Preparation method and application of waterproof fabric for down jacket

By using hot press composite technology to form a multi-layer structure in down jacket fabrics, the problem of insufficient waterproof performance of traditional down jacket fabrics is solved, and higher water resistance and wear resistance are achieved, while maintaining good breathability and comfort.

CN118578752BActive Publication Date: 2024-11-29HANGZHOU JINGYU TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411072238.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-29
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Traditional down jacket fabrics have shortcomings in waterproof performance, and the waterproof coating or film layer is prone to wear or fall off, affecting breathability and softness.

Method used

The multi-layer structure is formed in the down jacket fabric by using hot pressing composite technology, including the base layer, the first waterproof layer, the second waterproof layer and the wear-resistant layer. The wear-resistant layer is formed by amine decomposition and mist polymerization to improve waterproof performance and resistance. Abrasive.

Benefits of technology

It significantly improves the waterproofness and wear resistance of down jacket fabrics, while maintaining good breathability and comfort, and extending the service life of waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118578752B_ABST
    Figure CN118578752B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of clothing fabrics, and in particular to a preparation method and application of a waterproof fabric for a down jacket. In the invention, a second waterproof layer and a base layer are respectively hot-pressed and composited on both sides of a first waterproof layer, and then the surface of the second waterproof layer is composited to form a wear-resistant layer, wherein the wear-resistant layer can effectively improve the wear resistance of the waterproof fabric for the down jacket, and the second waterproof layer can be used to block the intrusion of liquid water, thereby improving the waterproofness and the air permeability. Even if a small amount of gaseous water enters or the user sweats, the first waterproof layer can transfer water molecules to a dry side. In addition, the base layer is compositely used, and the heat generation of the base layer can improve the warmth retention on the one hand, and can also accelerate the evaporation of water molecules in the first waterproof layer in contact with the base layer, thereby further improving the waterproof performance of the waterproof fabric for the down jacket, thereby improving the comfort of the user, and having broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of clothing fabrics, and in particular to a preparation method and application of waterproof fabrics for down jackets. Background Art

[0002] Down jackets are popular among consumers because of their light weight and warmth. Fabrics are an important component of down jackets, and their structure and performance will greatly affect the appearance, comfort and durability of down jackets. Down jacket fabrics generally use high-density fabrics, such as polyester taffeta, nylon taffeta, nylon taffeta, coated poplin, T / C cloth, etc. Although traditional down jacket fabrics have excellent warmth retention, they have obvious deficiencies in waterproof performance. Currently, the waterproof effect is usually achieved by applying a waterproof coating or bonding a waterproof membrane to the outer layer of the fabric in the market.

[0003] For example, patent document CN117322689A discloses a nano-waterproof, oil-proof and dust-proof down jacket and a preparation method thereof. The invention prepares the down jacket fabric by spraying a nano-waterproof layer and a nano-oil-proof layer on the fabric; patent document CN114261161A discloses a multi-layer composite fabric for a down jacket and a preparation method thereof. The invention increases the waterproofness of the fabric by coating glass microbeads, etc. However, these methods have problems: first, the coating or film layer is easily worn or falls off during washing, resulting in a decrease in the waterproof performance; second, the coating or film layer will affect the air permeability and softness of the fabric, reducing the wearing comfort.

[0004] Therefore, according to the above-mentioned related technologies, it is urgent to develop a preparation method and application of waterproof fabrics for down jackets. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a preparation method and application of waterproof fabric for down jackets, so as to further improve the waterproof property of the waterproof fabric for down jackets.

[0006] Based on the above purpose, the present invention provides a preparation method and application of waterproof fabric for down jackets.

[0007] A method for preparing a waterproof fabric for a down jacket comprises the following steps:

[0008] The second waterproof layer and the base layer are respectively laminated by hot pressing on both sides of the first waterproof layer, and then the surface of the second waterproof layer is treated by aminolysis and then a wear-resistant layer is formed on the surface by mist polymerization to obtain a waterproof fabric for down clothing;

[0009] The thickness ratio of the base layer, the first waterproof layer, the second waterproof layer and the wear-resistant layer is 10-12:4-6:2-3:2-4;

[0010] The base layer is graphene-modified polyurethane fiber;

[0011] The first waterproof layer is a thermoplastic polyurethane fiber membrane;

[0012] The second waterproof layer is a polymer-modified composite nanofiber membrane, and the polymer-modified composite nanofiber membrane is a polyurethane nanofiber membrane with SiO2 particles grafted on the surface;

[0013] The wear-resistant layer is a polyurethane layer, and the treatment agent used in the aminolysis treatment is ethanolamine.

[0014] Preferably, the preparation method of the base layer is as follows:

[0015] Step A1. Adding a thermoplastic polyurethane elastomer to N,N-dimethylformamide, stirring at 40-45° C. for 4.5-5 h, adding graphene powder, and dispersing to obtain a uniform thermoplastic polyurethane spinning solution;

[0016] Step A2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a speed of 15-16 mL / h to form gel-state thermoplastic polyurethane fibers, which are then air-dried to obtain graphene-modified polyurethane fibers. The obtained graphene-modified polyurethane fibers are woven by a textile machine to obtain a base layer.

