Polarizing plate and display device
The polarizing plate with a λ/4 layer of controlled moisture permeability and ellipticity addresses eye strain and durability issues, ensuring reduced strain and improved polarizer longevity.
Patent Information
- Application Number
- PCT/JP2026/018006
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-05-08
- Filing Date
- 2026-05-12
- Publication Date
- 2026-11-19
Smart Images

Figure JP2026018006_19112026_PF_FP_ABST
Abstract
Description
Polarizing plate and display device
[0001] This disclosure relates to polarizing plates and display devices.
[0002] In display devices, polarizing plates are often placed on the display elements to prevent a decrease in visibility due to ambient light. For example, Patent Document 1 discloses a polarizing plate with a predetermined configuration.
[0003] Japanese Patent Publication No. 2024-114638
[0004] Recently, there has been a growing need for display devices that are easy on the human eye, and in particular, there is a demand for display devices that do not cause eye strain during viewing. The present inventors investigated the characteristics of a display device including a polarizing plate described in Patent Document 1 and found that it easily causes eye strain during viewing, and that improvement is necessary. Furthermore, polarizing plates applied to such display devices are required to have excellent durability of the polarizer under high temperature and high humidity conditions.
[0005] The embodiments of this disclosure aim to provide a polarizing plate that can form a display device that reduces eye strain when viewed by an observer compared to a case without the configuration of the embodiments of this disclosure, and that suppresses the degradation of the polarizer even under high temperature and high humidity conditions compared to a case without the configuration of the embodiments of this disclosure. Furthermore, the embodiments of this disclosure also aim to provide a display device.
[0006] One embodiment of the present disclosure is a polarizing plate for use in a display device, comprising a λ / 4 layer and a polarizer, wherein the λ / 4 layer is a layer containing a liquid crystal compound, and the moisture permeability of the λ / 4 layer at a temperature of 40°C and a relative humidity of 90% is 500 g / m². 2 - The polarizer is less than or equal to 0.80, and when light is shone onto the polarizer from the polarizer side, the average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is 0.80 or higher, and when the polarizer is applied to a display device, the λ / 4 layer is positioned so that it faces the viewing side.
[0007] According to embodiments of this disclosure, it is possible to create a display device that reduces eye strain when viewed by an observer compared to a case without the configuration of the embodiments of this disclosure, and it is possible to provide a polarizing plate that suppresses the degradation of the polarizer even under high temperature and high humidity conditions compared to a case without the configuration of the embodiments of this disclosure. Furthermore, according to embodiments of this disclosure, a display device can be provided.
[0008] This figure shows an example of a display device of the present disclosure. This figure shows another example of a display device of the present disclosure.
[0009] The embodiments of this disclosure are described in detail below. The descriptions of the constituent elements described below may be based on representative embodiments of this disclosure, but this disclosure is not limited to such embodiments. Furthermore, the embodiments and examples described below may be combined with each other.
[0010] In this specification, numerical ranges expressed using "~" mean a range that includes the numbers before and after "~" as the lower and upper limits. Also, in this specification, if there are two or more types of a component, unless otherwise specified, the "content" of that component means the total content of those two or more components. In this specification, in numerical ranges described in stages, the upper or lower limit stated in one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Also, in numerical ranges described in this specification, the upper or lower limit stated in one numerical range may be replaced with the values shown in the examples.
[0011] In this specification, the "absorption axis" refers to the polarization direction in which the absorbance is maximum when linearly polarized light is incident on the element. The "in-plane lagging axis" refers to the direction in which the refractive index is maximum.
[0012] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and thickness retardation at wavelength λ, respectively. Unless otherwise specified, wavelength λ is assumed to be 550 nm. Furthermore, in this specification, Re(λ) and Rth(λ) are values measured at wavelength λ using an AxoScan (manufactured by Axometrics). Specifically, by inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d) into the AxoScan, the following can be calculated: In-plane retardation axis direction (°) Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d Note that R0(λ) is displayed as a numerical value calculated by the AxoScan, but it means Re(λ).
[0013] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Corporation) with a sodium lamp (λ = 589 nm) as the light source. Wavelength dependence can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Corporation) in combination with an interference filter. Values from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can also be used. Examples of average refractive index values for major optical films are given below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).
[0014] In this specification, A plates and C plates are defined as follows: There are two types of A plates: positive A plates and negative A plates. When the refractive index in the in-plane slow axis direction (the direction in which the refractive index is maximum in the plane) of the film is nx, the refractive index in the direction perpendicular to the in-plane slow axis is ny, and the refractive index in the thickness direction is nz, a positive A plate satisfies the relationship given by equation (A1), and a negative A plate satisfies the relationship given by equation (A2). Note that a positive A plate has a positive Rth value, and a negative A plate has a negative Rth value. Equation (A1) nx > ny ≈ nz Equation (A2) ny < nx ≈ nz Note that the above "≈" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. "Substantially identical" means, for example, that when (ny - nz) × d (where d is the film thickness) is -10 to 10 nm, preferably -5 to 5 nm, it is included in "ny ≈ nz", and when (nx - nz) × d is -10 to 10 nm, preferably -5 to 5 nm, it is included in "nx ≈ nz". There are two types of C plates: positive C plates and negative C plates. A positive C plate satisfies the relationship in equation (C1), and a negative C plate satisfies the relationship in equation (C2). Note that a positive C plate shows a negative Rth value, and a negative C plate shows a positive Rth value. Equation (C1) nz > nx ≈ ny Equation (C2) nz < nx ≈ ny Note that the above "≈" includes not only cases where the two are completely identical, but also cases where the two are substantially identical. "Substantially identical" means that, for example, when (nx - ny) × d (where d is the thickness of the film) is 0 to 10 nm, preferably 0 to 5 nm, it is included in "nx ≈ ny".
[0015] In this specification, unless otherwise specified, the refractive index is the refractive index at a wavelength of 550 nm. In this specification, unless otherwise specified, the in-plane slow axis is defined at a wavelength of 550 nm.
[0016] The polarizing plate of this disclosure (hereinafter also simply referred to as "this polarizing plate") will be described in detail below. This polarizing plate comprises a λ / 4 layer and a polarizer, and is a polarizing plate applied to a display device, wherein the λ / 4 layer is a layer containing a liquid crystal compound, and the moisture permeability of the λ / 4 layer at a temperature of 40°C and a relative humidity of 90% is 500 g / m². 2 - The polarizer is less than or equal to 0.80, and when light is shone onto the polarizer from the polarizer side, the average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is 0.80 or greater, and when the polarizer is applied to a display device, it is positioned so that the λ / 4 layer is on the viewing side.
[0017] The reason why the polarizing plate having the above configuration can solve the problem is not necessarily clear, but the inventors speculate as follows. Note that the following speculation does not limit the mechanism by which the effect is obtained. In other words, even if the effect is obtained by a mechanism other than those described below, it is included within the scope of this disclosure. The inventors, in their investigation of the prior art, found that eye strain when an observer views a display device with a polarizing plate positioned on the viewing side is related to the ellipticity of the light emitted from the display device. More specifically, they found that eye strain is suppressed when the observer views light with an ellipticity closer to 1 and closer to circular polarization. As shown in the embodiments described later, when an observer views a display device including this polarizing plate, eye strain is suppressed, and as a result, the number of blinks after observing the display device for a certain period of time is reduced. Note that blinking has the function of relaxing the muscles around the eyes and improving blood circulation; therefore, when eye strain accumulates, the number of blinks tends to increase in an attempt to improve blood circulation. Furthermore, in this polarizing plate, the moisture permeability of the λ / 4 layer is below a predetermined value, which suppresses the transmission of moisture to the polarizer, and as a result, it is believed that the degradation of the polarizer under high temperature and high humidity conditions is suppressed. In addition, in a display device including this polarizing plate, the λ / 4 layer is positioned on the viewing side of the polarizer, so the transmission of moisture to the polarizer is suppressed.
[0018] Figure 1 shows an example of a display device according to the present disclosure. The display device 100A includes an organic electroluminescent display element (organic EL display element) 12, a phase difference layer 14, a polarizer 16, a λ / 4 layer 18, and a substrate 20. The polarizing plate 10 of the present disclosure includes a polarizer 16, a λ / 4 layer 18, and a substrate 20. The λ / 4 layer 18 is positioned on the viewing side of the polarizer 16. The display device 100A is viewed from the substrate 20 side. As described above, if the substrate 20 is positioned outside the display device 100A and the substrate 20 contains an ultraviolet absorber as described later, the durability of the polarizing plate 10 against ambient light is improved. In addition, the light emitted from the organic EL display element 12, indicated by the white arrow, becomes linearly polarized after passing through the polarizer 16, and then becomes circularly polarized after passing through the λ / 4 layer 18, and enters the observer's eye of the display device 100A while maintaining that polarization state. As described above, eye strain is suppressed when light with an average ellipticity greater than a predetermined value enters the observer's eye. In Figure 1, the polarizing plate 10 also includes the base material 20, but it is sufficient that it includes at least the polarizer 16 and the λ / 4 layer 18. In Figure 1, the phase difference layer 14 and the polarizer 16 function as an anti-reflective film that prevents the reflection of ambient light. Note that the phase difference layer 14 and the base material 20 are arbitrary components and do not have to be included in the display device 100A. Also, as will be described later, adhesion layers (not shown) may be placed between each component. The characteristics of the polarizing plate and each component will be described in detail below.
[0019] <Average Ellipticity> Below, we will first describe in detail the average ellipticity, which is one of the characteristic features of this polarizer. In this polarizer, when light is shone onto the polarizer from the polarizer side, the average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is 0.80 or higher. In particular, an average ellipticity of 0.84 or higher is preferred in that it is possible to form a display device that further suppresses eye strain when viewed by an observer. There is no particular upper limit to the average ellipticity, but it may be 1.00 or less, 0.95 or less, or 0.90 or less. First, ellipticity is the ratio of the minor axis to the major axis of circularly polarized light. For example, the ellipticity when the light is perfectly circularly polarized is 1.00, and the ellipticity when the light is perfectly linearly polarized is 0. The average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is the average value of the ellipticity at each wavelength in 10 nm increments between 400 and 780 nm. In other words, the ellipticity is calculated at each wavelength in the 400-780 nm range, at 10 nm intervals (400 nm, 410 nm, 420 nm, ..., 770 nm, 780 nm), and these values are then given an arithmetic mean. When irradiating the polarizer plate with light from the polarizer side, the light is incident from the direction normal to the main surface of the polarizer plate. The above average ellipticity can be measured, for example, using an AxoScan OPMF-1 (manufactured by OptoScience). More specifically, the ellipticity in the 400-780 nm range can be measured, for example, using an AxoScan OPMF-1 (manufactured by OptoScience).
