A method for removing welding slag and particles inside small precision stainless steel welded parts

Through degreasing, pickling, multiple soaking, rinsing and ultrasonic cleaning, combined with high-pressure circulating water flow and high-temperature oven drying, the problem of removing welding slag and particles in small precision stainless steel welded parts is solved, and thorough cleaning in the hole is achieved and improved Quality of use of parts.

CN115889350BActive Publication Date: 2024-11-15ANHUI YINGYOU OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211552077.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-11-15
Estimated Expiration
2042-12-05

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove welding slag and particles inside small precision stainless steel welded parts, resulting in residual in the holes and affecting the quality of parts use.

Method used

Using degreasing, pickling, multiple soaking, rinsing, ultrasonic cleaning and high-temperature oven drying, combined with high-pressure circulating water flow and compressed dry air, we gradually remove welding slag and particles inside the welded parts to ensure thorough cleaning of the holes.

Benefits of technology

It significantly improves the cleaning effect in the welded holes, ensures the processing quality, fills the gap in the treatment of the welded holes in the prior art, and facilitates the subsequent application of the welded parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115889350B_ABST
    Figure CN115889350B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for removing welding slag and particles inside a small precision stainless steel welded part, comprising the following steps: Step 1: degreasing: soaking the precision welded part with a degreasing agent to obtain a degreased precision welded part; Step 2: soaking once: taking out the degreased precision welded part obtained in step 1, and putting it into a pure water tank for overflow soaking to obtain a precision welded part after soaking once, wherein the soaking time is more than 1 hour; Step 3: pickling: soaking the soaked precision welded part obtained in step 2 with hydrochloric acid to obtain a pickled precision welded part, wherein the mass ratio of hydrochloric acid to water is 10-20:80-90. The present invention is subjected to the processes of degreasing, pickling, multiple cleaning and drying of precision stainless steel welded parts, and has an obvious treatment effect on the hole of the welded part, and no particles of welding slag and debris will remain in the hole, thereby ensuring the treatment quality, filling the gap in the treatment of the hole of the welded part in the current production of precision parts, and facilitating the subsequent application of the welded part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cleaning treatment of precision welded parts, and in particular to a method for removing welding slag and particles inside a small precision stainless steel welded part. Background Art

[0002] After decades of development and innovation, the machining industry has evolved from the initial basic processing to precision and high-end development. The products involved have also moved from domestic to global, and the requirements for the products involved are getting higher and higher. When producing small precision products, welding slag and debris will be left inside the product during the welding and drilling process. The current conventional cleaning methods can only remove welding slag and debris on the surface, but have poor effect on removing welding slag and debris in the hole, resulting in residual particles in the hole, affecting the use of parts.

[0003] To this end, we propose a method for removing welding slag and particles inside small precision stainless steel welded parts to solve the above problems. Summary of the invention

[0004] The object of the present invention is to provide a method for removing welding slag and particles inside a small precision stainless steel welded part, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for removing welding slag and particles inside a small precision stainless steel welded part, comprising the following steps:

[0006] Step 1: Degreasing: Soak the precision welded parts in a degreasing agent to obtain degreased precision welded parts;

[0007] Step 2: Soaking once: After the degreased precision welded parts obtained in step 1 are fished out, they are placed in a pure water tank for overflow soaking to obtain precision welded parts after soaking once, wherein the soaking time is more than 1 hour;

[0008] Step 3: pickling: the soaked precision welded parts obtained in step 2 are soaked in hydrochloric acid to obtain pickled precision welded parts, wherein the mass ratio of hydrochloric acid to water is 10-20:80-90;

[0009] Step 4: secondary soaking: after the pickling precision welded parts obtained in step 3 are fished out, they are placed in a pure water tank and soaked for more than 1 hour to obtain secondary soaked precision welded parts;

[0010] Step 5: Rinse: Use a high-pressure water gun to rinse the precision welded parts after the second immersion. The rinsing time is 10 minutes to obtain the rinsed precision welded parts.

