Laser cladding nickel-based superalloy wear-resistant gradient coating and preparation method thereof

The preparation of nickel-based high-temperature alloy wear-resistant gradient coating through laser cladding technology solves the problems of poor density and low binding force of traditional coatings in high temperature environments, and achieves the high wear resistance, high temperature resistance and long life of the coating , suitable for high temperature, high pressure and high speed working conditions.

CN119040881AActive Publication Date: 2024-11-29TAIER (ANHUI) IND TECH SERVICE CO LTD

Patent Information

Application Number
CN202411197335.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Traditional nickel-based high-temperature alloy coatings have problems such as poor density, low binding force and easy peeling in high temperature environments, which are difficult to meet the requirements of long-term and stable operation.

Method used

Laser cladding technology is used to prepare a wear-resistant gradient coating of nickel-based high-temperature alloy. By reasonably selecting and controlling the metal powder composition and ratio of different layers, a transition layer, functional layer and ceramic particle enhancement layer are formed, and the thickness of the cladding layer is accurately controlled. and mass, reduce interfacial stress and crack risks, and enhance bond strength.

Benefits of technology

It significantly improves the wear and high temperature resistance of the coating, extends the service life, enhances the stability and mechanical strength of the material in high-temperature environments, and reduces wear and surface damage under high-speed flow or high load.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040881A_ABST
    Figure CN119040881A_ABST
Patent Text Reader

Abstract

The invention discloses a laser cladding nickel-based superalloy wear-resistant gradient coating. The coating comprises a transition layer-1, a transition layer-2 and a functional layer from inside to outside of a matrix, wherein the transition layer-1 is made of nickel-based high-temperature alloy powder; the transition layer-2 is made of nickel-based high-temperature alloy ceramic particle enhanced alloy powder; nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected by the functional layer comprises the following components in percentage by mass: 4.0 to 8.0 percent of C, 10.0 to 17.0 percent of Cr, 30.0 to 44.0 percent of Ni, 1.6 to 2.6 percent of Mo, 0.1 to 0.4 percent of Co, 0.06 to 0.3 percent of Al, 16.0 to 32.0 percent of Ti and the balance of Fe. According to the invention, the components and proportion of the metal powder of different layers are reasonably selected and controlled, so that the high temperature resistance and wear resistance of the coating are improved, and the service life of the coating is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material surface, and in particular relates to a preparation method of a nickel-based high-temperature alloy wear-resistant gradient coating and a laser cladding coating. Background Art

[0002] If the working environment of the parts involves high temperature, high-speed flow and wear, the surface of traditional materials often cannot meet the requirements of long-term stable operation. Nickel-based high-temperature alloys are widely used in aerospace, energy and chemical industries because of their excellent oxidation resistance, creep resistance and mechanical properties in high temperature environments.

[0003] Nickel-based high-temperature alloy coatings can usually be obtained by thermal spraying or laser cladding, but both methods have their own disadvantages: First, the nickel-based high-temperature alloy coating prepared by thermal spraying is thin, generally 0.3-0.5mm; and the bonding force between the coatings is low, and the coating is prone to peeling; Second, the nickel-based high-temperature alloy prepared by laser cladding is prone to cracks, and the density of the coating is poor. Summary of the invention

[0004] The problem to be solved by the present invention is to provide a laser cladding nickel-based high-temperature alloy wear-resistant gradient coating, which reasonably selects and controls the composition and ratio of metal powders in different layers, improves the high temperature resistance and wear resistance of the coating, and prolongs the service life of the coating. At the same time, the present invention provides a method for preparing the coating, which accurately controls the thickness and quality of the cladding layer through laser cladding technology, so that the coating has good density, strong bonding force between the coatings, and is not easy to fall off, thereby prolonging the service life of the coating.

[0005] The invention discloses a laser cladding nickel-based high-temperature alloy wear-resistant gradient coating, which comprises a transition layer-1, a transition layer-2 and a functional layer from the inside to the outside of a substrate; wherein: the transition layer-1 uses a nickel-based high-temperature alloy powder having a composition mass percentage of: C: 0.05-0.08, Cr: 17.0-21.0, Ni: 50.0-55.0, Mo: 2.8-3.3, Co: 0.5-1.0, Al: 0.3-0.7, and the balance is Fe; the transition layer-2 uses a nickel-based high-temperature alloy ceramic particle reinforced alloy powder having a composition mass percentage of: C: 1.8-2.5, Cr: 10.0-17.0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, W: 18.0-38.0, and the balance is Fe; the composition mass percentage of the nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected for the functional layer is: C: 4.0-8.0, Cr: 10.0-17.0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, Ti: 16.0-32.0, and the balance is Fe.

