiments herein relate to a method for extracting an impurity from a molybdenum concentrate. The method includes extracting one or more impurity components with an extraction composition, separating the molybdenum concentrate from the one or more components and the extraction composition, separating the extraction composition from the one or more components, and repeating the extracting. The separated one or more impurity components have a purity in a range from 10% to 90%, when separated from the extraction composition.

[0006] The one or more impurity components includes one or more minerals, one or more salts, or any combination thereof from the molybdenum concentrate. The extraction composition comprises an aqueous solution of an organic acid selected from the group consisting of citric acid, oxalic acid, formic acid, lactic acid, acetic acid, malic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid and combinations thereof.

[0007] Other aspects and advantages of the claimed subject matter will be apparent from the following description and the appended claims.BRIEF DESCRIPTION OF DRAWINGS

[0008] FIG. 1 is a simplified block flow diagram of an extraction process that recycles an extraction composition in accordance with one or more embodiments.

[0009] FIG. 2A is a graph showing percentages of dissolved elements after an initial leach with oxalic acid and a post regeneration leach.

[0010] FIG. 2B is a graph showing percentages of dissolved elements after an initial leach with tartaric acid and a post regeneration leach.DETAILED DESCRIPTION

[0011] In the following detailed description of embodiments of the disclosure, numerous specific details are set forth in order to provide a more thorough understanding of the disclosure. However, it will be apparent to one of ordinary skill in the art that the disclosure may be practiced without these specific details. In otherPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1instances, well-known features have not been described in detail to avoid unnecessarily complicating the description.

[0012] In the following description, any component described with regard to the figure, in various embodiments disclosed herein, may be equivalent to one or more like- named components described with regard to any other embodiment and / or figure. For brevity, descriptions of these components will not be repeated with regard to each embodiment and / or figure. Thus, each and every embodiment of the components of each embodiment and / or figure is incorporated by reference and assumed to be optionally present within every other figure having one or more like-named components. Additionally, in accordance with various embodiments disclosed herein, any description of the components of a figure is to be interpreted as an optional embodiment which may be implemented in addition to, in conjunction with, or in place of the embodiments described with regard to a corresponding like-named component in any other embodiment and / or figure.

[0013] Throughout the application, ordinal numbers (for example, first, second, third) may be used as an adjective for an element (that is, any noun in the application). The use of ordinal numbers does not imply or create a particular ordering of the elements or limit any element to being only a single element unless expressly disclosed, such as by the use of the terms “before,” “after,” “single,” and other such terminology. Rather, the use of ordinal numbers is to distinguish between the elements. By way of an example, a first element is distinct from a second element, and the first element may encompass more than one element and succeed (or precede) the second element in an ordering of elements.

[0014] It is to be understood that the singular forms “a,” “an,” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “an organic acid” includes reference to one or more of such organic acids.

[0015] Terms such as “approximately” or “substantially” mean that the recited characteristic, parameter, or value need not be achieved exactly, but that deviations or variations, including, for example, tolerances, measurement error, measurement accuracy limitations, and other factors known to those of skill in the art, may occur in amounts that do not preclude the effect the characteristic was intended to provide.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1

[0016] It is to be understood that one or more of the steps shown in the flowcharts may be omitted, repeated, or performed in a different order than shown. Accordingly, the scope disclosed should not be considered limited to the specific arrangement of steps shown in the flowcharts.

[0017] Although multiple dependent claims are not introduced, it would be apparent to one of ordinary skill that the subject matter of the dependent claims of one or more embodiments may be combined with other dependent claims.

[0018] One or more embodiments of the present disclosure are directed to compositions, systems, and methods for enrichment of ore materials, such as a molybdenum-containing ore concentrate (or “molybdenum concentrate”) thereof. For example, in one or more embodiments, methods for selectively removing one or more components (e.g., gangue and impurities) to improve ore grade, selectively removing gangue or impurities from ore to improve processing, extracting metals of value from gangue are described (e.g., as leaching processes). As one of ordinary skill may appreciate, the term “gangue” as used herein refers to the material proximate to or in which ore is found having relatively little value as compared to the ore material.

[0019] A method in accordance with the present disclosure may include solubilizing of select metals and / or impurities (e.g., non-metal components) from a molybdenum concentrate, which can include molybdenum-containing ore materials, such as ore tailings and / or from ore substrates and / or gangue material. For example, one or more embodiments may include using an extraction composition to selectively solubilize impurities including, but not limited to, fluorine (F), iron (Fe), copper (Cu), lead (Pb), magnesium (Mg), aluminum (Al), silicon (Si), arsenic (As), calcium (Ca), Zinc (Zn) among others, or combinations thereof from molybdenum concentrate. A method may include introducing solid molybdenum concentrate and a liquid extraction composition (e.g., a liquid biosolvent) to a container or system for an agitated leach. The selective solubilization of such embodiments is achieved while keeping molybdenum in the solid ore material, thereby improving the purity of molybdenum in the treated ore material.

[0020] A leachate with solubilized gangue material can be separated from the solids including the metal of value (i.e., molybdenum). The impurities may be removed from the solution to regenerate an extraction composition (e.g., a biosolvent), which can bePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1reused with a new untreated molybdenum concentrate (e.g., in an agitated leach). In some embodiments, the selective solubilization of metals and / or cations from molybdenum-containing ore materials may support carbon sequestration.

[0021] Organic acids, such as citric acid and mixtures of organic acids including gluconic and oxalic acid, have been used to solubilize certain atoms from ore materials. Previously, citric acid was often found to solubilize iron atoms and / or non-targeted atoms, which decreases the value of the ore material in further downstream processes. However, advantageously, one or more embodiments of the present disclosure unexpectedly show selective removal of Al, Si, Cu, F, Pb, As, Mg, Ca, Zn, and / or Fe, relative to other components including, but not limited to, molybdenum from molybdenum-containing ore materials (e.g., a molybdenum concentrate), which significantly improves the value of the molybdenum material in further downstream processes.

[0022] The composition, system, and / or method of one or more embodiments may be directed to the enrichment or upgrading of molybdenum ore materials by selectively removing one or more components, including, but not limited to, Al, Si, Cu, F, Pb, As, Mg, Ca, Zn, and / or Fe from a molybdenum concentrate. One or more embodiments herein may relate to a method for advantageously improving a grade of a molybdenum ore material by selectively reducing Al, Si, Cu, F, Pb, As, Mg, Ca, Zn, and Fe from the molybdenum ore material (e.g., a molybdenum concentrate). This selectivity may be achieved via solubilization of a component that can include one or more of Al, Si, Cu, F, Pb, As, Mg, Ca, Zn, and Fe while keeping most of the metals of value (e.g., molybdenum) in the solid ore material.

[0023] As used herein, the term “organic acid” may include an individual organic acid and / or mixtures of organic acids that are produced by microbes (e.g., in a biobroth), or organic acids from other biological sources (e.g., in a plant produced biobroth), or organic acids that are synthetically made. The “organic acid” as used throughout this disclosure can include a mixture of an organic acid and the respective conjugate base.

