Method for determining the fracture toughness curve and the delamination mode mix ratio of a composite unsymmetric laminate
Patent Information
- Application Number
- CN202310353080.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2026-11-03
- Estimated Expiration
- 2043-04-04
AI Technical Summary
然而,分层长度测量通常很困难,因为这需要全程观测裂纹发展并与载荷位移数据相匹配
[0044](1)利用本发明的方法确定ADCB层压板的断裂韧性曲线及分层模式混合比仅需要在试验过程记录载荷位移曲线以及测量特定的分层长度aT,无需测量全过程的裂纹长度。这大大降低了试验的复杂度,方便进行快速测试;
Smart Images

Figure CN116451452B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of determining the fracture toughness curve of fiber-reinforced composite laminates, and specifically to a method for determining the fracture toughness curve and the mixing ratio of the layering mode of an arbitrary layup composite asymmetric laminate. Background Technology
[0002] Delamination is one of the main forms of damage in composite laminates. The occurrence and propagation of delamination significantly reduce the mechanical properties of materials and structures, and can even lead to catastrophic accidents. These severely limit the application of composite materials in engineering. To achieve damage-tolerant design, accurate data on the interlaminar fracture toughness of composite structures is essential for predicting delamination propagation behavior and structural strength.
[0003] The asymmetrical double cantilever beam (ADCB) test has been used to determine mixed I / II delamination under type I loading and can also be used to determine the fracture toughness of most bimaterial interfaces over a wide range of mixing ratios. ADCB testing is simple and easy to conduct, and mixed I / II delamination caused by type I loading is ubiquitous in practical delamination problems, and mixed delamination due to geometric or material asymmetry also exists in engineering structures. During delamination propagation, toughening phenomena such as fiber bridging occur at the trailing edge of the crack tip. The bridging fibers bear the load and reduce the local stress at the crack tip. This toughening mechanism causes the apparent fracture toughness to increase with increasing delamination length. To accurately characterize the I / II mixed delamination propagation behavior of ADCB laminates, it is necessary to obtain the interlaminar fracture toughness curve and the corresponding delamination mode mixing ratio.
[0004] Existing research indicates that characterizing the I / II mixed-type interlaminar fracture toughness curve of ADCB laminates requires full-length measurement of the delamination length. However, measuring the delamination length is often difficult because it requires continuous observation of crack propagation and matching with load-displacement data. This introduces human error and other errors, leading to inaccurate data calculations. Furthermore, the mode mixing ratio throughout the ADCB delamination process is difficult to calculate. The ideal goal is to obtain accurate fracture toughness curves and mode mixing ratios with as few measurement parameters as possible. Therefore, it is necessary to establish a rapid method for determining the fracture toughness curve and mode mixing ratio of ADCB laminates that is easy to apply in engineering. Summary of the Invention
[0005] The technical problem this invention aims to solve is to provide a method for determining the fracture toughness curve and delamination mode mixing ratio of an asymmetric composite laminate. It proposes an equivalent delamination length concept using a global correction method, and further, a method for determining the fracture toughness curve of an ADCB laminate based on this concept. This significantly reduces the amount of experimental data required to determine the interlaminar fracture toughness curve of a fiber-reinforced composite ADCB laminate. This method can also significantly shorten the experimental cycle and reduce experimental costs.
[0006] The technical solution adopted by this invention to solve the above-mentioned technical problems is as follows: a method for determining the fracture toughness curve and delamination mode mixing ratio of a composite asymmetric laminate, comprising the following steps:
[0007] Step 1: Design and manufacture fiber-reinforced composite laminate samples with different thicknesses of upper and lower sub-laminated plates but arbitrary layup.
