A radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy and a preparation method thereof
Through high-energy ball milling and rapid hot-pressing sintering technology, a W-Ta-Cr-V series multi-component alloy with high-density coherent and ordered nano-precipitated phases was prepared, which solved the problem of insufficient radiation resistance of nuclear materials under irradiation. problem, achieving low activation and refractory alloy materials suitable for advanced nuclear reactors.
Patent Information
- Application Number
- CN202410161426.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-02-05
AI Technical Summary
Existing nuclear materials show severe mechanical property deterioration, volume swelling and other problems under irradiation, and low activation requirements are difficult to achieve. Especially under the influence of high-energy neutron irradiation and helium ions in fusion reactors, the radiation resistance of materials Performance is insufficient.
The W-Ta-Cr-V series multi-component alloy raw material powders are mixed using high-energy ball milling and rapidly hot-pressed, sintered and heat-treated to prepare a block with a BCC disordered solid solution matrix and a high-density coherent ordered nanoprecipitate phase. alloy to improve its radiation resistance.
A low-activation, refractory W-Ta-Cr-V series multi-component alloy has been realized, which significantly reduces radiation hardening and helium bubble size, improves the radiation resistance of the material, and is suitable for advanced nuclear reactors and plasma materials. Surface radiation resistant coating.
Smart Images

Figure CN117947326B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a radiation-resistant, low-activation, refractory W-Ta-Cr-V series multi-component alloy and a preparation method thereof. Background Art
[0002] With the development of advanced nuclear reactor technology, the irradiation dose of nuclear materials is increasing. After the deuterium-tritium nuclear fusion reaction in the fusion reactor, in addition to the high-energy neutron irradiation produced by the reaction, 3.5MeV high-energy He ions can also be produced. The energy of the reaction products is much higher than that of the fission reactor nuclear reaction products, and the materials will be affected by gas atoms such as helium, hydrogen and their isotopes. The corresponding radiation damage of nuclear energy materials is also more severe. The adverse effects of irradiation on materials are mainly manifested in irradiation dislocations, holes, helium bubbles, irradiation hardening and embrittlement. In severe cases, it will cause serious deterioration of the mechanical properties of the materials, volume swelling, etc., threatening the safe operation of the reactor. Therefore, in the development of advanced nuclear reactors, one of the important issues that must be solved first is materials, and the radiation resistance of materials must be effectively improved. At the same time, in order to avoid the generation of highly radioactive products after reaction with neutrons, the materials also have low activation requirements.
[0003] In recent years, due to lattice distortion effects and hysteresis diffusion, multi-component alloys have shown unique advantages in radiation resistance. Due to the slow diffusion of atoms, the increase in the composition complexity of single-phase concentrated solid solution alloys will significantly inhibit the level of radiation-induced segregation [C Lu, T Yang, K Jin, et al. Acta Materialia. 2017, 127: 98-107.]. In addition, lattice distortion and high-density vacancies in high-entropy alloys can increase the nucleation points of helium bubbles, avoiding the preferential nucleation growth of helium bubbles at grain boundaries, thereby reducing grain boundary brittleness [Y Lu, H Huang, X Gao, et al. Journal of Materials Science & Technology. 2019, 35 (3): 369-373.].
[0004] As one of the metals with the highest melting point, tungsten has the advantages of low physical sputtering rate, low tritium retention, and low swelling after irradiation, and is an important candidate material in nuclear reactors. However, pure tungsten has some disadvantages, such as low recrystallization temperature, easy formation of volatile oxides under accident conditions, and insufficient high-temperature strength. Adding low-activation alloying elements to tungsten to form a concentrated solid solution alloy can effectively improve the shortcomings of pure tungsten and significantly improve the radiation resistance without increasing the induced radioactivity. The W-Ta-Cr-V alloy film prepared by magnetron sputtering has good radiation resistance, and no irradiation dislocation loops are observed even when the irradiation dose reaches 8dpa [O El-Atwani, N Li, M Li, et al. Science Advances. 2019, 5(3): v2002.]. However, the research on low-activation tungsten-containing multi-component alloys is still in its early stages, and most studies use costly film preparation methods such as magnetron sputtering, which makes it difficult to prepare bulk alloys. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] One of the objects of the present invention is to provide a radiation resistant, low-activation, refractory W-Ta-Cr-V multi-component alloy, the atomic percentages of which are W 13-16%, Ta 13-16%, Cr 30-35%, and V 33-38%.