[0024] As used herein, the terms “biosolvent” and “biobroth” refer to a solution including inorganic and / or organic acids and their respective conjugate bases, one or more biobroths, ionic liquids, or any combination thereof. The biosolvent of one or more embodiments may be either derived biologically or synthetically and may or mayPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1not include silicase and / or other enzymes. The term “biobroth” may refer to a solution produced and obtained from a natural and / or engineered organic acid-producing microbe, such as via a fermentation process, a natural and / or engineered organic acidproducing plant, or combinations thereof. The organic acid-producing microbe may produce an organic acid or a mixture of organic acids. The organic acid-producing microbe may produce one or more organic acids and one or more components, such as primary metabolites, secondary metabolites, antibodies, salts, ions, organelles, cellular components, extracellular components, biomolecules (e.g., polysaccharides, proteins, enzymes, amino acids, nucleic acids, lipids, carbohydrates, among others), or any combination thereof. The term “engineered microbe” may be a microbe that has been altered, such as with genetic engineering, for example, to modulate acid or other biobroth component production.

[0025] The terms “biosolvent” and “biobroth” may refer to a complex mixture of components derived from an organism, such as a broth obtained from a culture of a microbe, such as a fungus. The complex mixture can include inorganic and / or organic acids and their respective conjugate bases, ionic liquids, amino acids, cellular components derived from a microbe, extracellular components derived from a microbe, or any combination thereof. For example, the biobroth can include one or more enzymes, such as silicase. The natural and / or engineered microbe may include, but is not limited to, a microorganism of a genus selected from the group consisting of Aspergillus, Acetobacter, Bacillus, Propionibacterium, Corynebacterium, Rhizopus, Clostridium, Fusobacterium, Pseudomonas, Bifidobacterium, Saccharomyces, Enterobacter , Escherichia (e.g., Escherichia coll), and combinations thereof. As a nonlimiting example, the biobroth of one or more embodiments may be obtained from an Aspergillus spp. culture, such as a supernatant, a cell lysate, or combinations thereof.

[0026] As used herein, the term “inorganic acid” may be an acid that is derived from an inorganic compound (e.g., a mineral acid). The inorganic acid of one or more embodiments may include a protic acid.

[0027] As used herein, the term “gangue” refers to the impurity material that surrounds or is closely mixed with a wanted mineral in an ore deposit. Although termed “impurities” it is understood that value can be obtained from certain elements in thePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1gangue, and that such elements are impurities with respect to the wanted material in the ore deposit.

[0028] As used herein, the phrase “total mass loss” refers to the difference between a mass of a material after a certain treatment from a mass of a material before a certain treatment. For example, “total mass loss” may refer to a change in mass in an ore material before and after exposure to an extraction process in accordance with one or more embodiments.

[0029] As used herein, the phrase “total volume loss” refers to the difference between a volume of a material after a certain treatment from a volume of a material before a certain treatment. For example, “total volume loss” may refer to a change in volume in an extraction composition (e.g., before an extraction process as compared to an extracted solution that has been separated from solid material obtained after an extraction process) in accordance with one or more embodiments.

[0030] As used herein, the terms “load” or “leach” refers to the process of transferring one or more components from a first material to a second material. For example, the process of “loading” or “leaching” may include transferring one or more components from an ore material to an extraction composition that may be a leaching composition in accordance with one or more embodiments.

[0031] As used herein, the terms “strip” or “separate” refers to the removal of a first component (e.g., an impurity component, a biobroth, a biosolvent, an organic acid, etc.) from a second component (e.g., a mixture, solution, ore material, etc.).

[0032] As used herein, the terms “recycle” or “regenerate” refers to the recovery of a material (e.g., a component of an extraction composition, an extraction composition, or both such that the material may be reused in subsequent processes.

[0033] As disclosed herein, one or more embodiments may relate to combinations of inorganic acids and organic acids and conjugate bases, and optionally one or more additives, at adjusted pH and oxidation-reduction potential to selectively (a) remove impurities from ore to improve ore grade, (b) remove impurities from ore to improve processing, and (c) extract metals of value from gangue. These combinations selectively solubilize impurities to a greater extent than previous work and open the possibility of using these technological improvements in mining industry processes.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1

[0034] EXTRACTION COMPOSITION AND MIXTURE

[0035] In one aspect, embodiments herein relate to an extraction composition. In another aspect, embodiments herein relate to an extraction mixture including an extraction composition and an ore material. As used herein, the term “ore material” refers to a molybdenum concentrate, which can include one or more of a molybdenum- containing ore, molybdenum concentrate after flotation, molybdenum ore tailings, waste rock including molybdenum, among other molybdenum ore materials. The ore material may include solids containing or derivatives of molybdenum sulfides, molybdenum oxides, molybdenum carbonates, molybdenum hydroxides, among others, and combinations thereof. The molybdenum concentrate of one or more embodiments may include molybdenum sulfide. The molybdenum concentrate of one or more embodiments may include molybdenum-containing ore tailings, a concentrate derived from molybdenum-containing ore tailings, a molybdenum concentrate obtained prior to a flotation process, a molybdenum concentrate following a flotation process, or any combination thereof. A concentrate of the molybdenum-containing ore may include molybdenum-containing ore tailings.

[0036] The extraction composition may include one or more selected from a biosolvent, a biobroth, or any combination thereof. The extraction composition may include a biosolvent that has been synthetically produced, such as a biosolvent prepared in a laboratory environment. The extraction composition may include a biobroth obtained from a natural and / or engineered microbe or another biological source (e.g., plant derived). The extraction composition may be a biosolvent or a biobroth. The extraction composition may be configured to selectively extract one or more components from a molybdenum concentrate. In one or more embodiments, the extraction composition is configured to extract a Pb component, a Mg component, an Al component, an Fe component, a Si component, a F component, a Cu component, an As component, a Ca component or any combination thereof. In some embodiments, the extraction composition is configured to selectively extract a magnesium component with an iron component being solubilized to a lesser extent.

[0037] The extraction composition may include an aqueous solution. The aqueous solution includes water. The water may include, but is not limited to, Milli-Q water, distilled water, deionized water, tap water, fresh water from surface or subsurfacePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1sources, formation water, natural and synthetic brines, brackish water, natural and synthetic sea water, potable water, non-potable water, process water, other waters, and combinations thereof, that are suitable for use for treating a molybdenum-containing ore and / or a concentrate thereof. As used herein, “Milli-Q water” is water purified using a Millipore Milli-Q laboratory water system. In one or more embodiments, the basic Milli-Q water meets ASTM Type I standards, having greater than 18.0 MegaOhms»centimeter (Mf cm) resistivity at 25EC due to ions, less than 10 parts per billion (ppb) organics, less than 0.03 endotoxin per milliliter (EU / mL) of pyrogens, less than 1 particulate per mL (pariculate / mL), less than 10 ppb silica, and less than 1 bacterial colony forming unit per mL (cfu / mL).

[0038] In one or more embodiments, the water used may naturally contain contaminants, such as salts, ions, minerals, organics, and combinations thereof, as long as the contaminants do not interfere with extraction of target metal atoms and / or impurities from an ore material. In one or more embodiments, one or more additives may be added to the extraction composition to enhance the selectivity for one or more components, efficiency for removing the one or more components, or combinations thereof.