[0020] The method for controlling the average ellipticity described above is not particularly limited, and methods for controlling the wavelength dispersion of each component constituting the polarizer include controlling the wavelength dispersion of each component. For example, the value of the average ellipticity can be adjusted by controlling the wavelength dispersion of the λ / 4 layer at each wavelength. More specifically, by forming the liquid crystal layer with two or more liquid crystal layers having different orientation states of liquid crystal compounds, the ellipticity at each wavelength from low wavelength to high wavelength can be increased, thereby improving the average ellipticity. In addition to the above, negative wavelength dispersion can be achieved by forming the λ / 4 layer using a liquid crystal compound with inverse wavelength dispersion, thereby improving the average ellipticity.
[0021] <Organic EL Display Element> The configuration of an organic EL display element is not particularly limited, but it usually includes at least a pair of electrodes (cathode and anode) and an organic light-emitting layer disposed between the electrodes. In addition, the organic EL display element usually includes connection terminals for connecting to an IC (integrated circuit) together with the organic light-emitting layer. Furthermore, the organic EL display element may include other components, for example, a sealing layer that covers the organic light-emitting layer.
[0022] <Phase Difference Layer> The phase difference layer is a layer placed between the organic EL display element and the polarizer. The phase difference layer is used in combination with the polarizer, and the polarizer plate, which includes the phase difference layer and the polarizer, functions as an anti-reflective film that prevents the reflection of ambient light. The phase difference layer is a layer that exhibits the optimal in-plane retardation according to its function, but from the viewpoint of anti-reflection, it is preferably a λ / 4 layer. The λ / 4 layer is a layer that has the function of converting linearly polarized light of a certain wavelength to circularly polarized light (or circularly polarized light to linearly polarized light). More specifically, it is a layer in which the in-plane retardation at a predetermined wavelength λnm is λ / 4 (or an odd multiple thereof). Among these, the in-plane retardation Re(550) of the λ / 4 layer at a wavelength of 550 nm is preferably 100 to 200 nm, more preferably 120 to 160 nm, and even more preferably 130 to 150 nm.
[0023] The phase difference layer may exhibit forward dispersiveness (a characteristic in which in-plane retardation decreases as the measurement wavelength increases) or inverse dispersiveness (a characteristic in which in-plane retardation increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, it is preferable that the above-mentioned forward and inverse dispersiveness be exhibited in the visible light range.
[0024] The phase difference layer (especially the λ / 4 layer) is not particularly limited in its composition and can include a layer containing a liquid crystal compound and a stretched film obtained by stretching a polymer. Among these, a layer containing a liquid crystal compound is preferred as the phase difference layer (especially the λ / 4 layer), a layer with a fixed liquid crystal compound is more preferred, and a layer with a fixed horizontally oriented rod-shaped liquid crystal compound is even more preferred. The state in which the rod-shaped liquid crystal compound is horizontally oriented means that the long axis of the rod-shaped liquid crystal compound and the main surface of the phase difference layer are parallel. However, it is not required that they be strictly parallel, and it is preferable that the angle between the long axis of the rod-shaped liquid crystal compound and the main surface of the phase difference layer is within the range of 0 ± 10°. As the layer containing the liquid crystal compound, a twisted liquid crystal layer containing a liquid crystal compound twisted along the helical axis can also be mentioned. The phase difference layer may be a single layer or a multi-layer structure. For example, when the phase difference layer is a λ / 4 layer and has a multi-layer structure, a broadband λ / 4 layer obtained by laminating a λ / 4 layer and a λ / 2 layer can be mentioned. Furthermore, the phase difference layer may be a broadband λ / 4 layer including a twisted liquid crystal layer. Specific examples of the phase difference layer (especially the λ / 4 layer) include, for example, the single-layer or multi-layer liquid crystal compound-containing layer (a layer in which the liquid crystal compound is fixed) described in Example 18 of WO2025 / 028229, Example 3 of WO2025 / 052975, Example 1 of WO2019 / 022156, and Example 1 of WO2025 / 198026.
[0025] When this polarizing plate is observed from the retardation layer side, clockwise rotation is represented by a positive angle and counterclockwise rotation by a negative angle, and the direction of the absorption axis of the polarizer is defined as 0°, the direction of the in-plane slow axis of the λ / 4 layer (corresponding to the outer-side retardation layer) and the direction of the in-plane slow axis of the retardation layer (corresponding to the inner-side retardation layer), which will be described later, are each independently preferably in the range of +45°±5° or in the range of -45°±5°. For example, one of the direction of the in-plane slow axis of the λ / 4 layer and the direction of the in-plane slow axis of the retardation layer may be in the range of +45°±5°, and the other may be in the range of -45°±5°. Regardless of whether the two in-plane slow axes are in the range of +45°±5° or the range of -45°±5°, the optical effect remains unchanged. However, the physical properties of the polarizing plate may change depending on the angle setting of the in-plane slow axis, and an optimal design can be appropriately performed in view of the relationship with the bending axis, the relationship with the stretching direction during molding, curling, and the like.
[0026] The thickness of the retardation layer is not particularly limited, and is preferably 10 μm or less, more preferably 0.1 to 5.0 μm. The thickness of the retardation layer is intended to mean the average thickness of the retardation layer. The average thickness is determined by measuring the thickness at any 5 or more points of the retardation layer and arithmetically averaging the measured values.
[0027] <Polarizer> The polarizer is not particularly limited as long as it is a member having a function of converting natural light into specific linearly polarized light, and examples thereof include an absorption-type polarizer. The type of the polarizer is not particularly limited, and commonly used polarizers can be used, and examples thereof include iodine-based polarizers, dye-based polarizers using a dichroic substance, and polyene-based polarizers. The iodine-based polarizer and the dye-based polarizer are generally produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching the resulting product.
[0028] The polarizer is also preferably a polarizer formed using a composition containing a dichroic substance and a liquid crystal compound having a polymerizable group. The dichroic substance is not particularly limited, and examples thereof include visible light absorbing substances (dichroic dyes), luminescent substances (fluorescent substances, phosphorescent substances), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, carbon nanotubes, and inorganic substances (for example, quantum rods), and conventionally known dichroic substances (dichroic dyes) can be used.
[0029] The positional relationship between the absorption axis of the polarizer and the in-plane slow axis of the λ / 4 layer described later is not particularly limited as long as the above-mentioned average ellipticity falls within a predetermined range. For example, the angle formed by the absorption axis of the polarizer and the in-plane slow axis of the λ / 4 layer is preferably in the range of 45±10° (35 to 55°).
[0030] When the λ / 4 layer is in the first preferred embodiment described later, the angle formed by the absorption axis of the polarizer and the in-plane slow axis of the liquid crystal layer (A) is preferably in the range of 76±10° (66 to 86°). When the λ / 4 layer is in the second preferred embodiment described later, the angle formed by the absorption axis of the polarizer and the in-plane slow axis of the layer formed by fixing a homogeneously aligned rod-like liquid crystal compound is preferably in the range of 11.5±10° (1.5 to 21.5°).
[0031] The thickness of the polarizer is not particularly limited, but from the viewpoint of reducing the thickness of the polarizing plate, it is preferably 40 μm or less, and more preferably 25 μm or less. The lower limit is not particularly limited, but it is often 5 μm or more. The thickness of the polarizer described above means the average thickness of the polarizer. The average thickness is obtained by measuring the thickness at any 5 or more points of the polarizer and arithmetically averaging the measured values.
[0032] <λ / 4 layer> The λ / 4 layer is positioned so as to be on the viewing side when the polarizing plate is incorporated into the display device. The definition and preferred embodiment of the λ / 4 layer are the same as the definition and preferred embodiment of the λ / 4 layer described above as a preferred embodiment of the phase difference layer. As described above, the λ / 4 layer may be a single layer or a multi-layer structure. In particular, it is preferable to include two or more liquid crystal layers with different orientation states of liquid crystal compounds, in order to form a display device that further suppresses eye strain when viewed by an observer. There is no particular upper limit to the number of liquid crystal layers included, but it is often four or fewer, and three or fewer is preferable. In particular, it is preferable that the λ / 4 layer includes a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed, in order to further suppress the deterioration of the polarizer under high temperature and high humidity conditions. That is, when the λ / 4 layer includes two or more liquid crystal layers with different orientation states of liquid crystal compounds, it is preferable that at least one of the two or more liquid crystal layers is a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed. Furthermore, in order to further suppress the degradation of the polarizer under high temperature and high humidity conditions, it is preferable that the λ / 4 layer includes a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed, and a liquid crystal layer containing a liquid crystal compound that is torsionally oriented with the thickness direction as the helical axis. In other words, when the λ / 4 layer includes two or more liquid crystal layers with different orientation states of liquid crystal compounds, it is preferable that at least one of the two or more liquid crystal layers is a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed, and at least one of the two or more liquid crystal layers is a liquid crystal layer containing a liquid crystal compound that is torsionally oriented with the thickness direction as the helical axis. The layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed, and the liquid crystal layer containing a liquid crystal compound that is torsionally oriented with the thickness direction as the helical axis will be described in detail later.
[0033] The moisture permeability of the λ / 4 layer at a temperature of 40°C and relative humidity of 90% is 500 g / m². 2 - It is less than 400 g / m². In particular, the degradation of this polarizer under high temperature and high humidity conditions is more suppressed. 2 - Preferably less than 350 g / m 2 - days or less is preferable. The lower limit of the above moisture permeability is not particularly limited, but 5 g / m 2 - May be more than 100g / m2 ·day or more. Examples of the method for measuring the moisture permeability include a method in which a λ / 4 layer as a measurement sample is prepared, and the moisture permeability of the measurement sample is measured under the conditions of a temperature of 40°C and a relative humidity of 90% described in JIS Z-0208 (1976). In the above measurement, the measurement sample may be adjusted to a predetermined size. Further, in the above measurement, the measurement sample is subjected to humidity conditioning for 24 hours in advance under the conditions of a temperature of 40°C and a relative humidity of 90%, and then subjected to the measurement. Further, as the measurement sample, a laminate including the λ / 4 layer and other members may be used. In the case of using a laminate including such other members other than the λ / 4 layer, the moisture permeability of the other members may be measured separately, and the moisture permeability of the λ / 4 layer may be calculated from the moisture permeability of the laminate and the moisture permeability of the other members. As the method for calculating the moisture permeability of the λ / 4 layer, the moisture permeability can be calculated using the following formula.