[0008] To solve the above technical problems, the present invention provides the following technical solutions: a radiation-resistant, low-activation, refractory W-Ta-Cr-V multi-component alloy, comprising: mixing raw material powders uniformly and preliminarily alloying them by a high-energy ball milling method, and then preparing a bulk alloy material with target structure and performance by rapid hot pressing (FHP) and heat treatment at an appropriate temperature.
[0009] As a preferred embodiment of the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, the alloy has the following characteristics:
[0010] (a) The alloy is based on a BCC disordered solid solution with dispersed high-density coherent ordered nano-precipitates, wherein the area fraction of the nano-precipitates is greater than 20% and the thickness of the precipitate layer is less than 80 nm;
[0011] (b) At room temperature, the irradiation dose of 400keV helium ions is 2×10 17 ions / cm 2 , the average helium bubble size in the alloy is less than 1 nm, and the radiation hardening is not higher than 20%;
[0012] (c) 450°C, 400keV helium ion irradiation dose 2×10 17 ions / cm 2 The average helium bubble size in the alloy is less than 1.5 nm, and the radiation hardening is not higher than 30%.
[0013] Another object of the present invention is to provide a method for preparing a radiation-resistant, low-activation, refractory W-Ta-Cr-V multi-component alloy, comprising the steps of preparing raw material powders according to the atomic percentage of the alloy, performing high-energy ball milling under inert gas protection conditions, sieving the powders, sintering in a mold, and heat treating to obtain the alloy.
[0014] As a preferred solution of the preparation method of the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, wherein: high-energy ball milling uses cemented carbide balls and cemented carbide tanks, the ball milling speed is 200-300rpm under argon protection, and the total ball milling time is 2000-3000min.
[0015] As a preferred solution of the method for preparing the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, the mass ratio of the cemented carbide ball to the total powder of each component of the alloy is 5:1 to 10:1.
[0016] As a preferred solution of the method for preparing the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, the vacuum degree during sintering is 30-40 Pa, and the heating rate is 50-150°C / min.
[0017] As a preferred solution of the method for preparing the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, the sintering temperature is 1400-1700°C and the holding time is 5-30 minutes.
[0018] As a preferred solution of the method for preparing the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy of the present invention, wherein: after heat treatment at 1100-1300°C for 30-90 minutes, air cooling or water cooling quenching is performed.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The W-Ta-Cr-V multi-component alloy of the present invention uses all low-activation elements, has less transmutation activation products, and has low-activation characteristics. After serving in a nuclear reactor, the induced radioactivity is greatly reduced.
[0021] (2) The W-Ta-Cr-V multi-component alloy of the present invention is based on a BCC disordered solid solution, has a high-density coherent ordered nano-precipitate phase, a large degree of lattice distortion, and a diffusion hysteresis, and exhibits excellent resistance to helium ion irradiation compared to pure tungsten. After room temperature and high temperature helium ion irradiation, the radiation hardening of pure W is 49.2% and 54.9%, respectively, while the radiation hardening of the W-Ta-Cr-V multi-component alloy of the present invention is only 13.1% and 16.1%.
[0022] (3) Aiming at the high requirements of advanced nuclear energy systems for the radiation resistance of materials, the present invention has developed a radiation-resistant, low-activation, refractory W-Ta-Cr-V multi-component alloy by selecting low-activation elements and combining powder metallurgy methods. The alloy has complex composition, high lattice distortion, and contains a high-density coherent ordered nano-precipitation phase structure. After high-energy helium ion irradiation, it exhibits better radiation resistance than pure W materials, and is expected to be used in advanced nuclear reactor radiation-resistant materials or surface radiation-resistant coatings for plasma-facing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0024] Figure 1 This is an electron microscope image of the backscattered morphology of the alloy material of Example 1 of the present invention after rapid hot pressing and sintering.