[0039] In one or more embodiments, the aqueous solution includes a first organic acid, an optional additional organic acid, and an optional inorganic acid. The extraction composition may include a plurality of organic acids. For example, the extraction composition may include two or more, three or more organic acids, four or more organic acids, five or more organic acids, six or more organic acids, eight or more organic acids, or ten or more organic acids, etc. The first organic acid may include one or more organic acids, two or more organic acids, or a plurality of organic acids. In some embodiments, when the first organic acid includes two or more organic acids, a main organic acid component may be present as compared to a minor organic acid component.

[0040] In some embodiments, the first organic acid, the optional additional organic acid, or both are naturally occurring such that at least a portion of the aqueous solution may be or may be isolated from a “biobroth.” In one or more embodiments, the biosolvent includes purified (e.g. purified individual organic acids and / or purified mixtures of organic acids) or mixtures of unpurified organic acids. The biosolvent of one or more embodiments may be used with single or mixtures of inorganic acids. ThePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1first organic acid may be an acid selected from the group consisting of citric acid, malic acid, formic acid, lactic acid, acetic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic, and combinations thereof. As a nonlimiting example, the first organic acid may include oxalic acid, citric acid, lactic acid, gluconic acid, tartaric acid, ascorbic acid, or combinations thereof as a minor component. In one or more embodiments, the first organic acid includes oxalic acid, citric acid, lactic acid, gluconic acid, tartaric, or combinations thereof as a main component. The first organic acid may be gluconic acid, citric acid, or lactic acid. In some embodiments, the first organic acid, the optional additional organic acid, or both are synthetically produced, such as in a laboratory.

[0041] In one or more embodiments, the first organic acid is present in the aqueous solution in a concentration in a range between 0.01 M (Molar) to 4 M. For example, the concentration of the first organic acid may be in a range having a lower limit of any one of a non-zero value, 0.010 M, 0.015 M, 0.020 M, 0.025 M, 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M, 0.250 M, 0.5 M, 0.6 M, 0.8 M, 0.9 M, 1 M, 1.5 M, 2M, 2.5 M, 3M, 3.5 M, and 3.9 M and an upper limit of any one of 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M, 0.250 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, 1.0 M, 1.1 M, 1.2 M, 1.5 M, 2 M, 2.5 M, 3 M, 3.5 M, 3.9 M, 3.95 M, and 4 M, where any lower limit can be paired with any mathematically compatible upper limit. As a non-limiting example, the concentration of the first organic acid may be present in a biosolvent at a concentration in a range from a non-zero value to 2.5 M, such as 0.05 M to 2.5 M.

[0042] The additional organic acid may include one or more organic acids, two or more organic acids, or a plurality of organic acids. In some embodiments, when the additional organic acid includes two or more organic acids, a main organic acid component may be present as compared to a minor organic acid component. The additional organic acid may include an acid selected from the group consisting of citric acid, malic acid, formic acid, lactic acid, acetic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid, and combinations thereof.

[0043] In one or more embodiments, when the first organic acid is, or includes as a main component, oxalic acid, the additional organic acid comprises an acid selectedPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1from the group consisting of gluconic acid, oxalic acid, lactic acid, acetic acid, malic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid, and combinations thereof. In one or more embodiments, when the first organic acid is, or includes as the main component, gluconic acid, the additional organic acid comprises an acid selected from the group consisting of oxalic acid, lactic acid, acetic acid, citric acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid, and combinations thereof.

[0044] In one or more embodiments, the additional organic acid is present in the aqueous solution in a concentration in a range between 0 M to 3.0 M. For example, the concentration of the first organic acid may be in a range having a lower limit of any one of 0 M, a non-zero value, 0.005 M, 0.010 M, 0.015 M, 0.020 M, 0.025 M, 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M, 0.250 M, 0.5 M, 0.6 M, 0.8 M, and 0.9 M and an upper limit of any one of 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M, 0.250 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, 1.0 M, 1.1 M, 1.5 M, 2.0 M, 2.1 M, 2.2 M, 2.5 M, 2.75 M, 2.9 M, and 3.0 M where any lower limit can be paired with any mathematically compatible upper limit.

[0045] In some embodiments, a ratio of the first organic acid to the additional organic acid is a concentration ratio in a range from 1 :0 to 1 : less than or equal to (<) 1. In one or more embodiments, the concentration ratio of the first organic acid to the additional organic acid is in a range having a lower limit of any one of 1:0, 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, and 1:0.75, and an upper limit of any one of 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1 :0.5, 1 : 0.6, 1 :0.7, 1 :0.75, 1 :0.8, 1 :0.85, 1 :0.9, 1 :0.95, 1 :0.99, and 1 : 1, where any lower limit can be paired with any mathematically compatible upper limit.

[0046] In one or more embodiments, the extraction composition includes an inorganic acid. The inorganic acid may include an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and combinations thereof. The inorganic acid may be included in the aqueous fluid in an amount in a range from 0 M or a non-zero concentration to 3.0 M. For example, the concentration of the inorganic acid may be in a range having a lower limit of any one of 0 M, 0.005 M, 0.010 M, 0.015 M, 0.020 M, 0.025 M, 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M,PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO10.250 M, 0.5 M, 0.6 M, 0.8 M, and 0.9 M and an upper limit of any one of 0.05 M, 0.075 M, 0.09 M, 0.10 M, 0.125 M, 0.150 M, 0.250 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, 1.0 M, 1.1 M, 1.5 M, 2.0 M, 2.1 M, 2.2 M, 2.5 M, 2.75 M, 2.9 M, and 3.0 M, where any lower limit can be paired with any mathematically compatible upper limit.

[0047] The extraction composition of one or more embodiments has a pH in a range from a non-zero value to 7. In some embodiments, the pH of the extraction composition is in a range having a lower limit of any one of a non-zero value, 0.05, 0.09, 0.10, 0.2, 0.25, 0.5, 0.75, 1, 1.2, 1.5, 1.7, 1.9, 2.0, 2.2, 2.5, 2.7, 2.9, 3.0, 3.2, 3.5, 3.7, 3.9, 4.0, 4.5, 5.0, and 6.0, and an upper limit of any one of 1, 1.2, 1.5, 1.7, 1.9, 2.0, 2.2, 2.5, 2.7, 2.9, 3.0, 3.2, 3.5, 3.7, 3.9, 4.0, 4.2, 4.5, 5.0, 5.5, 6.0, 6.5, and 7.0, where any lower limit can be paired with any mathematically compatible upper limit. As a non-limiting example, a pH of an extraction composition may be in a range of 0.09 to 4.2, such as from 0.1 to 4.0.

[0048] METHOD FOR EXTRACTING ONE OR MORE COMPONENTS FROM A MOL YB DENUM-CONTAINING ORE MATERIAL

[0049] In another aspect, embodiments herein relate to a method for extracting a metal from an ore material, such as a molybdenum concentrate. The method may include leaching an impurity from the ore material. In one or more embodiments, the method includes providing an extraction composition and an ore material. The method may include selectively solubilizing an impurity component including one or more minerals, salt, or any combination thereof having Pb, F, Fe, Al, Mg, Si, Ca, As, Zn, and Cu from a molybdenum concentrate into an extraction composition.