[0008] Step 2: For the above specimens, an ADCB layering test is conducted using a double cantilever beam test apparatus by applying a type I load, and the test load, displacement, and specific layering length 'a' are recorded. T ;
[0009] Step 3: Establish a two-dimensional ADCB mechanical model based on the reinforced beam theory and calculate the theoretical compliance C. eq Compare it with the test flexibility C exp The equivalent crack length 'a' is obtained by matching and iterative calculation using the program. eq The equivalent crack length a eq Substituting into the calculation formula based on the reinforced beam theory, we obtain G. T (a eq ) and the mode mixing ratio G of the entire stratified process I / G T ;
[0010] Step 4: Obtain the specific layer length 'a' through measurement. T Combined with the equivalent crack length a in step 3 eq Obtain the global correction coefficient
[0011] Step 5, obtain the result with a through a global correction method. eq One-to-one correspondence G T ;
[0012] Step 6, by comparing with the equivalent crack length a eq One-to-one correspondence G T and G I / G T Restored to G corresponding one-to-one with the actual layer length a T and G I / G TThus, the fracture toughness curves of the ADCB laminate I / II hybrid type and the mode mixing ratio of the whole process were obtained;
[0013] Furthermore, the pre-crack length, specimen width, and upper and lower sublaminated plate thicknesses of the test specimen in step 1 can be determined according to research needs;
[0014] Furthermore, in step 2, the testing machine should perform the static tensile test using a low-speed displacement control mode, with a loading rate typically 0.1 mm / min or slower. The load-displacement data P-δ should be recorded by the testing machine.
[0015] In step 2, a T The crack length measured when the ADCB laminate fracture process zone has fully developed during the test, i.e., when the crack is about to begin self-similar propagation;
[0016] In step 3, the hybrid stratification problem of the ADCB test will be simplified into a two-dimensional mechanical model based on the reinforced beam theory.
[0017] In step 3, based on a simplified two-dimensional mechanical model, the ADCB specimen is mechanically analyzed using classical laminate theory and Timoshenko beam theory to obtain the specimen's compliance C under load. eq and energy release rate G T (a eq ). Among them, C eq For the equivalent layer length a eq A function of the load P. C eq The expression is:
[0018]
[0019] Where, δ eq The specific expression for the displacement at the loading end derived from this simplified two-dimensional mechanical model is as follows:
[0020]
[0021] In the formula, d and c are the equivalent bending and shear compliance coefficients of the sublaminated plate, respectively; φ and w are the differences in rotation angle and longitudinal displacement of the crack tips of the upper and lower sublaminated plates derived from this simplified two-dimensional mechanical model, respectively; and subscripts 1 and 2 represent the upper and lower sublaminated plates, respectively. B is the actual width of the laminate, and P is the current test load. The specific expressions for φ and w are as follows:
[0022]
[0023]
[0024]
[0025]
[0026] In the formula, b is the equivalent coupling flexibility coefficient of the sublayer, where subscripts 1 and 2 represent the upper and lower sublayers, respectively. k z γ is the interfacial elastic constant. i η i (i = 1, 2, ..., 6) are the constant coefficients and characteristic roots derived from the reinforced beam theory, respectively. s The expression is: k s = (-d2H2+d1H1) / 2+(b2+b1) In step 3, G T (a eq The specific expression for ) is:
[0027]
[0028] In the formula, k x The interfacial elastic constant;
[0029] In step 3, the calculation process of the mechanical model is compiled into a Matlab program, and the calculation process is implemented using the program;
[0030] Furthermore, in step 3, the compliance C is specifically calculated. eq The process includes: (1) inputting the load displacement data of the ADCB laminate, the mechanical properties of the composite material single layer used, and the geometric information of the laminate into the Matlab program; (2) calculating the equivalent delamination length a corresponding to each pair of load displacement data using the compliance matching method based on the load displacement data P-δ. eq The specific expression for the flexibility matching method is as follows:
[0031]
[0032] Where C is the flexibility obtained from the experiment; (3) then the total energy release rate G corresponding to the current equivalent stratification length is obtained. T (a eq ), G I (a eq ) and G I / G T Among them, G I (a eq The calculation expression for ) is as follows:
[0033]
[0034] G I / G T The calculation formula is:
[0035]
[0036] In step 4, the global correction coefficient The calculation formula is:
[0037]
[0038] In the formula, a0 is the initial pre-existing crack length. eq,0 The initial equivalent crack length is obtained through step 3. eq,T The actual layer length a is obtained through step 3. T The equivalent layer length at that time;
[0039] In step 5, the specific expression for the global correction method is:
[0040]
[0041] In step 6, a eq -G T a eq -G I / G T Restore to aG T 、aG I / G T The reduction formula involving 'a' is:
[0042]
[0043] The advantages of this invention compared to the prior art are:
[0044] (1) Determining the fracture toughness curve and delamination mode mixing ratio of the ADCB laminate using the method of the present invention only requires recording the load-displacement curve and measuring a specific delamination length a during the test. T There is no need to measure the crack length throughout the entire process. This greatly reduces the complexity of the test and facilitates rapid testing;
[0045] (2) It avoids the use of finite element method, thus saving a lot of computational costs. The Matlab program can calculate the fracture toughness curve and the mixing ratio of the layering mode in a short time.
