A kind of styrene tar nano-dispersion synergist and its manufacturing method
By adding nanodispersion synergists to styrene tar, the problem that the existing technology cannot effectively utilize tar is solved, uniform dispersion and stability of tar is achieved, waste treatment costs are reduced, and the national standard indicators are met, and waste is turned into treasure purpose.
Patent Information
- Application Number
- CN202310374903.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-12-24
- Estimated Expiration
- 2043-04-10
AI Technical Summary
The existing technology cannot effectively utilize styrene tar, resulting in insufficient utilization of resources and waste production in the treatment method, which cannot achieve the purpose of "turning waste into treasure".
By adding nanodispersion synergists to styrene tar, including the T154 ash-free dispersant polyisobutylene succinimide, modified graphene material and modified nanomesoporous alumina, the tar reaches GB/ T 9581-2011 "Carbon Black Raw Oil Ethylene Tar" product quality indicators, used as carbon black raw material or heavy fuel oil.
It achieves uniform dispersion and stability of styrene tar, reduces waste treatment costs, complies with national standard indicators, and achieves the goal of turning waste into treasure.
Smart Images

Figure BDA0004170021650000051 
Figure BDA0004170021650000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmentally friendly treatment of styrene tar, and in particular to a styrene tar nano-dispersion synergist and a preparation method thereof. Background Art
[0002] Styrene tar is a distillation byproduct in the production process of styrene. Its composition is relatively complex, containing high-boiling point byproducts, polymer residues, inhibitors, etc. Since styrene tar has been included in the National List of Hazardous Wastes, it needs to be treated in an environmentally friendly manner.
[0003] With the growth of my country's demand for styrene, my country's styrene production has been rising in the past five years. Zhejiang Petrochemical, Hengli Petrochemical, Satellite Chemical, Anqing Petrochemical, Maoming Petrochemical and other companies have successively built / expanded large-scale styrene production facilities, and domestic production capacity has exceeded 10 million tons / year. If 10kg of tar is produced for every ton of styrene produced, 100,000 tons of tar will be produced each year. Such a large amount of styrene tar needs to be disposed of in a reasonable, efficient and legal way to make use of its resources.
[0004] There are three main ways to utilize styrene tar resources:
[0005] 1. As a heating furnace fuel
[0006] 2. Refining in the coking unit
[0007] 3. Send to catalytic cracking unit for refining.
[0008] The above three treatment methods still cannot fully utilize styrene tar, and waste will be generated, which cannot achieve the purpose of "turning waste into treasure and making full use of resources". Through countless experiments, the technical personnel of our company have developed a styrene tar environmental protection treatment agent. By adding a certain amount of styrene tar environmental protection treatment agent to styrene tar, styrene tar can be blended into carbon black raw material oil or heavy fuel oil, and finally make styrene tar meet the technical index requirements for raw material oil in GB / T 9581-2011 "Carbon Black Raw Material Ethylene Tar", and can be used as carbon black raw material oil or heavy fuel oil to achieve the purpose of turning waste into treasure. Summary of the invention
[0009] The purpose of the present invention is to make up for the defects of the existing technology and provide a styrene tar nano-dispersion synergist. By adding the nano-dispersion synergist to the styrene tar and fully stirring it, the styrene tar finally reaches the product quality index of GB / T 9581-2011 "Carbon black raw material oil ethylene tar", and can be used as a carbon black raw material or heavy fuel oil, thereby achieving the purpose of turning waste into treasure.
[0010] The present invention is achieved through the following technical solutions:
[0011] A styrene tar nano-dispersion synergist, characterized in that it comprises the following raw materials in parts by weight: 30-50 parts of T154 ashless dispersant polyisobutylene succinimide, 0.1-0.3 parts of modified graphene material, 0.1-0.2 parts of modified nano-mesoporous alumina, and 40-60 parts of heavy aromatic solvent oil.
[0012] The preparation method of the modified graphene material is as follows:
[0013] (1) Slowly add an appropriate amount of monoethanolamine to an appropriate amount of 2-methyltetrahydrofuran, and stir the reaction at 50-60° C. for 4-5 hours to obtain an intermediate;
[0014] (2) Add concentrated sulfuric acid into an ultrasonic agitator, add graphene under stirring, and ultrasonically stir for 1-2 hours, then add the intermediate obtained in step (1), adjust the pH value to 8-10, and ultrasonically stir the reaction at a temperature of 60-65° C. for 2-3 hours to obtain a monoethanolamine-modified graphene material.