[0050] The method may include preparing the extraction composition by obtaining the first organic acid and, optionally, the additional organic acid, the inorganic acid, or combinations thereof. One or more organic acids of the extraction composition may be obtained via synthetic laboratory procedures. The first organic acid, the additional organic acid, the inorganic acid, or combinations thereof may be microbially produced, plant produced, or both such that the first organic acid, the additional organic acid, the inorganic acid, or combinations thereof may be collected from a microbe, a plant, or both (e.g., in the form of a biobroth). In some embodiments, the first organic acid, the additional organic acid, the inorganic acid, or combinations thereof is collected from aPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1plant extract, a microbial cell lysate, a microbial supernatant, or combinations thereof. One or more organic acids of the extraction composition may be purified.

[0051] The method may include forming a mixture including an extraction composition and an ore material. The extraction composition and the ore material may be as previously described herein. An extraction composition, an ore material, or both may be introduced (or added) to an extraction unit of an extraction zone, such as an agitated leaching tank of an extraction system. In some embodiments, the extraction zone is a laboratory extraction unit that is a container capable of being manually agitated or stirred for the extraction process. The extraction unit may be a container capable of being automatically agitated or stirred for the extraction process, such as with a control system in electrical connection with the extraction unit. In some embodiments, the method includes providing an extraction system capable of performing one or more leaching processes. The extraction system may include one or more flow lines, valves, pumps, storage tanks, an extraction zone including an extraction unit (e.g., one or more agitated leaching tanks), among one or more additional units known to those skilled in the art for mineral leaching. One or more components of the extraction system may be an add-on component capable of being incorporated to one or more industrial mining processes.

[0052] In some embodiments, the extraction zone includes a plurality of leaching tanks positioned in parallel or in series. In one or more embodiments, one or more leaching tanks of the plurality of leaching tanks are in fluid communication with a subsequent leaching tank of the plurality of leaching tanks. In some embodiments, plurality of leaching tanks are positioned in a cross- or counter-current design, in locked cycle leaching, or combinations thereof.

[0053] The ore material may be added to the extraction zone in an amount in a range from 5 to 70 wt% based on the total weight of the extraction mixture. The ore material may be added to the extraction unit in an amount in a range having a lower limit of any one of 5 wt%, 7.5 wt%, 8 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt %, 40 wt%, 45 wt%, 48 wt%, and 50 wt % and an upper limit of any one of 15 wt%, 20 wt%, 25 wt%, 30 wt %, 40 wt%, 45 wt%, 48 wt%, 50 wt%, 52 wt%, 55 wt%, 57 wt%, 60 wt%, 62 wt%, 65 wt%, 68 wt%, and 70 wt%, where any lower limit can be paired with any mathematically compatible upper limit.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1

[0054] The extraction composition may be added to the extraction unit in an amount in a range from 30 to 95 wt% based on the total weight of the extraction mixture. The extraction composition may be added to the extraction unit in an amount in a range having a lower limit of any one of 30 wt%, 35 wt%, 38 wt%, 40 wt%, 42 wt%, 45 wt%, 47.5 wt%, 48 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt %, 70 wt%, 75 wt%, 78 wt%, and 80 wt % and an upper limit of any one of 55 wt%, 60 wt%, 65 wt%, 70 wt %, 75 wt %, 80 wt%, 85 wt%, 88 wt%, 90 wt%, 91 wt%, 92 wt%, 93 wt%, 94 wt%, and 95 wt%, where any lower limit can be paired with any mathematically compatible upper limit.

[0055] The mixture of the extraction composition and the ore material may be agitated in the extraction zone. The mixture may be heated while agitating to promote the selective removal of one or more components from the ore material. Agitating the extraction mixture in the extraction zone may form an extracted solution (or a “liquid mixture”) including the organic acid, the magnesium component, and, optionally, one or more additional components extracted from the molybdenum-containing ore and / or concentrate thereof. The extraction mixture may be agitated in the extraction unit for a period of time in a range having a lower limit of any one of 0.1 hour (h), 0.25 h, 0.5 h, 1 h, 2 h, 3, h, 4 h, 5 h, 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, and 20 h, and an upper limit of any one of 4 h, 5 h, 6 h, 7 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, and 26 h, where any lower limit can be paired with mathematically compatible upper limit. The mixture may be heated (e.g., in the extraction unit) at a temperature in a range from 15 °C, 20 °C, 25 °C, 27 °C, 28 °C, 29 °C, 30 °C, 35 °C, 40 °C, 45 °C, 50 °C, 60 °C, 70 °C, 80 °C, 90 °C, 95 °C, and 99 °C and an upper limit of any one of 35 °C, 40 °C, 45 °C, 50 °C, 55 °C, 60 °C, 65 °C, 70 °C, 75 °C, 80 °C, 90 °C, 95 °C, 99 °C, 100 °C, and 105 °C, where any lower limit can be paired with any mathematically compatible upper limit. In a non-limiting example, the method may include adjusting a temperature of the extraction zone to a temperature in a range from 20 to 100 °C and performing the extraction zone for a period of time in a range from 0.5 to 24 hours.

[0056] During the agitating step, one or more components may be selectively transferred from the ore material to the extraction composition, thereby forming an extraction mixture including a treated ore material and an extracted solution. The extracted solution of one or more embodiments includes the extraction composition andPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1one or more components removed from the ore material (i.e., an impurity component) that may include one or more selected from a Pb component, a Cu component, a Mg component, an Fe component, a Si component, an Al component, a F component, an As component, a Ca component, among other components (e.g., a lesser amount of molybdenum component). In some embodiments, the one or more components can include a Fe component, and / or a molybdenum component as relatively minor components compared to the F, Pb, Cu, Mg, Al, As, Ca, Zn, and Si components. In such embodiments, the method of extraction is selective for the F, Pb, Cu, Mg, Al, As, Ca, Zn, and / or Si components removal from the ore material.

[0057] The one or more components may include an impurity in the form of a mineral, an oxide, a salt, or any combination thereof. The Cu component may include one or more of a Cu mineral, elemental Cu, a Cu oxide, a Cu salt having a Cu cation, or any other form of Cu. The Ca component may include one or more of a Ca mineral, elemental Ca, a Ca oxide, a Ca salt having a Ca cation, or any other form of Ca. The As component may include one or more of a As mineral, elemental As, a As oxide, a As salt having a As cation, or any other form of As. The Mg component may include one or more of a Mg mineral, elemental Mg, a Mg oxide, a Mg salt having a Mg cation, or any other form of Mg. The Al component may include one or more of an Al mineral, elemental Al, an Al oxide, an Al salt having an Al cation, or any other form of Al. The Si component may include one or more of a Si mineral, elemental Si, a Si oxide, a Si salt, or any other form of Si. The Fe component may include one or more of a Fe mineral, elemental Fe, a Fe oxide, a Fe salt having a Fe cation, or any other form of Fe. The F component may include one or more of a fluoride ion, diatomic fluorine, or any other form of F. A molybdenum component may include a molybdenum mineral, elemental molybdenum, a molybdenum oxide, a molybdenum salt having a molybdenum cation, or any other form of molybdenum.