[0046] (3) The calculation results using the method of the present invention have been verified by experiments, and the obtained values are in good agreement with the experimental values, which shows that the calculation method of the present invention has good accuracy. Attached Figure Description
[0047] Figure 1 This is a flowchart illustrating the implementation of the present invention;
[0048] Figure 2These are load-displacement curves obtained from ADCB laminate delamination tests.
[0049] Figure 3 It is a two-dimensional ADCB mechanical model based on the reinforced beam theory;
[0050] Figure 4 It is ADCB laminate Ca eq Or C eq -a eq curve;
[0051] Figure 5 It is ADCB laminate G T (a eq )-a e curve.
[0052] Figure 6 It is ADCB laminate G I / G T -a e curve;
[0053] Figure 7 It is ADCB laminate G T -a curve;
[0054] Figure 8 It is ADCB laminate G I / G T -a curve.
[0055] Figure 9 This is a comparison chart of the global correction coefficients, the actual correction coefficients, and their linear fit. Detailed Implementation
[0056] The present invention will be further described in detail below with reference to the embodiments.
[0057] The specific implementation examples and steps are as follows:
[0058] Step 1: Use a glass fiber / epoxy resin composite multidirectional sheet, taking the layup sequence (0°2 / 90° / 0°3) / / [45° / (0°2 / 90°)3 / 0°2] as an example. The thicknesses of the upper and lower sub-laminates are 2mm and 4mm respectively. The sheet width is 25mm, the length is 140mm, and the pre-crack length is 25mm. The mechanical properties of the unidirectional tape are: E 11 =23.07 GPa, E 22 =8.63GPa,ν 12 =0.27,ν 13 =ν 23 =0.33,G 12 =3.94 GPa, G 13 =G 23 =2.84 GPa;
[0059] Step 2: Following ASTM standard D5528-13, conduct a static delamination test on the composite ADCB: Attach a paper scale to one side of the specimen, install it onto the MTS testing machine using a quick-release hinge clamp, and set the machine to record the load-displacement data during the test. Place the camera on one side of the scale. Begin the test and obtain the P-δ curve as shown below. Figure 2 As shown, the specific layer length a was measured. T =35.19mm;
[0060] Step 3: Establish a two-dimensional ADCB mechanical model based on the reinforced beam theory, such as... Figure 3 As shown;
[0061] Based on a simplified two-dimensional mechanical model, the ADCB specimen was mechanically analyzed using classical laminate theory and Timoshenko beam theory, and the compliance C of the specimen under load was obtained. eq and energy release rate G T (a eq The expressions are equivalent layer lengths a. eq and the load P as a function, where C eq The expression is:
[0062]
[0063] Where, δ eq The specific expression for the displacement at the loading end derived from this simplified two-dimensional mechanical model is as follows:
[0064]
[0065] In the formula, d and c are the equivalent bending and shear compliance coefficients of the sublaminated plate, respectively; φ and w are the differences in rotation angle and longitudinal displacement of the crack tips of the upper and lower sublaminated plates derived from this simplified two-dimensional mechanical model, respectively; and subscripts 1 and 2 represent the upper and lower sublaminated plates, respectively. B is the actual width of the laminate, and P is the current test load. The specific expressions for φ and w are as follows:
[0066]
[0067]
[0068]
[0069]
[0070] In the formula, b is the equivalent coupling flexibility coefficient of the sublayer, where subscripts 1 and 2 represent the upper and lower sublayers, respectively. k z γ is the interfacial elastic constant. i η i (i = 1, 2, ..., 6) are the constant coefficients and characteristic roots derived from the reinforced beam theory, respectively. s The expression is:
