Barrier material and product having the same
By applying a barrier material composed of polysiloxane compounds doped with metal atoms and silane oligomers modified with metal alkoxides on the electronic device substrate, the moisture absorption problem of the substrate is solved, and efficient moisture removal and moisture resistance are achieved. The effect improves the moisture resistance and performance of the device.
Patent Information
- Application Number
- CN201980098216.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-05-08
AI Technical Summary
The prior art is difficult to effectively suppress the moisture absorption of electronic device substrates, especially in the case of moisture intrusion, resulting in a degradation of device performance.
A barrier material arranged on the substrate is used, and the water vapor transmission rate from one side of the substrate to the opposite side is low, so that moisture absorption can be effectively suppressed and moisture is released by heating and drying. This material consists of a polysiloxane compound doped with metal atoms and a silane oligomer modified with a metal alkoxide, and the solidified product of the composition for formation is ensured to ensure that the water vapor transmittance A2/A1 ratio is 1.3 or more.
It significantly inhibits the moisture absorption of the substrate, can effectively dry moisture in a high-temperature environment, and improves the moisture resistance and moisture resistance of electronic devices.
Smart Images

Figure CN114096406B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a barrier material and a product having the barrier material. Background Art
[0002] Conventionally, in order to prevent moisture from entering the gaps formed in electronic devices, studies have been conducted to seal electronic devices using barrier films, etc. For example, Patent Document 1 describes a barrier film laminate formed by laminating barrier films having an inorganic oxide layer.
[0003] Previous technical literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2011-093195 Summary of the invention
[0006] Technical issues to be solved by the invention
[0007] An object of the present invention is to provide a barrier material disposed on a substrate, which can suppress moisture absorption of the substrate at a high level, and a product including the barrier material.
[0008] Means for solving technical problems
[0009] The present invention provides a barrier material disposed on a substrate, wherein a water vapor permeability A1 from a side opposite to the substrate to the substrate side is smaller than a water vapor permeability A2 from the substrate side to the side opposite to the substrate.
[0010] According to this barrier material, even when moisture intrudes into the substrate side, the moisture can be released to the side opposite to the substrate, so that moisture absorption into the substrate can be significantly suppressed. In addition, according to this barrier material, by performing heating and drying in a state where the barrier material is arranged, the moisture in the substrate is released to the outside, and the substrate can be effectively dried.
[0011] In one embodiment, the ratio (A2 / A1) of the water vapor permeability A2 to the water vapor permeability A1 may be 1.3 or more.
[0012] The barrier material according to one embodiment may include a polysiloxane compound doped with metal atoms.
[0013] In one embodiment, the polysiloxane compound may have a silicon atom bonded to three oxygen atoms.
[0014] In one embodiment, the ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the polysiloxane compound may be 30% or more.
[0015] In one embodiment, 90% or more of oxygen atoms in the polysiloxane compound may be bonded to silicon atoms.
[0016] The barrier material according to one embodiment may be composed of a cured product of the barrier material-forming composition applied on the substrate. In this case, the barrier material-forming composition may include a silane oligomer at least partly modified with a metal alkoxide.
[0017] In one embodiment, the silane oligomer may have a silicon atom bonded to three oxygen atoms.
[0018] In one embodiment, the ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the silane oligomer may be 50% or more.
[0019] In one embodiment, the barrier material-forming composition may further contain a silane monomer.
[0020] The present invention also provides a product comprising a substrate and the barrier material disposed on the substrate.
[0021] Effects of the Invention
[0022] The present invention can provide a barrier material disposed on a substrate, which can suppress moisture absorption of the substrate at a high level, and a product including the barrier material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic cross-sectional view showing a preferred embodiment of the barrier material. DETAILED DESCRIPTION
[0024] Hereinafter, preferred embodiments of the present invention will be described. In this specification, the numerical range represented by "~" indicates a range including the numerical values recorded before and after "~" as the minimum value and the maximum value, respectively. "A or B" only needs to include any one of A and B, or both. The materials exemplified in this embodiment can be used alone or in combination of two or more unless otherwise specified.
[0025] <Barrier materials>
[0026] The barrier material according to the present embodiment is disposed on a substrate, and has a water vapor permeability A1 from the side opposite to the substrate to the substrate side that is smaller than a water vapor permeability A2 from the substrate side to the side opposite to the substrate. Figure 1 This is a schematic cross-sectional view showing a preferred embodiment of the barrier material. Figure 1 The barrier material 10 is disposed on the substrate 20, and the water vapor permeability A1 from the surface 11 on the side opposite to the substrate 20 to the surface 12 on the substrate 20 side is smaller than the water vapor permeability A2 from the surface 12 on the substrate 20 side to the surface 11 on the side opposite to the substrate 20. Figure 1 As shown, a plurality of barrier materials 10 may be formed on the substrate 20, and preferably, the water vapor permeability A1 of all of the barrier materials 10 is less than the water vapor permeability A2.
[0027] According to the barrier material of this embodiment, even when moisture intrudes into the substrate side, the moisture can be released to the side opposite to the substrate, so that moisture absorption into the substrate can be significantly suppressed. In addition, according to the barrier material of this embodiment, by performing heating and drying in a state where the barrier material is arranged, the moisture in the substrate is released to the outside, and the substrate can be effectively dried.
[0028] The ratio of the water vapor permeability A2 to the water vapor permeability A1 (A2 / A1) may be, for example, 1.1 or more, preferably 1.3 or more, and more preferably 1.5 or more. This more significantly exhibits the above-mentioned effect.
[0029] The upper limit of the ratio (A2 / A1) of the water vapor permeability A2 to the water vapor permeability A1 is not particularly limited. The ratio (A2 / A1) may be, for example, 30 or less, 20 or less, or 10 or less.
