Light-colored thermal insulation fiber and preparation method thereof

By using heat-storing and thermal insulation masterbatches and fiber-forming polymers in light-colored warm fibers, the existing fiber insulation performance is solved and the problem of insufficient color darkness is achieved. The color is warm and lightweight, suitable for a variety of clothing needs.

CN116043354BActive Publication Date: 2024-11-12POLY PLASTIC MASTERBATCH SUZHOU +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211338278.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-11-12
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The existing heating fibers have limited insulation properties and dark colors, which cannot meet the diverse needs of light-colored clothing, and traditional light-absorbing heating fibers do not conform to the concept of lightweight life.

Method used

Light-colored warm fibers composed of thermal insulation masterbatches and fiber-forming polymers are used to add light-absorbing and heating nanoceramic materials, organic near-infrared absorbers and germanium powder to the thermal insulation masterbatches, combined with an optimized preparation process, to form The fibers in the hollow structure improve infrared absorption and reflection capabilities, enhance warmth and improve fiber color.

Benefits of technology

The preparation of light-colored warm fibers is realized, the problem of dark color of traditional fibers is solved, and the warmth effect and the uniformity, softness and lightness of the fibers are improved. It is suitable for self-heating and warm products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003915367440000101
    Figure BDA0003915367440000101
Patent Text Reader

Abstract

The present application relates to a light-colored thermal insulation fiber, which is made of a light-absorbing and heat-generating masterbatch and a fiber-forming polymer. The light-absorbing and heat-generating masterbatch comprises the following raw materials in parts by weight: 70-90 parts of a masterbatch polymer, 0.2-20 parts of a light-absorbing and heat-generating nano-ceramic material, 1-10 parts of an organic near-infrared absorber, 2-10 parts of a dispersant, and 0.1-5 parts of germanium powder. The preparation method thereof comprises a melt extrusion process, a mixing process, a metering process, a filtering and spinning process, a cooling and molding process, and an oiling and winding process. By adjusting the composition, content, and process of the raw materials, the problem of the dark color of the traditional light-absorbing and heat-generating fiber is solved, the influence of the fiber color on the color of the fabric is avoided, the thermal insulation effect and flexibility of the fiber are further improved, and the fiber is endowed with far-infrared and negative ion functions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of fiber technology, D01F6 / 92, and specifically to a light-colored thermal insulation fiber and a preparation method thereof. Background Art

[0002] It is found through analysis that the source of human body heat is based on the heat formed by the body's own metabolism process on the one hand, and there are various heat radiations around the environment where the human body is located on the other hand. The most widespread is sunlight radiation, among which the energy of visible light (400-760nm) and near infrared light (760-2500nm) accounts for more than 80% of the total energy of sunlight radiation. The heat loss of the human body is mainly achieved through thermal radiation, thermal convection, thermal conduction and evaporative heat dissipation, among which most of the heat is lost through thermal radiation. For the human body that is active outdoors in cold conditions, how to make full use of the energy of outdoor sunlight radiation and reduce the heat dissipation of the human body is the key to achieving warmth preservation. The heat-generating fibers currently developed are mainly based on far-infrared fibers, but the thermal insulation performance of such fiber fabrics is limited, and the existing heat-generating fibers are all dark in color, which has a great influence on the color of the finished products made of the fibers, and cannot meet people's diverse needs for clothing.

[0003] Patent application document CN114763629A discloses a fabric with heating function and its preparation method. The raw materials of the thermal insulation fiber include PET, nanomaterials and rare earth materials. The fabric has good heating performance, but the use of nano bamboo charcoal and rare earth materials makes the fabric darker, which limits its application in light-colored clothing. Patent application document CN109881295A discloses a light-absorbing and heating functional fiber: it consists of a light-absorbing layer, a heating layer and a heat storage layer. By utilizing the synergistic effect of the three layers, the obtained fiber fabric not only has a strong light-absorbing and heating function, but also has a good thermal insulation effect, but it does not conform to the light life concept of contemporary people. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a light-colored thermal insulation fiber and a preparation method thereof.