[0058] The treated ore material may have a reduced concentration of one or more impurity components (e.g., one or more components described previously herein) as compared to the untreated ore material, such as a percent of the one or more impurity component concentration(s) in the untreated ore material. The method of one or more embodiments may reduce the one or more impurity components in a treated ore material as compared to an untreated ore material by a relative percent. The relative percent ofPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1an impurity component reduced in a treated ore material as compared to an untreated ore material may be in a range having a lower limit of any one of a non-zero value, 1 %, 2 %, 5 %, 10 %, 15 %, 20 %, 25 %, 30 %, 35 %, 40 %, 45 %, 50 %, 55 %, 60 %, 65 %, 70 %, 75 %, 80 %, 85 %, and 90 %, and an upper limit of any one of 10 %, 20 %, 25 %, 30 %, 35 %, 40 %, 45 %, 50 %, 55 %, 60 %, 65 %, 70 %, 75 %, 80 %, 85 %, 90 %, 95 %, 98 %, 99 %, 99.5 %, 99.8 %, 99.9 %, and 100 % where any lower limit can be paired with any mathematically compatible upper limit.

[0059] In one or more embodiments, an impurity component may be present in an extracted composition (i.e., a leachate) in an amount having a range from 0.05 wt% to 100 wt%. An amount of the impurity component may be present in a leachate in an amount having a lower limit of any one of a non-zero value, 0.05 wt%, 1 wt%, 2 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, and 90 wt%, and an upper limit of any one of 10 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, 98 wt%, 99 wt%, 99.5 wt%, 99.8 wt%, 99.9 wt%, and 100 wt%, where any lower limit can be paired with any mathematically compatible upper limit.

[0060] The method of one or more embodiments may reduce the one or more impurity components in an ore material to provide a total mass loss of the impurity component of about 1 wt% to about 100 wt%. The reduced one or more components content in an ore material may be reduced by an amount in a range having a lower limit of any one of 1 wt%, 2.5 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, and 75 wt% and an upper limit of any one of 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 95 wt%, and 100 wt%, where any lower limit can be paired with any mathematically compatible upper limit.

[0061] In one or more embodiments, the untreated ore material has one or more impurity component content in a range from 0.01 wt% to 85 wt%. The untreated ore material may have a concentration of one or more impurity components in a range having a lower limit of any one of 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.25 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, and 60 wt% and an upper limit of any one of 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, and 85 wt%, where any lower limit can be paired with any mathematically compatible upper limit.

[0062] In some embodiments, the treated ore material has a reduced one or more impurity component content as compared to the untreated ore material. In one or more embodiments, the treated ore material has a reduced impurity component content in a range from 0 wt% to 85 wt%. The treated ore material may have a concentration of one or more impurities in a range having a lower limit of any one of 0 wt%, a non-zero value, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.25 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, and 60 wt% and an upper limit of any one of 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, and 85 wt%, where any lower limit can be paired with any mathematically compatible upper limit. As a non-limiting example, the reduced one or more impurity component concentration in the treated ore material may be in a range from 0 to 85 wt%. In one or more embodiments, the amount of impurity components in a treated ore material is less than 85 wt%, less than 80 wt%, less than 75 wt%, less than 50 wt%, less than 25 wt%, or less than 10 wt%. In some embodiments, the ore material is upgraded by the selective removal of one or more of Pb, Fe, Cu, Mg, Al, F, and Si, while retaining metals of value (e.g., molybdenum) in the solid ore material.

[0063] In embodiments where an impurity is found in an ore material in a relatively low amount (e.g., about 0.001 wt% to about 5 wt%) and reduces the overall financial value of the ore material such impurities may be referred to as penalty elements (or “penalty components”), which may be considered non-applicable for further processing. In embodiments described herein, all penalties are impurities but not all impurities are penalties. These penalty elements may render an ore material unsuitable for further use. Some non-limiting examples of penalty elements include one or more selected from Pb, Fe, Cu, Mg, arsenic (As), chromium (Cr), Al, F, and Si, among others. In embodiments in which penalty elements are present in a relatively low amounts in the ore material, the method may advantageously remove one or more impurityPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1components in a relative percentage of 20 % or more, 30 % or more, 40 % or more, 50% or more, 60 % or more, 70 % or more from the ore material. In embodiments where the ore material is or includes gangue, the method may advantageously increase the value of the ore material via removal of the penalty element while maintaining a relatively large percentage of gangue (e.g., 95 %).

[0064] In one or more embodiments, the untreated ore material has one or more impurity component content in a range from 0.001 wt% to 99.999 wt%. The treated ore material may have a concentration of one or more impurity components in a range having a lower limit of any one of 0.001 wt%, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.25 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, and 60 wt% and an upper limit of any one of 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 92.5 wt%, 95 wt%, 97.5 wt%, 99 wt%, 99.5 wt%, 99.9 wt%, 99.99 wt%, and 99.999 wt%, where any lower limit can be paired with any mathematically compatible upper limit.

[0065] In some embodiments, the treated ore material has a reduced one or more impurity component content as compared to the untreated ore material. In one or more embodiments, the treated ore material has a reduced impurity component content in a range from 0 wt% to 100 wt%. The treated ore material may have a concentration of one or more impurities in a range having a lower limit of any one of 0 wt%, 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.25 wt%, 0.5 wt%, 1.0 wt%, 1.5 wt%, 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, and 60 wt% and an upper limit of any one of 2.0 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, 92.5 wt%, 95 wt%, 96 wt%, 97 wt%, 98 wt%, 99 wt%, 99.95 wt%, 99.99, and 100 wt%, where any lower limit can be paired with any mathematically compatible upper limit. As a non-limiting example, the reduced one or more impurity component concentration in the treated ore material may be in a range from 0 to 95 wt%. In one or more embodiments, the amount of impurity components in a treated ore material is less than 98 wt%, less than 95 wt%, less than 90 wt%, 85 wt%, less than 80 wt%, less than 75 wt%, less than 50 wt%, less than 25 wt%, or less than 10PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1wt%. In some embodiments, the ore material is upgraded by the selective removal of one or more of Pb, Fe, Cu, Ca, As, Mg, Al, F, and Si, while retaining metals of value (e.g., molybdenum) in the solid ore material.

[0066] A method of one or more embodiments may include separating a treated ore material from the extraction mixture to collect the treated ore and the extracted solution. The treated ore material may be in the form of a solid such that the separation of the treated ore material from the extracted solution can be performed by a method for separating solids from liquids known to those skilled in the art. In some embodiments, the separation includes decanting, filtration, filtration, membrane filtration, gravity filtration, centrifugation, among others known to those skilled in the art. The separated treated ore material may be washed and dried. In some embodiments, the separated treated ore is transferred for further processing.

[0067] The separation of the one or more components described previously, and if present, one or more additional metallic components (e.g., a molybdenum component) from the extracted solution may be performed such that the extraction composition is regenerated. The extracted solution may be fed to a processing unit to regenerate the extraction composition. In some embodiments, separating the one or more components from the extracted solution includes extracting the one or more components from the extracted solution with one or more water treatment techniques. The extraction of the one or more components from the extracted solution may include performing one or more water treatment techniques selected from the group consisting of feeding the extracted solution through an ion exchange system, extracting the impurity component via solvent extraction, chromatography, filtration, nanofiltration, membrane filtration, osmotic separation (e.g., via reverse osmosis), using adsorption and / or absorption materials, precipitation including, but not limited to, pH control, precipitation via ion addition (e.g., anion addition such as via the addition of phosphates, sulfates, among other anions to the extracted solution), among other precipitation techniques known to those skilled in the art, electrodeionization, and combinations thereof. The water treatment technique may include introducing the extracted solution to an ion exchange column, solvent extraction (e.g., biphasic solvent extraction), or both.