[0030] The water vapor permeability A1 can be, for example, 5000 g / m 2 ·day or less, and preferably 4000 g / m2 from the viewpoint of further suppressing the intrusion of water into the substrate side. 2 ·Day or less, more preferably 3000g / m 2 The lower limit of the water vapor permeability A1 is not particularly limited. The water vapor permeability A1 may be, for example, 100 g / m 2 ·day or more. The water vapor transmission rate A1 is a value at 40°C and 95%RH per 20 μm thickness.
[0031] The water vapor transmission rate A2 can be, for example, 500 g / m 2 ·day or more, and preferably 2000 g / m2 from the viewpoint of more significantly obtaining the above-mentioned effect by releasing the water intruding into the substrate side. 2 day or more, more preferably 4000g / m 2 The upper limit of the water vapor permeability A2 is not particularly limited. The water vapor permeability A2 may be, for example, 10000 g / m 2·day or less. The water vapor transmission rate A2 is a value at 40°C and 95% RH per 20 μm thickness.
[0032] In addition, in this specification, the water vapor permeability A1 and the water vapor permeability A2 show the value measured by the method of JIS K7129.
[0033] The material constituting the barrier material according to the present embodiment is not particularly limited.
[0034] In a preferred embodiment, the barrier material preferably comprises a polysiloxane compound, and more preferably comprises a polysiloxane compound doped with metal atoms. Such a barrier material can easily control the voids in the barrier material by controlling the structure of silicon atoms in the polysiloxane compound, and can easily satisfy the above-mentioned relationship between the water vapor permeability A1 and the water vapor permeability A2.
[0035] The polysiloxane compound has a siloxane skeleton, and in the polysiloxane compound, metal atoms are bonded to silicon atoms constituting the polysiloxane skeleton via oxygen atoms.
[0036] The silicon atom contained in the polysiloxane compound can be divided into a silicon atom bonded to one oxygen atom (M unit), a silicon atom bonded to two oxygen atoms (D unit), a silicon atom bonded to three oxygen atoms (T unit), and a silicon atom bonded to four oxygen atoms (Q unit). Examples of the M unit, the D unit, the T unit, and the Q unit include the formulas (M), (D), (T), and (Q) described later, respectively.
[0037] In the polysiloxane compound, the ratio of the total number of T units and Q units to the total number of silicon atoms may be, for example, 30% or more, preferably 50% or more, more preferably 70% or more, further preferably 90% or more, and may be 100%. According to such a polysiloxane compound, the moisture resistance of the barrier material is further improved.
[0038] In a preferred embodiment, the polysiloxane compound preferably contains T units. The content of T units in the polysiloxane compound may be, for example, 10% or more, 20% or more, 30% or more, 40% or more, or 50% or more, preferably 70% or more, more preferably 80% or more, further preferably 90% or more, and may be 100% relative to the total number of silicon atoms. Such a polysiloxane compound tends to further improve flexibility and dehumidification properties.
[0039] In the polysiloxane compound, the molar ratio (M / Si) of the metal atoms M to the total number of silicon atoms (Si) may be, for example, 0.0001 or more, preferably 0.001 or more. Thus, there is a tendency that the curability becomes better. Furthermore, the molar ratio (M / Si) may be, for example, 0.5 or less, preferably 0.2 or less. Thus, there is a tendency that the transparency becomes further better.
[0040] In the polysiloxane compound, most of the oxygen atoms are preferably bonded to at least one silicon atom. When a small amount of alcoholic hydroxyl groups (C-OH) or ether bonds (COC) are present in the polysiloxane compound, the moisture resistance and dehumidification properties tend to be further improved. For example, among the oxygen atoms in the polysiloxane compound, preferably 90% or more are bonded to silicon atoms, more preferably 95% or more are bonded to silicon atoms, and even more preferably 99% or more are bonded to silicon atoms.
[0041] The barrier material may be transparent. Such a barrier material can be suitable for applications requiring transparency, for example, it can be preferably used as a coating material on an image sensor in an image sensor package. In addition, here, transparency means that the visible light transmittance (transmittance at 550 nm) per 1 mm thickness is 80% or more.
[0042] The visible light transmittance (550 nm transmittance) of the barrier material per 1 mm thickness is preferably 80% or more, more preferably 85% or more, and further preferably 90% or more. The visible light transmittance of the barrier material is measured using a spectrophotometer.
[0043] The shape of the barrier material is not particularly limited. The barrier material may be formed into a film, for example, and such a barrier material can be used as a moisture-proof barrier film. Furthermore, the barrier material may be formed in a manner covering the substrate, in which case the substrate can be prevented from contacting with moisture.
[0044] The barrier material can be constituted by, for example, a cured product of a barrier material-forming composition described below. A preferred embodiment of the barrier material-forming composition will be described below.
[0045] <Barrier material forming composition>
[0046] The barrier material-forming composition of the present embodiment contains a silane oligomer, at least a part of which is modified with a metal alkoxide.
[0047] This composition can easily form a barrier material satisfying the relationship between the water vapor permeability A1 and the water vapor permeability A2 on a substrate by appropriately adjusting the composition of silicon atoms (ratios of M units, D units, T units, and Q units) in the silane oligomer.
[0048] The barrier material-forming composition may be, for example, in a liquid state or a paste state. From the viewpoint of easy application to a substrate, the barrier material-forming composition is preferably a liquid composition.
[0049] A silane oligomer is a polymer of a silane monomer and has a structure in which a plurality of silicon atoms are linked via oxygen atoms. In this specification, a silane oligomer refers to a polymer having a molecular weight of 100,000 or less.