[0025] Figure 2 These are backscattered electron microscope images of the alloy material of Example 1 of the present invention after heat treatment at 1000, 1100, and 1200° C. for 1 hour.
[0026] Figure 3 This is the XRD spectrum of the bulk material of Example 1 of the present invention.
[0027] Figure 4 It is the transmission electron microscope HAADF-STEM morphology image and selected area electron diffraction image of the alloy material in Example 1 of the present invention.
[0028] Figure 5 This is an element distribution diagram of the coherent ordered nano-precipitates and the matrix in the alloy of Example 1 of the present invention.
[0029] Figure 6 This is a helium bubble morphology image of the alloy material of Example 1 of the present invention after room temperature helium ion irradiation.
[0030] Figure 7This is a helium bubble morphology diagram of the alloy material of Example 1 of the present invention after helium ion irradiation at 450°C.
[0031] Figure 8 This is a comparison chart of hardness-indentation depth of the block material before and after irradiation in Example 1 of the present invention.
[0032] Fig. 9 This is an electron microscope image of the backscattered morphology of the alloy material of Example 2 of the present invention after rapid hot pressing and sintering.
[0033] Fig.10 These are backscattered electron microscope images of the alloy material of Example 2 of the present invention after heat treatment at 1000, 1100, and 1200° C. for 1 hour.
[0034] Fig.11 This is the XRD spectrum of the bulk material of Example 2 of the present invention.
[0035] Fig.12 This is a helium bubble morphology diagram of pure W in comparative example 1 of the present invention after helium ion irradiation at 450°C.
[0036] Fig.13 This is a comparison chart of hardness-indentation depth of pure W before and after irradiation in comparative example 1 of the present invention.
[0037] Fig.14 is W of Comparative Example 2 of the present invention 25 Ta 25 Cr 25 V 25 XRD patterns of sintered alloys.
[0038] Fig.15 is W of Comparative Example 2 of the present invention 25 Ta 25 Cr 25 V 25 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0039] Fig.16 is W of Comparative Example 2 of the present invention 25 Ta 25 Cr 25 V 25 Element distribution diagram of sintered alloy.
[0040] Fig.17 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr 15 V 15 XRD patterns of sintered alloys.
[0041] Fig.18 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr15 V 15 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0042] Fig.19 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr 15 V 15 Element distribution diagram of sintered alloy.
[0043] Fig. 20 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr 15 V 15 XRD patterns of sintered alloys.
[0044] Fig.21 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr 15 V 15 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0045] Fig. 22 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr 15 V 15 Element distribution diagram of sintered alloy. DETAILED DESCRIPTION
[0046] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0047] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0048] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0049] Unless otherwise specified, the raw materials used in the examples were purchased commercially.
[0050] The W-Ta-Cr-V alloy provided by the present invention can be prepared by the following steps:
[0051] 1) Raw material powder weighing ratio and canning
[0052] Take W, Ta(-H), Cr, V powders with a purity higher than 99.9% and particles smaller than 200 mesh as raw materials, and weigh them according to the atomic percentage ratio in air or under argon protection. Put the above powders into a cemented carbide ball mill, and put cemented carbide balls in a ball-to-material ratio of 5:1 to 10:1, where the total volume of the powder raw materials and cemented carbide balls must be less than three-quarters of the volume of the ball mill. Seal the ball mill under argon protection to ensure that the subsequent powder will not oxidize during the ball milling process.
[0053] 2) High energy ball milling
[0054] Install the ball milling jar on the ball mill according to the equipment requirements, and first ball mill at 100rpm for about 100 minutes to make the powder preliminarily mixed and even. Then set the ball milling time to 2000-3000 minutes and the ball milling speed to 200-300rpm (to reduce the ball milling temperature rise, the machine can be stopped for 5-10 minutes for cooling every 20-30 minutes of ball milling).