[0034]
[0035] Wtotal represents the moisture permeability of the entire laminate. W 1 , W 2 ·· represents the moisture permeability of each individual layer.
[0036] The method for adjusting the moisture permeability of the λ / 4 layer is not particularly limited, and examples thereof include a method of adjusting the type of liquid crystal compound to be used, and a method of selecting the layer structure of the λ / 4 layer. More specifically, when a rod-like liquid crystal compound is used as the liquid crystal compound, the moisture permeability of the λ / 4 layer tends to be lower than when a discotic liquid crystal compound is used. Further, when a forward wavelength dispersion liquid crystal compound is used as the liquid crystal compound, the moisture permeability of the λ / 4 layer tends to be lower than when a reverse wavelength dispersion liquid crystal compound is used. Further, a method of reducing the moisture permeability of the λ / 4 layer by making the layer structure of the λ / 4 layer a multilayer structure to increase the thickness thereof may also be mentioned.
[0037] The λ / 4 layer is a layer containing a liquid crystal compound. The liquid crystal layer constituting the λ / 4 layer is also a layer containing a liquid crystal compound. Either a polymer liquid crystal compound or a low-molecular-weight liquid crystal compound can be used as the liquid crystal compound. Here, "polymer liquid crystal compound" refers to a liquid crystal compound having repeating units in its chemical structure. "Low-molecular-weight liquid crystal compound" refers to a liquid crystal compound that does not have repeating units in its chemical structure. The liquid crystal compound may be a rod-shaped liquid crystal compound or a disc-shaped liquid crystal compound, but a rod-shaped liquid crystal compound is preferred in that it has lower moisture permeability as described above. As the rod-shaped liquid crystal compound, known compounds can be used, for example, the compounds described in claim 1 of Japanese Patent Publication No. 11-513019 and paragraphs 0026 to 0098 of Japanese Patent Application Publication No. 2005-289980. Known compounds can be used as the disc-shaped liquid crystal compound, for example, the compounds described in paragraphs 0020 to 0067 of Japanese Patent Application Publication No. 2007-108732 and paragraphs 0013 to 0108 of Japanese Patent Application Publication No. 2010-244038.
[0038] The liquid crystal compound is preferably a forward-wavelength-dispersive liquid crystal compound. A forward-wavelength-dispersive liquid crystal compound is one in which, when the in-plane retardation (Re) value at a specific wavelength (visible light range) of a phase difference film made by aligning (horizontally oriented) this liquid crystal compound is measured, the Re value or Rth value decreases as the measured wavelength increases. A reverse-wavelength-dispersive liquid crystal compound is one in which, when the in-plane retardation (Re) value at a specific wavelength (visible light range) of a phase difference film made by aligning (horizontally oriented) this liquid crystal compound is measured, the Re value or Rth value increases as the measured wavelength increases.
[0039] The liquid crystal compounds in the λ / 4 layer and the liquid crystal layer may be fixed. In this specification, "fixed" means that the orientation of the liquid crystal compound is maintained. Specifically, it is preferable that the layer is non-fluid and can maintain a stable fixed orientation without being altered by an external field or force, usually in a temperature range of 0 to 50°C, or -30 to 70°C under more severe conditions. Furthermore, the liquid crystal compounds in the λ / 4 layer and the liquid crystal layer do not necessarily have to exhibit liquid crystalline properties. For example, when the λ / 4 layer and the liquid crystal layer are formed using a polymerizable liquid crystal compound, the liquid crystal compound may lose its liquid crystalline properties due to the curing reaction, resulting in increased molecular weight.
[0040] The λ / 4 layer and the liquid crystal layer are preferably layers formed using a composition containing a polymerizable liquid crystal compound. A polymerizable liquid crystal compound is a liquid crystal compound having polymerizable groups. Examples of polymerizable groups include unsaturated polymerizable groups, epoxy groups, and azilidinyl groups, with unsaturated polymerizable groups being preferred and ethylenically unsaturated polymerizable groups being more preferred.
[0041] The λ / 4 layer may exhibit forward dispersiveness (in-plane retardation decreases as the measurement wavelength increases) or inverse dispersiveness (in-plane retardation increases as the measurement wavelength increases), but inverse dispersiveness is preferred. Furthermore, both forward and inverse dispersiveness are preferably exhibited in the visible light range.
[0042] When the λ / 4 layer includes two or more liquid crystal layers with different orientation states of liquid crystal compounds, the types of liquid crystal layers are not particularly limited, but examples include A-plate, C-plate, and a liquid crystal layer containing a liquid crystal compound that is torsionally oriented with the thickness direction as the helical axis.
[0043] The definition of A-plate is as described above. A-plate can also be used as a so-called λ / 4 layer or λ / 2 layer. The definition of λ / 4 layer is as described above. A λ / 2 layer is an optical anisotropic layer in which the in-plane retardation Re(λ) at a specific wavelength λnm satisfies Re(λ) ≈ λ / 2. This equation only needs to be achieved at any wavelength in the visible light region (for example, 550 nm). In particular, when A-plate is used as a λ / 2 layer, the in-plane retardation Re(550) of A-plate at a wavelength of 550 nm is preferably 210 to 300 nm.
[0044] The definition of C plate is as described above. The retardation in the thickness direction of the C plate at a wavelength of 550 nm is not particularly limited, but -120 to -20 nm is preferred, and -100 to -30 nm is more preferred. Alternatively, the retardation in the thickness direction of the C plate at a wavelength of 550 nm is not particularly limited, but 10 to 80 nm is preferred, and 20 to 60 nm is more preferred.
[0045] In a liquid crystal layer containing a liquid crystal compound that is torsion-oriented with the thickness direction as the helical axis (hereinafter also referred to as the "torsed liquid crystal layer"), the torsion angle of the liquid crystal compound (torsion angle in the orientation direction of the liquid crystal compound) is not particularly limited, and is often greater than 0° and less than or equal to 360°. A range of 80±30° (50 to 110°) is preferred, and a range of 80±20° (60 to 100°) is more preferred, as it is easier to use as a λ / 4 layer. The value of the product Δnd of the refractive index anisotropy Δn of the torsed liquid crystal layer and the thickness d of the torsed liquid crystal layer at a wavelength of 550 nm is not particularly limited, but is preferably 40 to 280 nm, more preferably 100 to 200 nm, and even more preferably 160 to 200 nm. The above torsion angle and Δnd are measured using an AxoScan (polarimeter) device from Axometrics Inc. and its device analysis software.
[0046] Furthermore, when we say that the liquid crystal compound is torsion-oriented, we mean that the liquid crystal compound is twisted from one main surface to the other main surface of the torsion liquid crystal layer, with the thickness direction of the torsion liquid crystal layer as the helical axis. Consequently, the orientation direction of the liquid crystal compound (in-plane slow phase axis direction) differs depending on its position in the thickness direction of the torsion liquid crystal layer. In torsion orientation, the molecular axis of the liquid crystal compound (long axis in the case of a rod-shaped liquid crystal compound, and axis perpendicular to the disk surface in the case of a disc-shaped liquid crystal compound) is arranged to be parallel to the main surface of the torsion liquid crystal layer. However, strict parallelism is not required; it is preferable that the angle between the molecular axis of the liquid crystal compound and the main surface of the torsion liquid crystal layer be in the range of 0 to 20°, and more preferably in the range of 0 to 10°. The type of liquid crystal compound used is not particularly limited, and examples include the liquid crystal compounds described above in the λ / 4 layer section. The torsion-oriented liquid crystal compound may be fixed. In particular, the twisted liquid crystal layer is preferably formed by twisting and oriented a liquid crystal compound having polymerizable groups, and then polymerizing the liquid crystal compound to fix it in place.
[0047] A first preferred embodiment of the λ / 4 layer is a λ / 4 layer having, in this order, a liquid crystal layer (A) which is a layer in which vertically oriented disc-shaped liquid crystal compounds are fixed, a liquid crystal layer (B) which is a layer in which rod-shaped liquid crystal compounds twisted along a helical axis extending in the thickness direction are fixed, and a liquid crystal layer (C) which is a layer in which vertically oriented rod-shaped liquid crystal compounds are fixed. The in-plane retardation at a wavelength of 550 nm of the layer in which the vertically oriented disc-shaped liquid crystal compounds are fixed is preferably 140 to 220 nm, and more preferably 150 to 200 nm. The layer in which the vertically oriented disc-shaped liquid crystal compounds are fixed is preferably formed by vertically oriented a disc-shaped liquid crystal compound having polymerizable groups, and then polymerizing the disc-shaped liquid crystal compound to fix the disc-shaped liquid crystal compound.
[0048] The preferred range of the torsion angle and Δnd for a layer formed by fixing rod-shaped liquid crystal compounds that are twisted and oriented along a spiral axis extending in the thickness direction is the same as the preferred range of the torsion angle and Δnd for the twisted liquid crystal layer described above.
[0049] The in-plane retardation at a wavelength of 550 nm of the layer formed by fixing vertically oriented rod-shaped liquid crystal compounds is preferably 0 to 10 nm. Furthermore, the retardation in the thickness direction at a wavelength of 550 nm of the layer formed by fixing vertically oriented rod-shaped liquid crystal compounds is preferably -120 to -20 nm, more preferably -110 to -30 nm, and even more preferably -100 to -40 nm. The layer formed by fixing vertically oriented rod-shaped liquid crystal compounds is preferably formed by vertically oriented rod-shaped liquid crystal compounds having polymerizable groups, and then polymerizing the rod-shaped liquid crystal compounds to fix them.