[0050] In this specification, the metal alkoxide-modified silane oligomer is a compound formed by the reaction of the silane oligomer and the metal alkoxide, and can be said to be a compound having a structure in which a silicon atom derived from the silane oligomer and a metal atom derived from the metal alkoxide are bonded via an oxygen atom.
[0051] The silane oligomer modified with a metal alkoxide (hereinafter referred to as a "modified silane oligomer" depending on the situation) may be a reactant between a silane oligomer and a metal alkoxide, or a reactant between a silane monomer and a metal alkoxide. In the latter case, it may be a reactant formed by a silane monomer reacting with a metal alkoxide and further reacting with other silane monomers to form a silane oligomer structure, or it may be a reactant formed by a silane oligomer formed by a reaction between silane monomers and a metal alkoxide.
[0052] In addition, in the composition according to the present embodiment, it is not necessary that all of the silane oligomers contained in the composition be modified with a metal alkoxide, and it is sufficient that at least a part of the silane oligomers be modified with a metal alkoxide.
[0053] The silicon atoms contained in the silicon-oxygen oligomer can be divided into silicon atoms bonded to one oxygen atom (M unit), silicon atoms bonded to two oxygen atoms (D unit), silicon atoms bonded to three oxygen atoms (T unit) and silicon atoms bonded to four oxygen atoms (Q unit). The following formulas (M), (D), (T) and (Q) can be exemplified as the M unit, the D unit, the T unit and the Q unit, respectively.
[0054]
[0055] In the above formula, R represents an atom (such as a hydrogen atom) or an atomic group (such as an alkyl group) other than an oxygen atom bonded to silicon. Information on the content of these units can be obtained by Si-NMR.
[0056] In the silane oligomer, the ratio of the total number of T units and Q units to the total number of silicon atoms is preferably 50% or more, more preferably 70% or more, further preferably 90% or more, and may be 100%. According to such a silane oligomer, a barrier material with further excellent moisture resistance can be obtained.
[0057] As a preferred embodiment, the silane oligomer preferably contains T units. The content of T units in the silane oligomer relative to the total number of silicon atoms is, for example, 10% or more, preferably 20% or more, 30% or more, 40% or more, 50% or more, 70% or more, 80% or more, or 90% or more, and may be 100%. Such silane oligomers tend to have further improved flexibility and dehumidification properties.
[0058] As another embodiment, the silane oligomer may mainly contain Q units. In this case, the content of Q units in the silane oligomer relative to the total number of silicon atoms is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, further preferably 90% or more, and may be 100%. Such silane oligomers tend to have further improved moisture resistance and transparency.
[0059] The silane oligomer preferably has an alkyl group or an aryl group as R in the above formulas (M), (D), (T) and (Q).
[0060] The alkyl group is preferably an alkyl group having no more than 6 carbon atoms, and more preferably an alkyl group having no more than 4 carbon atoms. Specific examples of the alkyl group include methyl, ethyl, propyl, and butyl groups, among which methyl, ethoxy, and propyl groups are preferred, and methyl groups are more preferred.
[0061] Examples of the aryl group include phenyl and substituted phenyl. Examples of the substituent of the substituted phenyl include alkyl, vinyl, mercapto, amino, nitro, cyano, etc. Examples of the aryl group include phenyl.
[0062] The weight average molecular weight of the silane oligomer can be, for example, more than 400, preferably more than 600, more preferably more than 1000. And, the weight average molecular weight of the silane oligomer can be, for example, less than 30000, preferably less than 10000, more preferably less than 6000. If the weight average molecular weight of the silane oligomer is large, there is a tendency that flexibility and dehumidification are further improved, and if it is small, there is a tendency that moisture resistance and transparency are further improved. In addition, in this specification, the weight average molecular weight of the silane oligomer represents the value of the weight average molecular weight expressed in terms of polystyrene measured by gel permeation chromatography (GPC).
[0063] Metal alkoxides can be, for example, 1 ) n M represents a metal atom with a valence of n, R 1 represents an alkyl group. n represents a positive number of 1 or more.
[0064] n is preferably 2-5, more preferably 3-4.
[0065] M includes aluminum, titanium, zirconium, niobium, etc., among which aluminum, titanium, zirconium, and aluminum are preferred. That is, metal alkoxides include aluminum alkoxides, titanium alkoxides, zirconium alkoxides, and niobium alkoxides, among which aluminum alkoxides, titanium alkoxides, and zirconium alkoxides are preferred, and aluminum alkoxides are more preferred.
[0066] As R 1 , preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 2 to 4 carbon atoms. 1 Specific examples of the alkyl group include methyl, ethyl, propyl, and butyl. Among these, ethyl, propyl, and butyl are preferred, and propyl and butyl are more preferred.
[0067] The composition involved in this embodiment may include a modified silane oligomer formed by modifying a silane oligomer with 0.1 to 50 parts by mass of a metal alkoxide relative to 100 parts by mass of the silane oligomer. The amount of the metal alkoxide is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and preferably 30 parts by mass or less, more preferably 20 parts by mass or less relative to 100 parts by mass of the silane oligomer. If the amount of the metal alkoxide is large, there is a tendency for the curability to become better, and by reducing the amount of the metal alkoxide, there is a tendency for the transparency to be further improved.
[0068] The composition of the present embodiment may further include a silane monomer. By adding a silane monomer, for example, the content of the T unit and the Q unit in the barrier material can be adjusted, and the barrier material can be given effects such as transparency and flexibility according to the application. In addition, by adding a silane monomer, there is a tendency to obtain a barrier material with further excellent moisture resistance.