[0015] Furthermore, the mass ratio of the graphene material, monoethanolamine and 2-methyltetrahydrofuran is 100:4-6:3-5.
[0016] Furthermore, the preparation method of the modified nano-mesoporous alumina is as follows: fully dissolve the TM-200S water-soluble titanate coupling agent in water to obtain a titanate coupling agent aqueous solution with a mass percentage of 3-4%, then add nano-mesoporous alumina equivalent to 0.3-0.5% of the weight of the solution to the solution for reaction for 3-4 hours, filter and vacuum dry at 100-110°C to obtain a first-modified nano-mesoporous alumina, then disperse the first-modified nano-mesoporous alumina in anhydrous ethanol to form a suspension, add triethyl (trifluoromethyl) silane to a 75% mass percentage ethanol aqueous solution to prepare a modifier, stir the suspension, add the modifier to the suspension under stirring, after the addition is completed, the mixed solution is kept at a constant temperature of 32±2°C in a water bath under stirring, and stirred at a constant temperature for more than 6 hours, then the solid-liquid separation continues to stir the suspension for 3-4 hours, the solid phase is washed 3 times with anhydrous ethanol, washed 2 times with deionized water, and dried to obtain modified nano-mesoporous alumina.
[0017] Furthermore, the mass ratio of triethyl (trifluoromethyl) silane to ethanol aqueous solution in the modifier is 4-5:100.
[0018] Furthermore, the mass percentage of nano-mesoporous alumina in the suspension is 20-30%.
[0019] Furthermore, the mass ratio of the modifier to the suspension is 100:1-2.
[0020] Furthermore, the particle size of the nano-mesoporous alumina is 30-40 nm, and the pore size is 6-7 nm.
[0021] Furthermore, the method for preparing the styrene tar nano-dispersion synergist is characterized by comprising the following steps:
[0022] Add T154 ashless dispersant polyisobutylene succinimide to heavy aromatic solvent oil, stir thoroughly, then add modified graphene material, stir ultrasonically at 50-55°C for 5-6h, finally add modified nano-mesoporous alumina, stir ultrasonically to obtain the finished product.
[0023] Furthermore, the invention also comprises the following raw materials in weight percentage: 5-6% isopropanol and 3-8% modified polyether.
[0024] Usage: Add 3-8% by mass into the styrene tar to be treated and stir thoroughly for 30 minutes.
[0025] The advantages of the present invention are:
[0026] The invention adds monoethanolamine modified graphene material to conventional ashless dispersant polyisobutylene succinimide, and grafts monoethanolamine with the graphene material to further improve the dispersibility of the graphene material to the polymer; adds modified nano-mesoporous alumina, and the combination of the nano-mesoporous alumina and the monoethanolamine modified graphene material can further adsorb colloid in the tar. The styrene tar nano-dispersion synergist obtained by the invention has an excellent dispersing effect. The styrene tar nano-dispersion synergist is added to styrene tar, and after sufficient stirring, the styrene tar is dispersed into carbon black raw materials or heavy fuel oil with uniform and stable components. Various indicators meet the product quality indicator requirements of the national standard GB / T9581-2011 "carbon black raw material oil ethylene tar" after detection. DETAILED DESCRIPTION
[0027] Example 1
[0028] A styrene tar nano-dispersion synergist, characterized in that it comprises the following raw materials in parts by weight: 42 parts of T154 ashless dispersant polyisobutylene succinimide, 0.2 parts of modified graphene material, 0.15 parts of modified nano-mesoporous alumina, and 55 parts of heavy aromatic solvent oil.
[0029] The preparation method of the monoethanolamine modified graphene material is as follows:
[0030] (1) Slowly add an appropriate amount of monoethanolamine to an appropriate amount of 2-methyltetrahydrofuran, and stir the reaction at 55°C for 4.5 hours to obtain an intermediate;
[0031] (2) Add concentrated sulfuric acid into an ultrasonic agitator, add graphene under stirring, and ultrasonically stir for 1.5 hours. Then, add the intermediate obtained in step (1), adjust the pH value to 9, and ultrasonically stir the reaction at 62° C. for 2.5 hours to obtain a monoethanolamine-modified graphene material.