[0071] k s = (-d2H2+d1H1) / 2+(b2+b1)
[0072] The results were compiled into a Matlab program;
[0073] Input the load displacement P-δ data, material elastic modulus, Poisson's ratio, sample ply, thickness, width and single-layer thickness information obtained from the experiment into the program;
[0074] The program is run iteratively to calculate the equivalent crack length 'a' corresponding to each pair of P-δ using the compliance matching method. eq and energy release rate G T (a eq ), G I (a eq ), where G T (a eq The specific expression for ) is:
[0075]
[0076] In the formula, k x Let G be the interfacial elastic constant. I (a eq The calculation expression for ) is as follows:
[0077]
[0078] The specific expression for the flexibility matching method is as follows:
[0079]
[0080] Where C is the compliance obtained from the experiment, Ca is obtained. eq Or C eq -a eq As shown in the picture Figure 4 As shown, G is obtained. T (a eq )-a eq like Figure 5 As shown;
[0081] Calculate the mixing ratio of the stratified modes, where the proportion of type I is G. I / G T With aeq The size of the one-to-one correspondence is G I (a eq ) / G T (a eq ), to obtain G I / G T -a eq As shown in the picture Figure 6 As shown;
[0082] Step 4: Place a T The equivalent crack length a corresponding to step 3 eq The global correction coefficient is obtained. The calculation formula is:
[0083]
[0084] Step 5: Obtain the result related to a through a global correction method. eq One-to-one correspondence G T G T The calculation formula is as follows:
[0085]
[0086] In the formula, G T (a eq The result obtained in step 3 is ) The global correction coefficients calculated in step 4;
[0087] Step 6: By comparing with the equivalent crack length a eq One-to-one correspondence G T and G I / G T Restored to G corresponding one-to-one with the actual layer length a T and G I / G T The specific formula is as follows:
[0088]
[0089] The fracture toughness curve of the ADCB laminate as a function of delamination length is obtained as follows: Figure 7 As shown, the experimental results were calculated using modified elastic beam theory. The layering pattern of the ADCB laminate, varying with layer length, was obtained, for example... Figure 8 As shown, the calculation results agree well with the experimental or finite element results, verifying the applicability of the fracture toughness curve and delamination mode mixing ratio determination method of the composite material ADCB laminate proposed in this invention.
[0090] Furthermore, to illustrate the effectiveness of the global correction method of the present invention in step 4, the actual correction coefficients representing the crack propagation process were also calculated. The actual correction factor changes with each step of crack propagation, and its calculation formula is as follows:
[0091]
[0092] The actual correction coefficient requires measuring the entire crack process. In this specific embodiment, only the global correction coefficient used in this invention is listed to demonstrate its effectiveness and efficiency. The relationship between the global correction coefficient, the actual correction coefficient, and their linear fit with 'a' can be obtained as shown in the figure below. Figure 9 As shown, the linear fit between the global correction coefficient and the actual correction coefficient is good. The parts of this invention not described in detail are well-known techniques to those skilled in the art.
[0093] The above description is only a part of the specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the protection scope of the present invention.