[0006] Among them, the powder particle size of transition layer-1 nickel-based high-temperature alloy powder is 100-270 mesh; the particle size of transition layer-2 nickel-based high-temperature alloy ceramic particle reinforced alloy powder is 100-270 mesh; the particle size of functional layer nickel-based high-temperature alloy ceramic particle reinforced alloy powder is 100-270 mesh.

[0007] Among them, the thickness of transition layer-1 is 0.2-2 mm, the thickness of transition layer-2 is 0.2-2 mm, and the thickness of the functional layer is 0.2-2 mm.

[0008] The present invention provides a method for preparing a laser cladding nickel-based high-temperature alloy wear-resistant gradient coating, which specifically comprises the following steps:

[0009] Step 1, preparing alloy powders for transition layer and functional layer;

[0010] Step 2: Matrix preparation;

[0011] Step 3, laser cladding transition layer-1: laser cladding transition layer-1 on the surface of the metal substrate by high-power semiconductor laser, using pneumatic powder feeding or gravity powder feeding method to feed powder with a powder thickness of 0.5-2.5mm;

[0012] Step 4: Turn to remove the surface oxide scale and make the surface flat and bright;

[0013] Step 5, laser cladding transition layer-2: laser cladding transition layer-2 on the surface of transition layer-1 by high-power semiconductor laser, using pneumatic powder feeding or gravity powder feeding method to feed powder with a powder thickness of 0.5-2.5 mm;

[0014] Step 6: Grind with a grinding wheel to remove the surface oxide scale to obtain a flat and bright surface;

[0015] Step 7, laser cladding functional layer: a high-power semiconductor laser is used to laser clad the functional layer on the surface of transition layer-2, and powder is fed by pneumatic powder feeding or gravity powder feeding, with a powder feeding thickness of 0.5-2.5 mm.

[0016] Specifically, step 2 includes: removing oil stains and oxide scale on the surface of the substrate by oxyacetylene roasting or shot peening after turning.

[0017] Among them, in step 3: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 500-700mm / min, and overlap rate is 50%-70%.

[0018] Among them, in step 5: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 360-600mm / min, and overlap rate is 50%-70%.

[0019] Among them, in step 7: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 360-600mm / min, overlap rate is 50%-70%,

[0020] Wherein, in step 5: the alloy powder of transition layer-2 is mixed evenly by a mechanical powder mixer before cladding, and the mixing time is 2-3 hours; in step 7: the alloy powder of the functional layer is mixed evenly by a mechanical powder mixer before cladding, and the mixing time is 2-3 hours.

[0021] Among them, in step 1: after the three alloy powders are prepared, they are placed in a drying oven for 2 hours, the temperature is set at 150°C, and water vapor in the powder is removed.