[0005] Firstly, the present application provides a light-colored thermal insulation fiber, which is made of heat-storage thermal insulation masterbatch and fiber-forming polymer.

[0006] Furthermore, based on the total weight of the heat storage and thermal insulation masterbatch and the fiber-forming polymer, the fiber comprises 5-20wt% of the heat storage and thermal insulation masterbatch and 80-95wt% of the fiber-forming polymer.

[0007] The fiber-forming polymer is selected from one or more combinations of PLA, polyester, and polyamide, including but not limited to PA66, PA6, PET, PBT, and the like.

[0008] Furthermore, the heat storage and heat preservation masterbatch comprises the following raw materials in parts by weight: 70-90 parts of masterbatch polymer, 0.2-20 parts of light-absorbing and heat-generating nano-ceramic material, 1-10 parts of organic near-infrared absorber, 2-10 parts of dispersant, and 0.1-5 parts of germanium powder.

[0009] Furthermore, the heat storage and heat preservation masterbatch comprises the following raw materials in percentage by weight: 70-90 parts of masterbatch polymer, 5-10 parts of light-absorbing and heat-generating nano-ceramic material, 2-5 parts of organic near-infrared absorber, 1-5 parts of dispersant, and 0.5-0.8 parts of germanium powder.

[0010] Furthermore, the masterbatch polymer is selected from at least one of polyamide, polypropylene, polyethylene, polyethylene terephthalate, and polybutylene terephthalate.

[0011] Furthermore, the light-absorbing and heat-generating nano-ceramic material is selected from one or more of tungsten oxide, tin oxide, and titanium nitride.

[0012] Furthermore, the organic near-infrared absorber is selected from one or more of IRG-022, OPTION, and Omnistab NIR.

[0013] Light-absorbing and heat-generating nano-ceramic materials have a strong ability to absorb infrared light and have a very good heat generation and heat storage effect, but they are dark in color. Excessive addition will cause the color of the produced fibers to be darker, which is not conducive to obtaining colorful products through dyeing. Organic near-infrared absorbers not only have high near-infrared absorption, but can also compensate for the infrared absorption capacity of light-absorbing and heat-generating nano-ceramic materials at 760-900nm and improve infrared utilization. At the same time, organic near-infrared absorbers can help improve the color of the fibers and facilitate dyeing.

[0014] Furthermore, the average particle diameter of the light-absorbing and heat-generating nano-ceramic material is 5 nm-1 μm.

[0015] Furthermore, the average particle diameter of the light-absorbing and heat-generating nano-ceramic material is 10nm-500nm. When the particle size of the light-absorbing and heat-generating nano-ceramic material is too large, the structure of the masterbatch polymer cannot stabilize it well inside, and when the particle size is too small, the light-absorbing and heat-generating nano-ceramic material overlaps more inside and cannot effectively contact infrared light to absorb it, resulting in a waste of some materials.

[0016] Furthermore, the light-absorbing and heat-generating nano-ceramic material is tungsten oxide.

[0017] Furthermore, the tungsten oxide is cesium, silver or tantalum doped tungsten oxide.

[0018] Furthermore, in the cesium, silver or tantalum doped tungsten oxide, cesium, silver or tantalum accounts for 2.5-3% of the total mass of the cesium, silver or tantalum doped tungsten oxide.

[0019] Doping tungsten oxide with other elements will form defects on the surface of tungsten oxide and improve its light absorption capacity. However, if the doping amount of other elements is too high, the color of the light-absorbing and heat-generating nano-ceramic material will deepen, which is not conducive to the preparation of light-colored fibers. Therefore, it is necessary to select an appropriate doping amount to improve the light-absorbing and heat-generating capacity without affecting the fiber color too much.

[0020] Furthermore, the tungsten oxide is cesium-doped tungsten oxide. Since the radius of cesium atoms is large, cesium-doped tungsten oxide has a stronger ability to absorb light.

[0021] Furthermore, the dispersant is one or more of a silane coupling agent, an aluminate coupling agent, and a titanate coupling agent.

[0022] Furthermore, the silane coupling agent is one or more of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, aminoethylaminopropyltrimethoxysilane, anilinomethyltrimethoxysilane, and anilinomethyltriethoxysilane.