[0055] 3) Powder screening, storage and filling mold
[0056] Open the ball mill under argon protection, grind the powder after ball milling, and pass it through a 200-mesh standard sample sieve. Take a small amount of powder and place it in the air to observe whether the powder will spontaneously ignite or release a lot of heat to ensure the safety of the powder. The powder is molded or vacuum packed / stored in inert gas for later use.
[0057] 4) Sintering and heat treatment
[0058] The pre-alloyed powder after ball milling and screening is loaded into a graphite mold protected and lubricated by graphite paper, pre-pressed at 40MPa, and the symmetry of the upper and lower graphite pressure heads is adjusted. Through DC non-pulse rapid hot pressing (FHP) under vacuum (vacuum degree better than 40Pa), the powder is sintered into a dense bulk alloy material in a low-energy manner. The heating rate is 100℃ / min, the sintering temperature is 1400~1700℃, the holding time is 5~30min, and the pressure is maintained at 30~50MPa during sintering. After sintering, the temperature is lowered to below 400℃ with the furnace, and then the furnace door is opened to demould and take out the alloy sample.
[0059] Heat treatment method: Cut the sample into appropriate size, polish the oxide skin and seal the quartz tube in vacuum. Put it into the muffle furnace and heat it up with the furnace or put it in after reaching the target temperature. After keeping the target temperature for 1 hour, take out the quartz tube, smash it and quench it with water. In the actual production process, atmosphere protection, sheathing, anti-oxidation coating and other methods can be used to avoid oxidation during the heat treatment of materials.
[0060] 5) Helium ion irradiation
[0061] The samples were polished until the surface was stress-free and then irradiated with high-energy helium ions at room temperature or 450°C. The specific irradiation parameters were: irradiation voltage 400 keV, irradiation dose 2×10 17 ions / cm 2 .
[0062] The change of material hardness with depth before and after irradiation was characterized by the continuous stiffness method in nanoindentation, using a Berkovich indenter, a sample Poisson’s ratio of 0.26, a target load of 1000 mN, a target depth of 1000 nm, and a frequency of 110 Hz.
[0063] Example 1
[0064] According to the chemical formula W 15 Ta 15 Cr 35 V 35 (atomic percentage) for mixing, high-energy ball milling at 200-300rpm for 2000min. The powder is loaded into a graphite mold, pre-pressed at 40MPa and then rapidly hot-pressed for sintering. The heating rate is 100℃ / min, the pressure is 50MPa, the sintering temperature is 1600℃, and the temperature is cooled with the furnace after keeping warm for 10min. The sintered block material is cut into appropriate sizes, the oxide scale is polished, and then heat treated at 1000, 1100, and 1200℃ for 1 hour respectively, and then water-cooled and quenched. At this point, W 15 Ta 15 Cr 35 V 35 The alloy preparation is completed.
[0065] Figure 1 This is a backscattered electron microscope image of the alloy material after rapid hot pressing sintering in Example 1. After sintering, submicron oxide particles are dispersed in the alloy grains, but there is no obvious precipitation in the matrix.
[0066] Figure 2 This is a backscattered electron microscope image of the alloy material of Example 1 after heat treatment at 1000-1200°C. After heat treatment at 1000-1200°C, as the heat treatment temperature increases, the number of coherent ordered nano-precipitates increases gradually, and the size also increases gradually, wherein 1200°C is a more suitable heat treatment temperature.
[0067] Figure 3 This is the XRD spectrum of the bulk material of Example 1 of the present invention. It can be seen that the sintered alloy is mainly composed of BCC matrix, with a small amount of oxides and C-rich second phase. After heat treatment at 1200°C, the content of the second phase increases slightly.
[0068] Figure 4The transmission electron microscope HAADF-STEM morphology image and selected area electron diffraction image of the alloy material of Example 1 of the present invention are shown in FIG. It can be seen that a high-density bamboo leaf-like nano-second phase is distributed in the alloy matrix, and the second phase is a three-fold periodic ordered structure.
[0069] Figure 5 This is the element distribution diagram of the coherent ordered nano-precipitates and the matrix in the alloy of Example 1. The coherent ordered nano-precipitates have an area percentage of 27.43%, an average width of 9.3 nm, and an average length of 106.0 nm. They are mainly enriched in Ta and C elements, wherein the C element mainly comes from the ball milling medium (WC-Co) and the carbon paper in contact during sintering.