[0022] The coating of the present invention has the following advantages: 1. The temperature gradient and thermal stress distribution between the coating surface and the substrate are fully considered. The coating is composed of three layers: transition layer-1, transition layer-2, and functional layer, which reduces the stress concentration at the interface between the coating and the substrate and is not prone to cracks, improves the bonding strength of the coating, effectively reduces the risk of coating peeling caused by thermal stress, and extends the service life of the substrate parts; 2. The components of the two transition layers and one functional layer are carefully designed according to the high-temperature alloy steel substrate and the working conditions: (i) Al and Ti in the functional layer can generate γ' phase (Ni3( Al, Ti)), Ni as the matrix element of γ' phase, works together with aluminum and titanium to promote the uniform precipitation and stability of γ' phase, and enhance the strength and creep resistance of the alloy at high temperature; (ii) Cr is present in all three layers: 1. Cr forms a stable chromium oxide layer (such as Cr2O3) in the alloy, which can protect the alloy matrix in high temperature and corrosive environment, and prevent further expansion of oxidation and corrosion; 2. Cr forms a solid solution in the alloy, and increases the strength and hardness of the material through the solid solution strengthening mechanism; 3. Cr promotes the uniform precipitation and stability of γ' phase (Ni3(Al, Ti)). The distribution and stability of Mo improve the high-temperature mechanical properties of the alloy; (III) All three layers contain Mo: 1. Mo and other elements (such as Al and Ti) work together to form a solid solution strengthening phase, which improves the bonding strength between the coatings; 2. Mo introduces lattice distortion to increase the difficulty of dislocation movement and improve the strength of the alloy; especially in high-temperature environments, the addition of Mo significantly improves the creep resistance of the alloy; 3. Mo and Cr and other elements work together to enhance the stability of the oxide film on the alloy surface and improve the corrosion resistance of the alloy in high-temperature oxidation environments; (IV) All three layers contain Co: 1. Co 1. Co forms a solid solution in the nickel matrix, which improves the strength of the alloy by increasing the difficulty of dislocation slip; 2. The solid solution strengthening effect of Co is particularly important for improving the high-temperature performance of the alloy. The addition of cobalt can improve the toughness of the alloy, especially in high-temperature environments; 3. The presence of Co helps to improve the plasticity and fracture resistance of the alloy at high temperatures; (V) The transition layer-2 contains C and W, and the functional layer contains C and Ti: W, Ti and C elements combine to form WC or TiC hard phases, which have very high hardness and wear resistance, so the hardness of the coating can be significantly improved, enabling it to resist wear and surface damage.

[0023] The laser cladding method of the present invention: in the cladding process of step 3, step 5 and step 7, suitable process parameters are determined, and the laser energy is controlled by adjusting the melting speed, so as to ensure the density and bonding strength of the coating; a uniform high-temperature alloy transition layer is formed on the surface of the metal substrate through step 3; a uniform nickel-based ceramic particle-reinforced surface coating is obtained on the surface of the transition layer-1 alloy through step 5, that is, a uniform wear-resistant transition layer showing a gradient change is obtained; and a uniform nickel-based ceramic particle-reinforced surface coating is obtained on the surface of the transition layer-2 alloy through step 7, that is, a uniform high-temperature wear-resistant functional layer showing a gradient change is obtained.

[0024] In summary, the gradient coating of the present invention: 1. Significantly improves the wear resistance of the base material, effectively reducing wear and surface damage under high-speed flow or high-load working conditions; 2. Has excellent high-temperature resistance, enhancing the stability of the material in high-temperature environments; 3. Has plasticity and fracture resistance, and will not crack; 4. Has good mechanical strength and enhanced fatigue life; 5. The wear resistance and high-temperature resistance of the gradient coating show a gradient improvement, and the coating has good density, strong bonding between the coatings, and is not easy to fall off, extending the service life. Therefore, the gradient coating of the present invention has been widely used under high-temperature, high-pressure, and high-speed working conditions, which greatly extends the service life of the base parts clad with the gradient coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the gradient coating of the present invention. DETAILED DESCRIPTION

[0026] In order to better understand the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0027] from Figure 1It can be seen that the laser cladding nickel-based high-temperature alloy wear-resistant gradient coating of the present invention comprises a transition layer-1, a transition layer-2, and a functional layer from the inside to the outside of the substrate; wherein: the composition mass percentage of the nickel-based high-temperature alloy powder selected for the transition layer-1 is: C: 0.05-0.08, Cr: 17.0-21.0, Ni: 50.0-55.0, Mo: 2.8-3.3, Co: 0.5-1.0, Al: 0.3-0.7, and the balance is Fe; the composition mass percentage of the nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected for the transition layer-2 is: C: 1.8-2. 5. Cr: 10.0-17.0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, W: 18.0-38.0, and the balance is Fe; the composition mass percentage of the nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected for the functional layer is: C: 4.0-8.0, Cr: 10.0-17.0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, Ti: 16.0-32.0, and the balance is Fe.