[0023] Furthermore, the average particle diameter of germanium powder is 200-800nm; germanium powder has the functions of infrared transmittance enhancement and far-infrared emission, which can reduce infrared emission on the fiber surface and enhance the infrared absorption capacity of light-absorbing and heat-generating nano-ceramic materials to enhance the warming effect of the prepared fiber; in addition, germanium metal powder is used to reflect visible light and ultraviolet light to achieve the purpose of improving the brightness of the fiber, further solving the problem of dark color of traditional light-absorbing and heat-generating fibers. At the same time, germanium metal powder can also give the fiber the functions of far-infrared emission and negative ions, producing certain health care effects.

[0024] Furthermore, the cross section of the fiber is a hollow structure, and the cross section shape of the hollow part is one of a single-hole circle, a single-hole triangle, a four-hole circle or a seven-hole circle.

[0025] Furthermore, the cross-sectional shape of the hollow portion of the fiber is a four-hole circle or a seven-hole circle.

[0026] Secondly, the present invention provides a method for preparing a light-colored thermal insulation fiber, comprising the following steps:

[0027] (1) mixing a heat storage and heat preservation masterbatch and a fiber-forming polymer in proportion to obtain a mixture;

[0028] (2) The mixture is sequentially subjected to a melt extrusion process, a mixing process, a metering process, a filtering and spinning process, a cooling and molding process, and an oiling and winding process to obtain a light-colored thermal insulation fiber.

[0029] Furthermore, in the melt extrusion process, the temperatures of the screw and the box are 250-300°C, the melt temperature is 250-300°C, the intrinsic viscosity is 0.5-1.0, and the screw extrusion pressure is 5-10MP.

[0030] Furthermore, a static mixer is used in the mixing process to mix and knead the materials to reduce the stratified flow caused by the high viscosity in the melt; the side wall distance of the static mixer is 1.5-3.5mm, the water hole diameter is 5-10mm, the space angle is 50-90°, and the device spacing is 10-18mm.

[0031] Furthermore, in the metering process, in order to ensure uniform fineness of the filaments, a pump is used for sample feeding, the pump speed is 15-40r / min, the weight of the melt transmitted by the pump per unit time is 150-400g / min, the fineness of the finished filaments is 8-9, the stretching multiple is 0.40-0.50mm, the fiber shrinkage coefficient is 1.05-1.15, and the metering pump efficiency is 98%.

[0032] Furthermore, in the filtering and spinning process, the spinning speed is 1500-5000 m / min, and the pressure of the components (spinneret, melt distribution melt filtration material and its assembly kit) is 10-25 MPa.

[0033] Furthermore, in the cooling and forming process, the temperature of the cooling air is 20-30°C, the humidity of the cooling air is 50-80%, the wind speed increases with the increase of the fiber, and the range is 0.2-0.6 m / min, the main air duct pressure is 1000-1400 Pa, and the wind speed distribution is one of linear, arc and S-shaped. Preferably, the wind speed type is S-shaped.

[0034] Furthermore, in the oiling and winding process, the winding speed is 1200-4000 m / min, and the oil tanker rotation speed is 0.3-0.8 rpm.

[0035] Furthermore, the light-colored thermal insulation fiber of the present application can be used in the manufacture of self-heating and thermal insulation products.

[0036] Beneficial effects:

[0037] 1. The light-colored thermal insulation fiber of the present application utilizes masterbatch polymer, light-absorbing and heat-generating nano-ceramic material, organic near-infrared absorber, dispersant and germanium powder to prepare heat-storage and thermal insulation masterbatch, which not only solves the problem of dark color of traditional light-absorbing and heat-generating fibers, avoids the influence of fiber color on fabric color, but also further improves the thermal insulation effect of the fiber.