[0011] Step 6: Three-time soaking: Put the rinsed precision welded parts obtained in step 5 into a pure water tank and soak them for more than 1 hour to obtain three-time soaked precision welded parts;

[0012] Step 7: Blow dry once: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after three immersions to obtain precision welded parts after one blow drying;

[0013] Step 8 High-pressure flushing: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the drying in step 7, and flush the hole to obtain the precision welded part after high-pressure flushing. The flushing time is 10 minutes for each hole.

[0014] Step 9: First ultrasonic cleaning: put the precision welded parts after high pressure washing obtained in step 8 into the tank of ultrasonic cleaning machine for 20 minutes of vibration cleaning to obtain precision welded parts after first cleaning;

[0015] Step 12: Blow dry for the second time: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after the first cleaning obtained in step 9, and obtain the precision welded parts after the second drying;

[0016] Step 11: Water flow test: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the second drying obtained in step 10, filter after water flow, and use a magnifying glass to test the distribution of particles on the surface of the filter paper after the filter paper is dried. If there are too many particles, return to step 8-step 11 until the particles are reduced to the standard to obtain the final precision welded part;

[0017] Step 12: Blow-dry three times: Use compressed dry air to blow dry the moisture in the holes of the final precision welded part obtained in step 11 to obtain a precision welded part after three-blow drying;

[0018] Step 13: Secondary ultrasonic cleaning: In a clean room, place the three-dried precision welded parts obtained in step 12 into an ultrasonic cleaning machine tank for 30 minutes of vibration cleaning;

[0019] Step 14: Four-time drying: Use compressed dry air to dry the moisture in the holes of the three-time drying precision welded parts obtained in step 13, and obtain the four-time drying precision welded parts;

[0020] Step 15: Clean room drying: The precision welded parts after four times of drying obtained in step 14 are placed in a high temperature oven for drying, wherein the temperature in the oven is 150°C and the drying time is 2 hours, to obtain the final dried precision welded parts;

[0021] Step 16: Finished product packaging: The final dried precision welded parts obtained in step 15 are placed in a clean room to naturally cool to room temperature, and then vacuum packaged and labeled to obtain the final product.

[0022] Preferably, the degreasing agent in step one is a mixture of NaOH, TX-10 and H2O, wherein the mass ratio of NaOH, TX-10 and H2O is 10-20:1-5:75-89, and the soaking time in step one is 1 hour and the soaking temperature is 50-60°C.

[0023] Preferably, the water used in steps 1 to 16 is ultrapure water with a resistivity greater than 15 MΩ.CM.

[0024] Preferably, in step three, the soaking temperature is room temperature and the soaking time is 10 minutes.

[0025] Preferably, in step five, the pressure of the high-pressure water gun is 0.8 MPa, the power is 80 W, and the flow rate is 10 L / Min.

[0026] Preferably, in step eight, the pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min.

[0027] Preferably, in step nine, the output voltage of the ultrasonic cleaning machine is 220V and the output current is 6A.

[0028] Preferably, the pressure of the high-pressure circulating water flow equipment in step 11 is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min. The filtration method in step 11 is suction filtration. The maximum magnification of the magnifying glass in step 11 is 500 times. The filter paper specification in step 11 is 0.1 μm.

[0029] Preferably, the clean room in step 13 is a Class 100 clean room used in the semiconductor industry, and the output voltage and output current of the ultrasonic cleaning machine in step 13 are 220V and 6A respectively.

[0030] Preferably, in step 15, the power supply parameters of the high temperature oven are AC380V / 50HZ, the temperature control is 100-600°C, and the rated power is 21KW.

[0031] Preferably, in step sixteen, the vacuum packaging bag is made of PE and the packaging method is double-layer vacuum packaging.