[0068] The biosolvent, the biobroth, one or more components of the biosolvent and / or the biobroth (e.g., an organic acid), one or more metals of value, or combinationsPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1thereofmay be separated from the extracted solution via feeding the extracted solution to a system configured to perform chromatography, filtration, nanofiltration, membrane filtration, osmotic separation (e.g. via reverse osmosis), using adsorption and / or absorption materials, precipitation including, but not limited to, pH control, precipitation via ion addition (e.g., anion addition such as via the addition of phosphates, sulfates, among other anions to the extracted solution), among other precipitation techniques known to those skilled in the art, electrodeionization, solvent extraction, ion exchange chromatograph and combinations thereof.

[0069] In one or more embodiments, one or more metals of value (e.g., molybdenum) are removed from the extracted solution via the one or more water treatment techniques. In one or more embodiments, a molybdenum component is selectively removed from the extracted solution, the extraction mixture, or both. As a non-limiting example, the molybdenum component may be removed (e.g., via electrowinning or other extraction methods) and recovered for further processing of an enriched solid molybdenum concentrate. In a non-limiting example, the extracted molybdenum component may be added to the enriched molybdenum material recovered from the extraction mixture. Advantageously, one or more embodiment methods may allow for a reduced or minimal loss of molybdenum from a molybdenum ore material even if relatively low amounts of leach into the extracted solution.

[0070] In some embodiments, separating the extraction composition or one or more components of the extraction composition includes extracting the extraction composition or one or more components of the extraction composition from the extraction mixture, the extracted solution, or both. The extraction may be performed with one or more water treatments techniques selected from a group consisting of centrifugation, feeding the extracted solution through an ion exchange system, extracting the magnesium component via solvent extraction, chromatography, nanofiltration, filtration, membrane filtration, using adsorption and / or absorption materials, precipitation including, but not limited to, pH control, precipitation via ion addition (e.g., anion addition such as via the addition of phosphates, sulfates, among other anions to the extracted solution), among other precipitation techniques known to those skilled in the art, electrodeionization, and combinations thereof.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1

[0071] An organic acid component of the extraction composition, a biosolvent component of the extraction composition, a biobroth component of the extraction composition, or combinations thereof may be separated from the extracted solution and / or the extraction mixture and may subsequently be used to form a regenerated extraction composition. For example, at least a portion of an extraction composition may be separated from the extraction mixture, the extracted solution, or combinations thereof by pH control and precipitation, precipitation including, but not limited to, pH control, precipitation via ion addition (e.g., cation addition such as via the addition of organic cations to the extracted solution), among other precipitation techniques known to those skilled in the art, electrodeionization, chromatography, ion exchange, or filtration. After this, the extracted portion may be recovered as a solid precipitate, in an aqueous solution, or both.

[0072] The regenerated extraction composition may be recovered and reused for subsequent extractions. For example, when the extracted portion is recovered as a solid precipitate, the precipitate may be redissolved to form the regenerated extraction composition. In some embodiments, the method includes repeating the extracting, such as with the regenerated extraction composition. In some embodiments, the regenerated extraction composition can be modified after recovery and prior to the repeating the extraction to add an organic acid, an inorganic acid or both, dilute the extraction composition, adjust a pH of the extraction composition (e.g., with a pH adjusting agent that does not interfere with the extraction process), or any combination thereof. The regenerated extraction composition may be transported (i.e., introduced) to the extraction zone, such that the regenerated extraction composition is recycled.

[0073] In one or more embodiments, the method includes altering extraction composition to alter the selective solubilization of an impurity element. Altering the extraction composition may include selecting the first organic acid and / or a main component of the extraction composition based on the impurity to be removed.

[0074] A simplified diagram of a non-limiting extraction process and recycling process may be as shown in FIG. 1. As shown in system 100 of FIG. 1 a molybdenum - containing ore material, an extraction composition, or both may be introduced to extraction zone 102 via feed line 101. An extracted solution may be introduced to component recovery zone 104 via input line 103 A. A treated metal ore material may bePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1recovered from extraction zone 102 via output line 103B. The treated ore material may be analyzed, such as weighed to determine a total mass difference from the untreated ore material. The component recovery zone 104 may include a component to selectively remove one or more selected from Pb, Fe, As, Ca, Cu, Mg, Al, F, Zn, and Si, among other metal atoms (e.g., via line 105B) from the extracted solution such that the extraction composition is regenerated. In one or more embodiments, F may be removed from a Si-containing mineral or ore material.

[0075] One or more impurity components may be separated (or “stripped”) from the extracted solution along with one or more additional metal components (e.g., an iron component, a nickel component, a cobalt component, among others) such that the extraction composition and a mixture of metallic components may be recovered. The magnesium component may be a main component of the mixture of metallic components. In one or more embodiments, each of the Pb, Fe, Cu, Mg, Al, F, Ca, As, Zn, and / or Si components and, if present, one or more additional metallic components (e.g., molybdenum) are recovered separately from the extracted solution as recovered components. In some embodiments, the recovered component has a purity in a range from 5% or greater, 10% or greater, 25% or greater, or 50% or greater. The recovered component may have a purity in a range from 5% to 100%. For example, the recovered component may have a purity in a range having a lower limit of any one of 1%, 5%, 7.5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, and 50%, and an upper limit of any one of 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 98%, 99%, 99.9%, 99.99%, and 100%, where any lower limit can be paired with any mathematically compatible upper limit.

[0076] The regenerated extraction composition may be fed to one or more extraction units of the extraction zone, such as via one or more flow lines (e.g., line 105 A) in fluid communication with the metal atom recovery zone 104 and the extraction zone 102. In some embodiments, the regenerated extraction composition is transported to a storage tank to be used in a subsequent extraction process, for example. In some embodiments, it may be determined via analysis of the extraction composition, recovery efficiency of one or more metal atoms, or both, that the regenerated extraction composition requires additional components (e.g., one or more additional components of the extraction composition). The analysis may be performed with a method or system capable ofPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1measuring metal atoms in a solid sample (e.g., an ore material), a liquid sample (e.g., an extracted solution, a regenerated extraction composition), or both. Analysis of one or more embodiments may include determination of total mass loss of the untreated ore material, analysis of a sample (e.g., an extracted solution sample) with absorption spectroscopy, fluorescence spectroscopy, high performance liquid chromatography (HPLC), gas chromatography (GC), mass spectrometry (MS), Infrared Spectroscopy (IR), inductively coupled plasma - optical emission spectrometry (ICP-OES) of a solution, X-ray fluorescence (XRF) of a solid sample, X-ray Diffraction (XRD), Modal Mineralogy analysis (e.g., QEMSCAN® analysis), oxidation-reduction potential (ORP), pH, conductivity or combinations thereof.