[0017] The mass ratio of the thermoplastic polyurethane elastomer, N,N-dimethylformamide and graphene powder in step A1 is 20-25:100-110:6-7.5.

[0018] Preferably, the preparation method of the first waterproof layer is as follows:

[0019] The polyurethane particles are dried in a drying oven at 70-75°C for 50-60 minutes, added into the barrel, and the differential nozzle is adjusted to 220-230°C. After the temperature is raised, the extruder is turned on and the material is run for 26-30 minutes. Then the speed of the extruder is adjusted to 1.5-2r / min to prepare the first waterproof layer.

[0020] Preferably, the preparation method of the second waterproof layer is as follows:

[0021] Step B1. N, N-dimethylformamide and butyl acetate are mixed evenly, polyurethane particles are added, and the mixture is stirred evenly in an oil bath at 26-28°C, 4,4'-dicyclohexylmethane diisocyanate and catalyst triethylamine are added, and the mixed solution is stirred in an oil bath at 60°C for 3 hours, and finally 3-aminopropyltriethoxysilane is added, and the stirring is continued for 6 hours to obtain a spinning solution, and the obtained spinning solution is subjected to electrospinning to obtain a polyurethane fiber membrane;

[0022] Step B2. Add ethyl orthosilicate and ethanol to water, stir evenly, add sodium dodecylbenzene sulfonate, stir for 26-30 minutes, add ammonia water to adjust the pH to 9-10, heat the mixed emulsion in a 60°C air drying oven for 2 hours, add a hydrophobic agent hexadecyltrimethoxysilane, and then put the polyurethane fiber membrane in to obtain a second waterproof layer;

[0023] Preferably, the amount ratio of N,N-dimethylformamide, butyl acetate, polyurethane particles, 4,4'-dicyclohexylmethane diisocyanate, catalyst triethylamine and 3-aminopropyltriethoxysilane in step B1 is 40-45mL: 60-65mL: 16-17.6g: 0.4-0.66g: 0.3-0.5g: 4-4.4g.

[0024] Preferably, the electrospinning conditions in step B1 are as follows: the relative humidity in the laboratory is 26%-30%, the temperature is 24-28°C, the spinning solution is loaded into a spinning syringe with a needle hole of 18G, the high voltage is continuously 25kV, the spinning rate is 2mL / h, and the spinning time lasts for 3h.

[0025] Preferably, the usage ratio of ethyl orthosilicate, ethanol, water, sodium dodecylbenzenesulfonate and hydrophobic agent hexadecyltrimethoxysilane in step B2 is 90-100 mL: 380-400 mL: 180-200 mL: 3-6 g: 3-5 g.

[0026] Preferably, the preparation method of the wear-resistant layer is as follows:

[0027] Step C1. Pour the ethanolamine acetone solution into the atomizing cup, place one side of the second waterproof layer 3-5 cm away from the mist outlet, perform atomization treatment for 3-5 minutes, and then place it flat in a 75-80°C oven for 2 hours to obtain a pre-treated layer;

[0028] Step C2. Pour the polyurethane prepolymer solution into the atomizing cup, place one side of the pretreatment layer 3-5 cm from the mist outlet for atomization treatment for 3-5 minutes, and then place it flat in a 55-60°C oven for 2 hours to obtain a wear-resistant layer.

[0029] The mass fraction of ethanolamine in the acetone solution of ethanolamine in step C1 is 18%-20%.

[0030] The preparation method of the polyurethane prepolymer solution in step C2 is as follows:

[0031] The acetone solution of toluene diisocyanate was added to the acetone solution of ethylene glycol, and the mixture was refluxed for 4 hours, and then stirred and cooled to room temperature to obtain a polyurethane prepolymer solution;

[0032] The volume ratio of the toluene diisocyanate acetone solution to the ethylene glycol acetone solution is 22-24 mL:19-20 mL;

[0033] The amount ratio of toluene diisocyanate to acetone in the toluene diisocyanate acetone solution is 2-4g:20mL;

[0034] The usage ratio of ethylene glycol to acetone in the ethylene glycol-acetone solution is 0.5-0.62 g:20 mL.

[0035] Beneficial effects of the present invention:

[0036] The present invention provides a preparation method and application of a waterproof fabric for a down jacket. The wear-resistant layer in the present invention can effectively improve the wear resistance of the waterproof fabric for the down jacket, and the second waterproof layer can be used to block the intrusion of liquid water, thereby improving the waterproofness of the waterproof fabric for the down jacket and improving its air permeability. Even if a small amount of gaseous water enters or the user sweats, the first waterproof layer can transfer water molecules to a dry side. In addition, the composite use of the base layer can increase the warmth retention of the waterproof fabric for the down jacket and accelerate the evaporation of water molecules in the first waterproof layer in contact with the base layer, thereby further improving the waterproof performance of the waterproof fabric for the down jacket and further improving the comfort of the user. The present invention has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 It is a schematic structural diagram of the waterproof fabric of the down jacket in the present invention.