[0070] Figure 6 This is a morphology of helium bubbles after room temperature helium ion irradiation of the alloy material of Example 1. a, b, and c are images taken in the focused, underfocused, and overfocused states, respectively. The helium bubbles appear as white particles when underfocused and as black particles when overfocused. There are relatively few helium bubbles in the second phase and at the interface.
[0071] Figure 7 This is a morphology of helium bubbles after 450°C helium ion irradiation of the alloy material of Example 1. After room temperature and 450°C helium ion irradiation, there are relatively few helium bubbles in the coherent ordered nano-precipitated phase, no helium bubble enrichment at the phase interface, and the average helium bubble size in the matrix is 0.86nm and 1.18nm, respectively.
[0072] Figure 8 This is a comparison chart of hardness and indentation depth before and after irradiation of the block material of Example 1. After room temperature helium ion irradiation, the alloy radiation hardening is 13.1%, and after 450°C helium ion irradiation, the alloy radiation hardening is 16.1%.
[0073] Example 2
[0074] According to the chemical formula W 15 Ta 15 Cr 35 V 35 (atomic percentage) for batching, high-energy ball milling at 200-300rpm for 2000min. The powder is loaded into a graphite mold, pre-pressed at 40MPa and then rapidly hot-pressed for sintering. The heating rate is 100℃ / min, the pressure is 50MPa, the sintering temperature is 1500℃, and the temperature is cooled with the furnace after keeping warm for 10min. The sintered block material is cut into appropriate sizes, the oxide scale is polished, and then heat-treated at 1000, 1100, and 1200℃ for 1 hour respectively, and then water-quenched. At this point, W 15 Ta 15 Cr 35 V 35 The alloy preparation is completed.
[0075] Fig. 9This is a backscattered electron microscope image of the alloy material after rapid hot pressing sintering of Example 2. After sintering, the alloy is a multiphase heterogeneous structure with dispersed oxide particles and no obvious precipitation in the matrix.
[0076] Fig.10 This is a backscattered electron microscope image of the alloy material of Example 2 after heat treatment at 1000-1200°C. After heat treatment at 1000-1200°C, as the heat treatment temperature increases, the number of coherent ordered nano-precipitates increases gradually, and the size also increases gradually, wherein 1200°C is a more suitable heat treatment temperature.
[0077] Fig.11 This is the XRD pattern of the bulk material of Example 2.
[0078] Comparative Example 1
[0079] A commercially purchased pure W plate was heat treated at 1300° C. for 1 hour and then irradiated with helium ions under the same irradiation conditions as in Example 1.
[0080] Fig.12 This is a morphology of helium bubbles in pure W after helium ion irradiation at 450°C in comparative example 1. The results show that after helium ion irradiation at 450°C, the average helium bubble size of pure W is 1.27nm, which is larger than that of WTaCrV alloy.
[0081] Fig.13 This is a comparison of the hardness and indentation depth of pure W before and after irradiation in Example 1. The room temperature and 450°C irradiation hardening are 49.2% and 54.9% respectively, which are much higher than the irradiation hardening of the WTaCrV alloy in Example 1.
[0082] Comparative Example 2
[0083] According to the chemical formula W 25 Ta 25 Cr 25 V 25 (atomic percentage) for batching, high-energy ball milling at 200-300rpm for 2000min. The powder is loaded into a graphite mold, pre-pressed at 40MPa and then rapidly hot-pressed for sintering. The heating rate is 100℃ / min, the pressure is 50MPa, the sintering temperature is 1500℃, and the temperature is cooled with the furnace after keeping warm for 10min. The sintered block material is cut into appropriate sizes, the oxide scale is polished, and then water-quenched after heat treatment at 1200℃ for 1 hour. At this point, W 25 Ta 25 Cr 25 V 25 The alloy preparation is completed.
[0084] Fig.14 is W of Comparative Example 2 25 Ta 25 Cr 25 V25 XRD patterns of sintered alloys.