[0077] A method of one or more embodiments may include providing a measurement system coupled to the extraction system to analyze one or more components of the extraction mixture, such as a regenerated extraction composition. The measurement system may include one or more components configured to perform the analytical methods including, but not limited to ICP-OES, absorption measurement, fluorescence measurements (e.g., excitation and / or emission), HPLC, IR, GC, MS, XRD, XRF, Modal Mineralogy (e.g., QEMSCAN®), ORP, pH, conductivity among others. The measurement system may include various pumps, flow control components, a control system, among other components. The measurement system may be configured to collect a sample and analyze one or more components of the extraction mixture e.g., a liquid sample of the extraction mixture) over set time intervals and time periods. In some embodiments, the analysis of a solid sample is performed at an off-site location after separation and collection from an extraction mixture.

[0078] In some embodiments, analysis of an extracted sample is carried out after each extraction in the extraction zone. Analysis of a regenerated extraction composition may be performed after processing through the metal atom recovery zone. In some embodiments, the extracted sample, the regenerated extraction solution, or both are continuously measured by one or more components of the extraction system. In some embodiments, the extraction system includes one or more sensors capable of collecting and / or transmitting data to a computer that may be a part of the extraction system or at an off-site location. In some embodiments, one or more parameters (e.g., recycled extraction composition make-up, temperature, pressure, residence time within thePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1extraction zone, etc.) is adjusted based on the data collected from the analytical measurements.

[0079] In some embodiments, an extraction composition storage tank 106 can be present in system 100 such that one or more components of the extraction composition may be introduced to the regenerated extraction composition via line 107. For example, an extraction composition make-up may be introduced to the regenerated extraction composition to regenerate the concentration of the acid(s) in the extraction composition, to increase the concentration of the extraction composition, or to dilute the extraction composition. In such embodiments, the adjusting of the regenerated extraction composition via introduction of the make-up may maintain or increase the extraction efficiency of target metal component(s), enhance the selectivity of target metal component s), or both.

[0080] In another aspect, embodiments herein relate to a method for improving a processing efficiency of an ore material. The method for improving a processing efficiency may include one or more steps of a method for extracting one or more impurity components from a molybdenum-containing ore material. The molybdenum - containing ore material may include a molybdenum concentrate as described previously. The method for improving a processing efficiency may include forming a mixture including an extraction composition and an ore material. The mixture may be as described previously. The method may include selectively removing one or more impurity components as described previously from the ore material.

[0081] The processing efficiency may be derived from the chemical processing of an enriched ore material to extract molybdenum (e.g., as elemental molybdenum). As a non-limiting example, the processing efficiency may refer to a conversion efficiency to produce molybdenum oxides (e.g., from molybdenum sulfides in a treated ore material). The processing efficiency may be derived from the conversion efficiency of molybdenum species within a treated concentrate to form molybdenum oxides. The conversion efficiency may be derived from the reduction efficiency of the molybdenum oxides with hydrogen gas to produce elemental molybdenum relative to the amount of molybdenum present in the enriched ore material. The chemical processing efficiency may be determined from the amount of elemental molybdenum recovered from afterPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1the molybdenum oxide conversion step and the reduction step relative to the amount of molybdenum present in the enriched ore material.

[0082] While the method may include one or more method steps as described above, one of ordinary skill in the art will appreciate that some or all of the blocks may be executed in different orders, may be combined or omitted, and some or all of the blocks may be executed in parallel. Furthermore, the blocks may be performed actively or passively. Alternative methods include the use of these combinations of organic acids and conjugate bases to selectively remove gangue from other molybdenum-containing materials, including, but not limited to, molybdenum carbonates, molybdenum oxides, molybdenum hydroxides, and combinations thereof. The methods according to the present invention can be used in ore processing applications to remove gangue from ore as part of a leach, separate, regenerate circuit.

[0083] The method of one or more embodiments may advantageously upgrade a molybdenum ore material (e.g., a molybdenum concentrate) as well as or better than traditional processes. The process of one or more embodiments may be cost-effective and can be adapted to equipment currently used in the mining industry. One or more embodiments of the present disclosure may advantageously improve the processing efficiency of the ore material after extraction as compared to traditional processes. Additionally, the compositions and methods of one or more embodiments unexpectedly alters the selective removal of a Pb, Fe, Cu, Mg, Al, F, As, Ca and Si components from a molybdenum ore material in a way that significantly differs operationally from how a more standard solvent (e.g., the inorganic acid, H2SO4) solubilizes atoms, salts, and / or minerals from a molybdenum ore material. Further, mixtures of certain concentrations of inorganic and organic acids may allow for reduced cost while retaining the advantage of selectively removing one or more of Pb, Fe, Cu, Mg, Al, F, As, Ca , Zn, and Si from molybdenum-containing ore material.

[0084] One or more embodiments of the present disclosure are advantageous as organic acids and their conjugate bases improve selective solubilization of impurities from ores. In some cases, addition of inorganic acids further improve the removal of gangue material and impurities. Another advantage demonstrated by the present invention is that using the disclosed process for molybdenum-containing ore material reduces the processing resources involved in the chemical processing of lithium-containing orePATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1materials, thereby permitting reduction in the carbon footprint and cost. Furthermore, the one or more embodiments for treating a molybdenum ore material, such as a molybdenum concentrate, has a concentration effect in which selectively solubilizing impurities can reduce the formation of slag and permit reduction in the carbon footprint and cost. Still another advantage of the present disclosure is that using the disclosed process for a molybdenum ore material, such as a molybdenum concentrate, exposes more molybdenum and allows molybdenum depressants to work more effectively and capture more value from the same amount of material.

[0085] EXAMPLES

[0086] The following examples are intended to demonstrate that multiple laboratory experiments were performed to highlight the selectivity for magnesium extraction in accordance with one or more embodiments of the disclosure. These examples are not intended to limit the scope of the present disclosure.

[0087] Example 1

[0088] Samples of molybdenum concentrates (40 grams) were separately subjected to agitated leaching experiments of 360 mL of various organic acids (e.g., 1 M citric acid, 1 M gluconic acid, 1 M lactic acid, and 2M lactic acid) for 24 hours at 60 °C. Untreated and treated solid samples were measured by ICP-OES following sodium peroxide fusion.

[0089] Changes in percent (%) composition of elements making up molybdenum concentrates after the 24 hour agitation leach in presence of various acids were determined and compiled in Table 1, below.

[0090] Table 1:Organic AcidCitric Oxalic Gluconic Phosphoric Sulfuric Element (IM) (IM) (IM) (IM) (IM)F -40.3% -88.1% -38.8% -14.9% -59.7% Bi -56% -67.2% -55.2% -5.6% -59.2% Fe -23.3% -38.3% -22.6% -11.7% -27.1% Mn -25.8% -51.6% -22.6% -16.1% -32.3%PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1Mo +5.01% +3.5% +3.7% +3.1% +4.8% Pb -61.4% -75.0% -58.6% -33.6% -56.4% S +5.0% +5.0% +6.6% +5.8% +7.5% Si -0.3% -20.1% +1.2% -3.0% -3.0% Sn -9.6% -37.7% +3.4% -10.3% -15.8% W +1.4% +0.3% +8.0% +3.3% +3.9% Zn -18.0% -29.3% -15.8% -10.5% -23.3% Al -11.7% -53.0% -11.8% +5.9% -5.9%

[0091] Negative values included in Table 1 indicate loss of elements from the solids into the leachate (i.e., the extraction composition) while positive values indicate upgrading of the elements in the remaining solids concentrate. Notably oxalic acid reduces F by 88%, Pb by 75%, Si by 20% , and Al by 53% while upgrading the Mo content.