[0032] Furthermore, the mass ratio of the graphene material, monoethanolamine and 2-methyltetrahydrofuran is 100:4-6:3-5.
[0033] Furthermore, the preparation method of the modified nano-mesoporous alumina is as follows: fully dissolve the TM-200S water-soluble titanate coupling agent in water to obtain a 3.5% by weight titanate coupling agent aqueous solution, then add nano-mesoporous alumina equivalent to 0.4% by weight of the solution to the solution for reaction for 3.5 hours, filter and vacuum dry at 100-110°C to obtain a first-modified nano-mesoporous alumina, then disperse the first-modified nano-mesoporous alumina in anhydrous ethanol to form a suspension, add triethyl (trifluoromethyl) silane to a 75% by weight ethanol aqueous solution to prepare a modifier, stir the suspension, add the modifier to the suspension under stirring, after the addition is completed, keep the mixed solution in a water bath under stirring at a constant temperature of 32±2°C, stir at a constant temperature for more than 6 hours, then continue to stir the suspension for 3.5 hours for solid-liquid separation, wash the solid phase with anhydrous ethanol 3 times, wash with deionized water 2 times, and dry to obtain modified nano-mesoporous alumina.
[0034] Furthermore, the mass ratio of triethyl (trifluoromethyl) silane to ethanol aqueous solution in the modifier is 4.5:100.
[0035] Furthermore, the mass percentage of nano-mesoporous alumina in the suspension is 25%.
[0036] Furthermore, the mass ratio of the modifier to the suspension is 100:1.5.
[0037] Furthermore, the particle size of the nano-mesoporous alumina is 30-40 nm, and the pore size is 6-7 nm.
[0038] Furthermore, the method for preparing the styrene tar nano-dispersion synergist comprises the following steps:
[0039] T154 ashless dispersant polyisobutylene succinimide is added to heavy aromatic solvent oil, and after sufficient stirring, the modified graphene material is added, and the reaction is carried out under ultrasonic stirring at a temperature of 53°C for 5.5 hours. Finally, the modified nano-mesoporous alumina is added and ultrasonic stirring is performed to obtain the finished product.
[0040] Furthermore, the styrene tar nano-dispersion synergist also includes the following component raw materials in percentage by weight: 5.5% isopropanol and 5% modified polyether.
[0041] The various indicators of the styrene tar nanodispersion synergist prepared by the above method are shown in Table 1 below.
[0042] Table 1
[0043] project Index value Detection Methods Appearance Brown liquid Visual inspection Solubility Soluble in aromatic hydrocarbons Visual inspection <![CDATA[Density (20 °C) g / cm 3 > ≥1 GB / T4472 Flash point (closed cup)℃ >85 GB / T267 Moisture% ≤0.05 GB / T260 Mechanical impurities m% none GB / T511
[0044] Comparative Example 1
[0045] A styrene tar dispersant, characterized in that it comprises the following raw materials in parts by weight: 42 parts of T154 ashless dispersant polyisobutylene succinimide and 55 parts of heavy aromatic solvent oil.
[0046] The preparation method is to directly mix the two raw materials and stir them evenly.
[0047] The dispersants prepared in Example 1 and Comparative Example 1 were added to the styrene tar to be treated in an amount of 5% by mass. After stirring for 30 minutes, the stirred styrene tar was tested. The results are shown in Tables 2 and 3 below, respectively.
[0048] Table 2
[0049]
[0050] Table 3
[0051]
[0052] It can be seen from Table 2 above that after the styrene tar nano-dispersed synergist of the present invention is added to styrene tar and stirred for 30 minutes, the Engler viscosity of the styrene tar is directly reduced to 1.5. The treated styrene tar meets the technical indicators of ethylene tar in GB / T 9581-2011 "Carbon black raw material oil ethylene tar", and can be used as a carbon black raw material or heavy fuel oil, achieving the purpose of turning waste into treasure.