[0039] In the figure: 1, base layer; 2, first waterproof layer; 3, second waterproof layer; 4, wear-resistant layer. DETAILED DESCRIPTION

[0040] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0041] The sources and properties of some of the raw materials used in the present invention are as follows:

[0042] Thermoplastic polyurethane elastomer was industrial grade and purchased from BASF Polyurethanes (China) Co., Ltd.;

[0043] N,N-dimethylformamide (DMF) was of AR specification and purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0044] Polyurethane particles were purchased from Shanghai Jingjian Plastic Co., Ltd., model 1180A.

[0045] Embodiment 1: A waterproof fabric for a down jacket, the waterproof fabric for the down jacket comprising a base layer 1, a first waterproof layer 2, a second waterproof layer 3 and a wear-resistant layer 4.

[0046] Embodiment 2: A method for preparing a waterproof fabric for a down jacket, comprising the following steps:

[0047] Step S1. adding 20 g of thermoplastic polyurethane elastomer to 100 g of N,N-dimethylformamide, stirring at 40° C. for 4.5 h, adding 6 g of graphene powder, and dispersing to obtain a uniform thermoplastic polyurethane spinning solution;

[0048] Step S2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a speed of 15 mL / h to form a gel-state thermoplastic polyurethane fiber, and then air-dried to obtain a graphene-modified polyurethane fiber, and the obtained graphene-modified polyurethane fiber is spun by a textile machine to obtain a substrate layer 1;

[0049] Step S3. Dry the polyurethane particles in a drying oven at 70°C for 50 minutes, add them into the barrel, adjust the differential nozzle to 220°C, turn on the extruder after the temperature rise is completed, run with the material for 26 minutes, and then adjust the extruder speed to 1.5r / min to prepare the first waterproof layer 2;

[0050] Step S4. 40 mL of N, N-dimethylformamide and 60 mL of butyl acetate were mixed evenly, 16 g of polyurethane particles were added, and the mixture was stirred evenly in an oil bath at 26°C, 0.4 g of 4,4'-dicyclohexylmethane diisocyanate and 0.3 g of catalyst triethylamine were added, and the mixed solution was stirred in an oil bath at 60°C for 3 h, and finally 4 g of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 6 h to obtain a spinning solution, and the obtained spinning solution was subjected to electrospinning. The conditions for electrospinning were as follows: the relative humidity of the laboratory was 26%, the temperature was 24°C, the spinning solution was loaded into a spinning syringe with a pinhole of 18G, the high voltage was maintained at 25 kV, the spinning rate was 2 mL / h, and the spinning time was continued for 3 h to obtain a polyurethane fiber membrane;

[0051] Step S5. 90 mL of tetraethyl orthosilicate and 380 mL of ethanol were added to 180 mL of water, stirred evenly, 3 g of sodium dodecylbenzene sulfonate was added, stirred for 26 min, ammonia water was added dropwise to adjust the pH to 9, the mixed emulsion was placed in a 60° C. air drying oven and heated for 2 h, 3 g of hydrophobic agent hexadecyltrimethoxysilane was added, and the polyurethane fiber membrane was placed therein to obtain a second waterproof layer 3;

[0052] Step S6. hot-pressing the second waterproof layer 3 and the base layer 1 on both sides of the first waterproof layer 2;

[0053] Step S7. Pour an ethanolamine acetone solution with a mass fraction of ethanolamine of 18% into the atomizing cup, place one side of the second waterproof layer 3 at 3 cm from the mist outlet, perform atomization treatment for 3 minutes, and then place it flat in a 75°C oven for 2 hours to obtain a pre-treated layer;

[0054] Step S8. Add 2 g of toluene diisocyanate to 20 mL of acetone to obtain an acetone solution of toluene diisocyanate, add 0.5 g to 20 mL of acetone to obtain an acetone solution of ethylene glycol, then add 22 mL of the acetone solution of toluene diisocyanate to 19 mL of the acetone solution of ethylene glycol, reflux for 4 h, stir and cool to room temperature to obtain a polyurethane prepolymer solution;

[0055] Step S9. Pour the polyurethane prepolymer solution into the atomizer cup, place one side of the pretreatment layer 3 cm away from the mist outlet for atomization treatment for 3 minutes, and then place it flat in a 55°C oven for 2 hours to obtain a wear-resistant layer 4. The overall waterproof fabric for down clothing is obtained, wherein the thickness ratio of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 is 10:4:2:2.