[0092] Example 2

[0093] Recycling of an extraction composition was evaluated with resin in solution using an AmberLite™ IRC120 H Ion Exchange Resin (DuPont™). Two extraction processes (or “leaching”) was performed on a 10 wt% molybdenum concentrate (200 g of solid) at 60 °C for 24 hours with oxalic acid (1 M, 2000 mL) and with tartaric acid (IM, 2000 mL). After 24 hours, any remaining solids were separated from the extracted solution. The extracted solution was then added to a beaker of resin (1.3g resin per mL of leachate) and stirred for 10 minutes at room temperature to remove the metal component (i.e., cations of Ca, Mg, Fe) and regenerate the extraction composition. After 10 minutes the resin was separated from the regenerated extraction composition. The regenerated extraction composition was used to treat a fresh molybdenum concentrate.

[0094] The same leaching conditions were used in the second leach 10 wt% molybdenum concentrate (47 g of solid) at 60 °C for 24 hours with oxalic acid (I M, 470 mL) and tartaric acid (IM, 470 mL). The percentage of dissolved elements in the extracted solution was determined after the first extraction and the second extraction,PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1and results are shown in FIG. 2A (showing results for oxalic acid) and FIG. 2B (showing results for tartaric acid). The percentage of dissolved element was assessed by combining total volume loss of the liquid extraction composition and ICP-OES measurements of the extracted solution. Data shown in FIG. 2A and 2B indicates that there is minimal loss in selectivity for removal of Ca, Mg, Fe from the molybdenum concentrate while maintaining molybdenum in the concentrate.

[0095] Although only a few example embodiments have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the example embodiments without materially departing from this invention. Accordingly, all such modifications are intended to be included within the scope of this disclosure as defined in the following claims.

Claims

PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1 CLAIMSWhat is claimed:

1. A mixture, comprising:a molybdenum concentrate; andan extraction composition comprising:an aqueous solution comprising:a first organic acid;an optional additional organic acid; andoptionally an inorganic acid,wherein the extraction composition is configured to selectively solubilize one or more impurity components from the molybdenum concentrate,wherein the one or more impurity components comprise one or more of an atom, a mineral, a salt of Pb, Mg, Al, Si, F, Cu, Zn, As, Ca, Fe, or any combination thereof.

2. The mixture of claim 1, wherein the first organic acid and / or the optional additional organic acid comprises an acid selected from the group consisting of citric acid, oxalic acid, formic acid, lactic acid, acetic acid, malic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid, and combinations thereof.

3. The mixture of claim 1 or claim 2, wherein the extraction composition is capable of solubilizing an extracted Pb component, Zn component, Cu component, Mg component, Al component, Si component, F component, Fe component, Ca component, As component, or any combination thereof at a concentration in a range from 1 wt% to 80 wt% in the extraction composition.

4. The mixture of any one of the preceding claims, wherein the molybdenum concentrate comprises molybdenum sulfides.PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO15. The mixture of any one of the preceding claims, wherein the inorganic acid comprises an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and combinations thereof.

6. The mixture of any one of the preceding claims, comprising the inorganic acid in an amount in a range from 0 to 2.5 M, and wherein a pH of the extraction composition is in a range from 0.1 to 7.

7. The mixture of any one of the preceding claims, wherein the aqueous solution is a biobroth obtained from a natural and / or engineered organic acid-producing microbe, a natural and / or engineered organic acid-producing plant, or combinations thereof.

8. The mixture of any one of the preceding claims, wherein a concentration ratio of the first organic acid to the additional acid is in a range from 1 : 0 to 1 : <1.

9. A method for improving a processing efficiency of a molybdenum concentrate, the method comprising:forming the mixture of any one of the preceding claims; andseparating a treated molybdenum concentrate from the mixture of any one of the preceding claims, wherein the treated molybdenum concentrate comprises: a reduced Pb component, Mg component, Zn component, Cu component, Al component, Si component, F component, Ca component, As component, and / or Fe component content of 10 to 90 relative % less than the molybdenum concentrate.

10. A method for extracting a metal from molybdenum concentrate, the method comprising:selectively solubilizing one or more impurity components from the molybdenum concentrate into an extraction composition,wherein the extraction composition comprises an aqueous solution of an organic acid, an optional additional organic acid, and an optional inorganic acid.

11. The method of claim 10, further comprising:separating a treated molybdenum concentrate thereof from a mixture comprising the extraction composition and a Pb component, Mg component, Cu component, AlPATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1component, Si component, F component, Ca component, As component, Zn component, and / or Fe component.

12. The method of claim 10 or claim 11, wherein selectively solubilizing comprises: introducing the extraction composition to an extraction zone;introducing the molybdenum concentrate to the extraction zone, thereby forming a mixture with the extraction composition;agitating the extraction mixture in the extraction zone to form a liquid mixture comprising the organic acid, the one or more components, and, optionally, one or more additional components extracted from the molybdenum concentrate; andseparating the liquid mixture from the molybdenum concentrate.

13. The method of claim 12, further comprising:separating the one or more components from the liquid mixture; andrecovering the extraction composition to produce a recovered extraction composition, wherein the separated one or more components has a purity in a range from 10% to 100% when separated from the liquid mixture.

14. The method of claim 13, further comprising:introducing the recovered extraction composition from the liquid mixture to the extraction zone, thereby recycling the extraction composition.

15. The method of claim 13 or claim 14, wherein separating the one or more components from the liquid mixture comprises extracting the one or more components from the liquid mixture with one or more water treatment techniques.

16. The method of claim 15, wherein extracting the one or more impurity components comprises performing one or more water treatment techniques selected from the group consisting of feeding the liquid mixture through an ion exchange system, using solvent extraction, chromatography, filtration, membrane filtration, osmotic separation, using adsorption and / or absorption materials, precipitation , electrodeionization, or combinations thereof.

17. The method of any one of claims 12 to 16, further comprising:PATENT APPLICATION ATTORNEY DOCKET NO. 19148-012WO1adjusting a temperature of the extraction zone to a temperature in a range from 20 to 100 °C;wherein the mixture is in the extraction zone for a period of time in a range from 0.5 to 24 hours.

18. A method for extracting an impurity from a molybdenum concentrate, the method comprising:extracting one or more impurity components comprising one or more minerals, one or more salts, or any combination thereof from the molybdenum concentrate with an extraction composition ,wherein the extraction composition comprises an aqueous solution of an organic acid selected from citric acid, oxalic acid, formic acid, lactic acid, acetic acid, malic acid, hydroxypropionic acid, phthalic acid, tartaric acid, hexadecenoic acid, heptadecanoic acid, gallic acid, aspartic acid, succinic acid, oleic acid, tannic acid, palmitic acid, ascorbic acid, and combinations thereof;separating the molybdenum concentrate from the one or more components and the extraction composition;separating the extraction composition from the one or more components; and repeating the extracting,wherein the separated one or more components have a purity in a range from 10% to 90%, when separated from the extraction composition.

19. The method of claim 18, wherein the separated molybdenum concentrate thereof comprises:a reduced Pb component, Cu component, Mg component, Al component, Si component, F component, Zn component, As component, Ca component, and / or Fe component content of 10 to 90 wt% less than the molybdenum concentrate.