[0069] The content of silane monomer is not particularly limited, but relative to 100 parts by mass of silane oligomer, for example, it can be more than 10 parts by mass, preferably more than 20 parts by mass, and more preferably more than 30 parts by mass. Thus, the above effect is more significantly exerted. In addition, the content of silane monomer can be, for example, less than 100 parts by mass, or less than 60 parts by mass, preferably less than 50 parts by mass, and more preferably less than 40 parts by mass. By being set within such a range, there is a tendency that curability becomes better. In addition, in this specification, "100 parts by mass of silane oligomer" refers to the mass of the metal alkoxide that does not include the modified silane oligomer, and the total amount of the silane oligomer part of the modified silane oligomer and the unmodified silane oligomer is set to 100 parts by mass.
[0070] As the silane monomer, a trifunctional monomer containing a silicon atom bonded to three oxygen atoms and a tetrafunctional monomer containing a silicon atom bonded to four oxygen atoms can be preferably used.
[0071] Examples of the trifunctional monomer include alkyltrialkoxysilane, aryltrialkoxysilane, etc. Alkyltrialkoxysilane is a silane compound having one alkyl group and three alkoxy groups bonded to a silicon atom. Also, aryltrialkoxysilane is a silane compound having one aryl group and three alkoxy groups bonded to a silicon atom.
[0072] As the alkyl group of the alkyltrialkoxysilane, an alkyl group having 6 or less carbon atoms is preferred, and an alkyl group having 4 or less carbon atoms is more preferred. Specific examples of the alkyl group include methyl, ethyl, propyl, butyl, etc., among which methyl, ethyl, propyl, and methyl are preferred. Furthermore, as the alkoxy group of the alkyltrialkoxysilane, an alkoxy group having 6 or less carbon atoms is preferred, and an alkoxy group having 4 or less carbon atoms is more preferred. Specific examples of the alkoxy group include methoxy, ethoxy, propoxy, butoxy, etc., among which methoxy, ethoxy, propoxy are preferred, and methoxy and ethoxy are more preferred.
[0073] As the aryl group of the aryltrialkoxysilane, phenyl, substituted phenyl, etc. can be mentioned. As the substituent of the substituted phenyl, alkyl, vinyl, mercapto, amino, nitro, cyano, etc. can be mentioned. As the aryl group, phenyl is preferred. And, as the alkoxy group of the aryltrialkoxysilane, an alkoxy group having a carbon number of 6 or less is preferred, and an alkoxy group having a carbon number of 4 or less is more preferred. As specific examples of the alkoxy group, methoxy, ethoxy, propoxy, butoxy, etc. can be mentioned, among which methoxy, ethoxy, propoxy, and methoxy and ethoxy are preferred.
[0074] Specific examples of the trifunctional monomer include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, and ethyltriethoxysilane.
[0075] Examples of the tetrafunctional monomer include tetraalkoxysilane, etc. Tetraalkoxysilane is a silane compound in which four alkoxy groups are bonded to a silicon atom.
[0076] The alkoxy group of the tetraalkoxysilane is preferably an alkoxy group having no more than 6 carbon atoms, and more preferably an alkoxy group having no more than 4 carbon atoms. Specific examples of the alkoxy group include methoxy, ethoxy, propoxy, butoxy, etc. Among these, methoxy, ethoxy, propoxy are preferred, and methoxy and ethoxy are more preferred.
[0077] Specific examples of the tetrafunctional monomer include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane.
[0078] Furthermore, as the silane monomer, a silane monomer having a reactive functional group selected from the group consisting of a vinyl group, an epoxy group, a glycidyl group, a (meth)acryloyl group, an amino group, an isocyanate group, an isocyanurate group, and a mercapto group (hereinafter also referred to as a reactive silane monomer) can also be used. If the composition contains such a silane monomer, a barrier material having further excellent followability and adhesion to a substrate can be formed.
[0079] Although the reason why the reactive silane monomer exerts the above-mentioned effects is not necessarily clear, it is believed that when forming a barrier material, a cross-linked structure other than a siloxane bond can be formed by the reaction between reactive functional groups, the reaction between reactive functional groups and silanol groups, etc., thereby achieving excellent moisture resistance and flexibility. In addition, it is also believed that when forming a barrier material, the reactive functional groups of the reactive silane monomers are bonded to the functional groups present on the surface of the object, thereby achieving more excellent moisture resistance and flexibility.
[0080] The reactive functional group possessed by the reactive silane monomer is preferably selected from the group consisting of a vinyl group, an epoxy group (more preferably a glycidyl group), a (meth)acryloyl group, an amino group, an isocyanate group, an isocyanurate group and a mercapto group, and an amino group is more preferred, from the viewpoint of further improving the flexibility of the barrier material and the adhesion to the parts.
[0081] The reactive silane monomer preferably has a silicon atom bonded to three oxygen atoms.
[0082] As the reactive silane monomer, for example, a silane monomer represented by the following formula (A-1) can be preferably used.
[0083]
[0084] In the formula, R A1 Represents a reactive functional group, L 1 represents an alkanediyl or oxyalkanediyl group (-OL 2 - represented by the group, L 2 represents an alkanediyl group. ), p represents an integer greater than or equal to 0 (preferably an integer of 0 to 3), R A2 represents an alkyl group or an aryl group.
[0085] When R A1 In the case of a vinyl group, p is preferably 0 to 3, and more preferably 0.
[0086] When R A1 When it is an epoxy group, a glycidyl group, a (meth)acryloyl group, an amino group, an isocyanate group, an isocyanurate group or a mercapto group, p is preferably an integer of 1 or more, more preferably 1 to 3, and even more preferably 1.
[0087] When RA1 When L is vinyl, glycidyl or (meth)acryloyl, 1 Preferred is oxyalkanediyl.