[0053] As can be seen from Table 3, after the conventional ashless dispersant of Comparative Example 1 was added to styrene tar and stirred for 30 minutes, the Engler viscosity of the styrene tar was still as high as 35, and the styrene tar could not be used as a carbon black raw material or heavy fuel oil. It is still a hazardous waste that needs to be treated and further environmental protection treatment is required.
[0054] It can be seen that the styrene tar nano-dispersion synergist of the present invention has a good dispersing effect, and can quickly disperse high-viscosity components rich in styrene tar, such as high-boiling point by-products, polymer residues, inhibitors and other components in a short time. After a certain amount of the nano-dispersion synergist of the present invention is added to the tar, the molecular bonds of raw materials such as polymers and high-boiling point by-products are destroyed, so that the tar can be effectively dispersed, the cost of waste treatment is greatly reduced, and the purpose of turning waste into treasure is achieved.
Claims
1. A styrene tar nanodispersion synergist, characterized in that: The invention comprises the following raw materials in parts by weight: 30-50 parts of T154 ashless dispersant polyisobutylene succinimide, 0.1-0.3 parts of modified graphene material, 0.1-0.2 parts of modified nano-mesoporous alumina, 40-60 parts of heavy aromatic solvent oil, The preparation method of the modified graphene material is as follows: (1) Slowly add an appropriate amount of monoethanolamine to an appropriate amount of 2-methyltetrahydrofuran, stir and react at 50-60°C for 4-5 hours to obtain an intermediate; (2) Add concentrated sulfuric acid to an ultrasonic agitator, add graphene under stirring, and ultrasonically stir for 1-2 hours, then add the intermediate obtained in step (1), adjust the pH value to 8-10, and ultrasonically stir the reaction at a temperature of 60-65° C. for 2-3 hours to obtain a monoethanolamine-modified graphene material. The preparation method of the modified nano-mesoporous alumina is as follows: fully dissolving TM-200S water-soluble titanate coupling agent in water to obtain a titanate coupling agent aqueous solution with a mass percentage of 3-4%, then adding nano-mesoporous alumina equivalent to 0.3-0.5% of the weight of the solution to the solution for reaction for 3-4 hours, filtering and vacuum drying at 100-110° C. to obtain a first-modified nano-mesoporous alumina, then dispersing the first-modified nano-mesoporous alumina in anhydrous ethanol to form a suspension, adding triethyl (trifluoromethyl) silane to an ethanol aqueous solution with a mass percentage of 75% to prepare a modifier, stirring the suspension, adding the modifier to the suspension under stirring, and after the addition is completed, the mixed solution is kept at a constant temperature of 32±2° C. in a water bath under stirring, and stirred at a constant temperature for more than 6 hours, and then the solid-liquid separation is continued to stir the suspension for 3-4 hours, the solid phase is washed 3 times with anhydrous ethanol, washed 2 times with deionized water, and dried to obtain the modified nano-mesoporous alumina.
2. A styrene tar nanodispersion synergist according to claim 1, characterized in that: The mass ratio of the graphene material, monoethanolamine and 2-methyltetrahydrofuran is 100:4-6:3-5.
3. A styrene tar nanodispersion synergist according to claim 1, characterized in that: The mass ratio of triethyl (trifluoromethyl) silane to ethanol aqueous solution in the modifier is 4-5:
100.
4. A styrene tar nanodispersion synergist according to claim 1, characterized in that: The mass percentage of nano-mesoporous alumina in the suspension is 20-30%.
5. A styrene tar nanodispersion synergist according to claim 1, characterized in that: The mass ratio of the modifier to the suspension is 100:1-2.
6. A styrene tar nanodispersion synergist according to claim 4, characterized in that: The particle size of the nano-mesoporous alumina is 30-40 nm, and the pore size is 6-7 nm.
7. The method for preparing a styrene tar nano-dispersion synergist according to claim 1, characterized in that: The steps include: Add T154 ashless dispersant polyisobutylene succinimide to heavy aromatic solvent oil, stir thoroughly, then add modified graphene material, stir ultrasonically at 50-55°C for 3-4h, finally add modified nano-mesoporous alumina, stir ultrasonically to obtain the finished product.
8. The styrene tar nanodispersion synergist according to any one of claims 1 to 7, characterized in that: The invention also comprises the following raw materials in weight percentage: 5-6% isopropanol and 3-8% modified polyether.