[0032] Preferably, the compressed dry air in step seven, step ten, step twelve and step fourteen is compressed dry air filtered through a 0.05 μm filter.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention subjects precision stainless steel welded parts to processes such as degreasing, pickling, multiple cleanings and drying, and has an obvious treatment effect on the holes of welded parts. No welding slag and debris particles will remain in the holes, thus ensuring the treatment quality. This fills the gap in the treatment of welded part holes in the current production of precision parts and is beneficial to the subsequent application of welded parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a flow chart of the steps of the present invention; DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Embodiment 1:

[0038] See also Figure 1 The present invention provides a technical solution: a method for removing welding slag and particles inside a small precision stainless steel welded part, comprising the following steps:

[0039] Step 1: Degreasing: Soak the precision welded parts in a degreasing agent to obtain degreased precision welded parts;

[0040] Step 2: Soak once: After the degreased precision welded parts obtained in step 1 are fished out, they are placed in a pure water tank for overflow soaking to obtain precision welded parts after one soaking, wherein the soaking time is more than 1 hour, and the overflow soaking is to remove the residual degreasing agent more completely;

[0041] Step 3: pickling: the soaked precision welded parts obtained in step 2 are soaked in hydrochloric acid to obtain pickled precision welded parts, wherein the mass ratio of hydrochloric acid to water is 10-20:80-90;

[0042] Step 4: Secondary soaking: After the pickling precision welded parts obtained in step 3 are fished out, they are placed in a pure water tank and soaked for more than 1 hour to obtain the precision welded parts after secondary soaking. The purpose of the overflow soaking is to remove the residual acid more completely.

[0043] Step 5: Rinse: Use a high-pressure water gun to rinse the precision welded parts after the second immersion. The rinsing time is 10 minutes to obtain the rinsed precision welded parts.

[0044] Step 6: Three-time soaking: Put the rinsed precision welded parts obtained in step 5 into a pure water tank and soak them for more than 1 hour to obtain three-time soaked precision welded parts;

[0045] Step 7: Blow dry once: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after three immersions to obtain precision welded parts after one blow drying;

[0046] Step 8 High-pressure flushing: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the drying in step 7, and flush the hole to obtain the precision welded part after high-pressure flushing. The flushing time is 10 minutes for each hole.

[0047] Step 9: First ultrasonic cleaning: put the precision welded parts after high pressure washing obtained in step 8 into the tank of ultrasonic cleaning machine for 20 minutes of vibration cleaning to obtain precision welded parts after first cleaning;

[0048] Step 12: Blow dry for the second time: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after the first cleaning obtained in step 9, and obtain the precision welded parts after the second drying;

[0049] Step 11: Water flow test: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the second drying obtained in step 10, filter after water flow, and use a magnifying glass to test the distribution of particles on the surface of the filter paper after the filter paper is dried. If there are too many particles, return to step 8-step 11 until the particles are reduced to the standard to obtain the final precision welded part;

[0050] Step 12: Blow-dry three times: Use compressed dry air to blow dry the moisture in the holes of the final precision welded part obtained in step 11 to obtain a precision welded part after three-blow drying;

[0051] Step 13: Secondary ultrasonic cleaning: In a clean room, place the three-dried precision welded parts obtained in step 12 into an ultrasonic cleaning machine tank for 30 minutes of vibration cleaning;

[0052] Step 14: Four-time drying: Use compressed dry air to dry the moisture in the holes of the three-time drying precision welded parts obtained in step 13, and obtain the four-time drying precision welded parts;

[0053] Step 15: Clean room drying: The precision welded parts after four times of drying obtained in step 14 are placed in a high temperature oven for drying, wherein the temperature in the oven is 150°C and the drying time is 2 hours, to obtain the final dried precision welded parts;

[0054] Step 16: Finished product packaging: The final dried precision welded parts obtained in step 15 are placed in a clean room to naturally cool to room temperature, and then vacuum packaged and labeled to obtain the final product.