Claims
1. A method for determining the fracture toughness curve and delamination mode mixing ratio of a composite asymmetric laminate, characterized in that... Includes the following steps: Step 1: Design and manufacture fiber-reinforced composite laminate samples with different thicknesses of upper and lower sub-laminated plates but arbitrary layup. Step 2: Using a double cantilever beam testing apparatus, conduct an ADCB delamination test on the above specimens by applying tensile load, and record the test load, displacement, and specific delamination length 'a'. T ; In step 2, a T The delamination length is the length corresponding to the moment when the fracture process zone of the laminate is fully developed and begins to self-similarly propagate. Step 3: Establish a two-dimensional ADCB mechanical model based on the reinforced beam theory, and calculate the theoretical compliance C. eq Compare it with the test flexibility C exp The equivalent crack length 'a' is obtained by matching and iterative calculation using the program. eq The equivalent crack length a eq Substituting into the calculation formula based on the reinforced beam theory, we obtain G. T (a eq ) and the mixing ratio G of the stratified whole-process mode I / G T ; In step 3, the hybrid stratification problem of the ADCB test will be simplified into a two-dimensional mechanical model based on the reinforced beam theory. In step 3, based on a simplified two-dimensional mechanical model, the ADCB specimen is mechanically analyzed using classical laminate theory and Timoshenko beam theory to obtain the specimen's compliance C under load. eq and energy release rate G T (a eq ); where C eq For the equivalent layer length a eq A function of load P; In step 3, the calculation process of the mechanical model is compiled into a Matlab program, and the calculation process is implemented using the program. In step 3, the compliance C is specifically calculated. eq The process includes: (1) inputting the load displacement data of the ADCB laminate, the mechanical properties of the composite material single layer used, and the geometric information of the laminate into the Matlab program; (2) calculating the equivalent delamination length a corresponding to each pair of load displacement data using the compliance matching method based on the load displacement data P-δ. eq (3) Then, the total energy release rate G corresponding to the current equivalent stratification length is obtained. T (a eq ), G I (a eq ) and G I / G T ; In step 3, the compliance C is calculated. eq The process involves δ eq The displacement at the loading end, derived from this simplified two-dimensional mechanical model, is expressed in the following specific expression: In the formula, d and c are the equivalent bending and shear compliance coefficients of the sublaminated plate, respectively; ϕ and w are the differences in rotation angle and longitudinal displacement of the crack tip between the upper and lower sublaminated plates derived from this simplified two-dimensional mechanical model, respectively; subscripts 1 and 2 represent the upper and lower sublaminated plates, respectively; B is the actual width of the laminate; and P is the current test load. The specific expressions for ϕ and w are as follows: In the formula, b is the equivalent coupling compliance coefficient of the sublayer, where subscripts 1 and 2 represent the upper and lower sublayers, respectively; H1 and H2 are the thicknesses of the upper and lower sublayers, respectively; k z γ is the transverse elastic constant of the interface; i η i (i = 1, 2, ..., 6) are the constant coefficients and characteristic roots derived from the reinforced beam theory, respectively; k s The expression is: In step 3, G T (a eq The specific expression for ) is: In the formula, k x G is the longitudinal elastic constant of the interface; in step 3, G I (a eq The calculation expression for ) is as follows: Step 4, by measuring the specific layer length a T Combined with the equivalent crack length a in step 3 eq Obtain the global correction coefficient ; In step 4, the global correction coefficient The calculation formula is: In the formula, a0 is the initial pre-existing crack length, a eq,0 Let a be the initial equivalent crack length. eq,T The actual layer length a is obtained through step 3. T Equivalent layer length at time; Step 5, obtain the result with a through a global correction method. eq One-to-one correspondence G T ; In step 5, the specific expression for the global correction method is: Step 6, by comparing with the equivalent crack length a eq One-to-one correspondence G T and G I / G T Restored to G corresponding one-to-one with the actual layer length a T and G I / G T Thus, the fracture toughness curves of the ADCB laminate I / II hybrid type and the mixing ratio of the delamination mode were obtained; In step 6, a eq -G T a eq - G I / G T Restore to aG T a-G I / G T The reduction formula involving 'a' is: 。
Citation Information
Patent Citations
Hybrid interlayer crack propagation analysis method for composite laminated plate
CN111062117A
Prediction method for I / II mixed fracture response surface of composite material
CN114896763A