[0050] It is preferable that the in-plane slow axis of liquid crystal layer (A) and the in-plane slow axis of liquid crystal layer (B) on the surface facing liquid crystal layer (A) are parallel. However, strict parallelism is not required; it is preferable that the angle between the in-plane slow axis of liquid crystal layer (A) and the in-plane slow axis of liquid crystal layer (B) on the surface facing liquid crystal layer (A) is in the range of 0 to 10°, and more preferably in the range of 0 to 5°. In a polarizing plate combining the first preferred embodiment of the λ / 4 layer and a polarizer, it is preferable to combine the first preferred embodiment of the λ / 4 layer and the polarizer such that the liquid crystal layer (A) is positioned closer to the polarizer than the liquid crystal layer (C). In a polarizing plate combining a first preferred embodiment of a λ / 4 layer and a polarizer, when observing the polarizing plate from the liquid crystal layer (C) side toward the liquid crystal layer (A) side, if the in-plane slow axis of the liquid crystal layer (A) is rotated clockwise by the aforementioned angle (in the range of 76 ± 10°) with respect to the absorption axis of the polarizer, it is preferable that the in-plane slow axis of the liquid crystal layer (B) on the surface opposite to the liquid crystal layer (A) side of the liquid crystal layer (B) is rotated counterclockwise with respect to the in-plane slow axis of the surface opposite to the liquid crystal layer (A) side of the liquid crystal layer (B).
[0051] Furthermore, a second preferred embodiment of the λ / 4 layer is a λ / 4 layer having a liquid crystal layer (E) which is a twisted liquid crystal layer and a liquid crystal layer (D) which is a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed. The preferred embodiment of the twisted liquid crystal layer is as described above. When the thickness of the layer on which the homogeneously oriented rod-shaped liquid crystal compounds are fixed is d, and the refractive index anisotropy of the layer measured at a wavelength of 550 nm is Δn, the product of the thickness d and the refractive index anisotropy Δn (Δnd) is preferably 100 to 240 nm, more preferably 120 to 220 nm, even more preferably 140 to 200 nm, and particularly preferably 160 to 200 nm. The ratio of the thicknesses of liquid crystal layer (D) and liquid crystal layer (E) (thickness of liquid crystal layer (D) / thickness of liquid crystal layer (E)) is not particularly limited, but is preferably 0.1 to 5.0, and more preferably 0.2 to 3.0.
[0052] In this specification, homogeneous orientation refers to a state in which the molecular axes of a liquid crystal compound (for example, the long axis in the case of a rod-shaped liquid crystal compound) are aligned horizontally and in the same direction with respect to the layer surface (optical uniaxiality). Here, horizontal does not require strict horizontal alignment, but rather means an orientation in which the inclination angle between the average molecular axis of the liquid crystal compound in the layer and the layer surface is less than 20°. Furthermore, the same direction does not require strict same direction alignment, but rather means that when the orientation of the in-plane slow axis is measured at any 20 positions in the plane, the maximum difference in the in-plane slow axis orientations among the 20 in-plane slow axis orientations (the difference between the two in-plane slow axis orientations with the largest difference among the 20 in-plane slow axis orientations) is less than 10°.
[0053] In a polarizing plate combining a second preferred embodiment of the λ / 4 layer with a polarizer, it is preferable to combine the second preferred embodiment of the λ / 4 layer with the polarizer such that the liquid crystal layer (D) is positioned closer to the polarizer than the liquid crystal layer (E). In a polarizing plate combining a second preferred embodiment of a λ / 4 layer and a polarizer, when observing the polarizing plate from the polarizer side toward the λ / 4 layer side, if the in-plane slow axis of the liquid crystal layer (D) is rotated counterclockwise by the aforementioned angle (in the range of 11.5 ± 10°) with respect to the absorption axis of the polarizer, it is preferable that the in-plane slow axis of the liquid crystal layer (E) on the surface opposite to the liquid crystal layer (D) side of the liquid crystal layer (E) is rotated counterclockwise with respect to the in-plane slow axis of the surface opposite to the liquid crystal layer (D) side of the liquid crystal layer (E). When observing from the polarizer side toward the λ / 4 layer side, if the in-plane slow axis of the liquid crystal layer (D) is rotated clockwise by the aforementioned angle (in the range of 11.5 ± 10°) with respect to the absorption axis of the polarizer, it is preferable that the in-plane slow axis of the liquid crystal layer (E) on the surface opposite to the liquid crystal layer (D) side of the liquid crystal layer (E) is rotated clockwise with respect to the in-plane slow axis of the surface opposite to the liquid crystal layer (D) side of the liquid crystal layer (E).
[0054] The method for manufacturing the λ / 4 layer is not particularly limited and can be manufactured by known methods. If the λ / 4 layer has a multilayer structure, it can be manufactured by methods described, for example, in International Publication No. 2021 / 033631 and International Publication No. 2021 / 033640. Also, if the λ / 4 layer has a multilayer structure, the above-mentioned liquid crystal layers may be bonded via an adhesion layer described later. In other words, the λ / 4 layer may include an adhesion layer. From the viewpoint of reducing the film thickness, there may be an embodiment in which multiple liquid crystal layers are adjacent to each other, that is, an embodiment in which there is no adhesion layer between multiple liquid crystal layers.
[0055] The thickness of the λ / 4 layer is not particularly limited, but is preferably 10 μm or less, more preferably 2.0 to 5.0 μm, and even more preferably 2.2 to 5.0 μm. The thickness of the λ / 4 layer mentioned above refers to the average thickness of the λ / 4 layer. The average thickness is obtained by measuring the thickness of any five or more points in the λ / 4 layer and taking their arithmetic mean.
[0056] <Substrate> This polarizing plate may contain a substrate. As described above, the substrate may be located on the opposite side of the polarizer side of the λ / 4 layer. The substrate preferably contains a polymer. In other words, the substrate is preferably a polymer film. Examples of polymer film materials include cellulose polymers; acrylic polymers such as polymethyl methacrylate; thermoplastic norbornene polymers; polycarbonate polymers; polyester polymers such as polyethylene terephthalate and polyethylene naphthalate; styrene polymers such as polystyrene and acrylonitrile styrene copolymers; polyolefin polymers such as polyethylene, polypropylene, and ethylene-propylene copolymers; vinyl chloride polymers; amide polymers such as nylon and aromatic polyamides; imide polymers; sulfone polymers; polyethersulfone polymers; polyetheretherketone polymers; polyphenylene sulfide polymers; vinylidene chloride polymers; vinyl alcohol polymers; vinyl butyral polymers; arylate polymers; polyoxymethylene polymers; epoxy polymers; or polymers which are mixtures of these polymers. Among these, cellulose-based polymers are preferred as materials for polymer films, and cellulose acylates are more preferred.
[0057] The substrate may contain an ultraviolet absorber. The type of ultraviolet absorber is not particularly limited, and known ultraviolet absorbers can be used. Examples of ultraviolet absorbers include compounds selected from the group consisting of merocyanine compounds (especially diethylamino-phenylsulfonyl ultraviolet absorbers), benzophenone compounds, benzoxazinon compounds, anthracene compounds, benzotriazole compounds, indole compounds, methine compounds, benzodithiol compounds, and hydroxyphenyltriazine compounds. The wavelength range of ultraviolet light absorbed by the ultraviolet absorber is not particularly limited, but ultraviolet absorbers with a maximum absorption wavelength in the wavelength range of 300 to 400 nm are preferably used. The content of the ultraviolet absorber is preferably 0.1 to 20% by mass, and more preferably 1 to 10% by mass, based on the total mass of the substrate.
[0058] The thickness of the substrate is not particularly limited, but is preferably 1 to 200 μm, and more preferably 10 to 100 μm. The above-mentioned substrate thickness refers to the average thickness of the substrate. The above average thickness is obtained by measuring the thickness of five or more arbitrary points on the substrate and taking the arithmetic mean of them.
[0059] <Other Components> This polarizing plate may include other components besides the λ / 4 layer, polarizer, and substrate. For example, this polarizing plate may include a hard coat layer, alignment film, adhesion layer, and substrate.
[0060] (Hard Coat Layer) This polarizing plate may include a hard coat layer. Preferably, this polarizing plate includes the hard coat layer on the side opposite to the λ / 4 layer side of the substrate. The presence of the hard coat layer improves durability.
[0061] The composition of the hard coat layer is not particularly limited, and known hard coat layers can be used, such as organic hard coat layers, inorganic hard coat layers, and organic-inorganic hybrid hard coat layers. The hard coat layer is preferably formed using a hard coat layer forming composition containing polymerizable monomers. The hard coat layer may optionally contain fillers.
[0062] The polymerizable monomers included in the hard coat layer forming composition are not particularly limited, but polymerizable monomers in which the ratio of the molecular weight of the polymerizable monomer to the number of polymerizable groups is 120 or less are preferred in terms of superior hardness of the polarizing plate. The above ratio is more preferably 100 or less. The lower limit of the above ratio is not particularly limited, but may be 70 or more. The type of polymerizable group that the polymerizable monomer has is not particularly limited, and examples include radical polymerizable groups and cationic polymerizable groups, with radical polymerizable groups being preferred. Examples of radical polymerizable groups include acryloyl groups and methacryloyl groups. The number of polymerizable groups that the polymerizable monomer has is not particularly limited, and may be 2 or more, or 3 to 6.
[0063] The method for producing the hard coat layer is not particularly limited, but as described above, a method using a hard coat layer forming composition containing a polymerizable monomer (preferably a polyfunctional monomer) is preferred. More specifically, a method is to apply the hard coat layer forming composition onto a surface to be coated, and then cure the resulting coating film to form a hard coat layer.
[0064] The thickness of the hard coat layer is preferably 1.0 to 20.0 μm, and more preferably 1.5 to 15.0 μm.
[0065] (Alignment film) This polarizer may include an alignment film. Known alignment films can be used as the alignment film. Examples include a rubbing-treated alignment film and an optical alignment film.
[0066] (Adhesion Layer) This polarizing plate may further include an adhesion layer to enhance the adhesion between components. The adhesion layer is a layer selected from the group consisting of an adhesive layer and a tack layer. The tack layer is a layer formed using an adhesive. Examples of adhesives include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. The adhesive layer is a layer formed by curing an adhesive. Examples of adhesives include curable adhesives such as active energy ray-curable adhesives and thermosetting adhesives. Examples of active energy ray-curable adhesives include electron beam-curable adhesives, ultraviolet-curable adhesives, and visible light-curable adhesives, with ultraviolet-curable adhesives being preferred. In other words, it is preferable that the adhesion layer is a layer formed by curing an ultraviolet-curable adhesive.
[0067] In this polarizing plate, it is preferable that at least one of the substrate, hard coat layer, and adhesion layer contains an ultraviolet absorber. In this polarizing plate, the substrate may be included on the side opposite to the λ / 4 layer side of the polarizer. Examples of substrate types include those described above.
[0068] A display device including this polarizing plate may also include other components as described above, similar to this polarizing plate. For example, the substrate may be placed between the phase difference layer and the display element in the display device.