[0085] Fig.15 is W of Comparative Example 2 25 Ta 25 Cr 25 V 25 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0086] Fig.16 is W of Comparative Example 2 25 Ta 25 Cr 25 V 25 Element distribution diagram of sintered alloy.
[0087] After sintering, the alloy is a multiphase heterogeneous structure, mainly BCC matrix, with intermetallic compound phase and a small amount of oxide. The matrix is rich in W and Ta elements, with a size of about 2μm, and a Cr-V-rich second phase with a size of 10-40μm is distributed in the alloy. After heat treatment at 1200℃, cracks appeared in the alloy due to thermal stress, but the cracks were repaired by precipitation of low-melting point elements, and the matrix grains gradually transformed into equiaxed shapes, and no nano-second phase precipitation was observed. Example 1 alloy micro-Vickers hardness 797±19HV, W 25 Ta 25 Cr 25 V 25 Alloy hardness 1005±19HV.
[0088] Comparative Example 3
[0089] According to the chemical formula W 35 Ta 35 Cr 15 V 15 (atomic percentage) for batching, high-energy ball milling at 200-300rpm for 2000min. The powder is loaded into a graphite mold, pre-pressed at 40MPa and then rapidly hot-pressed for sintering. The heating rate is 100℃ / min, the pressure is 50MPa, the sintering temperature is 1500℃, and the temperature is cooled with the furnace after keeping warm for 10min. The sintered block material is cut into appropriate sizes, the oxide scale is polished, and then water-quenched after heat treatment at 1200℃ for 1 hour. At this point, W 35 Ta 35 Cr 15 V 15 The alloy preparation is completed.
[0090] Fig.17 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr 15 V 15 XRD patterns of sintered alloys.
[0091] Fig.18 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr 15 V 15 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0092] Fig.19 is W of Comparative Example 3 of the present invention 35 Ta 35 Cr 15 V 15 Element distribution diagram of sintered alloy.
[0093] After sintering, the alloy is mainly composed of BCC matrix, with a small amount of intermetallic compound phase and oxide. The matrix is rich in W and Ta elements, with a size of about 5μm, and a Cr-V-rich second phase with a size of 10 to 40μm is distributed in the alloy. After heat treatment at 1200℃, there is no obvious change in the alloy structure, and no nano-second phase precipitation is observed. Example 1 alloy micro-Vickers hardness 797±19HV, W 35 Ta 35 Cr 15 V 15 Alloy hardness 834±13HV.
[0094] Comparative Example 4
[0095] According to the chemical formula W 60 Ta 10 Cr 15 V 15 (atomic percentage) for batching, high-energy ball milling at 200-300rpm for 2000min. The powder is loaded into a graphite mold, pre-pressed at 40MPa and then rapidly hot-pressed for sintering. The heating rate is 100℃ / min, the pressure is 50MPa, the sintering temperature is 1500℃, and the temperature is cooled with the furnace after keeping warm for 10min. The sintered block material is cut into appropriate sizes, the oxide scale is polished, and then water-quenched after heat treatment at 1200℃ for 1 hour. At this point, W 60 Ta 10 Cr 15 V 15 The alloy preparation is completed.
[0096] Fig. 20 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr 15 V 15 XRD patterns of sintered alloys.
[0097] Fig.21 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr15 V 15 Backscattered electron microscopy images of the alloy in the sintered state and the 1200℃ heat-treated state.
[0098] Fig. 22 is W of Comparative Example 4 of the present invention 60 Ta 10 Cr 15 V 15 Element distribution diagram of sintered alloy.
[0099] After sintering, the alloy XRD image only shows BCC phase. The results of scanning electron microscopy show that nano and submicron second phases are dispersed at the grain boundaries. EDS results show that the matrix is rich in W and Ta elements, with a size of about 3μm, and nano and submicron Ta-VO enriched second phases are distributed in the alloy. After heat treatment at 1200℃, there is no obvious change in the alloy structure, and no nano second phase precipitation is observed. Example 1 alloy micro Vickers hardness 797±19HV, W 60 Ta 10 Cr 15 V 15 Alloy hardness 903±10HV.