[0028] Example 1

[0029] Step 1. According to the metal substrate and working conditions, the transition layer and functional layer alloy powders are prepared: the nickel-based high-temperature alloy powder composition and mass percentage selected for transition layer-1 are: C: 0.06, Cr: 20.0, Ni: 55.0, Mo: 3.0, Co: 0.6, Al: 0.4, and the balance is Fe, and they are mixed; the alloy powder particle size is 100-270 mesh; the nickel-based ceramic reinforced alloy powder composition and mass percentage selected for transition layer-2 are: C: 2.0, Cr: 16.0, Ni: 43.0, Mo: 2.4, Co: 0 .3, Al: 0.25, W: 18.7, the balance is Fe, mixed; the alloy powder particle size is 100-270 mesh; the nickel-based ceramic reinforced alloy powder composition and mass percentage selected for the functional layer are: C: 5.0, Cr: 16.0, Ni: 43.0, Mo: 2.4, Co: 0.3, Al: 0.2, Ti: 17.0, the balance is Fe, mixed; the alloy powder particle size is 100-270 mesh; the prepared three powders are placed in a drying oven for 2 hours, the temperature is set at 150°C, and water vapor in the powder is removed.

[0030] Step 2, substrate preparation: remove oil stains and oxide scale on the substrate surface by oxyacetylene baking or shot peening after turning.

[0031] Step 3, laser cladding transition layer-1: laser cladding is performed on the surface of the metal substrate using a high-power semiconductor laser, and powder is fed by pneumatic powder feeding or gravity powder feeding, with a powder feeding thickness of 1.7 mm. The laser process parameters are: laser wavelength 1064 nm, power 3000 W, spot size 5 mm diameter circular spot, scanning speed 600 mm / min, overlap rate 50%, and as the semiconductor laser moves, a uniform high-temperature alloy transition layer is formed on the bottom layer, and the thickness of the transition layer-1 is 1.5 mm;

[0032] Step 4: Turning to remove the surface oxide scale of transition layer-1 to obtain a flat and bright surface;

[0033] Step 5, laser cladding transition layer-2: a high-power semiconductor laser is used to perform laser cladding on the surface of transition layer-1, and powder is fed by pneumatic powder feeding or gravity powder feeding, and the powder feeding thickness is 1.7 mm, wherein the laser process parameters are: laser wavelength 1064 nm, power 2500 W, spot size is a circular spot with a diameter of 5 mm, scanning speed 480 mm / min, overlap rate 50%, and as the semiconductor laser moves, a uniform nickel-based ceramic particle-enhanced surface coating is obtained on the surface of the transition layer-1 alloy, and a uniform gradient wear-resistant transition layer is obtained, and the thickness of transition layer-2 is 1.5 mm;

[0034] Step 6: Grind with a grinding wheel to remove the surface oxide scale to obtain a flat and bright surface;

[0035] Step 7, laser cladding functional layer: use a high-power semiconductor laser to perform laser cladding on the surface of transition layer-2, and use pneumatic powder feeding or gravity powder feeding to feed powder, with a powder feeding thickness of 1.7 mm. The laser process parameters are: laser wavelength 1064 nm, power 2500 W, spot size is a circular spot with a diameter of 5 mm, scanning speed 480 mm / min, overlap rate 50%, and as the semiconductor laser moves, a uniform nickel-based ceramic particle-enhanced surface coating is obtained on the surface of the transition layer-2 alloy, and a uniform high-temperature wear-resistant functional layer with a gradient change is obtained, and the thickness of the functional layer is 1.5 mm.

[0036] Example 2

[0037] Step 1: According to the metal substrate and working conditions, the transition layer and functional layer alloy powders are prepared: the transition layer-1 uses the nickel-based high-temperature alloy powder with the following composition and mass percentage: C: 0.07, Cr: 18.0, Ni: 52.0, Mo: 3.2, Co: 0.8, Al: 0.6, and the balance is Fe, and the alloy powder particle size is 100-270 mesh; the transition layer-2 uses the nickel-based ceramic reinforced alloy powder with the following composition and mass percentage: C: 2.4, Cr: 12.0, Ni: 33.0, Mo: 1.8, Co: 0. 36, Al: 0.25, W: 37.5, the balance is Fe, mixed; the alloy powder particle size is 100-270 mesh; the nickel-based ceramic reinforced alloy powder composition and mass percentage selected for the functional layer are: C: 7.0, Cr: 12.0, Ni: 33.0, Mo: 1.8, Co: 0.36, Al: 0.25, Ti: 30.0, the balance is Fe, mixed; the alloy powder particle size is 100-270 mesh; the prepared three powders are placed in a drying oven for 2 hours, the temperature is set at 150°C, and water vapor in the powder is removed.

[0038] Step 2, substrate preparation: remove oil stains and oxide scale on the substrate surface by oxyacetylene baking or shot peening after turning.