[0088] When R A1 When L is an amino group, an isocyanate group, an isocyanurate group or a mercapto group, 1 Alkanediyl is preferred.
[0089] As L 1 and L 2 The alkanediyl group in the above-mentioned is preferably an alkanediyl group having 2 to 10 carbon atoms, and more preferably an alkanediyl group having 2 to 8 carbon atoms.
[0090] As R A2 The alkyl group in the above-mentioned group is preferably an alkyl group having no more than 6 carbon atoms, and more preferably an alkyl group having no more than 4 carbon atoms. Specific examples of the alkyl group include methyl, ethyl, propyl (n-propyl, isopropyl), butyl (n-butyl, sec-butyl, isobutyl, tert-butyl), and the like.
[0091] In R A2 The aryl group in the embodiment is preferably phenyl.
[0092] R A2 An alkyl group is preferred.
[0093] Relative to 100 parts by mass of silane oligomer, the content of reactive silane monomer can be, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more. Thus, there is a tendency that the followability and adhesion are further improved. In addition, the content of reactive silane monomer can be, for example, 5 parts by mass or less, preferably 4 parts by mass or less, more preferably 2 parts by mass or less. Thus, there is a tendency that the thermal stability of the cured product is further improved.
[0094] The composition according to the present embodiment may further contain a liquid medium. Examples of the liquid medium include water and organic solvents.
[0095] Examples of the organic solvent include alcohols, ethers, ketones, esters, hydrocarbons, etc. In addition to these, acetonitrile, acetamide, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, etc. can also be used.
[0096] The composition may contain water and alcohol as a liquid medium. By using such a liquid medium, a barrier material having excellent transparency can be easily obtained.
[0097] As the alcohol, an alcohol that can be vaporized by heating when forming the barrier material is preferred. As the alcohol, for example, an alcohol having 6 or less carbon atoms is preferred, and an alcohol having 1 to 4 carbon atoms is more preferred.
[0098] As alcohols, for example, alcohols corresponding to the alkoxy groups of metal alkoxides can be used. That is, for example, when the metal alkoxide has a tert-butoxy group, tert-butanol can be used as the alcohol. This tends to further improve transparency.
[0099] The content of the liquid medium is not particularly limited, and can be set to a content that provides a viscosity suitable for the coating composition. The viscosity of the composition is not particularly limited and can be appropriately adjusted according to the thickness of the barrier material to be produced, the coating method, the shape of the object, and the like.
[0100] The viscosity of the composition at 25° C. may be, for example, 1 to 6000 mPa·s, preferably 5 to 3000 mPa·s. Such a composition can be applied to an object more easily to form a barrier material on the object.
[0101] In the composition involved in this embodiment, the molar ratio (M / Si) of the metal atoms M derived from the metal alkoxide to the total number of silicon atoms derived from the silane oligomer and the silane monomer can be, for example, 0.0001 or more, preferably 0.001 or more. Thus, there is a tendency that the curability becomes better. In addition, the above-mentioned molar ratio (M / Si) can be, for example, 0.5 or less, preferably 0.2 or less. Thus, there is a tendency that the transparency is further improved.
[0102] The composition according to the present embodiment may further contain a curing catalyst. The curing catalyst is not particularly limited as long as it promotes the polymerization reaction of the silane oligomer and the silane monomer.
[0103] Examples of curing catalysts include acid catalysts such as hydrochloric acid, nitric acid, sulfuric acid, acetic acid, phosphoric acid, etc.; metal catalysts such as tin, titanium, aluminum, zinc, iron, cobalt, manganese, etc.; and base catalysts such as aliphatic amines, ammonium hydroxide, tetraethylammonium hydroxide, sodium carbonate, sodium hydroxide, etc.
[0104] For example, the content of the curing catalyst may be 0.1 parts by mass or more, preferably 1 part by mass or more, and may be 20 parts by mass or less, preferably 10 parts by mass or less, based on 100 parts by mass of the silane oligomer.
[0105] The composition involved in this embodiment may also contain other components other than those mentioned above. As other components, for example, resins, metal oxide particles, metal oxide fibers, etc. having hydroxyl groups in the molecular structure may be cited. As resins having hydroxyl groups in the molecular structure, for example, polyvinyl alcohol, etc. may be cited. In addition, as metal oxide particles, for example, silica particles, alumina particles, etc. may be cited, and these particles are preferably nano-sized (for example, particle diameters are 1 nm or more and less than 1000 nm) (that is, preferably nano-silica particles and nano-alumina particles). As metal oxide fibers, for example, alumina fibers, etc. may be cited, and the fiber diameters of these metal oxide fibers are preferably nano-sized (for example, fiber diameters are 1 nm or more and less than 1000 nm) (that is, preferably alumina nanofibers).
[0106] The content of the above-mentioned other components is not particularly limited as long as it is within the range that the above-mentioned effects can be obtained, and for example, it can be 50 parts by mass or less, preferably 40 parts by mass or less, relative to 100 parts by mass of the silane oligomer. In addition, the content of the above-mentioned other components can be, for example, 10 parts by mass or more, or 20 parts by mass or more, relative to 100 parts by mass of the silane oligomer.
[0107] As a method for producing the composition according to the present embodiment, the following method can be mentioned.
[0108] <Method 1 for producing composition>
[0109] The production method includes a modification step of modifying at least a portion of the silane oligomer with the metal alkoxide by reacting the silane oligomer with the metal alkoxide. In the modification step, the metal alkoxide reacts with the silane oligomer to form a metal atom-oxygen atom-silicon atom bond.