[0100] It can be seen from the examples and comparative examples that W prepared by powder metallurgy and subjected to appropriate heat treatment 15 Ta 15 Cr 35 V 35 The alloy has a high-density coherent ordered nano-precipitated phase structure. Combined with the hysteretic diffusion and severe lattice distortion in high entropy alloys, this type of alloy has excellent radiation resistance. Under the same irradiation conditions, the helium bubble size is smaller than that of pure tungsten, and the degree of radiation hardening is much less than that of pure tungsten. Therefore, through the alloy component system and preparation method provided by the present invention, a low-activation, radiation-resistant refractory alloy material can be obtained, which has excellent radiation-resistant service potential and provides a new material choice for the development of advanced nuclear reactors.
[0101] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a radiation-resistant, low-activation, refractory W-Ta-Cr-V multi-component alloy, characterized in that: The alloy raw material powder includes W 13-16%, Ta 13-16%, Cr 30-35%, and V 33-38% by atomic percentage. The raw material powder is weighed and put into a cemented carbide ball with a ball-to-material ratio of 5:1-10:1, and the ball mill is sealed; High-energy ball milling is performed under vacuum or inert gas protection conditions, powder is screened, molded and sintered, and heat-treated to obtain an alloy; the heat treatment temperature is 1200° C.; Wherein, the prepared alloy is any one of (a) to (c): (a) The alloy is based on a BCC disordered solid solution and dispersed with a high-density coherent ordered nano-precipitate phase, wherein the area percentage of the nano-precipitate phase is greater than 20% and the thickness of the precipitate phase layer is less than 80 nm; (b) At room temperature, 400 keV helium ion irradiation dose 2×10 17 ions / cm 2 , the average helium bubble size in the alloy is less than 1 nm, and the radiation hardening is not higher than 20%; (c) 450°C, 400 keV helium ion irradiation dose 2×10 17 ions / cm 2 , the average helium bubble size in the alloy is less than 1.5 nm, and the radiation hardening is not higher than 30%.
2. The method for preparing the radiation-resistant low-activation refractory W-Ta-Cr-V multi-component alloy according to claim 1, characterized in that: The alloy raw material powder is subjected to high-energy ball milling under inert gas protection conditions, using cemented carbide balls and cemented carbide lined containers, with a ball milling speed of 200-300 rpm and a total ball milling time of 2000-3000 min.
3. The method for preparing the radiation resistant low activation refractory W-Ta-Cr-V multi-component alloy according to claim 1, characterized in that: During the sintering, the initial vacuum degree in the furnace is less than 40 MPa, and the heating rate is 50-150 °C / min.
4. The method for preparing the radiation resistant low activation refractory W-Ta-Cr-V multi-component alloy according to claim 1 or 3, characterized in that: The sintering temperature is 1400-1700°C, the holding time is 5-30 min, and the holding pressure is 30-50 MPa during sintering.
5. The method for preparing the radiation resistant low activation refractory W-Ta-Cr-V multi-component alloy according to claim 1, characterized in that: The sintering is performed at a sintering temperature of 1600° C., a holding time of 10 min, and a sintering pressure of 50 MPa.
6. The method for preparing the radiation resistant low activation refractory W-Ta-Cr-V multi-component alloy according to claim 1, characterized in that: After heat treatment at 1100-1300 °C for 30-90 min, air cooling or water cooling quenching is carried out.
7. The method for preparing the radiation resistant low activation refractory W-Ta-Cr-V multi-component alloy according to claim 6, characterized in that: After heat treatment at 1200 °C for 60 min, water cooling was performed.
Citation Information
Patent Citations
Oxide dispersion strengthened (ODS) high-entropy alloy and preparation method thereof
CN106435323A
Powder metallurgy refractory multi-principal-element high-entropy alloy and preparation method thereof
CN113549780A
Alloy and nuclear reactor component with alloy coating on surface
CN114774757A
High strength tungsten alloy with low activation and manufacturing method for the same
KR1020160126702A
KR20220039485A