[0039] Step 3, laser cladding transition layer-1: laser cladding is performed on the surface of the metal substrate using a high-power semiconductor laser, and powder is fed by pneumatic powder feeding or gravity powder feeding, with a powder feeding thickness of 0.55 mm. The laser process parameters are: laser wavelength 1064 nm, power 1000 W, spot size 5 mm diameter circular spot, scanning speed 660 mm / min, overlap rate 60%, and as the semiconductor laser moves, a uniform high-temperature alloy transition layer is formed on the bottom layer, and the thickness of the transition layer-1 is 0.2 mm;

[0040] Step 4: Turning to remove the surface oxide scale of transition layer-1 to obtain a flat and bright surface;

[0041] Step 5, laser cladding transition layer-2: a high-power semiconductor laser is used to perform laser cladding on the surface of transition layer-1, and powder is fed by pneumatic powder feeding or gravity powder feeding, and the powder feeding thickness is 1.2 mm. The laser process parameters are: laser wavelength 1064 nm, power 2000 W, spot size is a circular spot with a diameter of 5 mm, scanning speed 540 mm / min, overlap rate 60%, and as the semiconductor laser moves, a uniform nickel-based ceramic particle-enhanced surface coating is obtained on the surface of the transition layer-1 alloy, and a uniform gradient wear-resistant transition layer is obtained. The thickness of transition layer-2 is 1 mm;

[0042] Step 6: Grind with a grinding wheel to remove the surface oxide scale to obtain a flat and bright surface;

[0043] Step 7, laser cladding functional layer: use a high-power semiconductor laser to perform laser cladding on the surface of transition layer-2, and use pneumatic powder feeding or gravity powder feeding to feed powder, with a powder feeding thickness of 1.7 mm. The laser process parameters are: laser wavelength 1064 nm, power 2500 W, spot size is a circular spot with a diameter of 5 mm, scanning speed 480 mm / min, overlap rate 60%, and as the semiconductor laser moves, a uniform nickel-based ceramic particle-enhanced surface coating is obtained on the surface of the transition layer-2 alloy, and a uniform high-temperature wear-resistant functional layer with a gradient change is obtained, and the thickness of the functional layer is 1.5 mm.

[0044] In summary, the advantages of the coating of the present invention are: 1. The coating is divided into three layers from the substrate to the outside, namely, transition layer 1, transition layer 2 and functional layer, and the composition and ratio of each layer of metal powder are reasonably selected and controlled; considering the temperature gradient and thermal stress distribution, the risk of coating peeling caused by thermal stress is effectively reduced by controlling the gradient structure, and at the same time, the bonding strength between the coating and the substrate is enhanced; the wear resistance and high temperature resistance of the three coatings show a gradient change and become larger; therefore, the coating can significantly improve the wear resistance, high temperature resistance and mechanical strength of the substrate material, and effectively reduce the wear under high-speed flow or high-load working conditions. loss and surface damage, which enhances the stability and life of the material in a high temperature environment, and is therefore widely used under high temperature, high pressure and high speed working conditions; secondly, by precisely determining the process parameters of laser cladding, the density of the coating is ensured, cladding defects are avoided, the bonding strength is improved, a close bond between multiple layers of cladding is achieved, and a thick cladding layer is ensured, thereby obtaining a composite cladding layer with good surface properties, enhancing the stability of the material in a high temperature environment, thereby extending the service life of the coating, and significantly reducing the maintenance cycle and cost, which has a positive impact on the stability and reliability of equipment operation.

Claims

1. A laser cladding nickel-based high-temperature alloy wear-resistant gradient coating, characterized by: It includes transition layer-1, transition layer-2, and functional layer from the inside to the outside of the substrate; wherein: the composition mass percentage of the nickel-based high-temperature alloy powder selected for transition layer-1 is: C: 0.05-0.08, Cr: 17.0-21.0, Ni: 50.0-55.0, Mo: 2.8-3.3, Co: 0.5-1.0, Al: 0.3-0.7, and the balance is Fe; the composition mass percentage of the nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected for transition layer-2 is: C: 1.8-2.5, Cr: 10.0-17. 0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, W: 18.0-38.0, and the balance is Fe; the composition mass percentage of the nickel-based high-temperature alloy ceramic particle reinforced alloy powder selected for the functional layer is: C: 4.0-8.0, Cr: 10.0-17.0, Ni: 30.0-44.0, Mo: 1.6-2.6, Co: 0.1-0.4, Al: 0.06-0.3, Ti: 16.0-32.0, and the balance is Fe.