[0056] Embodiment 3: A method for preparing a waterproof fabric for a down jacket, comprising the following steps:

[0057] Step S1. Add 22 g of thermoplastic polyurethane elastomer to 104 g of N,N-dimethylformamide, stir at 42° C. for 4.6 h, add 6.5 g of graphene powder, disperse, and obtain a uniform thermoplastic polyurethane spinning solution;

[0058] Step S2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a speed of 15 mL / h to form a gel-state thermoplastic polyurethane fiber, and then air-dried to obtain a graphene-modified polyurethane fiber, and the obtained graphene-modified polyurethane fiber is spun by a textile machine to obtain a substrate layer 1;

[0059] Step S3. Dry the polyurethane particles in a drying oven at 72°C for 52 minutes, add them into the barrel, adjust the differential nozzle to 224°C, turn on the extruder after the temperature rise is completed, run with the material for 27 minutes, and then adjust the extruder speed to 1.7r / min to prepare the first waterproof layer 2;

[0060] Step S4. 42 mL of N, N-dimethylformamide and 62 mL of butyl acetate were mixed evenly, 16.6 g of polyurethane particles were added, and the mixture was stirred evenly in an oil bath at 27°C, 0.46 g of 4,4'-dicyclohexylmethane diisocyanate and 0.4 g of catalyst triethylamine were added, and the mixed solution was stirred in an oil bath at 60°C for 3 h, and finally 4.1 g of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 6 h to obtain a spinning solution, and the obtained spinning solution was subjected to electrospinning. The conditions for electrospinning were as follows: the relative humidity in the laboratory was 27%, the temperature was 25°C, the spinning solution was loaded into a spinning syringe with a pinhole of 18G, the high voltage was maintained at 25 kV, the spinning rate was 2 mL / h, and the spinning time was continued for 3 h to obtain a polyurethane fiber membrane;

[0061] Step S5. 94 mL of ethyl orthosilicate and 382 mL of ethanol were added to 185 mL of water, stirred evenly, 4 g of sodium dodecylbenzene sulfonate was added, stirred for 27 min, ammonia water was added dropwise to adjust the pH to 9, the mixed emulsion was placed in a 60° C. air drying oven and heated for 2 h, 4 g of hydrophobic agent hexadecyltrimethoxysilane was added, and the polyurethane fiber membrane was placed therein to obtain a second waterproof layer 3;

[0062] Step S6. hot-pressing the second waterproof layer 3 and the base layer 1 on both sides of the first waterproof layer 2;

[0063] Step S7. Pour an acetone solution of ethanolamine with a mass fraction of 19% into the atomizing cup, place one side of the second waterproof layer 3 at 4 cm from the mist outlet, perform atomization treatment for 4 minutes, and then place it flat in a 76°C oven for 2 hours to obtain a pre-treated layer;

[0064] Step S8. Add 3 g of toluene diisocyanate to 20 mL of acetone to obtain an acetone solution of toluene diisocyanate, add 0.52 g to 20 mL of acetone to obtain an acetone solution of ethylene glycol, then add 23 mL of the acetone solution of toluene diisocyanate to 19 mL of the acetone solution of ethylene glycol, reflux for 4 h, stir and cool to room temperature to obtain a polyurethane prepolymer solution;

[0065] Step S9. Pour the polyurethane prepolymer solution into the atomizer cup, place one side of the pretreatment layer 4 cm away from the mist outlet for atomization treatment for 4 minutes, and then place it flat in a 57°C oven for 2 hours to obtain a wear-resistant layer 4. The whole down jacket waterproof fabric is obtained, wherein the thickness ratio of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 is 11:5:2.5:3.

[0066] Embodiment 4: A method for preparing a waterproof fabric for a down jacket, comprising the following steps:

[0067] Step S1. adding 24 g of thermoplastic polyurethane elastomer to 108 g of N,N-dimethylformamide, stirring at 44° C. for 4.8 h, adding 7 g of graphene powder, and dispersing to obtain a uniform thermoplastic polyurethane spinning solution;

[0068] Step S2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a rate of 16 mL / h to form a gel-state thermoplastic polyurethane fiber, and then air-dried to obtain a graphene-modified polyurethane fiber, and the obtained graphene-modified polyurethane fiber is spun by a textile machine to obtain a substrate layer 1;

[0069] Step S3. Dry the polyurethane particles in a drying oven at 74°C for 58 minutes, add them into the barrel, adjust the differential nozzle to 228°C, turn on the extruder after the temperature rise is completed, run with the material for 28 minutes, and then adjust the extruder speed to 1.8r / min to prepare the first waterproof layer 2;

[0070] Step S4. 44 mL of N, N-dimethylformamide and 64 mL of butyl acetate were mixed evenly, 17 g of polyurethane particles were added, and the mixture was stirred evenly in an oil bath at 27°C, 0.6 g of 4,4'-dicyclohexylmethane diisocyanate and 0.4 g of catalyst triethylamine were added, and the mixed solution was stirred in an oil bath at 60°C for 3 h, and finally 4.3 g of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 6 h to obtain a spinning solution, and the obtained spinning solution was subjected to electrospinning. The conditions for electrospinning were: the relative humidity of the laboratory was 28%, the temperature was 27°C, the spinning solution was loaded into a spinning syringe with a pinhole of 18G, the high voltage was maintained at 25 kV, the spinning rate was 2 mL / h, and the spinning time was continued for 3 h to obtain a polyurethane fiber membrane;