[0069] The method for manufacturing the polarizing plate and the display device is not particularly limited, and one method is to bond the various components described above via an adhesion layer.
[0070] This polarizing plate is applied to a display device. When this polarizing plate is applied to a display device, it means that it is used as a component of the display device. When this polarizing plate is applied to a display device, it is positioned so that the λ / 4 layer faces the viewer side. In other words, in a display device including a display element and this polarizing plate, the polarizer is positioned closer to the display element than the λ / 4 layer. This polarizing plate may be directly laminated onto the display element in contact with it, or it may be laminated onto the display element via another layer (e.g., an adhesion layer, a phase difference layer, a substrate, etc.).
[0071] Figure 1 describes a display device 100A including an organic EL display element, but the display device of this disclosure is not limited to this embodiment. The type of display device is not particularly limited as long as the polarizing plate is placed on the viewing side within the display device. For example, the display device of this disclosure may be a liquid crystal display device including a liquid crystal display element and the polarizing plate. In addition to organic EL display devices, other examples of display devices including the polarizing plate include liquid crystal display devices, micro-LED display devices, head-up displays, and head-mounted displays.
[0072] Another example of a display device including this polarizing plate is shown in Figure 2. Display device 100B includes a polarizer 22, a liquid crystal cell 24, a phase difference layer 26, a polarizer 16, a λ / 4 layer 18, and a substrate 20. This polarizing plate 10 is composed of a polarizer 16 and a λ / 4 layer 18. Display device 100B is visible from the substrate 20 side, similar to display device 100A. Light emitted from a light source (not shown) passes through the polarizer 16 to become linearly polarized, and then passes through the λ / 4 layer 18 to become circularly polarized, and enters the observer's eye of display device 100B while maintaining its polarization state. Each component will be described in detail below. Note that the polarizer 16, the λ / 4 layer 18, and the substrate 20 have already been explained in the section above, so their explanation will be omitted.
[0073] The polarizer 22 can be made of the same material as the polarizer 16. The liquid crystal cell 24 can be any known liquid crystal cell. The liquid crystal cell is not particularly limited as long as it is a liquid crystal cell that constitutes a liquid crystal panel capable of electrically birefringent switching. Such a liquid crystal cell is preferably in VA (Vertical Alignment) mode, OCB (Optically Compensated Bend) mode, IPS (In-Plane-Switching) mode, or TN (Twisted Nematic) mode, but is not limited to these. The phase difference layer 26 can function as a so-called optical compensation layer. The phase difference layer 26 can be any known optical compensation layer. By having an optical compensation layer, color changes and contrast reductions when viewed from an oblique direction can be reduced, and a high display quality can be obtained. From the viewpoint of ease of manufacture, the optical compensation layer is preferably a polymer film or a film formed using a liquid crystal composition.
[0074] The features of this disclosure will be further described below with reference to examples and comparative examples. The materials, amounts used, proportions, processing content, and processing procedures shown in the following examples may be modified as appropriate, provided that they do not deviate from the spirit of this disclosure. Therefore, the scope of this disclosure should not be interpreted as being limited by the specific examples shown below.
[0075] <Example 1> (Preparation of Cellulose Acrylate Film) A cellulose acylate dope (1) with the following composition was placed in a mixing tank, stirred, and then heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare the dope. The solid content concentration of the dope was 23.5% by mass, the amount of plasticizer added was a ratio to the cellulose acylate, and the solvent of the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (by mass ratio).
[0076] -------------------------------------------------- Cellulose acylate dope (1) -------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity-average degree of polymerization 310) 100 parts by mass of sugar ester compound 1 (shown in chemical formula (S4)) 6.0 parts by mass of sugar ester compound 2 (shown in chemical formula (S5)) 2.0 parts by mass of silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 parts by mass of solvent (methylene chloride / methanol / butanol)
[0077]
[0078]
[0079] The dope prepared as described above was cast using a drum film-forming machine. Specifically, the dope was cast from the die onto a metal support cooled to 0°C, and then the resulting web (film) was peeled off. The drum was made of stainless steel (SUS).
[0080] After the web (film) obtained by casting was peeled from the drum, it was dried for 20 minutes in a tenter device at 30-40°C during film transport, with both ends of the web clipped with clips. Subsequently, the web was further dried by zone heating while being transported on a roll. The obtained web was knurled and then wound up. The thickness of the obtained cellulose acylate film was 80 μm.
[0081] (Single-sided saponification treatment) The cellulose acylate film described above is passed through a dielectric heating roll at a temperature of 60°C to raise the film surface temperature to 40°C. Then, an alkaline solution of the following composition is applied to the band surface of the film using a bar coater at a rate of 14 ml / m². 2 The material was coated and then transported for 10 seconds under a steam-type far-infrared heater manufactured by Noritake Co., Ltd., heated to 110°C. Subsequently, using the same bar coater, 3 ml / m of pure water was applied. 2 The film was then coated. Next, it was washed with water using a fountain coater and dewatered with an air knife three times, and then transported to a 70°C drying zone for 10 seconds to dry, thereby producing a cellulose acylate film with one side saponified.
[0082] -------------------------------------------------- Alkaline solution -------------------------------------------------- Potassium hydroxide 4.7 parts by mass Water 15.8 parts by mass Isopropanol 63.7 parts by mass Surfactant SF-1:C 14 H 29 O(CH 2 CH 2 O) 20 H 1.0 parts by mass, Propylene glycol 14.8 parts by mass --------------------------------------------------
[0083] (Formation of Orientation Film) An orientation film-forming composition with the following composition was continuously applied to the surface of the cellulose acylate film that had undergone alkali saponification treatment using a #14 wire bar. The resulting cellulose acylate film was then dried with hot air at 60°C for 60 seconds, and then with hot air at 100°C for 120 seconds.
[0084] ------------------------------------------------------------------ Composition for forming an oriented film ------------------------------------------------------------------ Modified polyvinyl alcohol-1 below 10 parts by mass Water 170 parts by mass Methanol 57 parts by mass ------------------------------------------------------------------
[0085] Modified polyvinyl alcohol-1 (In the formula, the numerical values listed for each repeating unit represent the content (mol%) of each repeat relative to the total number of repeating units.)
[0086]
[0087] (Formation of λ / 4 layers (2 liquid crystal layers)) The alignment film prepared above was continuously rubbed. At this time, the longitudinal direction of the long film and the transport direction were parallel, and the angle between the longitudinal direction of the film and the rotation axis of the rubbing roller was set to 78.5°. If the longitudinal direction of the film is set to 90°, and when observed from the film side, with the film width direction as the reference (0°) and clockwise direction represented as a positive value, the rotation axis of the rubbing roller is at -11.5°. In other words, the position of the rotation axis of the rubbing roller is the position obtained by rotating 78.5° clockwise with respect to the longitudinal direction of the film. Using the cellulose acylate film that underwent the above rubbing treatment as a support, a liquid crystal composition L1 with the following composition was applied using a Gieser coating machine to form a composition layer.
[0088] -------------------------------------------------- Liquid Crystal Composition L1 -------------------------------------------------- ・The following rod-shaped liquid crystal compound (A) 80 parts by mass ・The following rod-shaped liquid crystal compound (B) 17 parts by mass ・The following polymerizable compound (C) 3 parts by mass ・Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass ・Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by mass ・The following left-handed chiral agent (L2) 0.47 parts by mass ・The following right-handed chiral agent (R2) 0.42 parts by mass ・The following polymer (A) 0.08 parts by mass ・Methyl isobutyl ketone 78 parts by mass ・Ethyl propionate 78 parts by mass --------------------------------------------------
[0089] Rod-shaped liquid crystal compound (A) [A mixture of the following liquid crystal compounds (RA), (RB), and (RC) in a mass ratio of 84:14:2]
[0090]
[0091] Rod-shaped liquid crystal compound (B)
[0092]
[0093] Polymerizable compound (C) [In the following formula, Me represents a methyl group.]
[0094]
[0095] Left-hand torsional chiral agent (L2)
[0096]
[0097] Right-handed chiral agent (R2)
[0098]
[0099] Polymer (A) [Content of the left-hand repeating unit in the following formula relative to the total repeating units in Polymer (A): 70% by mass, Content of the right-hand repeating unit in the following formula relative to the total repeating units in Polymer (A): 30% by mass, Weight-average molecular weight: 9000]
[0100]
[0101] Next, the obtained composition layer was heated at 95°C for 60 seconds. This heating caused the rod-shaped liquid crystal compounds in the composition layer to be oriented in a predetermined direction. Subsequently, ultraviolet light was irradiated onto the composition layer at 30°C under oxygen-containing air (oxygen concentration: approximately 20 vol%) using a 365 nm LED (Light Emitting Diode) lamp (manufactured by Acroedge Co., Ltd.) (irradiation dose: 25 mJ / cm²). 2 Next, the resulting composition layer was heated at 95°C for 10 seconds. After that, nitrogen purging was performed to an oxygen concentration of 100 ppm by volume, and ultraviolet light was irradiated onto the composition layer at 80°C using a metal halide lamp (manufactured by I-Graphics Co., Ltd.) (irradiation dose: 500 mJ / cm²). 2), an optically anisotropic layer with a fixed orientation state of the liquid crystal compound was formed as a λ / 4 layer, and a laminate 1 [layer structure: cellulose acylate film / orientation film / λ / 4 layer (homogeneous layer / twisted liquid crystal layer)] was fabricated. Laminate 1 containing the λ / 4 layer fabricated by the procedure described above was cut parallel to the rubbing direction, and the liquid crystal layer was observed from the cross-sectional direction with a polarizing microscope. The thickness of the λ / 4 layer was 2.7 μm, and the orientation state of the liquid crystal compound in the second liquid crystal layer with a thickness of 1.3 μm on the cellulose acylate film (resin film) side of the λ / 4 layer was homogeneous orientation with no twist angle, while the liquid crystal compound in the first liquid crystal layer with a thickness of 1.4 μm on the opposite side of the cellulose acylate film (resin film) of the λ / 4 layer was twisted orientation. Furthermore, the optical properties of the laminate 1 containing the λ / 4 layer of Example 1 were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The product of the refractive index anisotropy Δn2 and thickness d2 of the second liquid crystal layer at a wavelength of 550 nm (Δn2d2) was 179 nm, the twist angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -11.5° on the cellulose acylate film side and -11.5° on the side in contact with the first liquid crystal layer. In addition, the product of the refractive index anisotropy Δn1 and thickness d1 of the first liquid crystal layer at a wavelength of 550 nm (Δn1d1) was 178 nm, the twist angle of the liquid crystal compound was 79.6°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -11.5° on the side in contact with the second liquid crystal layer and -91.1° on the air side. The angles described above are observed from the support (cellulose acylate film) side, with the longitudinal direction of the laminate 1 as the reference (0°), and clockwise directions are expressed as positive values.