2. The gradient coating according to claim 1, characterized in that: The powder particle size of transition layer-1 nickel-based high-temperature alloy powder is 100-270 mesh; the particle size of transition layer-2 nickel-based high-temperature alloy ceramic particle reinforced alloy powder is 100-270 mesh; the particle size of functional layer nickel-based high-temperature alloy ceramic particle reinforced alloy powder is 100-270 mesh.

3. The gradient coating according to claim 1, characterized in that: The thickness of the transition layer-1 is 0.2-2 mm, the thickness of the transition layer-2 is 0.2-2 mm, and the thickness of the functional layer is 0.2-2 mm.

4. A method for preparing a laser cladding nickel-based high-temperature alloy wear-resistant gradient coating, the specific steps are: Step 1, preparing alloy powders for transition layer and functional layer; Step 2: Matrix preparation; Step 3, laser cladding transition layer-1: laser cladding transition layer-1 on the surface of the metal substrate by high-power semiconductor laser, using pneumatic powder feeding or gravity powder feeding method to feed powder with a powder thickness of 0.5-2.5mm; Step 4: Turn to remove the surface oxide scale and make the surface flat and bright; Step 5, laser cladding transition layer-2: laser cladding transition layer-2 on the surface of transition layer-1 by high-power semiconductor laser, using pneumatic powder feeding or gravity powder feeding method to feed powder with a powder thickness of 0.5-2.5 mm; Step 6: Grind with a grinding wheel to remove the surface oxide scale to obtain a flat and bright surface; Step 7, laser cladding functional layer: a high-power semiconductor laser is used to laser clad the functional layer on the surface of transition layer-2, and powder is fed by pneumatic powder feeding or gravity powder feeding, with a powder feeding thickness of 0.5-2.5 mm.

5. The preparation method according to claim 4, characterized in that: Step 2 specifically includes: removing oil stains and oxide scale on the surface of the substrate by oxyacetylene baking or shot peening after turning.

6. The preparation method according to claim 4, characterized in that: In step 3: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 500-700mm / min, and overlap rate is 50%-70%.

7. The preparation method according to claim 4 is characterized in that: in step 5: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 360-600mm / min, and overlap rate is 50%-70%.

8. The preparation method according to claim 4, characterized in that: In step 7: the laser process parameters are: laser wavelength 1064nm, power 1000-4000W, spot size is a circular spot with a diameter of 5mm, scanning speed is 360-600mm / min, and overlap rate is 50%-70%.

9. The preparation method according to claim 4, characterized in that: In step 5: the alloy powder of transition layer-2 is mixed evenly with a mechanical powder mixer before cladding, and the mixing time is 2-3 hours; in step 7: the alloy powder of the functional layer is mixed evenly with a mechanical powder mixer before cladding, and the mixing time is 2-3 hours.

10. The preparation method according to claim 4, characterized in that: in step 1: after the three alloy powders are prepared, they are placed in a drying oven for 2 hours, set at a temperature of 150°C, to remove water vapor in the powders.

Citation Information

Patent Citations

  • Method for preparing WC cemented carbide anti-wear layer on petroleum drilling tool stabilizer through laser cladding

    CN103194748A

  • Method for laser cladding coating preparing process by using vacuum sintering method

    CN110714198A

  • Magnesium alloy surface gradient ceramic composite coating laser cladding preparation method

    CN114507853A

  • WC-Ni wear-resistant coating on 316L stainless steel surface and preparation method of WC-Ni wear-resistant coating

    CN115537803A

  • WC-ni wear-resistant coating on 316l stainless steel surface and preparation method therefor

    WO2024077654A1

Cited By

  • Gradient structure wear-resistant coating and preparation method thereof

    CN119243147A

  • Gradient nano composite high-entropy alloy coating system with self-monitoring function and preparation method

    CN121653635A

  • Gradient lap joint martensitic stainless steel surface laser cladding coating and preparation method thereof

    CN122279579A

  • Gradiently overlapped martensitic stainless steel surface laser cladding coating and method for preparing same

    CN122279579B