[0110] The above reaction can be carried out in a liquid medium. As the liquid medium, the same liquid medium as above can be exemplified. The amount of the liquid medium is not particularly limited, and can be, for example, an amount such that the concentration of the silane oligomer in the reaction solution becomes 50 to 99% by mass (preferably 80 to 95% by mass).
[0111] The reaction conditions of the above reaction are not particularly limited. For example, the reaction temperature of the above reaction may be 60 to 100° C., or 70 to 90° C. Also, the reaction time of the above reaction may be, for example, 0.5 to 5.0 hours, or 1.0 to 3.0 hours.
[0112] The present production method may further include a step of adding a silane oligomer to the reaction solution after the modification step. Thus, a composition containing a silane oligomer modified with a metal alkoxide and an unmodified silane oligomer can be obtained.
[0113] The present production method may further include a step of adding a silane monomer to the reaction solution after the modification step. That is, the present production method may be a method including a first step of preparing a silane oligomer at least partly modified with a metal alkoxide and a second step of mixing the modified silane oligomer and the silane monomer to obtain a composition for forming a barrier material, and the first step may be the above-mentioned modification step. Thus, a composition containing a silane monomer may be obtained.
[0114] The present production method may also include a step of adding other components to the reaction solution after the modification step. The present production method may also include a step of adding a liquid medium to the reaction solution after the modification step, or a step of replacing the liquid medium in the reaction solution after the modification step with another liquid medium. Through these steps, various modes of the above-mentioned composition can be prepared from the reaction solution after the modification step.
[0115] <Method 2 for producing composition>
[0116] The manufacturing method includes a modification step of reacting a silane monomer with a metal alkoxide to form a silane oligomer at least partly modified by the metal alkoxide. In the modification step, the silane oligomer is formed by polymerizing the silane monomer, and the formed silane oligomer may be modified by the metal alkoxide. In addition, in the modification step, after the silane monomer is modified by the metal alkoxide, the silane oligomer part may be formed by the reaction of the modified silane monomer with other silane monomers.
[0117] The above reaction can be carried out in a liquid medium. As the liquid medium, the same liquid medium as above can be exemplified. The amount of the liquid medium is not particularly limited, and can be, for example, an amount such that the concentration of the silane monomer in the reaction solution becomes 50 to 99% by mass (preferably 80 to 95% by mass).
[0118] The reaction conditions of the above reaction are not particularly limited. For example, the reaction temperature of the above reaction may be 60 to 100° C., or 70 to 90° C. Also, the reaction time of the above reaction may be, for example, 0.5 to 5.0 hours, or 1.0 to 3.0 hours.
[0119] The present production method may further include a step of adding a silane oligomer to the reaction solution after the modification step. Thus, a composition containing a silane oligomer modified with a metal alkoxide and an unmodified silane oligomer can be obtained.
[0120] The present production method may further include a step of adding a silane monomer to the reaction solution after the modification step. That is, the present production method may be a method including a first step of preparing a silane oligomer at least partly modified with a metal alkoxide and a second step of mixing the modified silane oligomer and the silane monomer to obtain a composition for forming a barrier material, and the first step may be the above-mentioned modification step. Thus, a composition containing a silane monomer may be obtained.
[0121] The present production method may also include a step of adding other components to the reaction solution after the modification step. The present production method may also include a step of adding a liquid medium to the reaction solution after the modification step, or a step of replacing the liquid medium in the reaction solution after the modification step with another liquid medium. Through these steps, various modes of the above-mentioned composition can be prepared from the reaction solution after the modification step.
[0122] <Method for producing barrier material>
[0123] The manufacturing method of the barrier material involved in this embodiment includes a heating step of heating the above-mentioned composition to form the barrier material. In this manufacturing method, the silane oligomer and the silane monomer in the composition are polymerized by heating to form a polysiloxane compound. At this time, in the above-mentioned composition, at least a part of the silane oligomer is modified by a metal alkoxide, so that the polysiloxane compound is doped with metal atoms derived from the metal alkoxide.
[0124] In the heating step, the liquid medium in the composition may be removed by heating. That is, the heating step may be a step of forming a barrier material including a polysiloxane compound by heating and drying the composition.
[0125] The heating temperature in the heating step is not particularly limited as long as it is a temperature at which the silane oligomer can be polymerized. Furthermore, when the composition contains a liquid medium, the heating temperature is preferably a temperature at which the liquid medium volatilizes. The heating temperature may be, for example, 70° C. or more, preferably 100° C. or more. Furthermore, the heating temperature may be, for example, 200° C. or less, preferably 170° C. or less.
[0126] The present production method may further include a coating step of coating the composition. In this case, the heating step may be said to be a step of heating the coated composition.
[0127] The method for applying the composition is not particularly limited and may be appropriately changed depending on the shape of the object to be applied, the thickness of the barrier material, and the like.
[0128] In the present production method, the composition may be applied to an object to be imparted with moisture resistance to form a barrier material on the object. In addition, in the present production method, after producing a barrier material in a predetermined shape, the produced barrier material may be applied to the object.
[0129] <Application of barrier materials>
[0130] The use of the barrier material according to the present embodiment is not particularly limited, and the barrier material can be preferably used in various applications requiring moisture resistance. For example, the barrier material can be preferably used as a moisture-proof barrier material for electronic devices.
[0131] The barrier material of this embodiment can fully suppress the damage caused by the expansion of water intruding into the interior under high temperature environment (for example, above 100°C). As a barrier material, it can be preferably used for applications such as moisture-proof barrier materials for electronic devices used in high temperature environments and moisture-proof barrier materials for electronic devices that undergo high temperature processes during installation. Specifically, it can be preferably used as moisture-proof barrier materials for power semiconductors, moisture-proof barrier materials for image sensors, and moisture-proof barrier materials for displays.