[0038] 2. The heat storage and thermal insulation masterbatch used in this application is added with light-absorbing heat-generating nano-ceramic material and organic near-infrared absorber. The light-absorbing heat-generating nano-ceramic material has a strong absorption capacity for infrared light and a very good heat generation and heat storage effect, but its color is darker. Excessive addition will cause the color of the produced fiber to be darker, which is not conducive to obtaining colorful products through dyeing. The organic near-infrared absorber not only has high near-infrared absorption, but can also compensate for the infrared absorption capacity of the light-absorbing heat-generating nano-ceramic material at 760-900nm and improve infrared utilization. At the same time, the organic near-infrared absorber helps to improve the color of the fiber and facilitates dyeing.

[0039] 3. The light-absorbing and heat-generating nano-ceramic material in the present application is preferably tungsten oxide doped with cesium, silver or tantalum. Doping with other elements will form defects on the surface of tungsten oxide, which can improve the light absorption capacity of the ceramic material and is conducive to obtaining fibers with better light-absorbing and heat-generating effects.

[0040] 4. Germanium powder is also added to the heat storage and thermal insulation masterbatch used in this application. Germanium powder has the functions of infrared transmittance enhancement and far-infrared emission, which can reduce infrared emission on the fiber surface and enhance the infrared absorption capacity of the light-absorbing and heat-generating nano-ceramic material to enhance the warming effect of the prepared fiber; in addition, germanium metal powder is used to reflect visible light and ultraviolet light to achieve the purpose of improving the brightness of the fiber, further solving the problem of dark color of traditional light-absorbing and heat-generating fibers. At the same time, germanium metal powder can also give the fiber the functions of far-infrared emission and negative ions, producing certain health care effects.

[0041] 5. The present application optimizes the fiber preparation process so that the fiber of the present application has excellent uniformity, softness, fluffiness and lightness, further enhancing and ensuring the flexibility, warmth retention and stability of the fiber. DETAILED DESCRIPTION

[0042] Unless otherwise specified, the substances used in the examples and comparative examples of the present application are common commercially available chemicals.

[0043] Example 1

[0044] Raw materials: 70 parts of masterbatch polymer (PET), 10 parts of light-absorbing and heat-generating nano-ceramic material (silver-doped tungsten oxide, in which silver accounts for 2.8% of the total mass of the silver-doped tungsten oxide), 2 parts of near-infrared absorber (IRG-022), 5 parts of dispersant (APTES), and 0.5 parts of germanium powder (average particle size is 800nm).

[0045] Preparation of heat storage and thermal insulation masterbatch: light-absorbing and heat-generating nano-ceramic material, near-infrared absorber, dispersant, germanium powder and masterbatch polymer are blended and extruded to prepare masterbatch.

[0046] The preparation method of the masterbatch is as follows:

[0047] (1) putting the above raw materials into a high-speed mixer, heating and stirring until the mixed powder is dry;

[0048] (2) Putting the mixed material into a twin-screw extruder for extrusion granulation: After being fully plasticized in the twin-screw, the mixed material is evenly dispersed by shearing through the dispersing element in the twin-screw, extruded through a circular orifice die, cooled in a water tank, and pulled to a pelletizer to be cut into cylindrical pellets with a length of 3 mm ± 1 mm and a diameter of 2.5 mm ± 1.5 mm; the twin-screw extruder is equipped with a vacuum device, and the aspect ratio of the twin-screw extruder is not less than 40:1; the process temperature during extrusion is 260°C.

[0049] After mixing, the following steps are performed:

[0050] (1) Melt extrusion process: the temperature of the screw and the box is 280°C, the melt temperature is 280°C, the intrinsic viscosity is 0.7, and the screw extrusion pressure is 7.5MP;

[0051] (2) Mixing process: A static mixer is installed at the head of the screw extruder in (1), the side wall distance of the static mixer is 2 mm, the water hole diameter is 6 mm, the space angle is 70°, and the device spacing is 14 mm;

[0052] (3) Metering process: the pump speed is 28 r / min, the weight of the melt delivered by the pump is 300 g / min, the fineness of the finished silk is 8, the stretching multiple is 0.4 mm, and the fiber shrinkage coefficient is 1.05;

[0053] (4) Filtration and spinning process: the spinning speed is 3500 m / min and the assembly pressure is 20 MPa.