[0071] Step S5. 98 mL of ethyl orthosilicate and 388 mL of ethanol were added to 190 mL of water, stirred evenly, 5 g of sodium dodecylbenzene sulfonate was added, stirred for 28 min, ammonia water was added dropwise to adjust the pH to 10, the mixed emulsion was placed in a 60° C. air drying oven and heated for 2 h, 4 g of a hydrophobic agent hexadecyltrimethoxysilane was added, and the polyurethane fiber membrane was placed therein to obtain a second waterproof layer 3;

[0072] Step S6. hot-pressing the second waterproof layer 3 and the base layer 1 on both sides of the first waterproof layer 2;

[0073] Step S7. Pour an acetone solution of ethanolamine with a mass fraction of 19% into the atomizing cup, place one side of the second waterproof layer 3 at 4 cm from the mist outlet, perform atomization treatment for 4 minutes, and then place it flat in a 78°C oven for 2 hours to obtain a pre-treated layer;

[0074] Step S8. Add 3 g of toluene diisocyanate to 20 mL of acetone to obtain an acetone solution of toluene diisocyanate, add 0.6 g to 20 mL of acetone to obtain an acetone solution of ethylene glycol, then add 23 mL of the acetone solution of toluene diisocyanate to 20 mL of the acetone solution of ethylene glycol, reflux for 4 h, stir and cool to room temperature to obtain a polyurethane prepolymer solution;

[0075] Step S9. Pour the polyurethane prepolymer solution into the atomizing cup, place one side of the pretreated layer 5 cm from the mist outlet for atomization treatment for 5 minutes, and then place it flat in a 58°C oven for 2 hours to obtain a wear-resistant layer 4, and the whole is a waterproof fabric for down clothing.

[0076] Embodiment 5: A method for preparing a waterproof fabric for a down jacket, comprising the following steps:

[0077] Step S1. adding 25 g of thermoplastic polyurethane elastomer to 110 g of N,N-dimethylformamide, stirring at 45° C. for 5 h, adding 7.5 g of graphene powder, and dispersing to obtain a uniform thermoplastic polyurethane spinning solution;

[0078] Step S2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a rate of 16 mL / h to form a gel-state thermoplastic polyurethane fiber, and then air-dried to obtain a graphene-modified polyurethane fiber, and the obtained graphene-modified polyurethane fiber is spun by a textile machine to obtain a substrate layer 1;

[0079] Step S3. Dry the polyurethane particles in a drying oven at 75°C for 60 minutes, add them into the barrel, adjust the differential nozzle to 230°C, turn on the extruder after the temperature rise is completed, run the extruder with the material for 30 minutes, and then adjust the speed of the extruder to 2r / min to prepare the first waterproof layer 2;

[0080] Step S4. 45 mL of N, N-dimethylformamide and 65 mL of butyl acetate were mixed evenly, 17.6 g of polyurethane particles were added, and the mixture was stirred evenly in an oil bath at 28°C, 0.66 g of 4,4'-dicyclohexylmethane diisocyanate and 0.5 g of catalyst triethylamine were added, and the mixed solution was stirred in an oil bath at 60°C for 3 h, and finally 4.4 g of 3-aminopropyltriethoxysilane was added, and the stirring was continued for 6 h to obtain a spinning solution, and the obtained spinning solution was subjected to electrospinning. The conditions for electrospinning were: the relative humidity of the laboratory was 30%, the temperature was 28°C, the spinning solution was loaded into a spinning syringe with a pinhole of 18G, the high voltage was maintained at 25 kV, the spinning rate was 2 mL / h, and the spinning time was continued for 3 h to obtain a polyurethane fiber membrane;

[0081] Step S5. Add 100 mL of ethyl orthosilicate and 400 mL of ethanol to 200 mL of water, stir evenly, add 6 g of sodium dodecylbenzene sulfonate, stir for 30 min, add ammonia water dropwise to adjust the pH to 10, heat the mixed emulsion in a 60° C. blast drying oven for 2 h, add 5 g of hydrophobic agent hexadecyltrimethoxysilane, and then put the polyurethane fiber membrane in to obtain a second waterproof layer 3;

[0082] Step S6. hot-pressing the second waterproof layer 3 and the base layer 1 on both sides of the first waterproof layer 2;

[0083] Step S7. Pour an acetone solution of ethanolamine with a mass fraction of ethanolamine of 20% into the atomizing cup, place one side of the second waterproof layer 3 at 5 cm from the mist outlet, perform atomization treatment for 5 minutes, and then place it flat in an oven at 80° C. for 2 hours to obtain a pre-treated layer;

[0084] Step S8. Add 4 g of toluene diisocyanate to 20 mL of acetone to obtain an acetone solution of toluene diisocyanate, add 0.62 g to 20 mL of acetone to obtain an acetone solution of ethylene glycol, then add 24 mL of the acetone solution of toluene diisocyanate to 20 mL of the acetone solution of ethylene glycol, reflux for 4 h, stir and cool to room temperature to obtain a polyurethane prepolymer solution;

[0085] Step S9. Pour the polyurethane prepolymer solution into the atomizer cup, place one side of the pretreatment layer 5 cm from the mist outlet for atomization treatment for 5 minutes, and then place it flat in a 60°C oven for 2 hours to obtain a wear-resistant layer 4. The whole down jacket waterproof fabric is obtained, wherein the thickness ratio of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 is 12:6:3:4.