[0132] Hereinafter, a preferred embodiment of the use of the barrier material will be described in detail, but the use of the barrier material is not limited to the following.
[0133] <Application Example 1>
[0134] The use involved in one embodiment relates to a product having a component that has been treated to prevent moisture. This product includes a component (substrate) and a barrier material formed on the component. The barrier material can be formed on one component or on multiple components. The barrier material can be formed, for example, in a manner that covers one or more components.
[0135] Such a product is produced by a production method comprising the following steps: a first step of applying the barrier material forming composition on a component; and a second step of heating the applied composition to form a barrier material on the component.
[0136] Specific examples of such applications include the following electronic devices.
[0137] (Electronic Devices A-1)
[0138] An electronic device according to one embodiment includes a substrate, a cover glass, an image sensor disposed between the substrate and the cover glass, a support member that supports the cover glass and the image sensor on the substrate, and the barrier material provided at a junction between the cover glass and the support member.
[0139] The barrier material has excellent moisture resistance and can fully suppress damage caused by expansion of moisture intruding into the interior even when used in a high temperature environment. Therefore, the electronic device has excellent moisture resistance and can fully prevent damage to the cover glass, support member, etc. caused by expansion of moisture even when moisture intrudes into the gap between the cover glass and the substrate.
[0140] Such an electronic device can be manufactured, for example, by a manufacturing method comprising the following steps: a coating step of coating a barrier material forming composition on a junction between a support member and a cover glass; and a barrier material forming step of heating the coated composition to form a barrier material on the junction.
[0141] (Electronic Devices A-2)
[0142] An electronic device according to one aspect includes a substrate, an image sensor disposed on the substrate, and the barrier material provided on the image sensor.
[0143] The barrier material can be made into a barrier material with excellent moisture resistance and transparency. Therefore, the barrier material can also be preferably used as a sealing material for sealing an image sensor. This electronic device can form an image sensor package without using a cover glass, so it can be expected to reduce the size of the device, improve operability, etc.
[0144] In this application, the visible light transmittance (550 nm) of the barrier material per 1 mm thickness is preferably 95% or more, more preferably 97% or more, and even more preferably 99% or more.
[0145] Such an electronic device can be produced, for example, by a production method including the following steps: a coating step of coating a barrier material forming composition on an image sensor; and a barrier material forming step of heating the coated composition to form a barrier material on the image sensor.
[0146] <Application Example 2>
[0147] The use according to one embodiment relates to a product having a moisture-proof component. The product comprises a moisture-proof component having a barrier material and a substrate, and may be, for example, an assembly of a plurality of components including the moisture-proof component.
[0148] Such a product can be produced by a production method comprising the following steps: a first step of applying the barrier material-forming composition on a substrate and heating it to produce a moisture-proof member having a barrier material and a substrate; and a second step of assembling a plurality of members including the moisture-proof member.
[0149] Specific examples of such applications include the following electronic devices.
[0150] (Electronic Devices B-1)
[0151] An electronic device according to one aspect includes a substrate, at least one device selected from the group consisting of a MEMS sensor, a wireless module, and a camera module, and a moisture-proof member having a barrier material and a base material.
[0152] The barrier material has excellent moisture resistance and dehumidification properties. Therefore, the electronic device has excellent moisture resistance and can fully prevent the degradation of the sensing characteristics caused by moisture absorption.
[0153] Such an electronic device can be produced, for example, by a production method comprising the steps of: preparing a moisture-proof member having a barrier material and a substrate by applying a barrier material-forming composition on a substrate and heating the substrate; and assembling a plurality of members including the moisture-proof member.
[0154] As mentioned above, although the preferred embodiment of the present invention was described, the present invention is not limited to the above-mentioned embodiment.
[0155] Example
[0156] Hereinafter, the present invention will be described in further detail using examples, but the present invention is not limited to these examples.
[0157] (Example 1)
[0158] [Preparation of barrier material forming composition]
[0159] 3.8 parts by mass of aluminum sec-butylate (manufactured by Matsumoto Fine Chemical Co., Ltd., product name: AL-3001, hereinafter abbreviated as "AL-3001"), 7.6 parts by mass of tert-butyl alcohol (manufactured by Wako Pure Chemical Industries, Ltd.), 0.3 parts by mass of water, 0.3 parts by mass of acetic acid, and 64.9 parts by mass of silane oligomer (manufactured by Momentive Performance Materials Inc., product name: XC31-B2733) were mixed, and then reacted at 70°C for 1 hour. Then, 23.4 parts by mass of tetraethoxysilane (manufactured by FUJIFILM Wako Pure Chemical Corporation, hereinafter abbreviated as "TEOS") were mixed, and then reacted at 25°C for 2 hours. Then, 1.7 parts by mass of a curing catalyst (manufactured by Momentive Performance Materials Inc., product name: CR-15, hereinafter abbreviated as "CR-15") was mixed to obtain a barrier material-forming composition.
[0160] [Production of barrier materials]
[0161] Preparation of samples for water vapor transmission rate measurement
[0162] In the sample for measuring the water vapor permeability, an acetate film (manufactured by HOLBEIN ART MATERIALS INC., with a thickness of 0.08 mm) was used as the substrate. The acetate film was coated by immersing it in a barrier material forming composition. At this time, the barrier forming composition was coated only on one side of the acetate film. Regarding the drying of the barrier forming composition, the coated substrate was dried at 150°C for 4 hours. The thickness of the barrier material formed was set to 20μm. In addition, the water vapor permeability can also be obtained by preparing a plurality of samples of barrier materials with different thicknesses, and calculating the water vapor permeability in a thickness of 20μm based on an approximate straight line obtained by plotting the thickness on the horizontal axis and the water vapor permeability on the vertical axis.