[0054] (5) Cooling and forming process: the temperature of the cooling air is 25°C, the humidity of the cooling air is 60%, the wind speed is 0.4 m / min, and the wind speed distribution is S-shaped.

[0055] (6) Oiling and winding process: the winding speed is 2800 m / min and the oil tanker speed is 0.5 rpm.

[0056] Example 2

[0057] Raw materials: 90 parts of masterbatch polymer (PET), 5 parts of light-absorbing and heat-generating nano-ceramic material (tantalum-doped tungsten oxide, in which tantalum accounts for 2.8% of the total mass of tantalum-doped tungsten oxide), 5 parts of near-infrared absorber (OPTION), 3 parts of dispersant (APTES), and 2 parts of germanium powder (average particle size is 200nm).

[0058] Preparation of heat storage and heat preservation masterbatch: light-absorbing and heat-generating nano-ceramic material, near-infrared absorber, dispersant, germanium powder and masterbatch polymer are blended and extruded to prepare masterbatch (specific preparation method is the same as that in Example 1).

[0059] Preparation of light-colored thermal insulation fiber: 15wt% of thermal storage masterbatch and 85wt% of fiber-forming polymer (PET) were mixed and then the following steps were performed:

[0060] (1) Melt extrusion process: the temperature of the screw and the box is 250°C, the melt temperature is 250°C, the intrinsic viscosity is 1.0, and the screw extrusion pressure is 10MP;

[0061] (2) Mixing process: a static mixer is installed at the head of the screw extruder in (1), the side wall distance of the static mixer is 1.5 mm, the water hole diameter is 5 mm, the space angle is 50°, and the device spacing is 10 mm;

[0062] (3) Metering process: the pump speed is 15 r / min, the weight of the melt delivered by the pump is 150 g / min, the fineness of the finished silk is 8, the stretching multiple is 0.40, and the fiber shrinkage coefficient is 1.15;

[0063] (4) Filtration and spinning process: the spinning speed is 1500 m / min and the assembly pressure is 10 MPa.

[0064] (5) Cooling and forming process: the temperature of the cooling air is 20°C, the humidity of the cooling air is 50%, the wind speed is 0.2 m / min, and the wind speed distribution is S-shaped.

[0065] (6) Oiling and winding process: the winding speed is 1200 m / min and the oil tanker speed is 0.3 rpm.

[0066] Example 3

[0067] Raw materials: 80 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, in which cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of germanium powder (average particle size of 500 nm).

[0068] Preparation of heat storage and heat preservation masterbatch: light-absorbing and heat-generating nano-ceramic material, near-infrared absorber, dispersant, germanium powder and masterbatch polymer are blended and extruded to prepare masterbatch (specific preparation method is the same as that in Example 1).

[0069] Preparation of light-colored thermal insulation fiber: 15wt% of thermal storage masterbatch and 85wt% of fiber-forming polymer (PET) were mixed and then the following steps were performed:

[0070] (1) Melt extrusion process: the temperature of the screw and the box is 300°C, the melt temperature is 300°C, the intrinsic viscosity is 0.5, and the screw extrusion pressure is 5MP;

[0071] (2) Mixing process: A static mixer is installed at the head of the screw extruder in (1), the side wall distance of the static mixer is 3.5 mm, the water hole diameter is 10 mm, the space angle is 90°, and the device spacing is 18 mm;

[0072] (3) Measuring process: the pump speed is 40 r / min, the weight of the melt delivered by the pump is 400 g / min, the fineness of the finished silk is 9, the stretching multiple is 0.50 mm, and the fiber shrinkage coefficient is 1.15;

[0073] (4) Filtration and spinning process: the spinning speed is 5000 m / min and the assembly pressure is 25 MPa.

[0074] (5) Cooling molding process: The temperature of the cooling air is 30°C, the humidity of the cooling air is 80%, the wind speed is 0.6 m / min, and the wind speed distribution is S-shaped.

[0075] (6) Oiling and winding process: the winding speed is 4000 m / min and the oil tanker speed is 0.8 rpm.