[0086] Comparative Example 1:

[0087] Compared with Example 1, the wear-resistant layer 4 is not provided in the preparation process of the waterproof fabric for the down jacket in this comparative example, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the waterproof fabric for the down jacket is obtained.

[0088] Comparative Example 2:

[0089] Compared with Example 1, the second waterproof layer 3 is not provided in the preparation process of the waterproof fabric for the down jacket in this comparative example, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the waterproof fabric for the down jacket is obtained.

[0090] Comparative Example 3:

[0091] Compared with Example 1, the first waterproof layer 2 is not provided in the preparation process of the waterproof fabric for the down jacket in this comparative example, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the waterproof fabric for the down jacket is obtained.

[0092] Comparative Example 4:

[0093] Compared with Example 1, the base layer 1 is not provided in the preparation process of the waterproof fabric for the down jacket in this comparative example, and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally the waterproof fabric for the down jacket is obtained.

[0094] Comparative Example 5:

[0095] Compared with Example 1, this comparative example only adjusts "the thickness ratio of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 is 10:4:2:2" to "the thickness ratio of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 is 2:10:2:2", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally a waterproof fabric for a down jacket is obtained.

[0096] Comparative Example 6:

[0097] Compared with Example 1, this comparative example only adjusts the composite order of the base layer 1, the first waterproof layer 2, the second waterproof layer 3 and the wear-resistant layer 4 to the base layer 1, the second waterproof layer 3, the first waterproof layer 2 and the wear-resistant layer 4, and the other steps and parameters are the same, which will not be repeated in this comparative example, and finally a waterproof fabric for a down jacket is obtained.

[0098] Performance Test:

[0099] Breaking Strength:

[0100] Referring to the GB / T3923 strip test standard, the YG065 electronic fabric strength tester was used to test the breaking strength of the polyester fabric. The waterproof fabrics of the down jackets prepared in Examples 2 to 5 and Comparative Examples 1 to 6 were cut into rectangles of 200 mm × 50 mm, and then clamped on the sample clamp of the instrument. The parameters were adjusted, the test was performed, and the breaking strength of each test was recorded. The average value of 20 repeated tests was taken as the final breaking strength.

[0101] Abrasion resistance test:

[0102] The wear resistance of the waterproof fabrics of the down jackets prepared in Examples 2 to 5 and Comparative Examples 1 to 6 was tested and analyzed using a Martindale abrasion tester. The mass of the sample holder was 200 g, the mass of the weight was 395 g, the effective diameter of the friction head was 38.0 ± 0.5 mm, and the abrasive was standard wool abrasive. Before the test, the samples were placed in the test environment in a relaxed state for more than 18 hours. Then, three groups of 50×50 mm 2 The polyester fabric sample is loaded into the holder and the wear test is carried out at the same time. During the test, the test is paused every 1000 wear cycles, the holder is removed, and the debris on the surface of the sample and the abrasive is gently cleaned with a brush, and then the test is continued until the sample has obvious holes, and the value on the reading disk is recorded at this time. The average value of the three groups of samples is the wear cycle number of the sample;

[0103] Air permeability test:

[0104] A set of test tubes were filled with deionized water, and the distance from the liquid surface to the tube mouth was set to 2 cm. The down jackets prepared in Examples 2 to 5 and Comparative Examples 1 to 6 were cut into 50×50 mm layers of waterproof fabric. 2 The mouth of the test tube is sealed with each group of samples to allow the deionized water in the test tube to evaporate at room temperature. 24 hours is a cycle. The weight loss of water in the test tube before and after 24 hours is weighed respectively. The air permeability calculation formula is as follows:

[0105] T(g / m 2 / d)=

[0106] Among them, m a is the mass of deionized water in the test tube before the test, m0 is the mass of deionized water in the test tube after the test, r is the inner wall radius of the test tube, and T is the air permeability, which is the mass of water permeated per square meter of surface per day, in g / m 2 / d, the air permeability test data is averaged after repeated experiments for more than 3 times;

[0107] Waterproof test:

[0108] Referring to GB / T4744-2013 standard, the waterproof fabrics of down jackets prepared in Examples 2 to 5 and Comparative Examples 1 to 6 were subjected to hydrostatic pressure test using a YG (B) 812D water permeability tester of Dayong Textile Instruments. The pressure increase rate was 6 kPa / min. When three water drops appeared on the sample, the pressure value at that time was recorded.