[0163] Preparation of samples for moisture absorption measurement
[0164] In the sample for measuring the moisture absorption rate, a laminate (manufactured by Hitachi Chemical Co., Ltd.) was used as the substrate. The substrate had copper foil on both sides, so the copper foil was removed by etching only one side. The etched surface was coated with a composition for forming a barrier material using a rod coater. Then, a barrier material with a thickness of 20 μm was formed by drying at 150°C for 4 hours. In addition, the type of laminate used for the substrate is arbitrary. In addition, the moisture absorption rate can also be obtained by preparing multiple samples of barrier materials with different thicknesses, and calculating the moisture absorption rate in a thickness of 20 μm based on an approximate straight line obtained by plotting the thickness on the horizontal axis and the moisture absorption rate on the vertical axis.
[0165] [Evaluation method]
[0166] (Measurement of water vapor transmission rate)
[0167] The water vapor transmission rate was measured using a water vapor transmission rate meter (LASSY L80-5000 manufactured by Systec Instruments). The measurement conditions were a temperature of 40°C, a humidity of 90% RH, and a measurement area of 19.6 cm. 2 According to the measured water vapor transmission rate J of the whole sample t The water vapor transmission rate A of the barrier material alone is calculated by the following formula.
[0168] A=J t {[2a+b+(b 2 +4aJ t ) 0.5 ] / [2(a+bJ t )]}
[0169] When measuring the water vapor transmission rate A1, the sample composed of a barrier material and a substrate is measured with the substrate on the low humidity side and the barrier material on the high humidity side.
[0170] When measuring the water vapor transmission rate A2, the sample composed of a barrier material and a substrate is measured with the substrate on the high humidity side and the barrier material on the low humidity side.
[0171] (Moisture absorption rate after moisture absorption treatment)
[0172] The sample was subjected to moisture absorption by keeping it in a constant humidity thermostat at 85°C and 85%RH for 168 hours. Then, the sample weight was measured, and the moisture absorption rate was calculated by measuring the weight change rate from the weight before moisture absorption treatment as shown in the following formula.
[0173] [Formula 1]
[0174]
[0175] (Dehumidification rate after dehumidification treatment)
[0176] The dehumidification treatment is performed by keeping the sample subjected to the moisture absorption treatment in a thermostat maintained at 120°C for 1 hour. Then, the weight of the sample is measured, and the moisture absorption rate after the dehumidification treatment is calculated by measuring the rate of change from the weight before the moisture absorption treatment. Using this value, the dehumidification rate is calculated by the following formula. When the water absorbed by the moisture absorption treatment can be completely removed by the dehumidification treatment, the dehumidification rate becomes 100%.
[0177] [Formula 2]
[0178]
[0179] (Example 2)
[0180] A barrier material was formed and evaluated in the same manner as in Example 1 except that the silane oligomer of Example 1 was changed to TSR165 (manufactured by Momentive Performance Materials Inc.), tetraethoxysilane was changed to phenyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-103), and the curing catalyst was changed to aminopropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBE-903). The results are shown in Table 1.
[0181] (Comparative Example 1)
[0182] OPTOACE WP-140 was used as Comparative Example 1. The preparation of the sample for measuring the water vapor transmission rate and the sample for measuring the moisture absorption rate was carried out in the same manner as in Example 1 except for the drying conditions. The drying conditions were carried out by keeping at room temperature for 24 hours.
[0183] (Comparative Example 2)
[0184] Using only the substrate, the moisture absorption rate after the moisture absorption treatment and the moisture desorption rate after the moisture desorption treatment were determined in the same manner as in Example 1. The results are shown in Table 1.
[0185] [Table 1]
[0186]
[0187] Explanation of symbols
[0188] 10-barrier material, 20-substrate.
Claims
1. A barrier material, which is disposed on a substrate, wherein: The invention is composed of a cured product of a barrier material-forming composition applied on the substrate. The barrier material-forming composition comprises a silane oligomer at least partly modified with a metal alkoxide and a silane monomer. The silane oligomer has a silicon atom bonded to three oxygen atoms, The silane monomer is selected from the group consisting of alkyltrialkoxysilane, aryltrialkoxysilane and tetraalkoxysilane, The content of the silane monomer is 20 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the silane oligomer. The water vapor permeability A1 of the barrier material from the side opposite to the substrate to the substrate side is smaller than the water vapor permeability A2 of the barrier material from the substrate side to the side opposite to the substrate.
2. The barrier material according to claim 1, wherein: The ratio of the water vapor permeability A2 to the water vapor permeability A1, that is, A2 / A1, is 1.3 or more.
3. The barrier material according to claim 1 or 2, comprising a polysiloxane compound doped with metal atoms, The ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the polysiloxane compound is 30% or more.
4. The barrier material according to claim 3, wherein: 90% or more of the oxygen atoms in the polysiloxane compound are bonded to silicon atoms.
5. The barrier material according to claim 1 or 2, wherein: The ratio of the total number of silicon atoms bonded to three oxygen atoms and silicon atoms bonded to four oxygen atoms to the total number of silicon atoms in the silane oligomer is 50% or more.
6. A product having: substrate; and The barrier material according to claim 1 or 2 is disposed on the substrate.
Citation Information
Patent Citations
Gas barrier laminated film
CN101065240A
Water-vapor barrier film, process for producing same, and electronic appliance including same
CN103596757A
Steam barrier resin, steam barrier coating agent, steam barrier film, and steam barrier laminate
CN104080820A
Gas barrier film and method for producing same
CN106457765A
Barrier laminated film
JP2002046208A