[0076] Example 4

[0077] It is basically the same as Example 3, except that: the light-absorbing and heat-generating nano-ceramic material used in this embodiment is silver-doped tungsten oxide, wherein silver accounts for 2.8% of the total mass of the silver-doped tungsten oxide.

[0078] Example 5

[0079] It is basically the same as Example 3, except that: the light-absorbing and heat-generating nano-ceramic material used in this embodiment is tantalum-doped tungsten oxide, wherein tantalum accounts for 2.8% of the total mass of the tantalum-doped tungsten oxide.

[0080] Example 6

[0081] It is basically the same as Example 3, except that the light-absorbing and heat-generating nano-ceramic material used in this example is titanium nitride.

[0082] Example 7

[0083] The embodiment is basically the same as the embodiment 3, except that: the light-absorbing and heat-generating nano-ceramic material used in the embodiment is cesium-doped tungsten oxide, wherein cesium accounts for 2.2% of the total mass of the cesium-doped tungsten oxide.

[0084] Example 8

[0085] The embodiment is basically the same as the embodiment 3, except that: the light-absorbing and heat-generating nano-ceramic material used in the embodiment is cesium-doped tungsten oxide, wherein cesium accounts for 3.3% of the total mass of the cesium-doped tungsten oxide.

[0086] Example 9

[0087] It is basically the same as Example 3, except that: the raw materials used in this example to prepare the heat storage and thermal insulation masterbatch are: 80 parts of masterbatch polymer (PET), 4 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 4.7 parts of germanium powder (average particle size is 500nm).

[0088] Example 10

[0089] It is basically the same as Example 3, except that: the raw materials used in this example to prepare the heat storage and thermal insulation masterbatch are: 75.7 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 5 parts of germanium powder (average particle size is 500nm).

[0090] Embodiment 11

[0091] It is basically the same as Example 3, except that: the raw materials used in this example to prepare the heat storage and thermal insulation masterbatch are: 80.5 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.2 parts of germanium powder (average particle size is 500nm).

[0092] Example 12

[0093] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this example are: 82.5 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 1 part of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of germanium powder (average particle size is 500nm).

[0094] Embodiment 13

[0095] It is basically the same as Example 3, except that: the raw materials used in this example to prepare the heat storage and thermal insulation masterbatch are: 77.5 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 6 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of germanium powder (average particle size is 500nm).

[0096] Comparative Example 1

[0097] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this comparative example are: 80 parts of masterbatch polymer (PET), 0 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 8.7 parts of germanium powder (average particle size is 500nm).

[0098] Comparative Example 2

[0099] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this comparative example are: 80 parts of masterbatch polymer (PET), 8.7 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0 parts of germanium powder (average particle size is 500nm).

[0100] Comparative Example 3

[0101] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this comparative example are: 80 parts of masterbatch polymer (PET), 11.5 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 0 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of germanium powder (average particle size is 500nm).

[0102] Comparative Example 4

[0103] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this comparative example are: 83.5 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 0 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of germanium powder (average particle size is 500nm).

[0104] Comparative Example 5

[0105] It is basically the same as Example 3, except that: the raw materials used in preparing the heat storage and thermal insulation masterbatch in this comparative example are: 80 parts of masterbatch polymer (PET), 8 parts of light-absorbing and heat-generating nano-ceramic material (cesium-doped tungsten oxide, wherein cesium accounts for 2.8% of the total mass of cesium-doped tungsten oxide), 3.5 parts of near-infrared absorber (Omnistab NIR), 2 parts of dispersant (APTES), and 0.7 parts of silicon powder (average particle size is 500nm).

[0106] Performance testing method:

[0107] (1) Fiber color: The fiber was wound onto a color card and the yarn Lab value was tested using a Sanx TS8210 spectrophotometer. The larger the L value, the lighter the yarn color; the smaller the b value, the bluer the yarn; and the larger the a value, the redder the yarn. Five samples were tested for each comparative example, and the average values ​​of the measured values ​​were recorded in Table 1.

[0108] (2) Heat absorption and warmth retention performance: Indoor far-infrared lamp test, test conditions: 150W infrared light source, receiving distance of about 45cm, illumination time of 10 minutes and stop illumination for 5 minutes, light source irradiates the fiber surface, infrared thermistor is used to detect and record the change of sample surface temperature.