[0055] Embodiment 2:

[0056] See also Figure 1, which is the second embodiment of the present invention, is based on the previous embodiment. In step one, the degreasing agent is a mixture of NaOH, TX-10 and H2O, wherein the mass ratio of NaOH, TX-10 and H2O is 10-20:1-5:75-89, and the soaking time in step one is 1 hour and the soaking temperature is 50-60°C.

[0057] The water used in step 1 to step 16 is ultrapure water with a resistivity of >15 MΩ.CM.

[0058] In step 3, the soaking temperature is room temperature and the soaking time is 10 minutes.

[0059] In step 5, the pressure of the high-pressure water gun is 0.8 MPa, the power is 80 W, and the flow rate is 10 L / Min.

[0060] In step eight, the pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min.

[0061] In step nine, the output voltage of the ultrasonic cleaning machine is 220V and the output current is 6A.

[0062] In step 11, the pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min. The filtration method in step 11 is suction filtration. The maximum magnification of the magnifying glass in step 11 is 500 times. The filter paper specification in step 11 is 0.1 μm.

[0063] The clean room in step 13 is a Class 100 clean room used in the semiconductor industry. The output voltage of the ultrasonic cleaning machine in step 13 is 220V and the output current is 6A.

[0064] In step 15, the power parameters of the high temperature oven are AC380V / 50HZ, the temperature control is 100-600℃, and the rated power is 21KW.

[0065] In step 16, the vacuum packaging bag is made of PE and the packaging method is double-layer vacuum packaging.

[0066] The compressed dry air in step 7, step 10, step 12 and step 14 is compressed dry air filtered through a 0.05 μm filter to prevent particles in the air from entering the hole, and the air gun nozzle is made of soft plastic to prevent scratches on precision welded parts.

[0067] Embodiment 3:

[0068] See also Figure 1, which is the third embodiment of the present invention. This embodiment is based on the above two embodiments and provides a specific application of a method for removing welding slag and particles inside a small precision stainless steel welded part. Step 1: degreasing: NaOH, TX-10 and H2O are mixed to prepare a degreasing agent, wherein NaOH:TX-10:H2O is 10:5:85, NaOH is a commercially available industrial grade 99% flake caustic soda, TX-10 is a commercially available industrial grade 99% product, and water is ultrapure water with a resistivity of >15MΩ.CM. The precision welded part is soaked in the degreasing agent to obtain a degreased precision welded part;

[0069] Step 2: Soaking once: After the degreased precision welded parts obtained in step 1 are fished out, they are placed in a pure water tank for overflow soaking to obtain precision welded parts after soaking once, wherein the soaking time is more than 1 hour;

[0070] Step 3: Pickling: The soaked precision welded parts obtained in step 2 are soaked in hydrochloric acid to obtain pickled precision welded parts, wherein the mass ratio of hydrochloric acid to water is 10:90;

[0071] Step 4: secondary soaking: after the pickling precision welded parts obtained in step 3 are fished out, they are placed in a pure water tank and soaked for more than 1 hour to obtain secondary soaked precision welded parts;

[0072] Step 5: Rinse: Use a high-pressure water gun to rinse the precision welded parts after the second immersion. The rinsing time is 10 minutes to obtain the rinsed precision welded parts. The pressure of the high-pressure water gun is 0.8 MPa, the power is 80 W, the flow rate is 10 L / Min, and the water used is room temperature ultrapure water with a resistivity of >15 MΩ.CM;

[0073] Step 6: Three-time soaking: Put the rinsed precision welded parts obtained in step 5 into a pure water tank and soak them for more than 1 hour to obtain three-time soaked precision welded parts;

[0074] Step 7: Blow dry once: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after three immersions to obtain the precision welded parts after one blow drying, wherein the compressed dry air is compressed dry air filtered through a 0.05 μm filter;

[0075] Step 8: High-pressure flushing: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the drying step 7, and flush the hole to obtain the precision welded part after high-pressure flushing. The flushing time is 10 minutes for each hole. The pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min.