[0102] (Preparation of outer film) A cellulose acylate film with a thickness of 25 μm was prepared using the same method as Example 18 in International Publication No. 2014 / 112575. UV-531, manufactured by Teisei Chemicals Co., Ltd., was added to this cellulose acylate film as an ultraviolet absorber. The amount added was 3 phr (per 100 resin).
[0103] Each component was added according to the composition described below for hard coat layer formation composition HC-1. The resulting composition was placed in a mixing tank, stirred, and filtered through a polypropylene filter with a pore size of 0.4 μm to obtain hard coat layer formation composition HC-1.
[0104] -------------------------------------------------- Composition HC-1 for forming a hard coat layer -------------------------------------------------- 33.6 parts by mass of A-TMMT below 1.4 parts by mass of Omnirad127 below 35.8 parts by mass of methyl ethyl ketone 29.2 parts by mass of methyl acetate --------------------------------------------------
[0105] A-TMMT: Pentaerythritol tetraacrylate (manufactured by Shin-Nakamura Chemical Industry Co., Ltd.) Omnirad127: Photopolymerization initiator (manufactured by IGM Resins Inc.)
[0106] Next, the 25 μm cellulose acylate film prepared above was coated with the hard coat layer-forming composition HC-1 using a die coater to form a coating layer. The resulting cellulose acylate film was then dried at 30°C for 90 seconds, followed by drying at 60°C for 1 minute. Next, while purging with nitrogen to maintain an oxygen concentration of 0.3 volume%, an illuminance of 200 mW / cm² was applied using a 160 W / cm² air-cooled metal halide lamp (manufactured by I-Graphics Co., Ltd.). 2 , irradiation amount 60mJ / cm 2 The coating layer was cured by irradiation with ultraviolet light to create a protective film with a 5 μm thick hard coat layer, which was used as the outer film. Next, the side of the outer film opposite to the side with the hard coat layer and the λ / 4 layer side of the laminate 1 containing the λ / 4 layer were bonded together via the UV adhesive 1 described below, and UV irradiation (metal halide lamp, 240 mJ / cm²) was applied from the side of the laminate 1 containing the λ / 4 layer. 2 , 150 mW / cm 2The layers were bonded together by ) . From the laminate obtained by bonding, the cellulose acylate film and alignment film were peeled off to produce an outer film laminate containing a liquid crystal layer [layer structure: outer film (HC layer / cellulose acylate film) / UV adhesive layer / λ / 4 layers (twisted liquid crystal layer / homogeneous layer)].
[0107] (Preparation of UV Adhesive 1) UV Adhesive 1 was prepared with the following composition: ───────────────────────────────── UV Adhesive 1 ───────────────────────────────── ・CEL2021P (manufactured by Daicel Corporation) 70 parts by mass ・1,4-Butanediol diglycidyl ether 20 parts by mass ・2-Ethylhexylglycidyl ether 10 parts by mass ・CPI-100P 2.25 parts by mass ─────────────────────────────────
[0108] CPI-100P
[0109]
[0110] (Preparation of inner film) Each component was added to a mixing tank with the composition described in Cellulose Acrylate Dope (2) below, stirred, and then heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare Cellulose Acrylate Dope (2). The solid content concentration of Cellulose Acrylate Dope (2) was 23.5% by mass, the amount of plasticizer added was a ratio to the cellulose acylate, and the solvent was methylene chloride / methanol / butanol = 81 / 18 / 1 (by mass ratio).
[0111] -------------------------------------------------- Cellulose acylate dope (2) -------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity-average degree of polymerization 310) 100 parts by mass Ester oligomer A (see below) 8.0 parts by mass Silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 parts by mass Solvent (methylene chloride / methanol / butanol)
[0112] Ester oligomer A: Condensate of ethanediol / adipic acid (1 / 1 molar ratio), number average molecular weight 1000, hydroxyl value 112
[0113] The cellulose acylate dope (2) prepared above was cast using a drum film-forming machine. The cellulose acylate dope (2) was cast from the die so as to be in contact with a metal support cooled to 0°C, and then the resulting web (film) was peeled off. The drum was made of SUS (stainless steel).
[0114] After the casting process, the resulting web (film) was peeled from the drum and dried for 20 minutes in a tenter device at 30-40°C during film transport, with clips holding both ends of the web in place. The film was then wound up to a thickness of 40 μm and used as the inner film.
[0115] The inner film prepared as described above was immersed in a 1.5 mol / L NaOH aqueous solution (saponification solution) maintained at 55°C for 2 minutes, then the film was rinsed with water, and subsequently immersed in a 0.05 mol / L sulfuric acid aqueous solution at 25°C for 30 seconds. After that, the film was rinsed under running water for 30 seconds to neutralize it. Then, the water was removed three times using an air knife, and after the water was removed, the film was left in a 70°C drying zone for 15 seconds to dry, thus producing a saponified inner film.
[0116] (Fabrication of polarizer) A polarizer with a film thickness of 26 μm was fabricated by adsorbing iodine onto a stretched polyvinyl alcohol film in accordance with Example 1 of Japanese Patent Application Publication No. 2001-141926.
[0117] (Fabrication of polarizing plate) One side of a polarizer fabricated by the method described above, with nothing bonded to either side, was bonded with the saponified inner film described above using a polyvinyl alcohol-based adhesive. The other side of the polarizer was bonded to the λ / 4 layer side of an outer film laminate containing a λ / 4 layer via UV adhesive 1, and the polarizer was irradiated with UV light from the inner film side (metal halide lamp, 240 mJ / cm²). 2 , 150 mW / cm 2 The layers were bonded together by ) . At this time, the in-plane slow axis of the outermost liquid crystal layer (homogeneous layer) contained in the outer film laminate was set to -11.5° with respect to the absorption axis of the polarizer. Note that the above angle represents the position of the in-plane slow axis of the homogeneous layer when the bonded product is observed from the polarizer side after bonding the polarizer, and the absorption axis of the polarizer is taken as the reference (0°), with clockwise angles being represented as "positive". At this time, the absorption axis direction of the polarizer and the longitudinal direction of the outer film laminate are parallel. A polarizing plate 1 [layer structure: outer film (HC layer / cellulose acylate film) / adhesive layer / λ / 4 layers (twisted liquid crystal layer / homogeneous layer) / UV adhesive layer / polarizer / polyvinyl alcohol-based adhesive layer / inner film / adhesive layer / protective film] was fabricated by peeling off one side of the protective film of the adhesive SK-2057 and bringing the exposed adhesive surface into contact with the inner film side of the above laminate, and then applying pressure with a rubber roller to bond them together.
[0118] <Example 2> The amount of liquid crystal composition L1 applied, the angle of the rotation axis of the rubbing roller (changed from -11.5° to -12.6°), and the irradiation amount of the 365 nm LED lamp (25 mJ / cm²) 2 From 24 mJ / cm 2Laminate 2, including the λ / 4 layer of Example 2, was fabricated following the same procedure as in Example 1, except that the following adjustments were made (changed to). Furthermore, polarizing plate 2 was fabricated following the same procedure as in Example 1, except that laminate 2 was used instead of laminate 1. The product of the refractive index anisotropy Δn2 and thickness d2 (Δn2d2) of the second liquid crystal layer of the λ / 4 layer in laminate 2 at a wavelength of 550 nm was 181.4 nm, the torsion angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -12.6° on the cellulose acylate film side and -12.6° on the side in contact with the first liquid crystal layer. Furthermore, the product of the refractive index anisotropy Δn1 and thickness d1 (Δn1d1) of the first liquid crystal layer of the λ / 4 layer in the laminate 2 at a wavelength of 550 nm was 176.3 nm, the twist angle of the liquid crystal compound was 79.0°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -12.6° on the side in contact with the second liquid crystal layer and -91.6° on the air side.
[0119] <Example 3> Liquid crystal composition L2 was used instead of liquid crystal composition L1, and the amount of liquid crystal composition L2 applied, the angle of the rotation axis of the rubbing roller (changed from -11.5° to -14.4°), and the irradiation amount of the 365 nm LED lamp (25 mJ / cm²) were changed. 2 From 27 mJ / cm 2 A laminate 3 containing the λ / 4 layer of Example 3 was fabricated following the same procedure as in Example 1, except that the following adjustments were made (changed to). Furthermore, a polarizing plate 3 was fabricated following the same procedure as in Example 1, except that laminate 3 was used instead of laminate 1. The product of the refractive index anisotropy Δn2 and thickness d2 (Δn2d2) of the second liquid crystal layer of the λ / 4 layer in laminate 3 at a wavelength of 550 nm was 180.1 nm, the torsion angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -14.4° on the cellulose acylate film side and -14.4° on the side in contact with the first liquid crystal layer. Furthermore, the product of the refractive index anisotropy Δn1 and thickness d1 (Δn1d1) of the first liquid crystal layer of the λ / 4 layer in the laminate 3 at a wavelength of 550 nm was 172.7 nm, the twist angle of the liquid crystal compound was 83.1°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -14.4° on the side in contact with the second liquid crystal layer and -97.5° on the air side.
[0120] -------------------------------------------------- Liquid Crystal Composition L2 -------------------------------------------------- ・The above rod-shaped liquid crystal compound (A) 80 parts by mass ・The above rod-shaped liquid crystal compound (B) 17 parts by mass ・The above polymerizable compound (C) 3 parts by mass ・Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass ・Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by mass ・The above left-handed chiral agent (L2) 0.50 parts by mass ・The above right-handed chiral agent (R2) 0.45 parts by mass ・The above polymer (A) 0.08 parts by mass ・Methyl isobutyl ketone 78 parts by mass ・Ethyl propionate 78 parts by mass --------------------------------------------------
[0121] <Example 4> A laminate 4 containing the λ / 4 layer of Example 4 was prepared by following the same procedure as in Example 2, except that the amount of coating was changed. Furthermore, a polarizing plate 4 was prepared by following the same procedure as in Example 1, except that laminate 4 was used instead of laminate 1. The product of the refractive index anisotropy Δn2 and thickness d2 (Δn2d2) of the second liquid crystal layer of the λ / 4 layer in laminate 4 at a wavelength of 550 nm was 146.0 nm, the twist angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -12.6° on the cellulose acylate film side and -12.6° on the side in contact with the first liquid crystal layer. Furthermore, the product of the refractive index anisotropy Δn1 and thickness d1 (Δn1d1) of the first liquid crystal layer of the λ / 4 layer in the laminate 4 at a wavelength of 550 nm was 176.3 nm, the twist angle of the liquid crystal compound was 79.0°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -12.6° on the side in contact with the second liquid crystal layer and -91.6° on the air side.