[0109] The results are shown in Table 1 below:

[0110] Table 1 Summary of test results of Examples 2 to 5 and Comparative Examples 1 to 6

[0111] project Breaking strength / N Wear times / times <![CDATA[Air permeability / g / m 2 / d]]> Waterproof / Pa Example 2 413.2 19012 856 3089 Example 3 411.8 18929 831 3122 Example 4 412.5 18993 881 3015 Example 5 412.6 19015 862 3109 Comparative Example 1 359.3 15835 759 2687 Comparative Example 2 379.2 17128 746 2735 Comparative Example 3 372.1 16981 764 2873 Comparative Example 4 361.7 16261 739 2706 Comparative Example 5 388.9 17852 804 2905 Comparative Example 6 398.5 18203 798 2986

[0112] Data Analysis:

[0113] It can be seen from Table 1 that the waterproof fabric of the down jacket prepared by the present invention has stronger mechanical properties, wear resistance, air permeability and waterproofness.

[0114] This may be due to: first, the wear-resistant layer 4 provided by the present invention is a polyurethane layer, in which the surface of the second waterproof layer 3 is degraded into small molecules with active hydrogen by first performing aminolysis on the second waterproof layer 3, and then the surface is modified with a polyurethane prepolymer by a mist polymerization method, so that the polyurethane prepolymer can react with the small molecules to form chemical bonds, and then treated with ethylene glycol to form a polyurethane layer on the surface, thereby improving the wear resistance of the waterproof fabric of the down jacket; secondly, the second waterproof layer 3 provided by the present invention is a polymer-modified composite nanofiber membrane, wherein the polymer-modified composite nanofiber membrane is a polyurethane nanofiber membrane with SiO2 particles grafted on the surface, and its pore size is between the liquid water diameter and the water vapor diameter, which can effectively prevent liquid water from penetrating and allow water vapor to penetrate, thereby achieving waterproofness and breathability at the same time; furthermore, even if a small amount of gaseous water penetrates into the first waterproof layer 2 from the second waterproof layer 3, or a small amount of gaseous water molecules penetrate into the first waterproof layer 2 due to sweating of the user, at this time, due to the The first waterproof layer 2 provided is a thermoplastic polyurethane fiber membrane. Since the thermoplastic polyurethane fiber membrane contains a small amount of hydrophilic groups, the presence of the hydrophilic groups will absorb water molecules, and then transfer the water molecules to the dry side through chain end transfer, so that the water molecules can evaporate quickly, thereby improving the comfort of the waterproof fabric of the down jacket; finally, the base layer 1 in the present invention is a graphene-modified polyurethane fiber. The introduction of graphene gives the material excellent antibacterial properties, and when a small amount of gaseous sweat evaporates from the human body, the hydrophilic groups on the graphene-modified polyurethane fiber and the water molecules in the surrounding air are combined through hydrogen bonds. According to the law of conservation of energy, the original kinetic energy of the water molecules is converted into thermal energy. In addition, since the graphene-modified polyurethane fiber can absorb the gaseous sweat evaporated from the human body, the gaseous water is converted into liquid water due to the drop in temperature, and the liquefaction heat will release a large amount of heat. In addition to improving the warmth retention, the heating phenomenon can also increase the evaporation rate of the water molecules in the first waterproof layer 2, further improving the waterproofness, thereby improving the comfort of the user.

[0115] In comparative example 5, the thickness of the base layer 1 is reduced, while the thickness of the first waterproof layer 2 is increased, and in comparative example 6, the arrangement order of the first waterproof layer 2 and the second waterproof layer 3 is reversed, and the performance of the waterproof fabric of the down jacket finally obtained is reduced.

[0116] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0117] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a waterproof fabric for a down jacket, characterized in that: The following steps are involved: The second waterproof layer (3) and the base layer (1) are respectively laminated by hot pressing on both sides of the first waterproof layer (2), and then the surface of the second waterproof layer (3) is subjected to an aminolysis treatment and then a wear-resistant layer (4) is formed on the surface by a mist polymerization method, thereby obtaining a waterproof fabric for a down jacket; The base layer (1) is graphene-modified polyurethane fiber; The first waterproof layer (2) is a thermoplastic polyurethane fiber membrane; The second waterproof layer (3) is a polymer-modified composite nanofiber membrane, and the polymer-modified composite nanofiber membrane is a polyurethane nanofiber membrane with SiO2 particles grafted on the surface; The wear-resistant layer (4) is a polyurethane layer, and the treatment agent used in the aminolysis treatment is ethanolamine; The thickness ratio of the base layer (1), the first waterproof layer (2), the second waterproof layer (3) and the wear-resistant layer (4) is 10-12:4-6:2-3:2-4; The preparation method of the substrate layer (1) is as follows: Step A1. Adding a thermoplastic polyurethane elastomer to N,N-dimethylformamide, stirring at 40-45° C. for 4.5-5 h, adding graphene powder, and dispersing to obtain a uniform thermoplastic polyurethane spinning solution; Step A2. The obtained thermoplastic polyurethane spinning solution is sucked into a syringe, and sprayed from a spinneret into a coagulation bath of deionized water at a rate of 15-16 mL / h to form a gel-state thermoplastic polyurethane fiber, which is then air-dried to obtain a graphene-modified polyurethane fiber. The obtained graphene-modified polyurethane fiber is spun by a textile machine to obtain a substrate layer (1); The mass ratio of the thermoplastic polyurethane elastomer, N,N-dimethylformamide and graphene powder in step A1 is 20-25:100-110:6-7.