[0076] Step 9: First ultrasonic cleaning: put the precision welded parts after high pressure washing obtained in step 8 into the tank of ultrasonic cleaning machine for 20 minutes of vibration cleaning to obtain the precision welded parts after first cleaning. The cleaning temperature is room temperature, the output voltage of the ultrasonic cleaning machine is 220V, and the output current is 6A.

[0077] Step 12: Blow dry for the second time: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after the first cleaning obtained in step 9, and obtain the precision welded parts after the second drying, wherein the compressed air is filtered through a 0.05μm filter;

[0078] Step 11: Water flow test: connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the secondary drying obtained in step 10, filter after water flow, and test the distribution of particles on the surface of the filter paper with a magnifying glass after the filter paper is dried. If there are too many particles, return to step 8-step 11 until the particles are reduced to the standard to obtain the final precision welded part. The pressure of the high-pressure circulating water flow equipment is 16mpa, the power is 1200W, the circulating water flow rate is 120L / Min, the filtering method is suction filtration, the maximum magnification of the magnifying glass used is 500 times, and the filter paper used is 0.1μm grade;

[0079] Step 12: Blow dry three times: Use compressed dry air to blow dry the moisture in the holes of the final precision welded part obtained in step 11 to obtain the precision welded part after three-blow drying, wherein the compressed dry air is compressed dry air filtered through a 0.05 μm filter;

[0080] Step 13: Secondary ultrasonic cleaning: In a clean room, the three-times-dried precision welded parts obtained in step 12 are placed in an ultrasonic cleaning machine tank for oscillation cleaning for 30 minutes. The clean room is a Class 100 clean room used in the semiconductor industry. The output voltage of the ultrasonic cleaning machine is 220V and the output current is 6A.

[0081] Step 14: Four-time drying: Use compressed dry air to dry the moisture in the holes of the three-time drying precision welded parts obtained in step 13, and obtain the four-time drying precision welded parts;

[0082] Step 15: Clean room drying: The precision welded parts after four times of drying obtained in step 14 are placed in a high temperature oven for drying, wherein the temperature in the oven is 150°C and the drying time is 2 hours, to obtain the final dried precision welded parts, wherein the compressed dry air is compressed dry air filtered through a 0.05 μm filter;

[0083] Step 16: Finished product packaging: Place the final dried precision welded parts obtained in step 15 in a clean room to naturally cool to room temperature, use double-layer vacuum packaging and affix a label to obtain the final product, and the packaging bag is made of PE.

[0084] Embodiment 4:

[0085] The present invention subjects precision stainless steel welded parts to processes such as degreasing, pickling, multiple cleanings and drying, and has an obvious treatment effect on the holes of welded parts. No welding slag and debris particles will remain in the holes, thus ensuring the treatment quality. This fills the gap in the treatment of welded part holes in the current production of precision parts and is beneficial to the subsequent application of welded parts.