[0122] <Example 5> A laminate 5 containing the λ / 4 layer of Example 5 was fabricated following the same procedure as in Example 2, except that the coating amount and the irradiation amount of the 365 nm LED lamp were changed. Furthermore, a polarizing plate 5 was fabricated following the same procedure as in Example 1, except that laminate 5 was used instead of laminate 1. The product of the refractive index anisotropy Δn2 and thickness d2 (Δn2d2) of the second liquid crystal layer of the λ / 4 layer in laminate 5 at a wavelength of 550 nm was 125.0 nm, the twist angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -12.6° on the cellulose acylate film side and -12.6° on the side in contact with the first liquid crystal layer. Furthermore, the product of the refractive index anisotropy Δn1 and thickness d1 (Δn1d1) of the first liquid crystal layer of the λ / 4 layer in the laminate 5 at a wavelength of 550 nm was 156.0 nm, the twist angle of the liquid crystal compound was 69.9°, and the orientation axis angle of the liquid crystal compound with respect to the longitudinal direction was -12.6° on the side in contact with the second liquid crystal layer and -82.5° on the air side.
[0123] <Comparative Example 1> An alignment film was prepared by performing a single-sided saponification treatment on the back side of a protective film with a hard coat layer with a thickness of 5 μm. A liquid crystal layer was formed on the alignment film according to the same procedure as in Example 2 to prepare a laminate C1 including the liquid crystal layer. Furthermore, a polarizing plate C1 [layer configuration: outer film (HC layer / cellulose acylate film) / alignment film / λ / 4 layers (homogenous layer / twisted liquid crystal layer) / UV adhesive layer / polarizer / polyvinyl alcohol-based adhesive layer / inner film / adhesive layer / protective film] was prepared according to the same procedure as in Example 2, except that laminate C1 was used instead of laminate 2. In polarizing plate C1, the positional relationship between the homogeneous layer and the twisted liquid crystal layer is different from that of the example.
[0124] <Comparative Example 2> In Example 1, the rotation axis of the rubbing roller was changed from 11.5° to 45.0°, and a liquid crystal composition C1 containing a rod-shaped liquid crystal compound of the following composition was applied using a Gieser coating machine to form a composition layer. Next, the obtained composition layer was heated at 95°C for 100 seconds. This heating caused the rod-shaped liquid crystal compound in the composition layer to be oriented in a predetermined direction. After that, nitrogen purging was performed to set the oxygen concentration to 100 ppm by volume, and ultraviolet light was irradiated onto the composition layer at 80°C using a metal halide lamp (manufactured by I-Graphics Co., Ltd.) (irradiation dose: 500 mJ / cm²). 2 A laminate C2 containing a λ / 4 layer was prepared in the same manner as in Example 1, except that a liquid crystal layer was formed in which the orientation state of the liquid crystal compound was fixed. Furthermore, a polarizing plate C2 was prepared following the same procedure as in Example 1, except that laminate C2 was used instead of laminate 1.
[0125] ------------------------------------------------------------------- Liquid Crystal Composition C1 ------------------------------------------------------------------- ・The above rod-shaped liquid crystal compound (A) 80 parts by mass ・The above rod-shaped liquid crystal compound (B) 17 parts by mass ・The above polymerizable compound (C) 3 parts by mass ・Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass ・Photopolymerization initiator (Irgacure 819, manufactured by BASF) 3 parts by mass ・The following polymer (B) 0.08 parts by mass ・Methyl isobutyl ketone 78 parts by mass ・Ethyl propionate 78 parts by mass -------------------------------------------------------------------
[0126] Polymer (B) [Content of the left-hand repeating unit in the following formula relative to the total repeating units in Polymer (B): 39% by mass, Content of the right-hand repeating unit in the following formula relative to the total repeating units in Polymer (B): 61% by mass]
[0127]
[0128] The optical properties of the laminate C2 fabricated as described above were determined using AxoScan from Axometrics and its analysis software (Multi-Layer Analysis). The product of Δn and thickness d (Δnd) at a wavelength of 550 nm in the λ / 4 layer was 137.5 nm, the torsion angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -45° on the side in contact with the substrate.
[0129] <Comparative Example 3> A laminate C3 containing a λ / 4 layer was prepared using the same procedure as in Comparative Example 2, except that the amount of coating was changed. Furthermore, a polarizing plate C3 was prepared using the same procedure as in Example 1, except that laminate C3 was used instead of laminate 1. The product of Δn and thickness d (Δnd) at a wavelength of 550 nm of the λ / 4 layer was 206.3 nm, the twist angle of the liquid crystal compound was 0°, and the orientation axis angle of the liquid crystal compound with respect to the long longitudinal direction was -45° on the side in contact with the substrate.
[0130] <Comparative Example 4> A photo-alignment film-forming material prepared according to the method described in Example 1 of International Publication No. 2016 / 002722 was applied to one side of the cellulose acylate film prepared using cellulose acylate dope (1) in Example 1 by die coating. The coating was then hardened by heating it to 125°C with hot air. Next, polarized ultraviolet light at 313 nm was irradiated while shielding only the edges of the long film to form an alignment layer. The polarization direction of the polarized ultraviolet light was set so that the orientation direction of the liquid crystal was 45° with respect to the longitudinal direction of the long film.
[0131] A liquid crystal composition C2 with the following composition was applied to the fabricated alignment layer using a coating device. The coating film formed on the alignment layer was heated to 120°C with hot air, then cooled to 60°C, and then heated at a wavelength of 365 nm using a high-pressure mercury lamp under a nitrogen atmosphere at 50 mJ / cm². 2 The coating is irradiated with ultraviolet light, followed by heating to 120°C while applying 300 mJ / cm² of UV light. 2 The coating film was irradiated with ultraviolet light. Following the above procedure, the orientation of the liquid crystal compound was fixed, and a λ / 4 layer was fabricated.
[0132] -------------------------------------------------- Liquid Crystal Composition C2 -------------------------------------------------- ・Polymerizable liquid crystal compound L-1 below 86 parts by mass ・Polymerizable liquid crystal compound L-2 below 14 parts by mass ・Polymerization initiator S-1 below 0.5 parts by mass ・Highsolve MTEM (manufactured by Toho Chemical Industry Co., Ltd.) 2 parts by mass ・Leveling agent (compound T-1 below) 0.2 parts by mass ・Methyl ethyl ketone (MEK) 174 parts by mass ・Cyclopentanone 44 parts by mass --------------------------------------------------
[0133] Polymerizable liquid crystal compound L-1
[0134]
[0135] Polymerizable liquid crystal compound L-2
[0136]
[0137] Polymerization initiator S-1
[0138]
[0139] Compound T-1 was a polymer containing units based on monomers represented by the following formulas (T-1-a), (T-1-b), and (T-1-c) in a molar ratio of (T-1-a):(T-1-b):(T-1-c) = 60:30:10. The weight-average molecular weight was 20,000.
[0140]
[0141] In this way, a laminate C4 was obtained in which an orientation layer and a λ / 4 layer were laminated on a cellulose acylate film. The in-plane retardation of the λ / 4 layer in the above laminate C4 at a wavelength of 550 nm was 142.5 nm, and its in-plane slow axis was 45° with respect to the length direction. Furthermore, a polarizing plate C4 was fabricated by following the same procedure as in Example 1, except that laminate C4 was used instead of laminate 1.
[0142] <Comparative Example 5> A laminate C5 containing a λ / 4 layer was prepared by following the same procedure as in Comparative Example 2, except that liquid crystal composition C1 was changed to liquid crystal composition C3. Furthermore, a polarizing plate C5 was prepared by following the same procedure as in Example 1, except that laminate C5 was used instead of laminate 1. The in-plane retardation of the λ / 4 layer at a wavelength of 550 nm was 137.5 nm. The average inclination angle of the disc surface of the disc-shaped liquid crystal compound with respect to the film surface was 90°, confirming that it was oriented perpendicular to the film surface. In addition, the angle of the in-plane slow axis of the λ / 4 layer was parallel to the rotation axis of the rubbing roller, and when the width direction of the film was set to 0° (the longitudinal direction was 90° counterclockwise and -90° clockwise), the in-plane slow axis was -45° when viewed from the λ / 4 layer side.
[0143] -------------------------------------------------- Liquid Crystal Composition C3 -------------------------------------------------- Disc-shaped liquid crystal compound 1 below 80 parts by mass Disc-shaped liquid crystal compound 2 below 20 parts by mass Alignment film interface orientation agent 1 below 0.55 parts by mass Fluorine-containing compound A below 0.1 parts by mass Fluorine-containing compound B below 0.05 parts by mass Fluorine-containing compound C below 0.21 parts by mass Ethylene oxide-modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 10 parts by mass Photopolymerization initiator (Irgacure 907, manufactured by BASF) 3.0 parts by mass Methyl ethyl ketone 200 parts by mass --------------------------------------------------
[0144] Disc-shaped liquid crystal compound 1
[0145]
[0146] Disc-shaped liquid crystal compound 2
[0147]
[0148] Orientation film interface orientation agent 1
[0149]
[0150] Fluorine-containing compound A (Hereinafter, a and b represent the content (mass%) of each repeating unit relative to the total repeating units, where a represents 90% by mass and b represents 10% by mass. Weight-average molecular weight: 15000.)
[0151]
[0152] Fluorine-containing compound B (The numerical values within each repeating unit represent the content (mass%) relative to the total number of repeating units. The content of the repeating unit on the left was 32.5% by mass, and the content of the repeating unit on the right was 67.5% by mass. Weight-average molecular weight: 15000.)
[0153]
[0154] Fluorine-containing compound C (The numerical values within each repeating unit represent the content (mass%) relative to the total number of repeating units. The content of the repeating unit on the left was 25% by mass, the content of the repeating unit in the middle was 25% by mass, and the content of the repeating unit on the right was 50% by mass. Weight-average molecular weight: 15000)
[0155]
[0156] <Comparative Example 6> (Preparation of λ / 4 plate) Norbornene-based resin pellets (ZEONOR1420, manufactured by Nippon Zeon Co., Ltd.) were molded using a T-die type film extrusion molding machine to obtain an unstretched cycloolefin polymer substrate with a thickness of 100 μm.