5.

2. The method for preparing waterproof fabric for down jackets according to claim 1, characterized in that: The preparation method of the first waterproof layer (2) is as follows: The polyurethane particles are dried in a drying oven at 70-75°C for 50-60 minutes, added to the barrel, and the differential nozzle is adjusted to 220-230°C. After the temperature is raised, the extruder is turned on and the material is run for 26-30 minutes. The speed of the extruder is then adjusted to 1.5-2 r / min to prepare the first waterproof layer (2).

3. The method for preparing waterproof fabric for down jackets according to claim 1, characterized in that: The preparation method of the second waterproof layer (3) is as follows: Step B1. N, N-dimethylformamide and butyl acetate are mixed evenly, polyurethane particles are added, and the mixture is stirred evenly in an oil bath at 26-28°C, 4,4'-dicyclohexylmethane diisocyanate and catalyst triethylamine are added, and the mixed solution is stirred in an oil bath at 60°C for 3 hours, and finally 3-aminopropyltriethoxysilane is added, and the stirring is continued for 6 hours to obtain a spinning solution, and the obtained spinning solution is subjected to electrospinning to obtain a polyurethane fiber membrane; Step B2. Add ethyl orthosilicate and ethanol to water, stir evenly, add sodium dodecylbenzene sulfonate, stir for 26-30 minutes, add ammonia water to adjust the pH to 9-10, place the mixed emulsion in a 60°C forced air drying oven and heat for 2 hours, then add hydrophobic agent hexadecyltrimethoxysilane, and then place the polyurethane fiber membrane to obtain a second waterproof layer (3).

4. The method for preparing waterproof fabric for down jackets according to claim 3, characterized in that: The amount ratio of N,N-dimethylformamide, butyl acetate, polyurethane particles, 4,4'-dicyclohexylmethane diisocyanate, catalyst triethylamine and 3-aminopropyltriethoxysilane in step B1 is 40-45mL: 60-65mL: 16-17.6g: 0.4-0.66g: 0.3-0.5g: 4-4.4g.

5. The method for preparing waterproof fabric for down jackets according to claim 3, characterized in that: The electrospinning conditions in step B1 are as follows: the relative humidity in the laboratory is 26%-30%, the temperature is 24-28°C, the spinning solution is loaded into a spinning syringe with a needle hole of 18G, the high voltage is continuously 25kV, the spinning rate is 2mL / h, and the spinning time lasts for 3h.

6. The method for preparing waterproof fabric for down jackets according to claim 3, characterized in that: The usage ratio of ethyl orthosilicate, ethanol, water, sodium dodecylbenzene sulfonate and hydrophobic agent hexadecyltrimethoxysilane in step B2 is 90-100 mL: 380-400 mL: 180-200 mL: 3-6 g: 3-5 g.

7. The method for preparing waterproof fabric for down jackets according to claim 1, characterized in that: The preparation method of the wear-resistant layer (4) is as follows: Step C1. Pour the ethanolamine acetone solution into the atomizing cup, place one side of the second waterproof layer (3) 3-5 cm away from the mist outlet, perform atomization treatment for 3-5 minutes, and then place it flat in a 75-80°C oven for 2 hours to obtain a pre-treated layer; Step C2. Pour the polyurethane prepolymer solution into the atomizing cup, place one side of the pretreatment layer 3-5 cm from the atomizing port for atomization treatment for 3-5 min, and then place it flat in a 55-60° C. oven for 2 h to obtain a wear-resistant layer (4).

8. The method for preparing waterproof fabric for down jackets according to claim 7, characterized in that: The mass fraction of ethanolamine in the acetone solution of ethanolamine in step C1 is 18%-20%; The preparation method of the polyurethane prepolymer solution in step C2 is as follows: The acetone solution of toluene diisocyanate was added to the acetone solution of ethylene glycol, and the mixture was refluxed for 4 hours, and then stirred and cooled to room temperature to obtain a polyurethane prepolymer solution; The volume ratio of the toluene diisocyanate acetone solution to the ethylene glycol acetone solution is 22-24 mL:19-20 mL; The amount ratio of toluene diisocyanate to acetone in the toluene diisocyanate acetone solution is 2-4g:20mL; The usage ratio of ethylene glycol to acetone in the ethylene glycol-acetone solution is 0.5-0.62 g:20 mL.

Citation Information

Patent Citations

  • Multi-layer composite fabric for down jacket and preparation method of multi-layer composite fabric

    CN114261161A

  • Nano waterproof, oil-proof and dust-proof down jacket and preparation method thereof

    CN117322689A

  • Coating fabric with high water pressure resistance and high moisture penetrability and preparation process thereof

    CN101929081A

  • Method for preparing super-hydrophobic microporous membrane by modifying polyurethane surface with SiO2 particles

    CN109908774A

  • Waterproof and moisture-permeable composite film for clothing and preparation method of waterproof and moisture-permeable composite film

    CN116444851A