[0109] (3) Tensile elongation and breaking strength: in accordance with GB / T 3923.1-2013 Textiles, Fiber elongation and tensile breaking strength.

[0110] The test results of the embodiments are shown in Table 1.

[0111] Performance test results:

[0112] Table 1

[0113]

[0114] As can be seen from Table 1, the fibers prepared in Examples 1-6 are light in color and easy to dye; they have high breaking strength and good fiber lightness; after 10 minutes of irradiation with a 150W infrared light source and the light source is removed for 5 minutes, the fiber surface temperature is still 10.6-16.3°C higher than the initial temperature, and has good light absorption, heat generation and warming effects. In Example 4, silver-doped tungsten oxide powder is used to replace the cesium-doped tungsten oxide powder in Example 3, and the surface temperature change value of the prepared fiber decreases from 16.0°C to 11.2°C, indicating that the cesium-doped tungsten oxide powder can play a better heating and warming effect in the fiber of this application. In Example 5, tungsten oxide powder doped with tantalum is used to replace the cesium-doped tungsten oxide powder in Example 3, and the surface temperature change value of the prepared fiber decreases from 16.0°C to 12.7°C, indicating that the heating and warming effect of the cesium-doped tungsten oxide powder in the fiber of this application is better than that of tantalum-doped tungsten oxide powder. In Example 6, titanium nitride is used to replace the cesium-doped tungsten oxide powder in Example 3. The surface temperature change value of the prepared fiber decreases from 16.0°C to 13.1°C, and the L value is reduced to 67, indicating that the heat generation and warmth retention effect of the cesium-doped tungsten oxide powder in the fiber of the present application is better than that of titanium nitride and the color is lighter.

[0115] From the comparison among Example 3, Example 7 and Example 8, it can be found that when the cesium doping content in tungsten oxide is 2.2%, the fiber prepared in Example 7 has a light color but poor heat-generating and warm-keeping effects; when the cesium doping content in tungsten oxide used in Example 8 is 3.3%, the prepared fiber has a good heat-generating and warm-keeping effect, but a darker color, indicating that when the cesium doping content in tungsten oxide is 2.5%-3%, the heat-generating and warm-keeping effect can both meet the demand and keep the fiber color light.

[0116] In Example 9, an equal amount of germanium powder is used to replace the heating nano-ceramic material (4 parts of heating nano-ceramic material and 4.7 parts of germanium powder are used in this example). The content of heating nano-ceramic material is relatively the least. Although the amount of germanium powder is increased accordingly, the heating and warming effect of the fiber is not good. By comparing Example 3, Example 10 and Example 11, it can be found that too much germanium content in the fiber will improve the heating and warming effect, but the high solid content in the fiber will seriously affect its breaking strength and elongation at break, affecting the fiber performance. Too little germanium content will affect the heating and warming effect.

[0117] By comparing Example 3, Example 12 and Example 13, it can be found that too much organic near-infrared absorber in the fiber will improve the heating and warmth-keeping effect, but will affect the fiber's breaking strength and elongation at break. Too little organic near-infrared absorber will affect the heating and warmth-keeping effect.

[0118] From the comparison between comparative example 1 and embodiment 3, it can be seen that no heating nano-ceramic material is added in comparative example 1, resulting in poor heating and warmth-keeping effect of the fiber. From the comparison between comparative example 2 and embodiment 3, it can be seen that no germanium powder is added in comparative example 2. Although more heating nano-ceramic material is added, the heating and warmth-keeping effect is not significantly improved, and the fiber color is deepened, and the fiber breaking strength and breaking elongation are affected to a certain extent, indicating that the addition of germanium powder can reflect visible light and ultraviolet light to improve the brightness of the fiber while ensuring the heating and warmth-keeping effect, and avoid the color and mechanical properties of the fiber being affected due to excessive use.