[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for removing welding slag and particles inside small precision stainless steel welded parts, characterized in that The following steps are involved: Step 1: Degreasing: soaking the precision welded parts with a degreasing agent to obtain a degreased precision welded parts. The degreasing agent in step 1 is a mixture of NaOH, TX-10 and H2O, wherein the mass ratio of NaOH, TX-10 and H2O is 10-20:1-5:75-89. The soaking time in step 1 is 1 hour and the soaking temperature is 50-60°C. Step 2: Soaking once: After the degreased precision welded parts obtained in step 1 are fished out, they are placed in a pure water tank for overflow soaking to obtain precision welded parts after soaking once, wherein the soaking time is more than 1 hour; Step 3: pickling: the soaked precision welded parts obtained in step 2 are soaked in hydrochloric acid to obtain pickled precision welded parts, wherein the mass ratio of hydrochloric acid to water is 10-20:80-90; Step 4: secondary soaking: after the pickling precision welded parts obtained in step 3 are fished out, they are placed in a pure water tank and soaked for more than 1 hour to obtain secondary soaked precision welded parts; Step 5: Rinse: Use a high-pressure water gun to rinse the precision welded parts after the second immersion. The rinsing time is 10 minutes to obtain the rinsed precision welded parts. Step 6: Three-time soaking: Put the rinsed precision welded parts obtained in step 5 into a pure water tank and soak them for more than 1 hour to obtain three-time soaked precision welded parts; Step 7: Blow dry once: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after three immersions to obtain precision welded parts after one blow drying; Step 8 High-pressure flushing: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the drying in step 7, and flush the hole to obtain the precision welded part after high-pressure flushing. The flushing time is 10 minutes for each hole. Step 9: First ultrasonic cleaning: put the precision welded parts after high pressure washing obtained in step 8 into the tank of ultrasonic cleaning machine for 20 minutes of vibration cleaning to obtain precision welded parts after first cleaning; Step 12: Blow dry for the second time: Use compressed dry air to blow dry the moisture in the holes of the precision welded parts after the first cleaning obtained in step 9, and obtain the precision welded parts after the second drying; Step 11: Water flow test: Connect the high-pressure circulating water flow equipment to the hole of the precision welded part after the second drying obtained in step 10, filter after water flow, and test the distribution of particles on the filter paper surface with a magnifying glass after the filter paper is dried. If there are too many particles, return to step 8-step 11 until the particles are reduced to the standard to obtain the final precision welded part; Step 12: Blow-dry three times: Use compressed dry air to blow dry the moisture in the holes of the final precision welded part obtained in step 11 to obtain a precision welded part after three-blow drying; Step 13: Secondary ultrasonic cleaning: In a clean room, place the three-dried precision welded parts obtained in step 12 into an ultrasonic cleaning machine tank for 30 minutes of vibration cleaning; Step 14: Four-time drying: Use compressed dry air to dry the moisture in the holes of the three-time drying precision welded parts obtained in step 13, and obtain the four-time drying precision welded parts; Step 15: Clean room drying: The precision welded parts after four times of drying obtained in step 14 are placed in a high temperature oven for drying, wherein the temperature in the oven is 150°C and the drying time is 2 hours, to obtain the final dried precision welded parts; Step 16: Finished product packaging: The final dried precision welded parts obtained in step 15 are placed in a clean room to naturally cool to room temperature, and then vacuum packaged and labeled to obtain the final product.

2. A method for removing welding slag and particles inside small precision stainless steel welded parts according to claim 1, characterized in that: In step 3, the soaking temperature is room temperature and the soaking time is 10 minutes.

3. A method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: In step 5, the pressure of the high-pressure water gun is 0.8 MPa, the power is 80 W, and the flow rate is 10 L / Min.

4. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: In step eight, the pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min.

5. The method for removing welding slag and particles inside small precision stainless steel welded parts according to claim 1, characterized in that: In step nine, the output voltage of the ultrasonic cleaning machine is 220V and the output current is 6A.

6. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: In the step 11, the pressure of the high-pressure circulating water flow equipment is 16 MPa, the power is 1200 W, and the circulating water flow rate is 120 L / Min. The filtering method in the step 11 is suction filtration. The maximum magnification of the magnifying glass in the step 11 is 500 times. The filter paper specification in the step 11 is 0.1 μm.

7. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: The clean room in step 13 is a Class 100 clean room used in the semiconductor industry, and the output voltage and output current of the ultrasonic cleaning machine in step 13 are 220V and 6A, respectively.

8. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: In the step 15, the power supply parameters of the high temperature oven are AC380V / 50HZ, the temperature control is 100-600°C, and the rated power is 21KW.

9. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: In the step 16, the vacuum packaging bag is made of PE and the packaging method is double-layer vacuum packaging.

10. The method for removing welding slag and particles inside a small precision stainless steel welded part according to claim 1, characterized in that: The compressed dry air in step seven, step ten, step twelve and step fourteen is compressed dry air filtered through a 0.05 μm filter.