[0157] The obtained unstretched cycloolefin polymer substrate was stretched longitudinally and then diagonally to obtain a diagonally stretched film corresponding to a λ / 4 plate. The stretching temperature and magnification of each film were adjusted so that the in-plane retardation at a wavelength of 550 nm was 142 nm and the in-plane slow axis orientation, with the longitudinal direction of the film as the reference (0°), was 45°.
[0158] (Preparation of polarizing plate C6) Polarizing plate C6 was prepared in the same procedure as in Example 1, except that the laminate 1 was replaced with the obliquely stretched film described above.
[0159] <Evaluation> (Moisture permeability of the λ / 4 layer) Film samples of 70 mm in diameter were cut from each of the laminates 1 to 5 containing the λ / 4 layer in each example and comparative example, laminates C1 to C5, and the obliquely stretched film which was the λ / 4 layer used in Comparative Example 6. Each cut film sample was conditioned at a temperature of 40°C and a relative humidity of 90% for 24 hours, and the moisture permeability was measured according to the method described in JIS Z-0208 (1976) (40°C as described in JIS was adopted). If the above film sample was a laminate containing layers other than the λ / 4 layer, the moisture permeability of the layers other than the λ / 4 layer was measured separately, and the moisture permeability of the λ / 4 layer was calculated using the following formula.
[0160]
[0161] Wtotal represents the total moisture permeability of the laminate. 1 , W 2 ... represents the moisture permeability of each individual layer.
[0162] (Measurement of Optical Properties) Using an AxoScan OPMF-1 (OptoScience Co., Ltd.), the in-plane retardation of the liquid crystal layer and the mean ellipticity of the polarizer were measured at 10 nm intervals in the wavelength range of 400 to 780 nm. When measuring the mean ellipticity of the polarizer, light was irradiated from the polarizer side along the direction normal to the main surface of the polarizer. The results of the mean ellipticity of the polarizer are shown in Table 1. Details of the measurement method for the mean ellipticity of the polarizer are as described above.
[0163] (Evaluation of Polarizer Durability) The protective film of the polarizer prepared above was peeled off, and the exposed adhesive side was bonded to glass. The change in orthogonal transmittance at a wavelength of 680 nm before and after placing the glass with the polarizer attached in an environment of 60°C and 95% relative humidity for a certain period of time was measured using an automatic polarizing film measuring device VAP-7070 manufactured by JASCO Corporation, and evaluated according to the following criteria. In the measurement of the orthogonal transmittance above, light was incident from the glass side of the glass with the polarizer attached. In the following evaluations, A or B is practically preferable. A: Change in orthogonal transmittance is less than 0.1% after 1000 hours B: Change in orthogonal transmittance is less than 0.1% after 750 hours, but the change in orthogonal transmittance is 0.1% or more after 1000 hours C: Change in orthogonal transmittance is less than 0.1% after 500 hours, but the change in orthogonal transmittance is 0.1% or more after 750 hours D: Change in orthogonal transmittance is 0 after 250 hours. Less than 1%, but the change in orthogonal transmittance after 500 hours was 0.1% or more. E: The change in orthogonal transmittance after 250 hours was 0.1% or more.
[0164] (Evaluation of eye strain) The front panel, including the touch sensor, polarizer, and cover glass, was peeled off from a commercially available smartphone (Galaxy A15, manufactured by SAMSUNG) to expose the organic EL panel. The liquid crystal layer side of the laminate 2, which includes the λ / 4 layer prepared in Example 2, was bonded to the surface of the panel via an adhesive so that the in-plane slow axis of the liquid crystal layer and the longitudinal direction of the panel were parallel. Furthermore, the polarizers in polarizers 1-5 and polarizers C1-C6 were bonded so that the angle between the absorption axis of the polarizers in polarizers in polarizers 1-5 and polarizers C1-C6 and the in-plane slow axis of the liquid crystal layer bonded to the panel was 45°. Polarizers 1-5 and polarizers C1-C6 were bonded so that the outer films in polarizers 1-5 and polarizers C1-C6 were located on the outside. An image was displayed on the panel with polarizers obtained in this way, and the number of blinks during the 5 minutes after 2.5 hours of viewing was recorded, and the number of blinks per minute was evaluated. A lower number of blinks indicates that eye strain is suppressed. The same evaluation was conducted before viewing. A blink count of 26 or less after viewing is preferable.
[0165]
[0166] As shown in Table 1, the polarizing plate exhibited the desired effect. A comparison of Examples 1-3 and Examples 4-5 confirmed that fatigue evaluation was superior when the average ellipticity was 0.84 or higher. A comparison of Example 5 with the other examples showed that the moisture permeability of the λ / 4 layer was 350 g / m². 2 - When the number of days was less than or equal to 1 day, it was confirmed that the polarizer durability was superior. In Comparative Examples 1-3 and 5-6, which did not meet the average ellipticity requirement, the number of blinks was higher than in the example. In Comparative Examples 2-5, which did not meet the λ / 4 layer moisture permeability requirement, the polarizer durability was inferior to that of the example.
[0167] (Note) (1) A polarizing plate comprising a λ / 4 layer and a polarizer, which is applied to a display device, wherein the λ / 4 layer is a layer containing a liquid crystal compound, and the moisture permeability of the λ / 4 layer at a temperature of 40°C and a relative humidity of 90% is 500 g / m². 2 (1) A polarizing plate having a mean ellipticity of 0.84 or more, wherein when light is shone from the polarizer side onto the polarizing plate, the average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is 0.80 or more, and the polarizing plate is arranged so that the λ / 4 layer faces the viewing side when applied to a display device. (2) The polarizing plate according to (1), wherein the average ellipticity is 0.84 or more. (3) A polarizing plate having a moisture permeability of 350 g / m 2- A polarizing plate according to (1) or (2), wherein the polarizing plate is less than or equal to day. (4) A polarizing plate according to any one of (1) to (3), wherein the λ / 4 layer comprises two or more liquid crystal layers having different orientation states of liquid crystal compounds. (5) A polarizing plate according to (4), wherein at least one of the two or more liquid crystal layers is a layer in which a homogeneously oriented rod-shaped liquid crystal compound is fixed. (6) A polarizing plate according to (5), wherein at least one of the two or more liquid crystal layers is a layer in which a homogeneously oriented rod-shaped liquid crystal compound is fixed, and at least one of the two or more liquid crystal layers is a liquid crystal layer containing a liquid crystal compound that is twisted with the thickness direction as the helical axis. (7) A polarizing plate according to any one of (1) to (6), wherein the λ / 4 layer comprises a substrate on the side opposite to the polarizer side. (8) A polarizing plate according to (7), wherein the substrate comprises a hard coat layer on the side opposite to the λ / 4 layer side. (9) A display device comprising a polarizing plate according to any one of (1) to (8). (10) A display device comprising an organic electroluminescent display element and a polarizing plate according to any one of (1) to (8), wherein the polarizer in the polarizing plate is positioned closer to the organic electroluminescent display element than the λ / 4 layer. (11) The display device according to (10), further comprising a phase difference layer between the organic electroluminescent display element and the polarizing plate. (12) A display device comprising a polarizer, a liquid crystal cell, and a polarizing plate according to any one of (1) to (8), wherein the polarizer in the polarizing plate is positioned closer to the liquid crystal cell than the λ / 4 layer.
[0168] (1) The polarizing plate according to (1) makes it possible to form a display device that suppresses eye strain when viewed by an observer, compared to a case without the configuration of the embodiment of this disclosure, and also suppresses the deterioration of the polarizer even under high temperature and high humidity conditions. (2) The polarizing plate according to (2) further suppresses eye strain. (3) The polarizing plate according to (3) further suppresses the deterioration of the polarizer.
[0169] 10 Polarizing plate 12 Organic EL display device 14 Phase difference layer 16 Polarizer 18 λ / 4 layer 20 Substrate 22 Polarizer 24 Liquid crystal cell 26 Optical compensation layer 100A, 100B Display device
Claims
1. A polarizing plate comprising a λ / 4 layer and a polarizer, applied to a display device, wherein the λ / 4 layer is a layer containing a liquid crystal compound, and the moisture permeability of the λ / 4 layer at a temperature of 40°C and a relative humidity of 90% is 500 g / m². 2 A polarizing plate having a value of 0.80 or less, wherein when light is irradiated onto the polarizing plate from the polarizer side, the average ellipticity of the transmitted light at wavelengths of 400 to 780 nm is 0.80 or more, and the polarizing plate is arranged so that the λ / 4 layer faces the viewing side when applied to a display device.
2. The polarizing plate according to claim 1, wherein the mean ellipticity is 0.84 or greater.
3. The aforementioned moisture permeability is 350 g / m². 2 A polarizing plate according to claim 1, wherein the day is less than or equal to [number] days.
4. The polarizing plate according to claim 1, wherein the λ / 4 layer comprises two or more liquid crystal layers having different orientation states of liquid crystal compounds.
5. The polarizing plate according to claim 4, wherein at least one of the two or more liquid crystal layers is a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed.
6. The polarizing plate according to claim 5, wherein at least one of the two or more liquid crystal layers is a layer on which homogeneously oriented rod-shaped liquid crystal compounds are fixed, and at least one of the two or more liquid crystal layers is a liquid crystal layer containing a torsionally oriented liquid crystal compound with the thickness direction as the helical axis.
7. The polarizing plate according to claim 1, wherein the λ / 4 layer includes a substrate on the side opposite to the polarizer side.
8. The polarizing plate according to claim 7, wherein the substrate includes a hard coat layer on the side opposite to the λ / 4 layer side.
9. A display device comprising a polarizing plate according to any one of claims 1 to 8.
10. A display device comprising an organic electroluminescent display element and a polarizing plate according to any one of claims 1 to 8, wherein the polarizer in the polarizing plate is positioned closer to the organic electroluminescent display element than the λ / 4 layer.
11. The display device according to claim 10, further comprising a phase difference layer between the organic electroluminescent display element and the polarizing plate.
12. A display device comprising a polarizer, a liquid crystal cell, and a polarizing plate according to any one of claims 1 to 8, wherein the polarizer in the polarizing plate is positioned on the liquid crystal cell side of the λ / 4 layer.