[0119] Comparison between Comparative Examples 3 and 4 and Example 3 shows that the heating and warming effect is significantly weakened by using polymer masterbatch instead of organic near-infrared absorber in Comparative Example 4. In Comparative Example 3, heating nano-ceramic material is used instead of organic near-infrared absorber. Although more heating nano-ceramic material is added, the heating and warming effect is not significantly improved, but the fiber color is significantly deepened and the fiber breaking strength and elongation at break are affected to a certain extent, indicating that the addition of organic near-infrared absorber can reduce the amount of heating nano-ceramic material while ensuring the heating and warming effect, avoiding the darkening of fiber color and the influence of mechanical properties due to excessive amount.

[0120] From the comparison between Comparative Example 5 and Example 3, it can be seen that silicon powder is added in Comparative Example 5 instead of germanium powder. It can be observed that the color of the fiber is significantly deepened, and the heating and warming effect is worse. This shows that although silicon powder also has a certain infrared transmittance enhancement effect, the effect is not as good as that of germanium powder, so the improvement of the fiber heating effect is not significant. In addition, silicon powder does not have the function of visible light reflection, so the fiber color is darker.

[0121] In summary, it can be seen from Examples 1 to 13, Comparative Examples 1 to 5 and Table 1 that the light-colored thermal insulation fiber provided by the present invention not only effectively solves the problem of dark color of traditional light-absorbing and heat-generating fibers, avoids the influence of fiber color on fabric color, but also further improves the thermal insulation effect of the fiber, and gives the fiber far-infrared and negative ion functions, is suitable for promotion in the chemical fiber field, and has broad development prospects.

Claims

1. A light-colored thermal insulation fiber made of light-absorbing and heat-generating masterbatch and fiber-forming polymer. It is characterized in that The light-absorbing and heat-generating masterbatch comprises the following raw materials in parts by weight: 70-90 parts of masterbatch polymer, 0.2-20 parts of light-absorbing and heat-generating nano-ceramic material, 1-10 parts of organic near-infrared absorber, 2-10 parts of dispersant, and 0.1-5 parts of germanium powder; The light-absorbing and heat-generating nano-ceramic material is tungsten oxide; The tungsten oxide is cesium-doped tungsten oxide; cesium in the cesium-doped tungsten oxide accounts for 2.5-3% of the total mass of the cesium-doped tungsten oxide; The average particle diameter of the light-absorbing and heat-generating nano-ceramic material is 10nm-500nm.

2. The light-colored thermal insulation fiber according to claim 1, It is characterized in that The masterbatch polymer is selected from at least one of polyamide, polypropylene, polyethylene, polyethylene terephthalate and polybutylene terephthalate.

3. The light-colored thermal insulation fiber according to claim 1, It is characterized in that The dispersant is one or more of a silane coupling agent, an aluminate coupling agent, and a titanate coupling agent.

4. The light-colored thermal insulation fiber according to claim 1, It is characterized in that The organic near-infrared absorber is one or more of IRG-022, OPTION, and Omnistab NIR.

5. The light-colored thermal insulation fiber according to claim 1, It is characterized in that The cross section of the fiber is a special-shaped hollow structure, and the shape of the special-shaped hollow cross section is one of a single-hole circle, a single-hole triangle, a four-hole circle or a seven-hole circle.

6. A method for preparing the light-colored thermal insulation fiber according to any one of claims 1 to 5, It is characterized in that The steps include: (1) mixing the light-absorbing heat-generating masterbatch and the fiber-forming polymer in proportion to obtain a mixture; (2) The mixture is sequentially subjected to a melt extrusion process, a mixing process, a metering process, a filtering and spinning process, a cooling and molding process, and an oiling and winding process to obtain a light-colored thermal insulation fiber.

7. The method for preparing the light-colored thermal insulation fiber according to claim 6, It is characterized in that In the melt extrusion process, the melt temperature is 250-300° C. and the screw extrusion pressure is 5-10 MPa.

8. The method for preparing the light-colored thermal insulation fiber according to claim 6, It is characterized in that In the cooling and forming process, the temperature of the cooling air is 20-30° C., the humidity of the cooling air is 50-80%, and the wind speed distribution is one of a linear type, an arc type, and an S type.